Silicon-carbon composite for secondary battery negative electrode material, and method for preparing same

A silicon-carbon composite with amorphous silicon particles and a carbon coating, produced via homogeneous reaction, addresses the volume expansion issue in silicon-based anodes, enhancing the performance and lifespan of secondary batteries by achieving efficient particle size and sphericity.

WO2024232580A1PCT designated stage expired Publication Date: 2024-11-14OCI CO LTD(KR)
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005838
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-26
Filing Date
2024-04-30
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Silicon-based anode materials for secondary batteries face significant volume expansion during charging and discharging, leading to structural deformation, reduced cycle life, and decreased performance due to limitations in particle size and manufacturing complexity in existing silicon-carbon composite production methods.

Method used

A silicon-carbon composite is developed with amorphous silicon particles of 10 nm or less and a carbon-based amorphous coating layer, produced through a homogeneous reaction without a substrate, achieving a particle size of 1 μm to 10 μm and high sphericity, which minimizes volume expansion and enhances performance.

Benefits of technology

The silicon-carbon composite improves initial discharge capacity, efficiency, and lifespan of secondary batteries by reducing structural deformation and maintaining high sphericity, thus addressing the limitations of existing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005838_14112024_PF_FP_ABST
    Figure KR2024005838_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a silicon-carbon composite for a negative electrode material of a secondary battery and a method for manufacturing same and, more specifically, to a silicon-carbon composite for a negative electrode material of a secondary battery and a method for efficiently manufacturing the same, wherein when applied as a negative electrode material, the silicon-carbon composite for a negative electrode material of a secondary battery is capable of improving characteristics of a secondary battery by minimizing a volume change of silicon particles during charging and discharging processes of a secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon-carbon composite for secondary battery anode material and method for manufacturing the same

[0001] The present invention relates to a silicon-carbon composite for use as a negative electrode material for a secondary battery and a method for producing the same, and more specifically, to a silicon-carbon composite for use as a negative electrode material for a secondary battery, which can improve the characteristics of a secondary battery when applied as a negative electrode material by minimizing changes in the volume of silicon particles during the charge / discharge process of a secondary battery, and a method for efficiently producing the same.

[0002] The performance of secondary batteries is based on the components of the cathode, anode, and electrolyte. Among these components, graphite-based materials, primarily used as anode materials, are commercially available due to their excellent electrochemical performance and low cost. However, their theoretical capacity is limited to 370 mAh / g, limiting their application to high-capacity secondary batteries.

[0003] To overcome the above limitations, non-graphite anode materials such as silicon, tin, and germanium are emerging as alternatives. Among them, silicon has a theoretical capacity of 4,000–4,200 mAh / g, can store a very large amount of lithium per unit weight, and exhibits a high capacity of nearly 10 times that of graphite, so it is attracting attention as a material to replace graphite. However, compared to its high theoretical capacity, it has limitations in that it experiences a large volume expansion of approximately 400% during the charge and discharge process, which causes problems such as destruction and pulverization of silicon particles, and reduced electronic conductivity with carbon additives and current collectors, ultimately leading to capacity loss and reduced cycle life of secondary batteries.

[0004] One way to solve this problem is a silicon-carbon composite that can suppress the volume expansion of silicon particles with a carbon-based material. By minimizing the size of the silicon particles within the composite, the structural deformation of the silicon particles between charge and discharge can be fundamentally suppressed, leading to additional performance improvements, thereby enabling the implementation of high-performance anode materials.

[0005] The method for manufacturing silicon-carbon composites is mainly to crush silicon to form silicon nanoparticles and then composite them with carbon-based materials to obtain ideal particle sizes of 1 ㎛ to 10 ㎛ (D 50 ) includes the process of making it have.

[0006] However, this method requires a complex manufacturing process and has the disadvantage of a particle size limit of 100 nm for pulverizing silicon particles. To produce silicon particles below the pulverization limit of 100 nm, the composite must be manufactured using chemical vapor deposition (CVD).

[0007] Looking at the conventional techniques for manufacturing silicon-carbon composites using the above chemical vapor deposition method, the composite particle size (D) is 1 ㎛ to 10 ㎛. 50 ) are mainly manufactured by heterogeneous reaction using a deposition substrate.

[0008] Specifically, Korean Patent Publication No. 10-2021-0071246 (“Prior Art Document 1”) and Korean Patent Publication No. 10-2020-0023870 (“Prior Art Document 2”) disclose a method of depositing a silicon layer on a base material having a size of 1 to 10 μm and using the silicon layer together with the base material as a negative electrode active material.

[0009] In addition, Korean Patent Publication No. 10-2022-0087143 (“Prior Art Document 3”) discloses a process of depositing a composite in the form of a film on a large matrix surface and then performing an additional grinding process to obtain the corresponding particle size.

[0010] The techniques disclosed in prior art documents 1 and 2 have the disadvantage of requiring complexity in that process conditions differ for each base material because the surface characteristics differ depending on the type of base material.

[0011] In the case of the technology disclosed in prior art document 3, since a grinding process is absolutely necessary, there is a high possibility that impurities will be mixed in, and since the sphericity of the final composite is low, when applied as an anode material in a secondary battery, it may cause the formation of an excessive SEI (solid-electrolyte interphase) layer, which may lead to a decrease in the performance of the secondary battery, which has limitations.

[0012] Therefore, in order to realize a negative electrode material (negative electrode active material) with high capacity retention, it is still necessary to develop a silicon-carbon composite that can suppress structural deformation of silicon particles during charge and discharge of a secondary battery and the technology to manufacture it.

[0013] [Prior Art Literature]

[0014] (Patent Document 1) Prior Art Document 1: Korean Patent Publication No. 10-2021-0071246

[0015] (Patent Document 2) Prior Art Document 2: Korean Patent Publication No. 10-2020-0023870

[0016] (Patent Document 3) Prior Art Document 3: Korean Patent Publication No. 10-2022-0087143

[0017] The purpose of the present invention is to provide a silicon-carbon composite for use as a negative electrode material of a secondary battery, which can improve the initial discharge capacity, initial efficiency, and lifespan characteristics of a secondary battery when applied as a negative electrode material of a secondary battery.

[0018] Another object of the present invention is to provide a method for efficiently manufacturing a silicon-carbon composite having excellent sphericity without using a substrate, unlike conventional manufacturing methods, in manufacturing a silicon-carbon composite for a secondary battery negative electrode material having the above-described excellent properties.

[0019] Another object of the present invention is to produce a silicon-carbon composite for use as a secondary battery negative electrode material having the above-described excellent properties, wherein the crystallite size of the silicon particles is 10 nm or less without a separate pulverization process, and the D of the silicon-carbon composite 50 A method for efficiently manufacturing a silicon-carbon composite having a particle size of 1 ㎛ to 10 ㎛ is provided.

[0020] The objectives of the present invention are not limited to those mentioned above. Other objectives and advantages of the present invention not mentioned above can be understood through the following description and will be more clearly understood through the embodiments of the present invention. Furthermore, it will be readily apparent that the objectives and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims.

[0021] In order to achieve the above purpose, according to the first aspect of the present invention, a silicon-carbon composite including silicon particles and a carbon material is provided.

[0022] The above silicon particles are amorphous silicon particles having an average crystallite size of 10 nm or less,

[0023] D of the above silicon-carbon composite 50 The value is 1 ㎛ to 10 ㎛, and the sphericity is 0.7 or more.

[0024] A silicon-carbon composite can be provided.

[0025] The sphericity of the above silicon-carbon composite may be 0.9 or more.

[0026] A carbon-based amorphous coating layer formed of a carbon-based coating material may be formed on the surface of the above silicon-carbon composite.

[0027] The above carbon-based coating material may include at least one selected from the group consisting of petroleum-based pitch, ethylene, acetylene, methane, ethane, epoxy resin, polyphenol, polyaniline, polyvinyl alcohol, polyvinyl chloride, and other cross-linked polymers.

[0028] Based on the total weight of the silicon-carbon composite, the silicon particles may comprise 55 to 70 wt%, and the carbon material may comprise 30 to 45 wt%.

[0029] According to a second aspect of the present invention, a negative electrode material for a secondary battery can be provided, comprising a silicon-carbon composite according to the first aspect of the present invention.

[0030] According to the third aspect of the present invention,

[0031] (S1) A step of heating a rotary kiln to a temperature of 400°C to 650°C while purging it with an inert gas; and

[0032] (S2) A step of simultaneously injecting silicon source gas and carbon source gas into the rotary kiln, performing a homogeneous reaction under atmospheric pressure conditions, and co-deposition of silicon and carbon to obtain a silicon-carbon composite;

[0033] The silicon-carbon composite obtained above comprises silicon particles and carbon materials,

[0034] The average crystallite size of the above silicon particles is 10 nm or less,

[0035] D of the above silicon-carbon composite 50 A method for producing a silicon-carbon composite having a particle size of 1 μm to 10 μm and a sphericity of 0.7 or more can be provided.

[0036] The above inert gas may include at least one of nitrogen gas and argon gas.

[0037] The above rotary kiln may be a chemical vapor deposition (CVD) reactor equipped with a rotary baffle.

[0038] The above silicon source gas may include at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, tetrachlorosilane (SiCl4) gas, and trimethylsilane (SiH(CH3)3) gas.

[0039] The above carbon source gas may include at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, ethylene gas, and acetylene gas.

[0040] The sphericity of the above silicon-carbon composite may be 0.9 or more.

[0041] In the above step (S2), the silicon-carbon composite can be obtained as a solid powder by cooling to room temperature of 15°C to 25°C.

[0042] After the reaction of (S2) is completed, a step of (S3) injecting a carbon-based source gas and an inert gas for a coating material to form a carbon-based amorphous coating layer on the result obtained in (S2) to obtain a final silicon-carbon composite may be further included.

[0043] The above step (S3) can be performed by chemical vapor deposition.

[0044] The above carbon-based source gas may be one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, ethylene gas, and propylene gas.

[0045] The present invention can provide a silicon-carbon composite including silicon particles whose particle size is adjusted to a condition that can prevent silicon cracking and minimize volume expansion even during charging and discharging of a secondary battery, and an anode material for a secondary battery including the same.

[0046] Due to the excellent properties of the silicon-carbon composite of the present invention, the initial discharge capacity, initial efficiency, and life characteristics of a secondary battery manufactured by including the composite as a negative electrode material can be improved.

[0047] The present invention can provide a method for manufacturing the silicon-carbon composite through a homogenous reaction without a substrate, and can efficiently manufacture a silicon-carbon composite having a high sphericity of 0.7 or more.

[0048] The present invention provides a silicon particle having a crystallite size of 10 nm or less without a separate grinding process, and D 50 A method for producing a silicon-carbon composite having a value of 1 ㎛ to 10 ㎛ can be provided.

[0049] In addition to the effects described above, the effects of the present invention are described together with the description of matters for carrying out the invention below.

[0050] Figure 1 briefly illustrates one embodiment of a method for manufacturing a silicon-carbon composite of the present invention.

[0051] Figure 2 briefly illustrates another embodiment of a method for manufacturing a silicon-carbon composite of the present invention.

[0052] Figure 3 is a SEM image for observing particles of a silicon-carbon composite in the cross-section of the electrode plate of Example 1 of the present invention.

[0053] Figure 4 is a SEM image for observing particles of a silicon-carbon composite in the cross-section of the electrode plate of Comparative Example 1 of the present invention.

[0054] Figure 5 is an analysis graph for calculating the silicon crystallite size through X-ray diffraction analysis of the silicon-carbon composite obtained in Example 1 of the present invention.

[0055] The aforementioned purposes, features, and advantages are described in detail below with reference to the drawings, so that those skilled in the art can easily implement the technical concepts of the present invention. In describing the present invention, if a detailed description of known technologies related to the present invention is deemed to unnecessarily obscure the gist of the present invention, a detailed description thereof will be omitted.

[0056] In this specification, when the terms "includes," "has," "consists of," "arranges," and "provides" are used for a component, other parts may be added, unless "only" is used. When a component is expressed in the singular, it includes the plural unless otherwise explicitly stated.

[0057] In this specification, "crystallite" refers to "crystal grains" or "crystallite", which means "a region of material in which atoms are arranged in an ordered and repeating pattern."

[0058] In this specification, “crystallite size” is measured through XRD (equipment name: panalytical - x'pert pro) analysis, and the crystallite size automatically derived through the Scherer equation for XRD data measured by the equipment is used.

[0059] In the present invention, "D 50 The "value" measurement is a particle size analyzer (PSA) method, which calculates the particle size through the scattering angle distribution of light scattered while passing through the powder sample of the sample to be measured, and the measuring equipment used was LS 13 320 Particle Size Analyzer (Beckman Coulter). Here, D50 The value refers to the particle size (size) value that accounts for 50% of the distribution of the entire powder in descending order of particle size (size).

[0060] In the present invention, in the case of "sphericity", the external appearance image of the particle is analyzed through a microscope (SEM, JSM-7100F and OM), the horizontal axis and vertical axis are designated to intersect at 90° from the center of the silicon particle, and the value is converted into a percentage of the length of the vertical axis relative to the length of the horizontal axis within the particle.

[0061] In interpreting the components in this specification, even if there is no separate explicit description, it is interpreted to include the range of error.

[0062]

[0063] Hereinafter, the present invention will be described in more detail.

[0064] silicon-carbon composites

[0065] The silicon-carbon composite of the present invention is a silicon-carbon composite including silicon particles and a carbon material, wherein the silicon particles are amorphous silicon particles having an average crystallite size of 10 nm or less, and the average particle diameter of the silicon-carbon composite may be 1 ㎛ to 10 ㎛, and the sphericity may be 0.7 or more, preferably the sphericity may be 0.8 or more, and most preferably the sphericity may be 0.9 or more.

[0066] D of the silicon-carbon composite of the present invention 50 It is desirable that the value be in the range of 1 ㎛ to 10 ㎛. D 50 If the value exceeds 10 ㎛, a separate process may be required to control the particle size through an additional spheroidization process or a grinding process. If a separate grinding process is performed, not only will inefficiency occur in the process, but the purity of the silicon particles may also decrease due to the introduction of impurities during the grinding process.

[0067] Also, D 50If the value is less than 1 ㎛, it is not uniformly mixed and dispersed when manufactured as a negative electrode material slurry due to low stability and dispersibility, and thus, when applied as a negative electrode material of a secondary battery, it may lower the performance of the secondary battery.

[0068] The silicon particles included in the silicon-carbon composite of the present invention may be amorphous silicon particles having an average crystallite size of 10 nm or less, preferably 1 to 5 nm, and more preferably 1 to 3 nm.

[0069] If the average crystallite size of the silicon particles exceeds 10 nm, there may be a problem of degrading during the charge / discharge cycle of the secondary battery when applied as an anode material of a secondary battery, thereby reducing the lifespan. Therefore, it is desirable to control the average crystallite size to 10 nm or less.

[0070] The silicon-carbon composite of the present invention has a sphericity of 0.7 or more, preferably 0.8 or more, and most preferably 0.9 or more. When a non-spherical silicon-carbon composite is used as an anode material for a secondary battery, there is a problem in that dispersibility is low and side reactions are likely to occur during the charge and discharge process of the secondary battery, which ultimately reduces the performance of the secondary battery. In addition, if the sphericity is less than 0.7, the surface area per unit mass increases, which may have the disadvantage of forming an unstable SEI layer (Solid Electrolyte Interphase Layer).

[0071] The silicon-carbon composite of the present invention can be formed by co-deposition without a separate substrate, and is advantageous in achieving high sphericity because there is no separate pulverization process.

[0072] According to one embodiment of the present invention, a carbon-based amorphous coating layer can be formed on the surface of the silicon-carbon composite using a carbon-based coating material, if necessary. Forming the coating layer in this way can more effectively protect silicon exposed to the outside of the silicon-carbon composite, improve the particle strength of the silicon-carbon composite, and increase electrical conductivity, thereby allowing for the control of the physical properties required for the silicon-carbon composite.

[0073] According to one embodiment of the present invention, the carbon-based coating material for forming the carbon-based amorphous coating layer may include, for example, one or more selected from the group consisting of petroleum pitch, ethylene, acetylene, methane, ethane, epoxy resin, polyphenol, polyaniline, polyvinyl alcohol, polyvinyl chloride, and other cross-linked polymers.

[0074] The thickness of the coating layer can be adjusted depending on the size of the silicon-carbon composite, and can be, for example, about 1 nm to 50 nm, for example, about 1 nm to 30 nm, for example, about 1 nm to 20 nm, for example, about 1 nm to 10 nm, for example, about 1 nm to 5 nm, but is not necessarily limited thereto.

[0075] Method for manufacturing silicon-carbon composites

[0076] In the present invention, unlike conventional techniques, a method for manufacturing a silicon-carbon composite without a substrate is devised, and the manufactured silicon-carbon composite can satisfy the characteristics of the silicon-carbon composite of the present invention described above.

[0077] Referring to FIG. 1, the method for manufacturing a silicon-carbon composite according to the present invention may include the following steps (S1) and (S2).

[0078] (S1) A step of heating a rotary kiln to a temperature of 400°C to 650°C while purging it with an inert gas; and

[0079] (S2) A step of simultaneously introducing silicon source gas and carbon source gas into the rotary kiln, performing a homogeneous reaction under atmospheric pressure conditions, and co-deposition of silicon and carbon to obtain a silicon-carbon composite.

[0080] The silicon-carbon composite obtained by the above manufacturing method comprises silicon particles and a carbon material, the average crystallite size of the silicon particles is 10 nm or less, and the D of the silicon-carbon composite 50 The value is 1 ㎛ to 10 ㎛, and the sphericity may be 0.7 or more, preferably 0.8 or more, and more preferably 0.9 or more.

[0081] As the homogeneous reaction proceeds as described above, silicon and carbon source gases can form a silicon-carbon complex through homogeneous reaction deposition (co-precipitation), and the turbulence generated inside the reaction device allows the silicon-carbon complex to grow.

[0082] In addition, in the present invention, the rotary kiln of step (S1) is a chemical vapor deposition reactor, and a rotary chemical vapor deposition reactor with a baffle added for uniform reactivity and prevention of agglomeration can be used, and thereby, by appropriately controlling the flow rates of silicon source gas and carbon source gas and the rotation speed of the kiln, the final particle size (D) of the silicon-carbon composite produced by the homogeneous reaction can be 50 ) and sphericity can be controlled, and once it has the ideal particle size and sphericity, it can be used as a cathode material without any additional processes.

[0083] The above step (S1) may be performed by sufficiently purging with an inert gas and then heating at a heating rate of, for example, 15°C / min until the target temperature of 400°C to 650°C is reached. Purging with an inert gas in this way is intended to control the overall reaction rate and obtain a uniform homogeneous reaction product, and the inert gas may include at least one of nitrogen gas and argon gas, but is not necessarily limited thereto.

[0084] The temperature conditions of the above step (S1) are for performing a homogeneous reaction, and may be, for example, 400°C to 650°C, or, for example, 420°C to 500°C.

[0085] When the target temperature is reached in the above step (S1), in step (S2), the silicon source gas and the carbon source gas may be simultaneously injected at a flow rate of 100 to 200 ml / min and a flow rate of 10 to 30 ml / min, respectively, and a homogeneous reaction may be performed for 30 minutes to 3 hours under atmospheric pressure conditions. For example, the silicon source gas may be injected at a flow rate of 125 ml / min and the carbon source gas may be injected at a flow rate of 25 ml / min, but the present invention is not limited thereto.

[0086] According to one embodiment of the present invention, the silicon source gas may include at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, tetrachlorosilane (SiCl4) gas, and trimethylsilane (SiH(CH3)3) gas, but is not necessarily limited thereto.

[0087] According to one embodiment of the present invention, the carbon source gas may include at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, ethylene gas, and acetylene gas, but is not necessarily limited thereto.

[0088] After the homogeneous reaction is completed in the above step (S2), the particles of the grown silicon-carbon composite are collected so that they can be recovered as a solid powder by cooling to room temperature of 15°C to 25°C. As a method for the collection, a method of moving the particles using a fluid such as air as a medium can be used, and for example, collection can be performed using a bag filter.

[0089] Referring to FIG. 2 according to one embodiment of the present invention, after the step (S2), the step (S3) may further include a step of forming a carbon-based amorphous coating layer on the result obtained in (S2) by injecting a carbon-based source gas and an inert gas for the coating material to obtain a final silicon-carbon composite.

[0090] For example, the carbon-based source gas and inert gas for the coating material can be reacted for 10 minutes to 2 hours while being injected at a flow rate of 20 ml / min to 80 ml / min and a flow rate of 300 ml / min to 600 ml / min, respectively, and for example, the carbon-based source gas and inert gas for the coating material can be reacted for 30 minutes while being injected at a flow rate of 50 ml / min and a flow rate of 450 ml / min, respectively, but the present invention is not limited thereto.

[0091] The above carbon-based amorphous coating layer is the same as that described with respect to the coating layer formed with a carbon-based coating material for coating formed on the surface of the silicon-carbon composite of the present invention.

[0092] At this time, the carbon-based source gas for forming the carbon-based coating layer for coating may be the same as or different from the carbon-based source gas used in the step (S2), and may be, for example, one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, ethylene gas, and propylene gas.

[0093] According to one embodiment of the present invention, the step (S3) may be performed by chemical vapor deposition (CVD), but is not necessarily limited thereto.

[0094] Hereinafter, the present invention will be described in more detail by way of examples. However, the following examples are merely illustrative of the present invention, and the scope of the present invention is not limited to the following examples.

[0095] [Manufacturing example]

[0096] Example 1

[0097] A rotary kiln sufficiently purged with argon (Ar) gas was heated to 450°C at a heating rate of 15°C / min, and then monosilane gas (SiH4) and ethylene (C2H4) gases were simultaneously introduced at flow rates of 125 ml / min and 25 ml / min, respectively, while maintaining the rotation speed of the reactor at 1.0 rpm. The reaction was performed for 2 hours under atmospheric pressure conditions to produce silicon-carbon composite particles. At the same temperature, ethylene (C2H4) gas and argon (Ar) gas, which are carbon source gases for coating, were introduced at flow rates of 50 ml / min and 450 ml / min, respectively, and the reaction was performed for an additional 30 minutes to form a carbon-based amorphous coating layer on the surface of the composite. After the above reaction was completed, the inside of the kiln was replaced with argon and cooled to ambient temperature to obtain the final silicon-carbon composite.

[0098] Comparative Example 1

[0099] A rotary kiln sufficiently purged with argon (Ar) gas was heated to 450°C at a heating rate of 15°C / min, and then monosilane (SiH4) gas and ethylene (C2H4) gas were simultaneously introduced at flow rates of 125 ml / min and 25 ml / min, respectively, toward a graphite plate, which is a base material deposition plate. After a reaction under atmospheric pressure for 2 hours, a silicon-carbon composite mass widely deposited on the base material plate was obtained. After the reaction was completed, the rotary kiln was replaced with argon gas and cooled to room temperature to recover the silicon-carbon composite mass. The silicon-carbon composite mass was processed to have a particle size similar to that of Example 1 through a pulverization process.

[0100] 5 g of the above-mentioned pulverized silicon-carbon composite particles were placed in a rotary kiln and heated to 450°C at a heating rate of 15°C / min. Then, ethylene (C2H4) gas and argon (Ar) gas were introduced at flow rates of 50 ml / min and 450 ml / min, respectively, and reacted for an additional 30 minutes to form a carbon coating layer on the surface of the silicon-carbon composite.

[0101] After the above reactions were completed, the inside of the furnace was replaced with argon and cooled to ambient temperature to obtain the final silicon-carbon composite.

[0102] Comparative Example 2

[0103] The same procedure as Example 1 was followed, except that the input flow rates of monosilane gas (SiH4) and ethylene (C2H4) gas were adjusted to 75 ml / min and 75 ml / min, respectively.

[0104] [Experimental Example]

[0105] Particle property measurements

[0106] D of the silicon-carbon composites manufactured in Example 1, Comparative Example 1 and Comparative Example 2 50 , the crystallite size and sphericity of silicon were measured and shown in Table 1 below.

[0107] Cross-sectional SEM images of the silicon carbon particles of the silicon-carbon composite manufactured in Example 1 and Comparative Example 1 are shown in FIGS. 3 and 4, respectively.

[0108] The XRD analysis graph of the silicon-carbon composite of Example 1 is shown in Fig. 5.

[0109] For silicon, the crystallite size is determined by observing the peak at the point where 2θ(theta) [unit: degree (°)] is 28° in the XRD analysis graph. In addition, if there is no peak in the XRD analysis graph, the measurement subject is judged to be amorphous, and if the peak is broadly distributed, the measurement subject is interpreted as a mixture of amorphous and crystalline forms.

[0110] Looking at Fig. 5, the silicon-carbon composite manufactured in Example 1 has a widely distributed peak at a point where 2θ is 28°, so it can be seen that amorphous silicon particles and crystalline silicon particles are mixed. Using XRD analysis data, the average crystallite size of the crystalline silicon particles calculated according to the Scherrer equation using [Highscore plus], a program within the XRD analysis equipment, was 1.6 nm.

[0111] The vertical axis “count” in Fig. 5 represents the signal that is generated when X-rays are incident on the sample and enter the detector, and is the same as the intensity of typical XRD analysis data.

[0112] The horizontal axis of Fig. 5, “Copper (Cu)”, refers to a source that generates X-ray radiation, and specifically, it refers to ‘XRD (X-ray diffraction) pattern obtained with Cu-K α radiation.’

[0113] Cathode slurry manufacturing

[0114] The silicon-carbon composite and artificial graphite (average particle size = 14 μm) manufactured in the above manufacturing example were mixed at a weight ratio of 20:80 to manufacture a negative electrode material.

[0115] The above-mentioned manufactured negative electrode material, conductive material (Super P: SWCNT = 9:1, weight ratio) and binder (CMC: SBR = 3:7, weight ratio) were mixed using a sinky mixer at a weight ratio of negative electrode material: conductive material: binder = 80:10:10 to obtain a negative electrode slurry.

[0116] cell test

[0117] The above-mentioned negative electrode slurry was applied to a copper foil having a thickness of 18 μm, dried in an oven at 80°C for 1 hour, and then heat-treated in a vacuum oven at 100°C for 12 hours to manufacture a negative electrode plate. The plate was punched to 16 mmΦ, and a coin cell using Li metal as a counter electrode was manufactured to confirm the electrochemical characteristics.

[0118] The charge / discharge conditions were charge CC / CV: 0.005 V / 0.005 C, discharge CC 1.5 V, and a rate of 0.1 C. The initial discharge capacity (IDC) and initial efficiency (ICE) measured using the TOSCAT-3100 half-cell device are shown in Table 1 below.

[0119] D 50 (㎛)Si crystallite size (nm)SphericityInitial discharge capacity (mAh / g)Initial efficiency (%)Example 15.421.60.91454589.0Comparative example 15.191.60.66554883.3Comparative example 20.421.60.92754756.9

[0120] As can be seen in Table 1 above, Example 1 produced a silicon-carbon composite by co-precipitation without a parent material, and thus was able to achieve a high sphericity of 0.914, and a smooth spherical particle surface was also observed in the SEM image of Fig. 3.

[0121] On the other hand, Comparative Example 1 was manufactured as a silicon-carbon composite by depositing using a base material and going through a pulverization process, so it can be seen that the sphericity is very low at 0.665, and this can be confirmed with the naked eye in the SEM image of Fig. 4 that the surface of the particle is uneven.

[0122] Comparative Example 2: D of silicon carbon composite 50 In this invention, the limit of 1㎛ or more was not satisfied, and accordingly, it was difficult to manufacture a uniform slurry because it was not well dispersed during slurry work, and as a result, the initial efficiency was very low in the coin cell test.

[0123]

[0124] This specification is not necessarily limited to these embodiments, and various modifications may be implemented without departing from the technical spirit of this specification. Therefore, the embodiments disclosed in this specification are not intended to limit the technical spirit of this specification, but to specifically explain it, and the scope of the technical spirit of this specification is not limited by these embodiments. Therefore, it should be understood that the embodiments described above are illustrative in all respects and not restrictive. The scope of protection of this specification should be interpreted by the claims, and all technical ideas within a scope equivalent thereto should be interpreted as being included in the scope of rights of this specification.

Claims

1. A silicon-carbon composite comprising silicon particles and carbon materials, The above silicon particles are amorphous silicon particles having an average crystallite size of 10 nm or less, The sphericity of the above silicon-carbon composite is 0.7 or more, Silicon-carbon composite.

2. In paragraph 1, The sphericity of the above silicon-carbon composite is 0.9 or more, Silicon-carbon composite.

3. In paragraph 1, A carbon-based amorphous coating layer formed of a carbon-based coating material is formed on the surface of the above silicon-carbon composite. Silicon-carbon composite.

4. In paragraph 1, The above carbon-based coating material comprises at least one selected from the group consisting of petroleum-based pitch, ethylene, acetylene, methane, ethane, epoxy resin, polyphenol, polyaniline, polyvinyl alcohol, polyvinyl chloride and other cross-linked polymers. Silicon-carbon composite.

5. In paragraph 1, Based on the total weight of the silicon-carbon composite, the silicon particles comprise 55 to 70 wt% and the carbon material comprises 30 to 45 wt%. Silicon-carbon composite.

6. A negative electrode material for a secondary battery, comprising a silicon-carbon composite according to any one of claims 1 to 5. 7.(S1) A step of heating the rotary kiln to a temperature of 400°C to 650°C while purging it with an inert gas; and (S2) A step of simultaneously injecting silicon source gas and carbon source gas into the rotary kiln, performing a homogeneous reaction under atmospheric pressure conditions, and co-deposition of silicon and carbon to obtain a silicon-carbon composite; The silicon-carbon composite obtained above comprises silicon particles and carbon materials, The average crystallite size of the above silicon particles is 10 nm or less, D of the above silicon-carbon composite 50 The value is 1 ㎛ to 10 ㎛, and the sphericity is 0.7 or more. Method for producing a silicon-carbon composite.

8. In paragraph 7, The above inert gas includes at least one of nitrogen gas and argon gas. Method for producing a silicon-carbon composite.

9. In paragraph 7, The above rotary kiln is a chemical vapor deposition (CVD) reactor equipped with a rotary baffle. Method for producing a silicon-carbon composite.

10. In paragraph 7, The above silicon source gas includes at least one selected from the group consisting of monosilane (SiH4) gas, disilane (Si2H6) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, trichlorosilane (SiHCl3) gas, tetrachlorosilane (SiCl4) gas, and trimethylsilane (SiH(CH3)3) gas. Method for producing a silicon-carbon composite.

11. In paragraph 7, The above carbon source gas comprises at least one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, ethylene gas and acetylene gas. Method for producing a silicon-carbon composite.

12. In paragraph 7, The sphericity of the above silicon-carbon composite is 0.9 or more, Method for producing a silicon-carbon composite.

13. In paragraph 7, A method for producing a silicon-carbon composite, wherein the silicon-carbon composite is cooled to a room temperature of 15°C to 25°C in the above step (S2) to obtain a solid powder.

14. In paragraph 7, After completion of the reaction of the above (S2), (S3) a step of forming a carbon-based amorphous coating layer on the result obtained in (S2) by injecting a carbon-based source gas and an inert gas for coating material to obtain a final silicon-carbon composite; further comprising; Method for producing a silicon-carbon composite.

15. In paragraph 14, The above step (S3) is performed by chemical vapor deposition. Method for producing a silicon-carbon composite.

16. In paragraph 14, The above carbon source gas is one selected from the group consisting of methane gas, ethane gas, propane gas, butane gas, acetylene gas, ethylene gas, and propylene gas. Method for producing a silicon-carbon composite.

Citation Information

Patent Citations

  • High performance silicon-based materials for lithium ion battery anodes

    EP3965185A1

  • Composite particles, their production method and uses

    JP7236613B1

  • Lamp control device and lamp system including the same

    KR1020240120181A

  • Waffle manufacturing device and waffle manufactured by the same that

    KR102348534B1

  • KR20200023870A