Lithium secondary battery anode having improved electrochemical characteristics by dry process and electrode additive content adjustment, method for manufacturing same, and lithium secondary battery comprising same

The controlled dry process and additive content in lithium secondary batteries, using PTFE and PVP, address lithium loss and SEI instability, enhancing electrochemical properties and stability.

WO2024232460A1PCT designated stage expired Publication Date: 2024-11-14KOREA INST OF CERAMIC ENG & TECH

Patent Information

Application Number
PCT/KR2023/006488
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-11
Filing Date
2023-05-12
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional lithium secondary batteries face issues with lithium loss and unstable solid electrolyte interface (SEI) due to side reactions of polytetrafluoroethylene (PTFE) dry binders during the lithiation process, leading to low initial coulombic efficiency and electrode deterioration.

Method used

A dry process is employed to mix negative electrode active materials, conductive materials, and polyvinylpyrrolidone (PVP) as an electrode additive in a strictly controlled content ratio with PTFE, minimizing side reactions and forming a stable SEI, thereby improving electrochemical properties.

Benefits of technology

The approach enhances initial coulombic efficiency and lifetime stability by suppressing PTFE side reactions, resulting in improved electrochemical performance and reduced lithium loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023006488_14112024_PF_FP_ABST
    Figure KR2023006488_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a lithium secondary battery anode having improved electrochemical characteristics by a dry process and the electrode additive content adjustment, a method for manufacturing same, and a lithium secondary battery comprising same, wherein the anode is formed by adding electrode additives to an anode active material, a conductive material, and a dry binder at a strictly limited content ratio and then mixing same through a dry process, so that side reactions of the dry binder PTFE is suppressed, resulting in the minimization in lithium loss and leading to the formation of a stable solid electrolyte interface (SEI), which can improve electrochemical characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

A negative electrode for a lithium secondary battery with improved electrochemical properties by controlling the content of dry process and electrode additives, a method for manufacturing the same, and a lithium secondary battery including the same

[0001] The present invention relates to an anode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control, a method for manufacturing the same, and a lithium secondary battery including the same, and more particularly, to an anode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control, in which an electrode additive is added to an anode active material, a conductive material, and a dry binder at a strictly limited content ratio and mixed through a dry process to form an anode, thereby suppressing side reactions of PTFE, which is a dry binder, minimizing lithium loss and improving electrochemical characteristics through the formation of a stable SEI (Solid electrolyte interface), a method for manufacturing the same, and a lithium secondary battery including the same.

[0002]

[0003] Conventional wet electrodes have been difficult to produce in thick films due to binder misalignment and other issues when manufacturing battery electrodes. To address this, efforts are currently underway to manufacture battery electrodes using a dry process.

[0004] Figure 1 is a schematic diagram for explaining the cause of lithium loss in a conventional lithium secondary battery, and will be described in more detail with reference to this.

[0005] As shown in Fig. 1, in the case of a dry process, since no solvent is used, unlike a general wet process, a dry binder, PTFE (polytetrafluoroethylene), which has fibrillation properties must be used.

[0006] However, when an electrode manufactured through a dry process is used as an anode, the low LUMO level of PTFE, a dry binder, causes a side reaction, resulting in lithium loss during the first lithiation reaction. Ultimately, this not only directly leads to low initial Coulombic efficiency, but also causes electrode deterioration due to the continuous decomposition and repeated volume changes of the dry binder during cycling, which in turn leads to the formation of an unstable solid electrolyte interface (SEI), which degrades electrochemical performance.

[0007] Related prior art literature includes Korean Patent Publication No. 10-2021-0030788 (published on March 18, 2021), which describes a negative electrode for a lithium secondary battery containing a surfactant, a method for manufacturing the same, and a lithium secondary battery containing the same.

[0008]

[0009] The purpose of the present invention is to provide a lithium secondary battery anode having improved electrochemical characteristics by a dry process in which an electrode additive is added to an anode active material, a conductive material, and a dry binder at a strictly limited content ratio and mixed in a dry process to form an anode, thereby suppressing side reactions of PTFE, a dry binder, minimizing lithium loss, and forming a stable SEI (Solid Electrolyte Interface), and a method for manufacturing the same, and a lithium secondary battery including the same.

[0010]

[0011] In order to achieve the above object, a method for manufacturing an anode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention comprises the steps of: (a) mixing an anode active material, a conductive material, a dry binder, and an electrode additive, and then mixing them using a dry process; (b) forming the mixed mixture into a sheet shape to form an electrode sheet; and (c) attaching the electrode sheet to an anode current collector, and then pressing it to form an anode for a lithium secondary battery; wherein in the step (a), the dry binder is polytetrafluoroethylene (PTFE), and the electrode additive is polyvinylpyrrolidone (PVP).

[0012] In the above step (a), the negative active material is composed of carbon alone or a silicon-carbon composite.

[0013] The above negative active material is made of the above silicon-carbon composite, and the silicon and carbon are mixed in a weight ratio of 5:95 to 20:80.

[0014] In the above step (a), the mixing is performed for 10 to 20 minutes using a rotating / rotating mixer.

[0015] After the step (c), the negative electrode for the lithium secondary battery comprises 87 to 97 wt% of the negative electrode active material; 0.5 to 4 wt% of the conductive material; 1 to 5 wt% of the dry binder; and 0.05 to 0.50 wt% of the electrode additive.

[0016] The above electrode additive is added in a content ratio of 0.08 to 0.15 wt%.

[0017]

[0018] In order to achieve the above object, a negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention comprises 87 to 97 wt% of a negative electrode active material; 0.5 to 4 wt% of a conductive agent; 1 to 5 wt% of a dry binder; and 0.05 to 0.50 wt% of an electrode additive, wherein the dry binder is polytetrafluoroethylene (PTFE) and the electrode additive is polyvinylpyrrolidone (PVP).

[0019] The above negative active material is composed of carbon alone or a silicon-carbon composite.

[0020] The above negative active material is made of the above silicon-carbon composite, and the silicon and carbon are mixed in a weight ratio of 5:95 to 20:80.

[0021] The above electrode additive is added in a content ratio of 0.08 to 0.15 wt%.

[0022]

[0023] In order to achieve the above object, a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention comprises: a positive electrode; an anode disposed to face the positive electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte solution impregnating the positive electrode, the negative electrode, and the separator, wherein the negative electrode comprises 87 to 97 wt% of a negative electrode active material, 0.5 to 4 wt% of a conductive material, 1 to 5 wt% of a dry binder, and 0.05 to 0.50 wt% of an electrode additive, wherein the dry binder is polytetrafluoroethylene (PTFE), and the electrode additive is polyvinylpyrrolidone (PVP).

[0024] The above negative active material is composed of carbon alone or a silicon-carbon composite.

[0025] The above negative active material is made of the above silicon-carbon composite, and the silicon and carbon are mixed in a weight ratio of 5:95 to 20:80.

[0026] The above electrode additive is added in a content ratio of 0.08 to 0.15 wt%.

[0027] The electrolyte solution comprises an electrolyte salt, an organic solvent, and an electrolyte additive, and the electrolyte additive comprises fluoroethylene carbonate (FEC).

[0028] The above electrolyte salt includes at least one selected from LiPF6, LiPO2F2, LiI, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, (SO2F)2, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiClO4, LiB(C2O4)2, LiF2BC2O4, LiPF44(C2O4), LiPF2(C2O4)22, LiSCN, and LiP(C2O4)3.

[0029] The organic solvent includes at least one selected from acetonitrile, propylene carbonate, ethylene carbonate, ethylmethyl carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, vinylene carbonate, tetrahydrofuran, 1,2-dioxane, 2-methyltetrahydrofuran, butyrolactone, and dimethylformamide.

[0030] The above electrolyte additive is added in an amount of 4 to 15 wt% of the total weight of the electrolyte.

[0031]

[0032] A negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to the present invention, a method for manufacturing the same, and a lithium secondary battery including the same form an negative electrode by adding an electrode additive to an negative electrode active material, a conductive material, and a dry binder at a strictly limited content ratio and mixing them through a dry process, thereby suppressing side reactions of PTFE, which is a dry binder, to minimize lithium loss and improving electrochemical characteristics through the formation of a stable SEI (Solid electrolyte interface).

[0033] In this way, the negative electrode for a lithium secondary battery and the method for manufacturing the same, which have improved electrochemical characteristics by the dry process and electrode additive content control according to the present invention, and the lithium secondary battery including the same, use PTFE as a dry binder used in the dry process, and by controlling the amount of PVP, which is an electrode additive, to an optimal content ratio, side reactions of PTFE are suppressed, thereby minimizing lithium loss, thereby improving ICE (initial coulombic efficiency) and life stability.

[0034] In addition, the anode for a lithium secondary battery and the method for manufacturing the same, which have improved electrochemical characteristics by the dry process and electrode additive content control according to the present invention, and the lithium secondary battery including the same, use carbon alone or a silicon-carbon composite as an anode active material, and by adding PVP as an electrode additive and strictly controlling the amount of FEC as an electrolyte additive, the improvement effect on the initial irreversibility of PTFE can be further increased.

[0035]

[0036] Figure 1 is a schematic diagram explaining the cause of lithium loss in a conventional lithium secondary battery.

[0037] Figure 2 is a process flow diagram showing a method for manufacturing a negative electrode for a lithium secondary battery with improved electrochemical characteristics by controlling the content of a dry process and electrode additive according to an embodiment of the present invention.

[0038] Figure 3 is a graph showing the results of evaluating the voltage characteristics of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1.

[0039] Figures 4 and 5 are graphs showing the results of evaluating cycle characteristics of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1.

[0040] Figure 6 is a graph showing the results of evaluating the voltage characteristics of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2.

[0041] Figures 7 and 8 are graphs showing the results of evaluating cycle characteristics of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2.

[0042] Figure 9 is a graph showing the results of evaluating the voltage characteristics of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3.

[0043] Figures 10 and 11 are graphs showing the results of evaluating cycle characteristics of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3.

[0044] Figure 12 is a graph showing the results of evaluating the voltage characteristics of lithium secondary batteries manufactured according to Example 7 and Comparative Example 4.

[0045] Figures 13 and 14 are graphs showing the results of evaluating cycle characteristics of lithium secondary batteries manufactured according to Example 7 and Comparative Example 4.

[0046]

[0047] The advantages and features of the present invention, and the methods for achieving them, will become clearer with reference to the embodiments described in detail below together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but may be implemented in various different forms. These embodiments are provided only to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims. Like reference numerals designate like elements throughout the specification.

[0048] Hereinafter, with reference to the attached drawings, a lithium secondary battery negative electrode having improved electrochemical characteristics by a dry process and electrode additive content control according to a preferred embodiment of the present invention, a method for manufacturing the same, and a lithium secondary battery including the same will be described in detail.

[0049]

[0050] A negative electrode for a lithium secondary battery having improved electrochemical characteristics by controlling the content of electrode additives and a dry process according to an embodiment of the present invention is formed by adding electrode additives to a negative electrode active material, a conductive material, and a dry binder at a strictly limited content ratio and mixing them through a dry process, thereby suppressing side reactions of PTFE, which is a dry binder, thereby minimizing lithium loss and improving electrochemical characteristics through the formation of a stable SEI (Solid Electrolyte Interface).

[0051] In this way, the negative electrode for a lithium secondary battery having improved electrochemical characteristics by controlling the dry process and electrode additive content according to an embodiment of the present invention uses PTFE as a dry binder used in the dry process, and by controlling the amount of PVP, an electrode additive, to an optimal content ratio, side reactions of PTFE are suppressed, thereby minimizing lithium loss, thereby improving ICE (initial coulombic efficiency) and life stability.

[0052] In addition, the negative electrode for a lithium secondary battery having improved electrochemical characteristics by controlling the dry process and electrode additive content according to an embodiment of the present invention uses carbon alone or a silicon-carbon composite as the negative electrode active material, and by adding PVP as an electrode additive and strictly controlling the amount of FEC as an electrolyte additive, the improvement effect on the initial irreversibility of PTFE can be further increased.

[0053]

[0054] To this end, a negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention comprises 87 to 97 wt% of a negative electrode active material, 0.5 to 4 wt% of a conductive agent, 1 to 5 wt% of a dry binder, and 0.05 to 0.50 wt% of an electrode additive.

[0055] The negative active material is composed of carbon alone or a silicon-carbon composite. Here, it is more preferable to use a silicon-carbon composite as the negative active material in terms of improving electrochemical characteristics. More specifically, it is preferable to use a silicon-carbon composite in which silicon and carbon are mixed in a weight ratio of 5:95 to 20:80 as the negative active material. At this time, if the silicon content is mixed at a weight ratio of less than 5, there is a problem that the energy density is excessively low due to the small amount of silicon, and if the silicon content exceeds a weight ratio of 20, there is a concern that the carbon may not be able to properly surround the silicon, and thus volume expansion may not be sufficiently suppressed.

[0056] It is preferable that such negative active material be added in a content ratio of 87 to 97 wt% of the total weight of the negative electrode for a lithium secondary battery, and a more preferable range is 90 to 96 wt%. If the amount of the negative active material added is less than 87 wt%, it is difficult to properly exhibit the effect of improving the electrochemical characteristics of the lithium secondary battery. Conversely, if the amount of the negative active material added exceeds 97 wt%, there is a great concern that the electrical conductivity of the lithium secondary battery may deteriorate.

[0057]

[0058] The conductive material may be a material that is conductive without causing a chemical change in the battery. Such conductive materials may include at least one selected from the group consisting of Super-P, carbon nanofibers, vapor-grown carbon fibers, Ketjen black, Denka black, acetylene black, carbon black, carbon nanotubes, multi-walled carbon nanotubes, and ordered mesoporous carbon.

[0059] These conductive agents are preferably added in a content ratio of 0.5 to 4 wt% of the total weight of the negative electrode for lithium secondary batteries, and a more preferred range is 0.8 to 1.5 wt%. If the amount of conductive agent added is less than 0.5 wt%, it may be difficult to ensure conductivity. Conversely, if the amount of conductive agent added exceeds 4 wt%, there is a high risk of reduced durability due to excessive use of the conductive agent.

[0060]

[0061] Dry binders are not slurry-based wet binders, but rather binders that are not mixed with organic solvents and possess fibrillating properties with a fibrous structure. For this purpose, polytetrafluoroethylene (PTFE) is preferably used as the dry binder. PTFE is an essential component for forming films through a dry process, and it possesses the characteristics of a fibrous structure and excellent processability.

[0062] It is preferable that such dry binder be added in a content ratio of 1 to 5 wt% of the total weight of the negative electrode for lithium secondary batteries, and a more preferable range is 2.5 to 3.5 wt%. If the amount of dry binder added is less than 1 wt%, the bonding force between the negative electrode active material and the negative electrode current collector may be weak, making it difficult to secure bonding strength. Conversely, if the amount of dry binder added exceeds 5 wt%, there is a high risk that electrical conductivity may be reduced due to excessive use of the dry binder.

[0063]

[0064] Electrode additives effectively suppress the initial irreversible reaction process caused by side reactions of PTFE, a dry binder, thereby improving ICE. Preferably, the electrode additive is polyvinylpyrrolidone (PVP).

[0065] These electrode additives are preferably added in a content ratio of 0.05 to 0.50 wt% of the total weight of the negative electrode for lithium secondary batteries, a more preferable range may be 0.08 to 0.35 wt%, and a most preferable range may be 0.08 to 0.15 wt%. If the amount of the electrode additive is less than 0.05 wt%, the amount is so small that it is difficult to properly exhibit the effect of improving the initial irreversible reaction of PTFE. On the other hand, if the amount of the electrode additive is excessively added exceeding 0.50 wt%, it is not preferable because it causes a problem of lowering the life characteristics of the lithium secondary battery.

[0066]

[0067] Hereinafter, with reference to the attached drawings, a method for manufacturing a negative electrode for a lithium secondary battery with improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention will be described.

[0068] Figure 2 is a process flow diagram showing a method for manufacturing a negative electrode for a lithium secondary battery with improved electrochemical characteristics by controlling the content of a dry process and electrode additive according to an embodiment of the present invention.

[0069] As illustrated in FIG. 2, a method for manufacturing a negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention includes a mixing step (S110), a film forming step (S120), and a press pressing step (S130).

[0070]

[0071] Mixing

[0072] In the mixing step (S110), the negative active material, conductive material, dry binder, and electrode additive are mixed and then mixed using a dry process.

[0073] The negative active material consists of carbon alone or a silicon-carbon composite. Here, the use of a silicon-carbon composite is more preferable for improving electrochemical properties. More specifically, the negative active material is preferably a silicon-carbon composite in which silicon and carbon are mixed in a weight ratio of 5:95 to 20:80.

[0074] The conductive material may be a material that is conductive without causing a chemical change in the battery. Such conductive materials may include at least one selected from the group consisting of Super-P, carbon nanofibers, vapor-grown carbon fibers, Ketjen black, Denka black, acetylene black, carbon black, carbon nanotubes, multi-walled carbon nanotubes, and ordered mesoporous carbon.

[0075] Dry binders are not slurry-based wet binders, but rather binders that are not mixed with organic solvents and possess fibrillation properties with a fibrous structure. For this purpose, polytetrafluoroethylene (PTFE) is preferably used as the dry binder. PTFE is an essential component for forming films through a dry process, and it possesses the characteristics of a fibrous structure and excellent processability.

[0076] Electrode additives effectively suppress the initial irreversible reaction process caused by side reactions of PTFE, a dry binder, thereby improving ICE. Preferably, the electrode additive is polyvinylpyrrolidone (PVP).

[0077] These electrode additives are preferably added in a content ratio of 0.05 to 0.50 wt% of the total weight of the mixed mixture, a more preferable range may be 0.08 to 0.35 wt%, and a most preferable range may be 0.08 to 0.15 wt%. If the amount of the electrode additive is less than 0.05 wt%, the amount is so small that it is difficult to properly exhibit the effect of improving the initial irreversible reaction of PTFE. On the other hand, if the amount of the electrode additive is excessively added exceeding 0.50 wt%, it is not preferable because it causes a problem of lowering the life characteristics of the lithium secondary battery.

[0078]

[0079] At this stage, mixing is preferably performed using a dry process, which involves mixing the material with a process / rotary mixer for 10 to 20 minutes without adding a solvent. This dry process utilizes the characteristic of PTFE, a dry binder, to fiberize when physical force is applied to create a sheet. This dry process eliminates the need for additional drying equipment after coating, resulting in significant savings in both time and cost.

[0080] In addition, in this stage, by applying a dry process that utilizes the characteristic of PTFE, a dry binder, to become fiberized when physical force is applied, the occurrence of binder unevenness can be prevented in advance, thereby enabling the implementation of an ultra-thick film.

[0081] In this dry process, since no solvent is used, unlike the general wet process, PTFE, a dry binder with fibrillation properties, is used. However, when using the dry process in the negative electrode manufacturing process, a lithium loss problem may occur in the first lithiation process due to a side reaction caused by the low LUMO level of PTFE. To solve this problem, in the present invention, an electrode additive is additionally added at a strictly limited content ratio of 0.05 to 0.5 wt%.

[0082] These electrode additives effectively suppress the initial irreversible reaction process caused by the side reaction of PTFE, a dry binder, thereby improving ICE. Thus, in the present invention, while PTFE is used as a dry binder in the dry process, the addition amount of PVP, an electrode additive, is adjusted to an optimal content ratio, thereby suppressing the side reaction of PTFE and minimizing lithium loss, thereby improving ICE and life stability.

[0083]

[0084] Unveiling

[0085] In the film forming step (S120), the mixed mixture is formed into a sheet shape to form an electrode sheet.

[0086] This film forming step (S120) forms a film from a mixed mixture into a sheet state, and forms an electrode sheet by forming the mixed mixture into a sheet state without using a solvent.

[0087]

[0088] Press compression

[0089] In the press compression step (S130), the electrode sheet is attached to the negative electrode collector and then press-compressed to form a negative electrode for a lithium secondary battery.

[0090] Here, the negative electrode current collector may be formed of one or more alloys selected from among aluminum (Al), copper (Cu), nickel (Ni), titanium (Ti), tungsten (W), iron (Fe), chromium (Cr), stainless steel, etc., which are metals having excellent conductivity. Here, the dimensions of the negative electrode current collector, such as the size or thickness, are not particularly limited. A conductive adhesive (not shown) and a conductive coating layer (not shown) may be further formed on the surface of the negative electrode current collector made of metal foil, as needed.

[0091] In this step, press compression can be performed by, for example, compression using a roll press molding machine. The roll press molding machine aims to increase electrode density and control the thickness of the electrode through rolling, and is composed of a controller that can control the thickness and heating temperature of the upper and lower rolls, and a winding unit that can unwind and wind the electrode. The rolling process proceeds as the rolled electrode passes through the roll press, and this is then wound into a roll again to complete the electrode. At this time, the pressing pressure of the press can be performed under the conditions of 5 to 20 ton / ㎠ and the temperature of the roll can be 50 to 150℃, but is not limited thereto.

[0092] With this, the method for manufacturing a negative electrode for a lithium secondary battery with improved electrochemical characteristics by controlling the dry process and electrode additive content according to an embodiment of the present invention can be completed.

[0093]

[0094] Hereinafter, a lithium secondary battery having improved electrochemical characteristics through a dry process and electrode additive content control according to an embodiment of the present invention will be described.

[0095] A lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control according to an embodiment of the present invention includes a positive electrode, a negative electrode, a separator, and an electrolyte.

[0096] The anode may be, but is not limited to, lithium metal. Any anode used in a lithium secondary battery may be used without limitation.

[0097] The cathode is arranged to face the anode. The cathode comprises 87 to 97 wt% of a cathode active material, 0.5 to 4 wt% of a conductive agent, 1 to 5 wt% of a dry binder, and 0.05 to 0.50 wt% of an electrode additive.

[0098] Here, it is preferable that the dry binder be polytetrafluoroethylene (PTFE).

[0099] Electrode additives effectively suppress the initial irreversible reaction process caused by side reactions of PTFE, a dry binder, thereby improving ICE. Preferably, the electrode additive is polyvinylpyrrolidone (PVP).

[0100] These electrode additives are preferably added in a content ratio of 0.05 to 0.50 wt% of the total weight of the negative electrode for lithium secondary batteries, a more preferable range may be 0.08 to 0.35 wt%, and a most preferable range may be 0.08 to 0.15 wt%. If the amount of the electrode additive is less than 0.05 wt%, the amount is so small that it is difficult to properly exhibit the effect of improving the initial irreversible reaction of PTFE. On the other hand, if the amount of the electrode additive is excessively added exceeding 0.50 wt%, it is not preferable because it causes a problem of lowering the life characteristics of the lithium secondary battery.

[0101] The separator is placed between the positive and negative electrodes to electrically isolate the positive and negative electrodes. Here, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, which may be used alone or in a laminated manner. In addition, the separator may be a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc., but is not limited thereto.

[0102] The electrolyte impregnates the anode, cathode and separator.

[0103] These electrolytes contain electrolyte salts, organic solvents and electrolyte additives.

[0104] Here, the electrolyte salt includes at least one selected from LiPF6, LiPO2F2, LiI, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, (SO2F)2, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiClO4, LiB(C2O4)2, LiF2BC2O4, LiPF44(C2O4), LiPF2(C2O4)22, LiSCN, and LiP(C2O4)3.

[0105] In addition, the organic solvent includes at least one selected from acetonitrile, propylene carbonate, ethylene carbonate, ethylmethyl carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, vinylene carbonate, tetrahydrofuran, 1,2-dioxane, 2-methyltetrahydrofuran, butyrolactone, and dimethylformamide.

[0106] The electrolyte additive is preferably fluoroethylene carbonate (FEC). This electrolyte additive improves the surface properties of the anode active material (carbon alone or a silicon-carbon composite). This minimizes the continuous decomposition and repetitive volume changes of the dry binder PTFE during cycling, thereby improving not only the life characteristics but also overall electrochemical properties, including initial coulombic efficiency and increased capacity.

[0107] It is preferable that the electrolyte additive be added in an amount of 4 to 15 wt% of the total weight of the electrolyte. More preferably, the electrolyte additive be added in an amount of 8 to 12 wt% of the total weight of the electrolyte. If the amount of the electrolyte additive is less than 4 wt%, the amount added may be insufficient, making it difficult to reduce the continuous decomposition and repeated volume changes of PTFE. Conversely, if the amount of the electrolyte additive is added in a large amount exceeding 15 wt%, it may only increase the amount of the electrolyte additive used without further increasing the effect, which is not economical.

[0108]

[0109] As discussed above, the negative electrode for a lithium secondary battery and the method for manufacturing the same, which have improved electrochemical characteristics by controlling the content of electrode additives and the dry process according to an embodiment of the present invention, and the lithium secondary battery including the same, form the negative electrode by adding an electrode additive to the negative electrode active material, conductive material, and dry binder at a strictly limited content ratio and mixing them through a dry process, thereby suppressing the side reaction of PTFE, which is a dry binder, to minimize the loss of lithium and improving the electrochemical characteristics through the formation of a stable SEI (Solid electrolyte interface).

[0110] In this way, the negative electrode for a lithium secondary battery and the method for manufacturing the same, which have improved electrochemical characteristics by controlling the dry process and electrode additive content according to an embodiment of the present invention, and the lithium secondary battery including the same, use PTFE as a dry binder used in the dry process, and by controlling the amount of PVP, which is an electrode additive, to an optimal content ratio, side reactions of PTFE are suppressed, thereby minimizing lithium loss, thereby improving ICE (initial coulombic efficiency) and life stability.

[0111] In addition, a negative electrode for a lithium secondary battery and a method for manufacturing the same, which have improved electrochemical characteristics by controlling the dry process and electrode additive content according to an embodiment of the present invention, and a lithium secondary battery including the same, use carbon alone or a silicon-carbon composite as a negative electrode active material, add PVP as an electrode additive, and strictly control the amount of FEC as an electrolyte additive, thereby further increasing the improvement effect on the initial irreversibility of PTFE.

[0112]

[0113] Example

[0114] Hereinafter, the structure and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.

[0115] Anything not described here is technically inferable enough to be understood by those skilled in this field, so its description will be omitted.

[0116]

[0117] 1. Lithium secondary battery manufacturing

[0118]

[0119] Example 1

[0120] After mixing 95.9 wt% of silicon-graphite composite, 1.0 wt% of super-P, 3.0 wt% of polytetrafluoroethylene (PTFE), and 0.1 wt% of polyvinylpyrrolidone (PVP), the mixture was mixed using a rotating / rotating mixer.

[0121] Next, the mixed mixture was formed into a sheet shape to manufacture an electrode sheet.

[0122] Next, the electrode sheet was attached to the copper foil and then pressed to manufacture the cathode.

[0123] Next, a 2032 coin cell was assembled using a negative electrode as the reference electrode, a positive electrode as the lithium metal as the working electrode, and a polyolefin film (Celgard 2400) as the separator, and then the cell was impregnated with an electrolyte to manufacture a half-cell type lithium secondary battery. The electrolyte used here was 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt%.

[0124]

[0125] Example 2

[0126] A lithium secondary battery was manufactured in the same manner as Example 1, except that the silicon-graphite composite was mixed in a content ratio of 95.7 wt%, Super-P 1 wt%, PTFE 3 wt%, and PVP 0.3 wt%.

[0127]

[0128] Example 3

[0129] A lithium secondary battery was manufactured in the same manner as Example 1, except that 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 5 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0130]

[0131] Example 4

[0132] A lithium secondary battery was manufactured in the same manner as in Example 2, except that 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 5 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0133]

[0134] Example 5

[0135] A lithium secondary battery was manufactured in the same manner as Example 1, except that 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 10 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0136]

[0137] Example 6

[0138] A lithium secondary battery was manufactured in the same manner as in Example 2, except that 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 10 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0139]

[0140] Example 7

[0141] A lithium secondary battery was manufactured in the same manner as in Example 1, except that graphite alone was used instead of the silicon-graphite composite, and 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + LiPO2F2 1 wt% + 12.5 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0142]

[0143] Comparative Example 1

[0144] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the silicon-graphite composite was mixed in a content ratio of 96 wt%, Super-P 1 wt%, and PTFE 3 wt% without adding PVP.

[0145]

[0146] Comparative Example 2

[0147] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the silicon-graphite composite was mixed at a content ratio of 96 wt%, Super-P 1 wt%, and PTFE 3 wt% without adding PVP, and 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 5 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0148]

[0149] Comparative Example 3

[0150] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the silicon-graphite composite was mixed at a content ratio of 96 wt%, Super-P 1 wt%, and PTFE 3 wt% without adding PVP, and 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + 10 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0151]

[0152] Comparative Example 4

[0153] A lithium secondary battery was manufactured in the same manner as in Comparative Example 1, except that graphite alone was used instead of the silicon-graphite composite, and 1.15 M LiPF6 / EC(ethylene carbonate) / EMC(ethylmethyl carbonate) / DEC(diethyl carbonate)(2 / 4 / 4)(v / v) VC 1 wt% + LiPO2F2 1 wt% + 12.5 wt% FEC(fluoroethylene carbonate, PANAX ETEC, Korea) was used as the electrolyte.

[0154]

[0155] 2. Physical property evaluation

[0156] Table 1 shows the results of the electrochemical characteristic evaluation of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1, and Fig. 3 is a graph showing the results of the voltage characteristic evaluation of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1. In addition, Figs. 4 and 5 are graphs showing the results of the cycle characteristic evaluation of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1.

[0157]

[0158] [Table 1]

[0159]

[0160] As shown in Table 1 and FIG. 3, the results of the electrochemical characteristic evaluation of lithium secondary batteries manufactured according to Examples 1 to 2 and Comparative Example 1 showed that when an electrolyte without FEC, an electrolyte additive, was used, improvement in ICE was clearly observed in Example 1, in which PVP was added at a content ratio of 0.1 wt%.

[0161] In addition, as shown in Table 1, Figures 4 and 5, the lithium secondary batteries manufactured according to Examples 1 and 2 showed improvement in ICE compared to the lithium secondary batteries manufactured according to Comparative Example 1, and there was no significant difference in capacity retention rate.

[0162]

[0163] Table 2 shows the results of the electrochemical characteristic evaluation of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2, and Fig. 6 is a graph showing the results of the voltage characteristic evaluation of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2. In addition, Figs. 7 and 8 are graphs showing the results of the cycle characteristic evaluation of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2.

[0164]

[0165] [Table 2]

[0166]

[0167] As shown in Table 2 and FIG. 6, the results of evaluating the electrochemical characteristics of lithium secondary batteries manufactured according to Examples 3 to 4 and Comparative Example 2 showed that when PVP was added, lithium loss in the first lithiation process was effectively suppressed, and this was confirmed to be most improved in Example 4, which had a high PVP content ratio.

[0168] In addition, as shown in Table 2, Figures 7 and 8, in the case of lithium secondary batteries manufactured in Examples 3 to 4 and Comparative Example 2, similar effects were shown in terms of discharge maintenance rate, but in the case of Examples 3 to 4, where PVP was added at 0.1 wt% and 0.3 wt%, ICE was effectively improved, and in the case of Example 4, where PVP was added at 0.3 wt%, the most distinct effect was shown.

[0169]

[0170] Table 3 shows the results of the electrochemical characteristic evaluation of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3, and Fig. 9 is a graph showing the results of the voltage characteristic evaluation of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3. In addition, Figs. 10 and 11 are graphs showing the results of the cycle characteristic evaluation of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3.

[0171]

[0172] [Table 3]

[0173]

[0174] As shown in Table 3 and Fig. 9, the results of evaluating the electrochemical characteristics of lithium secondary batteries manufactured according to Examples 5 to 6 and Comparative Example 3 confirmed that when PVP was added, the irreversible process caused by the side reaction of PTFE was effectively suppressed.

[0175] In addition, as shown in Table 3, Figs. 10 and 11, in the case of the lithium secondary batteries manufactured in Examples 5 to 6 and Comparative Example 3, there was no significant difference in terms of discharge maintenance rate, but in the case of Examples 5 to 6, where PVP was added at 0.1 wt% and 0.3 wt%, ICE was effectively improved. However, in the case of Examples 5 to 6, it was confirmed that there was no significant difference in the ICE improvement effect even when the amount of PVP added increased.

[0176]

[0177] Table 4 shows the results of the electrochemical characteristic evaluation of lithium secondary batteries manufactured according to Example 7 and Comparative Example 4, and Fig. 12 is a graph showing the results of the voltage characteristic evaluation of lithium secondary batteries manufactured according to Example 7 and Comparative Example 4. In addition, Figs. 13 and 14 are graphs showing the results of the cycle characteristic evaluation of lithium secondary batteries manufactured according to Example 7 and Comparative Example 4.

[0178]

[0179] [Table 4]

[0180]

[0181] As shown in Table 4 and Fig. 12, it was confirmed that, like the lithium secondary battery manufactured according to Example 7, the irreversible process due to the side reaction of PTFE was effectively suppressed when PVP was added to the graphite-only electrode, similar to the silicon-graphite electrode.

[0182] In addition, as shown in FIGS. 13 and 14, it was confirmed that, as in the lithium secondary battery manufactured according to Example 7, there was little difference in the discharge maintenance rate even in the graphite-only electrode, but the ICE was effectively improved by adding PVP at a content ratio of 0.3 wt%.

[0183]

[0184] While the above description focuses on specific embodiments of the present invention, those skilled in the art will appreciate that various modifications and variations can be made. Such modifications and variations, as long as they do not depart from the scope of the technical concept provided by the present invention, are considered to be within the scope of the present invention. Therefore, the scope of the present invention should be determined by the claims set forth below.

[0185]

[0186] [Explanation of symbols]

[0187] S110: Mixing stage

[0188] S120: Unveiling Stage

[0189] S130: Press compression stage

Claims

1. (a) A step of mixing a negative electrode active material, a conductive material, a dry binder and an electrode additive, and then mixing them using a dry process; (b) forming an electrode sheet by forming the mixed mixture into a sheet shape; and (c) a step of attaching the electrode sheet to a negative electrode collector and then pressing it to form a negative electrode for a lithium secondary battery; In the above step (a), the dry binder is polytetrafluoroethylene (PTFE), A method for manufacturing a negative electrode for a lithium secondary battery, wherein the electrode additive is polyvinylpyrrolidone (PVP), and the electrochemical characteristics are improved by a dry process and electrode additive content control.

2. In paragraph 1, In step (a) above, The above negative active material is A method for manufacturing a negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process characterized by being composed of carbon alone or a silicon-carbon composite and controlling the content of electrode additives.

3. In paragraph 2, The above negative active material is A method for manufacturing a negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and controlling the content of electrode additives, characterized in that the negative electrode is formed of the above silicon-carbon composite, wherein the silicon and carbon are mixed in a weight ratio of 5:95 to 20:

80.

4. In paragraph 1, In step (a) above, The above mixing is performed for 10 to 20 minutes using a rotating / rotating mixer, and is a method for manufacturing a negative electrode for a lithium secondary battery with improved electrochemical characteristics by controlling the dry process and electrode additive content.

5. In paragraph 1, After step (c) above, The above negative electrode for lithium secondary batteries is 87 to 97 wt% of the above negative active material; 0.5 to 4 wt% of the above-mentioned challenging agent; 1 to 5 wt% of the above dry binder; and 0.05 to 0.50 wt% of the above electrode additive; A method for manufacturing a negative electrode for a lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additives, characterized by including:

6. In paragraph 5, The above electrode additives are A method for manufacturing a negative electrode for a lithium secondary battery, wherein the electrochemical characteristics are improved by controlling the content of a dry process and electrode additive, characterized in that the content is added in a content ratio of 0.08 to 0.15 wt%.

7. 87 to 97 wt% of negative electrode active material; 0.5 to 4 wt% of the challenge agent; 1 to 5 wt% dry binder; and Contains 0.05 to 0.50 wt% of electrode additive; The above dry binder is polytetrafluoroethylene (PTFE), A negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and controlling the content of the electrode additive, wherein the electrode additive is polyvinylpyrrolidone (PVP).

8. In paragraph 7, The above negative active material is A negative electrode for a lithium secondary battery having improved electrochemical properties by a dry process and controlling the content of electrode additives, characterized by being composed of carbon alone or a silicon-carbon composite.

9. In paragraph 8, The above negative active material is A negative electrode for a lithium secondary battery having improved electrochemical characteristics by a dry process and controlling the content of electrode additives, characterized in that the negative electrode is made of the above silicon-carbon composite, wherein the silicon and carbon are mixed in a weight ratio of 5:95 to 20:

80.

10. In paragraph 7, The above electrode additives are A negative electrode for a lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additive, characterized in that the content is added at a content ratio of 0.08 to 0.15 wt%.

11. Bipolar; A cathode positioned opposite the anode; A separator disposed between the anode and cathode; and An electrolyte solution for impregnating the positive electrode, negative electrode and separator; The above negative electrode comprises 87 to 97 wt% of negative active material, 0.5 to 4 wt% of conductive material, 1 to 5 wt% of dry binder, and 0.05 to 0.50 wt% of electrode additive; The above dry binder is polytetrafluoroethylene (PTFE), A lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control, characterized in that the electrode additive is polyvinylpyrrolidone (PVP).

12. In paragraph 11, The above negative active material is A lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additives, characterized by being composed of carbon alone or a silicon-carbon composite.

13. In paragraph 11, The above negative active material is A lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control, characterized in that the lithium secondary battery is made of the above silicon-carbon composite, wherein the silicon and carbon are mixed in a weight ratio of 5:95 to 20:

80.

14. In paragraph 11, The above electrode additives are A lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additive, characterized in that the additive is added at a content ratio of 0.08 to 0.15 wt%.

15. In paragraph 11, The above electrolyte is Containing electrolyte salt, organic solvent and electrolyte additive, A lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additive, wherein the electrolyte additive is fluoroethylene carbonate (FEC).

16. In paragraph 15, The above electrolyte salt is A lithium secondary battery having improved electrochemical characteristics by a dry process and electrode additive content control, characterized in that it includes at least one selected from among LiPF6, LiPO2F2, LiI, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, (SO2F)2, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiClO4, LiB(C2O4)2, LiF2BC2O4, LiPF44(C2O4), LiPF2(C2O4)22, LiSCN and LiP(C2O4)3.

17. In paragraph 15, The above organic solvent is A lithium secondary battery having improved electrochemical characteristics by a dry process and controlling the content of electrode additives, characterized in that it comprises at least one selected from acetonitrile, propylene carbonate, ethylene carbonate, ethylmethyl carbonate, dimethyl carbonate, diethyl carbonate, butylene carbonate, vinylene carbonate, tetrahydrofuran, 1,2-dioxane, 2-methyltetrahydrofuran, butyrolactone, and dimethylformamide.

18. In paragraph 11, The above electrolyte additive is A lithium secondary battery having improved electrochemical characteristics by controlling the content of a dry process and electrode additive, characterized in that the additive is added at 4 to 15 wt% of the total weight of the electrolyte.

Citation Information

Patent Citations

  • Electric Double Layer Capacitor and manufacturing method of sheet type electrode for EDLC

    KR100581230B1

  • PDRN encapsulated chitosan nanoparticles included chitosan nanofilm and a method for preparing the same

    KR1020210013230A

  • Apparatus for processing wafer capable of positioning focus ring

    KR1020240022806A

  • Shaping device for beam of vehicle

    KR102132652B1

  • KR20220065688A

Cited By

  • Method for preparing negative electrode membrane by using semi-dry method, negative electrode membrane, secondary battery and electric device

    CN119495746A

  • Electrolyte adaptive to dry-method electrode plate, preparation method of electrolyte and lithium ion battery

    CN120109298A