Silicon-carbon composite for secondary battery anode material, and method for manufacturing same
The silicon-carbon composite addresses the volume expansion issue in silicon-based anode materials by using a porous carbon structure and carbon coating, enhancing the performance and longevity of secondary batteries.
Patent Information
- Application Number
- PCT/KR2024/005837
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-26
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-14
AI Technical Summary
Silicon-based anode materials for secondary batteries experience significant volume expansion during charging and discharging, leading to material destruction, reduced electronic conductivity, and decreased cycle life, limiting their application in high-capacity batteries.
A silicon-carbon composite is developed, comprising amorphous or mixed-state silicon particles with an average grain size of 10 nm or less, combined with a porous carbon structure having specific pore distributions and a carbon-based coating, to minimize volume expansion and enhance structural integrity.
The silicon-carbon composite improves the initial discharge capacity, efficiency, and lifespan of secondary batteries by accommodating volume expansion and maintaining electronic conductivity, resulting in stable battery performance over multiple cycles.
Smart Images

Figure KR2024005837_14112024_PF_FP_ABST
Abstract
Description
Silicon-carbon composite for secondary battery anode material and method for manufacturing the same
[0001] The present invention relates to a silicon-carbon composite for use as a negative electrode material for a secondary battery and a method for producing the same, and more specifically, to a silicon-carbon composite for use as a negative electrode material for a secondary battery and a method for producing the same, which can improve the characteristics of a secondary battery when applied as a negative electrode material by minimizing changes in the volume of silicon particles during the charge / discharge process of a secondary battery.
[0002] The performance improvement of secondary batteries is based on the components of positive electrode materials, negative electrode materials, and electrolyte.
[0003] Among the above components, graphite-based materials, which are mainly used as cathode materials, are commercially available due to their excellent electrochemical performance and low cost, but their theoretical capacity is limited to 370 mAh / g, which limits their application to high-capacity secondary batteries.
[0004] To overcome the above limitations, non-graphite anode materials such as silicon, tin, and germanium are emerging as alternative materials. Among them, silicon has a theoretical capacity of 4000-4200 mAh / g, can store a very large amount of lithium per unit weight, and exhibits a high capacity of nearly 10 times that of graphite, so it is attracting attention as a material to replace graphite. However, compared to its high theoretical capacity, it has a large volume expansion of approximately 400% during the charge and discharge process, which causes problems such as destruction and pulverization of silicon particles, and decreased electronic conductivity with carbon additives and current collectors, and ultimately leads to capacity loss and reduced cycle life of secondary batteries.
[0005] As a method for alleviating the volume expansion of silicon, a method for controlling the characteristics of silicon particles and a method for manufacturing a silicon-carbon composite (Si-C composite) by mixing carbon-based materials have been devised, and applying the composite as an anode material for secondary batteries to improve the performance of secondary batteries has emerged as an important task.
[0006] The purpose of the present invention is to provide a silicon-carbon composite as an anode material for a secondary battery, which can improve the initial discharge capacity, initial efficiency, and lifespan characteristics of a secondary battery when applied as an anode material for a secondary battery, and a method for producing the same.
[0007] The purpose of the present invention is not limited to the aforementioned purposes, and other unmentioned purposes and advantages of the present invention can be understood through the following description and will be more clearly understood through the embodiments of the present invention. Furthermore, it will be readily apparent that the purposes and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims.
[0008] In order to achieve the above purpose, according to the first aspect of the present invention,
[0009] A silicon-carbon composite comprising silicon particles and a porous carbon structure,
[0010] The above silicon particles exist in an amorphous or mixed state of amorphous and crystalline,
[0011] The average crystal grain size of the above crystalline silicon particles is 10 nm or less,
[0012] The above porous carbon structure includes micropores, mesopores and macropores,
[0013] Based on the total pore volume of 100 vol% of the above porous carbon structure, the micropores are contained at 10 to 30 vol%, the mesopores are contained at 20 to 40 vol%, and the macropores are contained at 40 to 60 vol%.
[0014] A silicon-carbon composite can be provided.
[0015] The total porosity of the above porous carbon structure is 0.6 to 1.5 cm 3 / g may be.
[0016] The specific surface area of the above porous carbon structure is 200 to 1,000 m 2 / g may be.
[0017] The average particle size of the above silicon particles may be 1 to 100 nm, and the average particle size of the above silicon-carbon composite particles may be 4 to 8 μm.
[0018] The above porous carbon structure may be formed of carbon black or a mixture of carbon black and a binder.
[0019] In the case of a mixture of the above carbon black and binder, when the total weight of the mixture is 100 wt%, the carbon black may be included in a ratio of 40 to 70 wt%, and the binder may be included in a ratio of 30 to 60 wt%.
[0020] The above binder may include at least one of phenolic resin, coal tar pitch, and polyacrylonitrile.
[0021] A coating layer may be formed on the surface of the above silicon-carbon composite using a carbon-based coating material.
[0022] When the total weight of the above silicon-carbon composite is 100 wt%, the content of silicon particles included in the above silicon-carbon composite may be 40 to 80 wt%.
[0023] The above silicon-carbon composite can satisfy the span value of Equation 1 below of 0.8 to 1.2.
[0024] <Formula 1> Span = (D 90 -D 10 ) / D 50
[0025] According to a second aspect of the present invention, a negative electrode material for a secondary battery comprising a silicon-carbon composite according to the first aspect of the present invention can be provided.
[0026] According to a third aspect of the present invention, there is provided a method for producing a silicon-carbon composite according to the first aspect of the present invention,
[0027] (a) a step of placing a porous carbon structure in a chemical vapor deposition (CVD) reactor;
[0028] (b) a step of supplying silicon source gas to a chemical vapor deposition (CVD) reactor and reacting under atmospheric pressure and a temperature of 400°C to 550°C to chemically vapor deposit silicon particles on the porous carbon structure; and
[0029] (c) a step of precipitating the result of (b) above as a solid to obtain a silicon-carbon composite; including;
[0030] A method for manufacturing a silicon-carbon composite can be provided.
[0031] The above step (a) can be performed under a carrier gas atmosphere.
[0032] The carrier gas may include at least one of nitrogen gas and argon gas.
[0033] Hydrogen (H2) gas can be additionally added to the above step (a).
[0034] The above silicon source gas may include at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, and trimethylsilane (SiH(CH3)3) gas.
[0035] After the above step (c), the method may further include the step of (d) forming a coating layer using a carbon-based coating material on the surface of the obtained silicon-carbon composite.
[0036] The above step (d) can be performed by any one of coating by chemical vapor deposition (CVD), coating by solution infiltration followed by solvent evaporation, coating by solution infiltration followed by solvent evaporation and annealing, coating by sol-gel, coating by vapor infiltration, coating by molten infiltration, and coating by atomic deposition.
[0037] The above step (d) may be a method of forming a carbon-based coating layer by chemical vapor deposition (CVD) using a carbon source gas including at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, and ethylene gas.
[0038] The present invention can provide silicon particles having a particle size adjusted to a condition that can prevent silicon cracking and minimize volume expansion even during charging and discharging of a secondary battery.
[0039] The present invention provides a carbon material having a void space capable of accommodating volume expansion of silicon, and a pore volume distribution that allows silicon to grow when manufacturing a silicon-carbon composite.
[0040] A novel silicon-carbon composite formed from the silicon particles and carbon material of the present invention can be provided.
[0041] Due to the excellent properties of the silicon-carbon composite of the present invention, the initial discharge capacity, initial efficiency, and life characteristics of a secondary battery manufactured by including the composite as an anode material can be improved.
[0042] In addition to the effects described above, the effects of the present invention are described together with the description of matters for carrying out the invention below.
[0043] Figure 1 shows a graph of the results of X-ray diffraction analysis of the silicon-carbon composite of Example 1, performed according to Experimental Example 1 of the present invention.
[0044] Figure 2 is a graph showing the discharge capacity measured in a 20-cycle experiment performed according to Experimental Example 2 of the present invention.
[0045] Figure 3 is a graph showing the efficiency measured in a 20-cycle experiment performed according to Experimental Example 2 of the present invention.
[0046] Figure 4 is a graph showing the capacity retention rate measured in a 20-cycle experiment performed according to Experimental Example 2 of the present invention.
[0047] The above-described objects, features, and advantages will be described in detail below with reference to the accompanying drawings, so that those skilled in the art can easily practice the technical idea of the present invention. In describing the present invention, if it is determined that a detailed description of known technologies related to the present invention may unnecessarily obscure the gist of the present invention, a detailed description thereof will be omitted. Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the drawings, the same reference numerals are used to indicate the same or similar components.
[0048] In this specification, when the terms "includes," "has," "consists of," "arranges," and "provides" are used for a component, other parts may be added, unless "only" is used. When a component is expressed in the singular, it includes the plural unless otherwise explicitly stated.
[0049] In this specification, micropore means a pore having an average size of 2 nm or less, mesopore means a pore having an average size of more than 2 nm and less than 50 nm, and macropore means a pore having an average size of 50 nm to 100 nm.
[0050] In this specification, particle size measurement is performed using the Particle size analyzer (PSA) method, which calculates the particle size through the scattering angle distribution of light scattered while passing through a powder sample of the target sample, and the measuring equipment used was an LS 13 320 Particle Size Analyzer (Beckman Coulter).
[0051] In the present invention, the average particle size of silicon in the silicon-carbon composite is measured through SEM (JSM-7100F) or TEM (JEM-2100F) analysis, and the size of silicon particles of at least 9 spots is measured, and the average value is used.
[0052] In the present invention, “crystal grain” refers to a crystallite or crystallite, and means “a region of a material in which atoms are aligned and arranged in a repeating pattern.”
[0053] In the present invention, the crystal grain size is measured through XRD (equipment name: panalytical - x'pert pro) analysis, and the crystal grain size automatically derived through the Scherer equation for the XRD data measured by the equipment is used.
[0054] In this specification, the specific surface area was measured by the BET method (nitrogen adsorption / desorption method).
[0055] In this specification, the porosity of micropores and mesopores was measured by the BET (Brunauer-Emmett-Teller) method (nitrogen adsorption / desorption method), and the porosity of macropores was measured by the mercury porosimetry method.
[0056] In interpreting the components in this specification, even if there is no separate explicit description, it is interpreted to include the range of error.
[0057]
[0058] Hereinafter, the present invention will be described in more detail.
[0059]
[0060] The silicon-carbon composite of the present invention is a silicon-carbon composite including silicon particles and a porous carbon structure, wherein the average particle size of the silicon particles may be 1 to 100 nm or less, the silicon particles may exist in an amorphous or a mixed state of amorphous and crystalline, the average crystal grain size of the crystalline silicon particles may be 10 nm or less, the porous carbon structure may include micropores, mesopores, and macropores, and the average particle size of the silicon-carbon composite particles may be 4 to 8 μm.
[0061]
[0062] As a result of the study conducted in the present invention, it was found that when amorphous silicon particles are included or crystalline silicon particles are mixed with amorphous silicon particles, and even if the crystalline silicon particles have an average grain size of 10 nm or less, when applied as an anode material, there is an advantage in solving the problem of deterioration in the performance of a secondary battery by preventing the surface of the silicon particles from breaking during discharge of the secondary battery.
[0063] If the average particle size of the above silicon particles exceeds 100 nm as nanoparticles, there may be a problem in which the surface of the silicon particles breaks during charging and discharging, resulting in a decrease in performance.
[0064] In addition, if the average particle size of the silicon-carbon composite particles exceeds 4 to 8 μm, there may be a problem that a process for controlling the particle size through an additional spheroidization process or a crushing process is required.
[0065] The porous carbon structure of the present invention has a pore volume including micropores, mesopores, and macropores, thereby providing empty space capable of accommodating expansion of silicon during charging and discharging of a secondary battery, thereby contributing to mitigating expansion of the silicon-carbon composite. In addition, it may be advantageous in obtaining silicon of the size and shape desired in the present invention by providing a nucleation site where silicon can grow.
[0066] According to one embodiment of the present invention, based on 100 vol% of the total pore volume of the porous carbon structure, the micropores may be 10 to 30 vol%, the mesopores may be 20 to 40 vol%, and the macropores may be 40 to 60 vol%. When the porous carbon structure of the present invention satisfies the pore distribution, silicon can be evenly impregnated into the porous carbon structure, and thus silicon expansion can be efficiently controlled during charging of the secondary battery, and there can be an advantage of high lifespan maintenance.
[0067] According to one embodiment of the present invention, the porous carbon structure may be formed of carbon black or a mixture of carbon black and a binder.
[0068] When manufacturing porous carbon structures, mixing a binder induces carbon black agglomeration, increasing the density of the porous carbon structure. Furthermore, the pore distribution can be controlled by adjusting the ratio of carbon black to binder.
[0069] From this point of view, when forming a porous carbon structure with a mixture of the carbon black and a binder according to one embodiment of the present invention, when the total weight of the mixture is 100 wt%, the carbon black may be included in a proportion of 40 to 70 wt%, and the binder may be included in a proportion of 30 to 60 wt%. More preferably, when the total weight of the mixture is 100 wt%, the carbon black may be included in a proportion of 50 to 65 wt%, and the binder may be included in a proportion of 35 to 50 wt%.
[0070]
[0071] As described below, when manufacturing the porous carbon structure, a carbonization process is performed, and the carbon present in the binder remains in the form of amorphous carbon, and other elements present in the binder disappear during the carbonization process.
[0072] According to one embodiment of the present invention, the carbon black may be selected from furnace black and acetylene black.
[0073] According to one embodiment of the present invention, the binder may include at least one of phenolic resin, coal tar pitch, and polyacrylonitrile.
[0074]
[0075] The method for manufacturing the porous carbon structure desired in the present invention generally includes a heat treatment step and an activation step of carbon black, and specifically, can be divided into the following two methods depending on whether the activation process is before or after the heat treatment.
[0076] A first method for manufacturing a porous carbon structure according to the present invention is a post-activation method, which may include the following steps.
[0077] (a-1) A step of mixing carbon black and a binder in a solvent;
[0078] (a-2) A step of spheroidizing the mixture of (a-1) by spray drying;
[0079] (a-3) a step of carbonizing the result of (a-2) above at 900 to 1100°C; and
[0080] (a-4) A step of steam activation of the result of (a-3) above at 900 to 1000°C.
[0081]
[0082] A second method for manufacturing a porous carbon structure according to the present invention is a pre-activation method for performing an activation step prior to heat treatment, which may include the following steps.
[0083] (b-1) A step of steam activating carbon black in pellet form at 900 to 1000°C;
[0084] (b-2) A step of disintegrating the carbon black of the resultant product of (b-1) and then mixing it with a binder in a solvent;
[0085] (b-3) a step of spray drying the mixture of (b-2) to form a sphere; and
[0086] (b-4) A step of carbonizing the result of (b-3) above at 900 to 1100°C.
[0087]
[0088] The contents regarding carbon black and binder in the first or second method are the same as those described above.
[0089] According to one embodiment of the present invention, the total porosity of the porous carbon structure is 0.6 to 1.5 cm 3 / g, and the specific surface area of the porous carbon structure is 200 to 1,000 m 2 / g. By using a porous carbon structure that satisfies such characteristics, the effect desired in the present invention can be achieved.
[0090] Specifically, if the total porosity of the porous carbon structure is too small, it cannot provide a buffering role when silicon expands, and thus, when applied as a negative electrode material for a secondary battery, there may be a problem that the lifespan of the secondary battery may be reduced.
[0091] On the other hand, if the total porosity of the porous carbon structure is too large, the specific surface area may increase excessively, which may cause a problem in that the charge / discharge efficiency of the secondary battery may decrease when applied as an anode material of the secondary battery. From this point of view, the total porosity of the porous carbon structure of the present invention may be, for example, 0.6 to 1.5 cm 3 / g can be, for example, 0.7 to 1.2 cm 3 / g may be.
[0092] The above total porosity is the sum of the porosities of all pores, including micropores, mesopores, and macropores. The porosity of micropores and mesopores is measured by the BET method, and the porosity of macropores is measured by the mercury porosimetry.
[0093]
[0094] In addition, if the specific surface area of the porous carbon structure is too small, the area where silicon can be deposited is reduced, resulting in a decrease in the silicon content in the negative electrode material, and there is a problem in that it is difficult to achieve the desired capacity of the secondary battery when applied as the negative electrode material of the secondary battery.
[0095] On the other hand, if the specific surface area of the porous carbon structure is too large, there is a disadvantage in that the charge / discharge efficiency of the secondary battery is lowered when applied as a negative electrode material of the secondary battery.
[0096] From this point of view, the specific surface area of the porous carbon structure of the present invention is, for example, 200 to 1,000 m 2 / g, and the specific surface area is, for example, 200-500m 2 / g, and the specific surface area is, for example, 200-300 m 2 / g may be.
[0097] According to one embodiment of the present invention, the silicon-carbon composite may have a span value of Equation 1 below of 0.8 to 1.2. The span value refers to the distribution of the composite particle size, and if it deviates from the span value, it means that the size of the composite particles is not uniform, and the degree of expansion of the silicon particles is different throughout the electrode, which may cause a problem of partial life degradation. Since the quality of the composite particles is excellent, there may be an advantage of increased life maintenance rate due to uniform volume expansion of the silicon particles throughout.
[0098] <Formula 1> Span = (D 90 -D 10 ) / D 50
[0099] In the above equation 1, D 10 value, D 50 Value and D 90 The values represent the particle size (size) values that account for 10%, 50%, and 90% of the total powder distribution, respectively, in descending order of particle size (size).
[0100]
[0101] According to one embodiment of the present invention, a coating layer using a carbon-based coating material can be formed on the surface of the silicon-carbon composite, if necessary. Forming the coating layer in this way can more effectively protect silicon exposed to the outside of the silicon-carbon composite, improve the particle strength of the silicon-carbon composite, and increase electrical conductivity, thereby controlling the physical properties required for the silicon-carbon composite. For example, the carbon-based coating material can be thermally decomposed, and then a coating layer can be formed using the thermally decomposed carbon-based coating material. The thickness of the coating layer is not particularly limited, but may be, for example, 1 to 100 nm, for example, 5 to 50 nm, or for example, 10 to 20 nm.
[0102] The carbon-based coating material for forming the above coating layer may include, but is not limited to, one or more selected from the group consisting of petroleum pitch, ethylene, acetylene, methane, ethane, epoxy resin, polyphenol, polyaniline, polyvinyl alcohol, polyvinyl chloride, and other cross-linked polymers. As a method for forming the above carbon-based coating layer, the carbon-based coating layer may be deposited by chemical vapor deposition (CVD) using a carbon source gas including one or more selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, and ethylene gas.
[0103] The carbon-based coating material may include a conductive polymer. For example, the conductive polymer may include, but is not necessarily limited to, one or more selected from the group consisting of polyacrylonitrile (PAN), polyaniline, polypyrrole, polyacetylene, polyphenylene, polyphenylene sulfide, polythiophene, poly(fluorene), polypyrene, polyazulene, polynaphthalene, polycarbazole, polyindole, polyazepine, poly(3,4-ethylenedioxythiophene) (PEDOT), poly(p-phenylene sulfide) (PPS), and poly(p-phenylene vinylene) (PPV).
[0104] As a coating method for forming the above coating layer, coating by chemical vapor deposition (CVD), coating by solution infiltration followed by solvent evaporation, coating by solution infiltration followed by solvent evaporation and annealing, coating by sol-gel, coating by vapor infiltration, coating by molten infiltration, coating by atomic deposition, etc. can be applied, but are not necessarily limited thereto.
[0105]
[0106] The present invention provides a method for producing a silicon-carbon composite, and the produced silicon-carbon composite can satisfy the characteristics of the silicon-carbon composite of the present invention described above.
[0107]
[0108] Specifically, the method for manufacturing the silicon-carbon composite of the present invention may include the following steps (a) to (c).
[0109] (a) a step of placing a porous carbon structure in a chemical vapor deposition (CVD) reactor;
[0110] (b) a step of supplying silicon source gas to a chemical vapor deposition (CVD) reactor and reacting under atmospheric pressure and a temperature of 400 to 500°C to chemically vapor deposit silicon particles on the porous carbon structure; and
[0111] (c) A step of precipitating the result of (b) above as a solid to obtain a silicon-carbon composite.
[0112]
[0113] According to one embodiment of the present invention, the reactor used in step (a) may be a tube furnace or a rotary tube furnace.
[0114] According to one embodiment of the present invention, the substrate may be a boat or a sus plate, but is not necessarily limited thereto.
[0115] According to one embodiment of the present invention, in order to control the overall reaction rate and obtain a uniform homogeneous reaction product, step (a) may be performed under an atmosphere of a carrier gas, which is an inert gas. The carrier gas may include at least one of nitrogen gas and argon gas, but is not necessarily limited thereto.
[0116] According to one embodiment of the present invention, in order to suppress the reactivity of Si radicals generated when Si-H bonds are broken during a homogeneous reaction and obtain a uniform Si-C composite, hydrogen (H2) gas may be additionally added in step (a). If hydrogen gas is not added, the thermal decomposition products of silicon gas may be mostly concentrated at the front of the reactor, which may cause a problem of uneven Si distribution.
[0117]
[0118] In order to satisfy the characteristics of the silicon particles, particularly the crystallinity and grain size characteristics, in the silicon-carbon composite according to one embodiment of the present invention, the ratio of the silicon source gas, the carrier gas, and the hydrogen gas can be adjusted. For example, when the total gas amount of the three types of gases is 1000 sccm, the silicon source gas can be 1 to 20 sccm, the carrier gas can be 400 to 600 sccm, and the hydrogen gas can be 400 to 600 sccm, but is not necessarily limited thereto.
[0119]
[0120] According to one embodiment of the present invention, the silicon source gas may include at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, and trimethylsilane (SiH(CH3)3) gas, but is not necessarily limited thereto.
[0121]
[0122] According to one embodiment of the present invention, the temperature condition of step (b) is for performing a homogeneous reaction, and may be, for example, 400°C to 550°C, for example, 450°C to 500°C, and may be advantageous in satisfying the characteristics of silicon particles in the silicon-carbon composite according to the present invention, particularly, the characteristics of crystallinity and crystal grain size, within the above temperature range, but is not necessarily limited thereto.
[0123]
[0124] According to one embodiment of the present invention, in step (c), the resultant of (b) may be cooled to room temperature of 23 to 25°C and deposited in a crucible to precipitate the solid.
[0125] According to one embodiment of the present invention, after step (c), the method may further include a step (d) of forming a coating layer using a carbon material for coating on the surface of the obtained silicon-carbon composite.
[0126] The above coating layer is the same as that described with respect to the coating layer formed of a carbon material for coating formed on the surface of the silicon-carbon composite of the present invention.
[0127] According to one embodiment of the present invention, the step (d) may be performed by any one of coating by chemical vapor deposition (CVD), coating by solution infiltration followed by solvent evaporation, coating by solution infiltration followed by solvent evaporation and annealing, coating by sol-gel, coating by vapor infiltration, coating by molten infiltration, and coating by atomic deposition, and may be performed by, for example, coating by chemical vapor deposition (CVD), but is not limited thereto.
[0128] According to one embodiment of the present invention, the step (d) may form a carbon-based coating layer by chemical vapor deposition (CVD) using a carbon source gas including at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, and ethylene gas.
[0129]
[0130] Hereinafter, the present invention will be described in more detail through examples and experimental examples. However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0131]
[0132] Example 1
[0133] Carbon black (OCI Carbon Black DC3501) and phenolic resin as a binder were mixed in isopropyl alcohol (IPA) at a ratio of 'carbon black: binder = 65:35 (by weight)', and then dried by spray drying to form spherical powder particles. Then, carbonization was performed at a temperature of approximately 1000°C, and steam activation was performed at a temperature of 950°C to produce a porous carbon structure. The pore ratio of the manufactured porous carbon structure was micropore: mesopore: macropore = 11:37:52 (by volume).
[0134] About 5 g of the above porous structure was placed on a crucible in a rotary tube furnace, which is a reaction device, and heated to a temperature of 455°C. Into the reaction device heated to 455°C, a mixture of monosilane gas and hydrogen gas (monosilane gas: hydrogen mixture gas = 50 sccm: 450 sccm) was injected at atmospheric pressure to perform a chemical vapor deposition reaction. After reacting for about 2 hours, the mixture was cooled to room temperature to obtain about 10 g of a gray-black solid silicon-carbon composite deposited in the crucible.
[0135] A chemical vapor deposition reaction was performed at 455°C for 2 hours while flowing a mixed gas of acetylene gas and argon gas (acetylene gas: argon gas = C2H2: Ar = 250 sccm: 250 sccm) over 2 g of the silicon-carbon composite obtained above, thereby forming a carbon coating layer of about 10 nm thickness on the surface of the silicon-carbon composite, thereby manufacturing the final silicon-carbon composite.
[0136]
[0137] Comparative Examples 1 to 3
[0138] A silicon-carbon composite was manufactured in the same manner as in Example 1, but porous carbon structures having different ratios of micropores, mesopores, and macropores contained in the porous carbon structure were prepared, and the specific ratios of the pores are as shown in Table 1 below.
[0139] Specifically, Comparative Example 1 corresponds to a case where the micropore ratio was higher than that specified in the present invention, the macropore ratio was lower, and the total porosity was also lower than that targeted in the present invention.
[0140] Comparative Example 2 corresponds to a case where the mesopore ratio is higher and the macropore ratio is lower than that specified in the present invention.
[0141] Comparative Example 3 corresponds to a case where the micropore ratio is higher and the macropore ratio is lower than that specified in the present invention.
[0142] [Table 1]
[0143]
[0144] In Table 1 above, ‘structural BET’ refers to the measurement of the specific surface area of the entire silicon-carbon composite structure.
[0145] In the above Table 1, 'BET' means that the porosity of micropores and mesopores belonging to those having an average pore size of 50 nm or less was measured by the BET method.
[0146] In the above Table 1, ‘mercury porosity method’ means that the porosity of macropores having an average pore size exceeding 50 nm was measured by mercury porosity method.
[0147]
[0148] Experimental Example 1 - XRD Analysis of Silicon Particles
[0149] The graph showing the results of analyzing the silicon particles in the silicon-carbon composite manufactured in Example 1 using X-ray diffraction analysis (XRD) is shown in Fig. 1.
[0150] For silicon, the grain size is determined by observing the peak at the point where 2θ(theta) [unit: degree (°)] is 28° in the XRD analysis graph. In addition, if there is no peak in the XRD analysis graph, the measurement subject is judged to be amorphous, and if the peak is broadly distributed, the measurement subject is interpreted as a mixture of amorphous and crystalline forms.
[0151] Looking at Figure 1, the silicon-carbon composite manufactured in Example 1 has a widely distributed peak at a point where 2θ is 28°, so it can be seen that it is a mixture of amorphous silicon particles and crystalline silicon particles. The average grain size of the crystalline silicon particles calculated using the Scherrer equation using XRD analysis data was 1.7 nm.
[0152] Comparative Examples 1 to 3 also used the same silicon source gas and silicon deposition method as Example 1, and as a result of performing XRD analysis, the crystal grain size was also measured to be 1.7 nm.
[0153]
[0154] Experimental Example 2 - Half-Cell Test
[0155] The silicon-carbon composites manufactured in Example 1 and Comparative Examples 1 to 3 were prepared as a negative electrode material. Separately, conductive carbon black (Super P) and carbon nanotube conductive material (SWCBT) were mixed (Super P: SWCNT = 9: 1, weight ratio) to prepare a conductive material. Separately, sodium salt of carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) were mixed (CMC: SBR = 3: 7, weight ratio) to prepare a binder. The negative electrode material, conductive material, and binder prepared above were mixed using a sinky mixer (negative electrode material: conductive material: binder = 8: 1: 1, weight ratio) to obtain a negative electrode slurry.
[0156] The above cathode slurry was applied to a copper foil having a thickness of 18 μm and dried at 80°C for 1 hour. Then, after heat treatment in a vacuum oven at 100°C for 12 hours, a cathode plate was manufactured by punching to 16 mmØ.
[0157] The fabricated cathode plate was fabricated into a coin cell using Li metal as a counter electrode, and its electrochemical characteristics were confirmed. The charge / discharge conditions were charge CC / CV: 0.005 V / 0.005 C, discharge CC 1.5 V, and the rate was 0.1 C.
[0158] Using the TOSCAT-3100 equipment, which is a half-cell device, 20 cycles of charge and discharge were performed, and the results of measuring the discharge capacity (mAh / g), efficiency (%), and capacity retention rate (CRR, %) are shown in Figures 2 to 4, respectively, and the results are summarized in Table 2 below.
[0159] [Table 2]
[0160]
[0161] As can be seen from Table 2 above, when the silicon-carbon composite of Example 1 manufactured using a specific porous structure in the present invention was used as a negative electrode material, it was found that the discharge capacity, efficiency, and capacity retention rate were all improved compared to Comparative Examples 1 to 3 that did not satisfy the specific porous structure in the present invention.
[0162]
[0163] In addition, referring to the graph of Fig. 3, it can be seen that Comparative Examples 1 to 3 exhibit a significant degree of fluctuation in efficiency values as the number of cycles increases, resulting in very unstable results when applied to secondary batteries. On the other hand, Example 1 exhibited a lesser degree of decrease in efficiency as the number of cycles increased compared to Comparative Examples 1 to 3, and it was also found that the secondary battery was operated very stably.
[0164]
[0165] Although the embodiments of the present specification have been described in more detail with reference to the attached drawings, the present specification is not necessarily limited to these embodiments, and various modifications may be implemented without departing from the technical spirit of the present specification. Therefore, the embodiments disclosed in this specification are not intended to limit the technical spirit of the present specification, but to explain, and the scope of the technical spirit of the present specification is not limited by these embodiments. Therefore, it should be understood that the embodiments described above are illustrative in all respects and not restrictive. The scope of protection of this specification should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of rights of this specification.
Claims
1. A silicon-carbon composite comprising silicon particles and a porous carbon structure, The above silicon particles exist in an amorphous or mixed state of amorphous and crystalline, The average crystal grain size of the above crystalline silicon particles is 10 nm or less, The above porous carbon structure includes micropores, mesopores and macropores, Based on the total pore volume of 100 vol% of the above porous carbon structure, the micropores are contained at 10 to 30 vol%, the mesopores are contained at 20 to 40 vol%, and the macropores are contained at 40 to 60 vol%. Silicon-carbon composite.
2. In paragraph 1, The total porosity of the above porous carbon structure is 0.6 to 1.5 cm 3 / g person, Silicon-carbon composite.
3. In paragraph 1, The specific surface area of the above porous carbon structure is 200 to 1,000 m 2 / g person, Silicon-carbon composite.
4. In paragraph 1, The average particle size of the above silicon particles is 1 to 100 nm, The average particle size of the above silicon-carbon composite particles is 4 to 8 μm. Silicon-carbon composite.
5. In paragraph 1, The above porous carbon structure is formed of carbon black or a mixture of carbon black and a binder. Silicon-carbon composite.
6. In paragraph 5, The above binder comprises at least one of phenolic resin, coal tar pitch, and polyacrylonitrile. Silicon-carbon composite.
7. In paragraph 5, In the case of a mixture of the above carbon black and binder, When the total weight of the above mixture is 100 wt%, the carbon black is included in a ratio of 40 to 70 wt%, and the binder is included in a ratio of 30 to 60 wt%. Silicon-carbon composite.
8. In paragraph 1, A coating layer is formed on the surface of the above silicon-carbon composite using a carbon-based coating material. Silicon-carbon composite.
9. In paragraph 1, When the total weight of the above silicon-carbon composite is 100 wt%, the content of silicon particles included in the silicon-carbon composite is 40 to 80 wt%. Silicon-carbon composite.
10. In paragraph 1, Satisfying that the span value of the following equation 1 is 0.8 to 1.2, Silicon-carbon composite. <Formula 1> Span = (D 90 -D 10 ) / D 50 11. A negative electrode material for a secondary battery, comprising a silicon-carbon composite according to any one of claims 1 to 10.
12. A method for producing a silicon-carbon composite according to any one of claims 1 to 10, (a) a step of placing a porous carbon structure in a chemical vapor deposition (CVD) reactor; (b) a step of supplying silicon source gas to a chemical vapor deposition (CVD) reactor and reacting under atmospheric pressure and a temperature of 400°C to 550°C to chemically vapor deposit silicon particles on the porous carbon structure; and (c) a step of precipitating the result of (b) above as a solid to obtain a silicon-carbon composite; including; Method for producing a silicon-carbon composite.
13. In paragraph 12, The above step (a) is performed under a carrier gas atmosphere, The carrier gas comprises at least one of nitrogen gas and argon gas. Method for producing a silicon-carbon composite.
14. In paragraph 12, In the above step (a), additional hydrogen (H2) gas is added. Method for producing a silicon-carbon composite.
15. In paragraph 12, The above silicon source gas includes at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, and trimethylsilane (SiH(CH3)3) gas. Method for producing a silicon-carbon composite.
16. In paragraph 12, After the step (c), further comprising the step (d) of forming a coating layer with a carbon-based coating material on the surface of the obtained silicon-carbon composite; Method for producing a silicon-carbon composite.
17. In paragraph 16, The above step (d) is performed by any one of coating by chemical vapor deposition (CVD), coating by solution infiltration followed by solvent evaporation, coating by solution infiltration followed by solvent evaporation and annealing, coating by sol-gel, coating by vapor infiltration, coating by molten infiltration, and coating by atomic deposition. Method for producing a silicon-carbon composite.
18. In paragraph 17, The above step (d) is a method of forming a carbon coating layer by chemical vapor deposition (CVD) using a carbon source gas including at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, and ethylene gas. Method for producing a silicon-carbon composite.
Citation Information
Patent Citations
Amorphous silicon-carbon composite material, preparation method and application thereof, and lithium ion secondary battery
CN115995542A
Hologram-based direct retinal projection-type augmented reality device for expanding FoV by replicating FoV
KR1020230167579A
.
KR102556283B1
Method of depositing silicon on carbon materials and forming an anode for use in lithium ion batteries
US20140349186A1
Anode active material for lithium secondary battery and method for producing same
WO2017052281A1
Cited By
Nano silicon-carbon composite material as well as preparation method and application thereof