Weld structure of battery can, current collecting plate, and cap, and battery cell employing same

The integrated welding of the current collector and cap within the battery can's design addresses inefficiencies in existing processes, enhancing energy density and production efficiency by eliminating the need for separate welding masks or jigs, resulting in improved welding performance and reduced costs.

WO2024232643A1PCT designated stage expired Publication Date: 2024-11-14LG ENERGY SOLUTION LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006147
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-11
Filing Date
2024-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The existing manufacturing process of battery cells using cylindrical cans is inefficient due to the need for separate welding masks or jigs, which wastes internal space and increases production costs and assembly time, hindering the increase in energy density and production efficiency.

Method used

A welded structure for the battery can, current collector, and cap is designed to eliminate the need for separate welding masks or jigs, integrating the welding of the current collector to the can and cap into a single process, optimizing internal space and reducing assembly time and costs.

Benefits of technology

This approach enhances welding performance, stability, and durability while reducing assembly man-hours and production costs, allowing for increased energy density and improved manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006147_14112024_PF_FP_ABST
    Figure KR2024006147_14112024_PF_FP_ABST
Patent Text Reader

Abstract

This battery cell comprises: a can having an electrode assembly accommodated therein; and a cap. The can is provided with: a bottom member; and a side wall member that is connected to the bottom member and extends upward from the bottom member in an axial direction. The cap covers an open end of the can, the open end being provided at the opposite end from the bottom member. The current collecting plate is connected, in the vicinity of the open end, to an electrode tab of the electrode assembly. The current collecting plate includes: a central portion electrically connected to the electrode tab; and a circumferential portion in electrical contact with the inner surface of a side wall of the can in the radial direction. The circumferential portion is also in contact with a lower portion of the cap. The radial inner surface of the side wall member, the radial outer surface of the cap, and the circumferential portion of the current collecting plate are all welded to each other.
Need to check novelty before this filing date? Find Prior Art

Description

Welding structure of battery can, collector plate and cap and battery cell using the same

[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0059345, dated May 8, 2023, and Korean Patent Application No. 10-2023-0135319, dated October 11, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention belongs to the field of batteries, and more specifically, relates to a welding structure of a battery can, a current collector plate, and a cap, and a battery cell using the same.

[0003] The process of manufacturing a battery cell using a cylindrical can includes the steps of deep drawing a metal sheet to form a circular bottom member and a circular tubular side wall member connected thereto, accommodating an electrode assembly therein, and then closing the open end of the side wall member by covering it with a cap.

[0004] Meanwhile, at one of the axial ends of the electrode assembly facing the open end, a current collector plate is provided that is in contact with and electrically connected to at least one electrode tab of the electrode assembly. The current collector plate is connected to the cap or the side wall member by welding or the like so as to be in contact with and electrically connected to the cap or the side wall member.

[0005] In the process of welding the current collector plate to the cap or side wall member, the current collector plate may be maintained in close contact with the cap or side wall member. To this end, a jig may be required to close the current collector plate to the cap or the side wall member, and in addition, a mask may be required to expose the welding area.

[0006] In order to adhere the collector plate to the cap or sidewall member through the mask or jig, a space may be provided inside the can to accommodate the mask or jig. However, this space remains empty after the mask or jig is removed, which may result in the can's internal volume not being efficiently utilized. This hinders the design of increasing the energy density per unit volume of the can.

[0007] Additionally, when closing the open end of the cylindrical can, a process of connecting the current collector plate to the cap or the side wall member, and a process of connecting the cap to the side wall member are each performed. This increase in the number of steps required to assemble battery cell components reduces the production efficiency of cylindrical battery cells and increases the production cost.

[0008] The present invention has been devised to solve the above-described problem, and provides a welding structure of a battery can, a current collector, and a cap, which enables a design to increase the energy density per unit volume of the can without wasting or sacrificing the internal space of the can when welding a current collector provided on the open end of the can to the can by omitting a separate welding mask or jig, and a battery cell using the welding structure.

[0009] Additionally or alternatively, the present invention aims to increase the production efficiency and reduce the production cost of cylindrical battery cells by integrating the process of welding the current collector to the can and the process of welding the cap to the side wall member into a single welding process.

[0010] Additionally or alternatively, the present invention seeks to increase the stability of the process by imparting the functions of a mask and a jig to the can, the collector plate, and the cap.

[0011] The present invention seeks to provide a shape of a can, a collector plate, and a cap, and an interlocking relationship thereof, which can secure weldability, increase process stability, and ensure durability of welding.

[0012] The technical tasks of the present invention are not limited to the purposes mentioned above, and other purposes and advantages of the present invention that are not mentioned can be understood by the following description and will be more clearly understood by the embodiments of the present invention.

[0013] According to one aspect of the present invention, a battery cell is provided. The battery cell may include an electrode assembly, a current collector, and a can.

[0014] The can may include a side wall member (side wall) extending along a central longitudinal axis and surrounding the interior volume thereof. The side wall member may define an opening to the interior volume of the can at the first longitudinal end.

[0015] The above electrode assembly can be accommodated in the internal volume of the can.

[0016] The opening of the above can can be closed by a cap.

[0017] The cap may cover the opening of the can so as to surround the internal volume.

[0018] The above current collector plate can be electrically connected to the above electrode assembly.

[0019] The above-mentioned collector plate may include a central portion and a peripheral portion. The peripheral portion is positioned around the central portion and is positioned further away from the longitudinal axis of the center than the central portion.

[0020] The above central portion can be electrically connected to the electrode tab of the electrode assembly.

[0021] The above circumferential portion can be in contact with the radially inner surface of the side wall member so as to be electrically connected to the can.

[0022] The above circumference may be in contact with the bottom surface of the cap. The bottom surface of the cap may be arranged to face the internal volume of the can in the longitudinal direction of the axis.

[0023] The radially inner surface of the side wall member, the radially outer surface of the cap, and the periphery of the collector plate are preferably welded to each other.

[0024] According to one aspect of the above battery cell, the radially inner surface of the side wall member may include a lateral step extending in a direction transverse to the longitudinal direction of the axis.

[0025] A first inner surface of the side wall member located on a first side of the lateral step in the longitudinal direction of the axis may have a first diameter. A second inner surface of the side wall member located on a second side of the lateral step in the longitudinal direction of the axis may have a second diameter. The second side may be arranged closer to the open end of the can than the first side. The second diameter may be larger than the first diameter.

[0026] The radial outer surface of the cap and the peripheral portion of the collector plate can be in contact with the second inner surface.

[0027] According to one aspect of the above battery cell, an outer diameter of a periphery of the current collector plate may be larger than a first diameter of a first inner surface of a side wall member of the can.

[0028] According to one aspect of the above battery cell, the periphery of the current collector plate can be in contact with the lateral step.

[0029] According to another aspect of the battery cell, the lateral step may be defined by a slope extending from a first diameter of the first inner surface to a second diameter of the second inner surface.

[0030] According to another aspect of the battery cell, a first thickness of the cap, measured in the longitudinal direction of the axis along a radially outer surface of the cap, may be thicker than a second thickness of the side wall member, measured in a radial direction perpendicular to the longitudinal direction of the axis along a second inner surface of the side wall member.

[0031] In an additional embodiment, the first thickness may be one to two times thicker than the second thickness.

[0032] According to one aspect of the above battery cell, the diameter of the radially outer surface of the cap may be smaller than the diameter of an adjacent portion of the radially inner surface of the side wall member adjacent thereto. In addition, the welding area may extend from the adjacent portion of the radially inner surface of the side wall member to the radially outer surface of the cap.

[0033] According to one aspect of the above battery cell, the cap may include an annular region extending along the radially outer surface. In addition, the thickness of the annular region of the cap along the longitudinal direction of the axis may be thinner than the thickness of the central region of the cap located along the longitudinal direction of the central axis.

[0034] In one embodiment, an inclined surface along the bottom of the cap may connect the annular region and the central region.

[0035] In one embodiment, the inclined surface may be in contact with the collector plate.

[0036] According to one aspect of the battery cell, the collector plate may include an axial step between the central portion and the peripheral portion, such that the peripheral portion may be offset toward the open end of the can relative to the central portion.

[0037] According to one aspect of the above battery cell, the longitudinal dimension of the central portion of the current collector plate may extend in a direction transverse to the axial direction, and the longitudinal dimension of the peripheral portion of the current collector plate may extend parallel to the axial direction. In this way, the peripheral portion may extend along the radially inner surface of the side wall member of the can to a distal end of the peripheral portion, wherein the distal end is in contact with the bottom surface of the cap.

[0038] According to another aspect of the present invention, a method for manufacturing a battery cell is provided.

[0039] The method may include the step of positioning the cap and the collector plate in an assembled position, one above the other, within the opening of the can. In this assembled position, the collector plate may be electrically connected to an electrode assembly housed within the interior volume of the can.

[0040] Additionally, in this assembly position, the periphery of the collector plate can be in contact with the radially inner surface of the side wall member surrounding the opening of the can.

[0041] Additionally, in this assembly position, the cap may be positioned on the current collector plate along the longitudinal direction of the central axis of the can. The cap may be positioned further away from the electrode assembly than the current collector plate.

[0042] Preferably, the method also includes the step of welding the radially inner surface of the side wall member, the radially outer surface of the cap, and the periphery of the collector plate to each other.

[0043] According to one aspect of this method, positioning the cap and the collector plate at the assembly position may include bringing the peripheral portion of the collector plate into contact with a lateral step defined on a radially inner surface of the side wall member of the can.

[0044] According to one aspect of the method, positioning the cap and the collector plate in the assembly position may include contacting an inclined surface positioned along the bottom surface of the cap with an annular portion of the collector plate extending along the periphery.

[0045] According to one aspect of this method, the step of welding the radially inner surface of the side wall member of the can may include the step of melting the material of the extension portion of the side wall member that protrudes above the cap along an axial direction extending parallel to the longitudinal direction of the central axis. As a result, the material of the extension portion can flow between the radially inner surface of the side wall and the radially outer surface of the cap to join them.

[0046] According to one aspect of the method, the step of welding the radially inner surface of the side wall member may include tack welding performed at a plurality of individual locations spaced apart from each other along the side wall member in a circumferential direction about a central longitudinal axis.

[0047] The method may further include the step of performing continuous welding along the side wall member to form a weld that substantially surrounds the cap in the circumferential direction.

[0048] According to one aspect of this method, the step of positioning the cap and the collector plate at the assembly position may include the step of inserting the electrode assembly to which the collector plate is joined into the internal space of the can.

[0049] According to an additional aspect of this invention, the step of positioning the cap and the collector plate at the assembly position may further include the step of inserting the cap into the opening of the can and bringing it into contact with the collector plate. Furthermore, after inserting the electrode assembly with the collector plate bonded thereto into the can, the cap may be inserted into the opening so that the cap comes into contact with the collector plate.

[0050] As a non-limiting effect according to the aspect of the present invention, there is improved welding performance that enables welding of the side wall member, the cap, and the collector plate together.

[0051] Additionally, the process stability can be improved by welding the side wall member, cap, and collector plate together.

[0052] Additionally, the durability of the welding area between the side wall member and the cap can be secured.

[0053] Additionally, by welding the sidewall members, cap and collector plate together at least as part of the same welding process, the assembly time and man-hours of the battery cell can be significantly reduced.

[0054] FIG. 1 is a perspective view of a cylindrical battery cell according to one aspect of the present invention.

[0055] Figure 2 is an exploded perspective view of the electrode assembly to be accommodated inside the can of Figure 1 before winding.

[0056] Fig. 3 is a perspective view of the electrode assembly of Fig. 2 in a pre-winding laminated state.

[0057] Fig. 4 is a perspective view of an assembled cylindrical jelly-roll-shaped electrode assembly by winding up the laminate of Fig. 3.

[0058] Fig. 5 is a perspective view showing a state in which a first collector plate is joined to an electrode tab of a first electrode of the electrode assembly of Fig. 4.

[0059] Fig. 6 is a perspective view showing a state in which a second collector plate is joined to an electrode tab of a second electrode of the electrode assembly of Fig. 4.

[0060] Figure 7 is a side cross-sectional view showing the process of positioning the electrode assembly with the current collector plate bonded inside the can.

[0061] Figure 8 is a side cross-sectional view showing the bonding process of the first collector plate and the first electrode terminal of the electrode assembly accommodated in the can.

[0062] Figure 9 is a side cross-sectional view showing the process of positioning a cap to cover the open end of a can containing an electrode assembly.

[0063] Figure 10 is an enlarged cross-sectional view of the open end of a battery cell with the open end of the can covered by a cap.

[0064] Figure 11 is an enlarged drawing showing the side wall member, current collector plate, and cap portion where welding is to be performed in the battery cell of Figure 10.

[0065] Figure 12 is a drawing showing the side wall member, collector plate, and cap portion of Figure 11 welded together.

[0066] Fig. 13 is an enlarged photograph of the welded portion corresponding to Fig. 11.

[0067] Fig. 14 is an enlarged view of the side wall member, current collector plate, and cap portion corresponding to Fig. 11 of a battery cell according to another sun.

[0068] Figure 15 is a diagram showing the location and size of stress concentration that vary depending on the welding length of the outer circumferential surface of the cap.

[0069] Figure 16 is a flowchart of a battery cell manufacturing process according to the present invention.

[0070] FIG. 17 is a perspective view of a battery pack including a plurality of battery cells according to the present invention.

[0071] Fig. 18 illustrates a vehicle equipped with the battery pack of Fig. 17.

[0072] [Explanation of symbols]

[0073] 10: Can 11: Side wall member 111: First inner surface 113: Inner diameter expansion portion 115: Second inner surface 117: Overhang portion t1: First thickness t2: Second thickness h1: First height h2: Second height 12: Bottom member 13: First electrode terminal 14: Gasket 15: Second electrode terminal 16: Cap 160: Cap body 161: Thickness reduction portion 17: Joint portion 171: Joint outer circumference 173: Collector plate mating surface t3: Third thickness (edge) t4: Fourth thickness (cap body) 19: Insulator 20: Electrode assembly 21: First electrode (positive electrode) 22: Second electrode (negative electrode) 23: Metal foil 24: Active material layer 25: Maintenance part 26: Non-conductive part 27: Electrode tab (notched tab) 28: Separator 31: First collector plate (positive collector plate) 312: Terminal connection part 313: Ring part 314: Electrode connection part 32: Second collector plate (negative collector plate) t5: Fifth thickness 321: Inner ring part 322: Hole 323: Electrode tab connection part 324: Can connection part 325: Butt outer circumference 326: Cap butt surface 327: First bend part 328: Second bend part W: Welding part S: Sealing part 70: Battery pack 71: Housing 72: Battery cell 80: Vehicle

[0074] The above-described objects, features, and advantages will be described in detail below with reference to the accompanying drawings, so that those skilled in the art can easily practice the technical idea of ​​the present invention. In describing the present invention, if it is determined that a detailed description of known technologies related to the present invention may unnecessarily obscure the gist of the present invention, a detailed description thereof will be omitted. Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the drawings, the same reference numerals are used to indicate the same or similar components.

[0075] Although terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another, and unless otherwise specified, a "first" component may also be a "second" component.

[0076] Throughout the specification, unless otherwise specifically stated, each element may be singular or plural.

[0077] Hereinafter, the phrase "any configuration is placed on (or below)" a component or "on (or below)" a component may mean that any configuration is placed in contact with the upper surface (or lower surface) of said component, and that other configurations may be interposed between said component and any configuration placed on (or below) said component.

[0078] Additionally, when it is described that a component is "connected," "coupled," or "connected" to another component, it should be understood that the components may be directly connected or connected to one another, but that other components may also be "interposed" between the components, or that each component may be "connected," "coupled," or "connected" through another component.

[0079] As used herein, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0080] Throughout the specification, when we refer to "A and / or B", this means A, B, or A and B, unless otherwise stated, and when we refer to "C through D", this means C or more and D or less, unless otherwise stated.

[0081] In describing the embodiments, the axial direction refers to the direction in which the central longitudinal axis forming the winding center of the jelly-roll-shaped electrode assembly extends, for example, the direction parallel to the central longitudinal axis. The radial direction refers to the direction approaching (centripetal) or moving away (centrifugal) from the axis, and the circumferential direction refers to the direction surrounding the axis.

[0082] Hereinafter, with reference to FIGS. 1 to 13, an embodiment of a battery cell to which the welding structure of the present invention is applied will be described in detail.

[0083] The battery cell of the embodiment may be, for example, a cylindrical battery cell having a form factor ratio (defined as the ratio of the diameter (Φ) to the height (H) of a cylindrical battery cell) of greater than about 0.4.

[0084] Here, the form factor refers to a value indicating the diameter and height of a cylindrical battery cell. The cylindrical battery cell may be, for example, a 46110 cell, a 48750 cell, a 48110 cell, a 48800 cell, or a 46800 cell. In the numerical value indicating the form factor, the first two numbers indicate the diameter of the cell, the next two numbers indicate the height of the cell, and the last number 0 indicates that the cross-section of the cell is circular.

[0085] The above battery cell may be a cylindrical battery cell having a roughly cylindrical shape, a diameter of approximately 46 mm, a height of approximately 110 mm, and a form factor ratio of 0.418.

[0086] According to another embodiment, a battery cell may be a cylindrical battery cell having a generally cylindrical shape, a diameter of approximately 48 mm, a height of approximately 75 mm, and a form factor ratio of 0.640.

[0087] According to another embodiment, a battery cell may be a cylindrical battery cell having a generally cylindrical shape, a diameter of approximately 48 mm, a height of approximately 110 mm, and a form factor ratio of 0.418.

[0088] According to another embodiment, a battery cell may be a cylindrical battery cell having a generally cylindrical shape, a diameter of approximately 48 mm, a height of approximately 80 mm, and a form factor ratio of 0.600.

[0089] According to another embodiment, a battery cell may be a cylindrical battery cell having a generally cylindrical shape, a diameter of approximately 46 mm, a height of approximately 80 mm, and a form factor ratio of 0.575.

[0090] The present invention can of course also be applied to battery cells having a form factor ratio of approximately 0.4 or less, such as 18650 cells, 21700 cells, etc. For 18650 cells, the diameter is approximately 18 mm, the height is approximately 65 mm, and the form factor ratio is 0.277. For 21700 cells, the diameter is approximately 21 mm, the height is approximately 70 mm, and the form factor ratio is 0.300.

[0091] The battery cell of the embodiment includes an electrode assembly (20), a current collector (31, 32) electrically connected to the electrode assembly (20), and a can (10) that accommodates the electrode assembly (20) and the current collector (31, 32).

[0092] The above can (10) includes a bottom member (12), a side wall member (11) connected to the bottom member (12) and extending in the axial direction, and a cap (16) covering an open end provided at one axial end of the side wall member (11).

[0093] The above-mentioned bottom member (12) may have a disc shape with a hole formed in the center, and the side wall member (11) may have a circular tube shape surrounding the internal volume of the can (11).

[0094] The above-mentioned bottom member (12) and side wall member (11) can be manufactured by forming a metal sheet with a nickel plated surface of steel using a deep drawing process, and trimming the front end of the side wall member (11) with a punch while holding it with a blank holder. Of course, the material of the can (10) is not limited to this.

[0095] A first electrode terminal (13) can be fitted into the hole. The first electrode terminal (13) can be fixed by riveting to the bottom member (12) with a gasket (14) interposed therebetween. The gasket (14) is interposed between the first electrode terminal (13) and the bottom member (12), sealing the inside and outside of the can (10) to prevent leakage of the electrolyte, and electrically insulating the first electrode terminal (13) from the bottom member (12).

[0096] However, the method of connecting the first electrode terminal (13) and the bottom member (12) is not limited to this. For example, if there is a structure that can seal between the first electrode terminal (13) and the bottom member (12) and electrically insulate the first electrode terminal (13) and the bottom member (12), various other fixing methods, such as i) bolt-nut joint method, ii) glass seal method, or iii) chrome coating & PP-MAH thermal bonding method, can also be applied.

[0097] The first electrode terminal (13) above may have a first polarity, and the can (10) may have a second polarity. That is, the bottom member (12) of the can (10), the side wall member (11) connected thereto, and the cap (16) connected to the side wall member (11), which will be described later, may all have a second polarity.

[0098] Accordingly, the battery cell may have both the first electrode terminal (13) and the second electrode terminal (15) positioned at the axial end, i.e., the closed end, provided with the bottom member (12). Then, the battery cell may have both the bus bar connected to the first electrode terminal (13) and the bus bar connected to the second electrode terminal (15) positioned on one side (upper) of the battery cell.

[0099] In one example, the first electrode terminal (13) may be a positive terminal and the second electrode terminal (15) may be a negative terminal. Of course, the opposite may also be true.

[0100] An electrode assembly (20) is accommodated within the can (10). The electrode assembly (20) is prepared by preparing a first electrode (21), a second electrode (22), and a separator (28) having a predetermined width and extending in the longitudinal direction as illustrated in FIG. 2, and forming a laminated body by sequentially stacking the first electrode (21), the separator (28), the second electrode (22), and the separator (28) as illustrated in FIG. 3, and then winding this around a core shaft as illustrated in FIG. 4, in the form of a jelly-roll.

[0101] The above first electrode (21) may be an anode, and the above second electrode (22) may be a cathode. Of course, the opposite may also be the case.

[0102] The above first electrode (21) and second electrode (22) are manufactured in the form of sheets. The electrode sheet is manufactured in the form of an active material layer (24) applied to the surface of a metal foil (23). The electrode sheet has a holding portion (25) region where the active material layer (24) is applied, and a non-coated portion (26) region where the active material layer (24) is not applied. The positive electrode sheet has a non-coated portion (26) region on one side in the width direction, and the negative electrode sheet has a non-coated portion (26) region on the other side in the width direction.

[0103] The first electrode (21) and the second electrode (22) are laminated so that their uncoated portions (26) are exposed or protrude in the width direction of the laminate. The uncoated portion (26) of the first electrode (21) protrudes from one axial end of the rolled jelly-roll, and the uncoated portion (26) of the second electrode (21) protrudes from the opposite axial end of the jelly-roll. The uncoated portion (26) itself functions as at least one electrode tab (27).

[0104] In the above-mentioned blank portion (26), notches can be formed at a predetermined interval to form flag-shaped notching tabs (27).

[0105] In the embodiment, the notching tabs (27) are exemplified as having an equilateral trapezoidal shape. However, their shapes may be various, such as a semicircle, a semi-ellipse, a triangle, a rectangle, a parallelogram, etc.

[0106] In addition, in the embodiment, a form in which the notching tabs (27) arranged along the longitudinal direction have the same width is exemplified. However, the width of the notching tabs may be gradually or stepwise widened from the core side to the outer periphery side.

[0107] In addition, as illustrated in FIGS. 2 and 3, the height of the notching tabs (27) gradually increases from the core side to the outer circumference side. However, differently from this, the height of these notching tabs may be implemented in a constant or gradually decreasing form.

[0108] In addition, in the embodiment, a structure is exemplified in which a notching tab (27) is deleted in a predetermined section of the centripetal end of the above-mentioned plain portion (26) and a predetermined section of the centrifugal end. However, it is obvious that, contrary to this, the notching tab may not be deleted in the centripetal end of the plain portion, the notching tab may not be deleted in the centrifugal end of the plain portion, or the notching tab may not be deleted in both sides.

[0109] In the jelly roll-shaped electrode assembly (20), the notched tab (27) can be bent radially and flattened as illustrated in FIG. 4. The notched tab (27) can be bent radially inward or outward. In the embodiment, a structure in which the notched tab (27) is bent radially inward is exemplified.

[0110] The above-mentioned notched tabs (27) can be bent one by one during the process of forming a jelly roll-shaped electrode assembly (20) by winding the laminate. Alternatively, the above-mentioned notched tabs (27) can be bent all at once after the laminate is wound to form a jelly roll-shaped electrode assembly.

[0111] The notched tabs (27) of the first electrode (21) and the notched tabs (27) of the second electrode (22), which are bent and overlapped in the radial direction in this way, can provide a plane that is substantially perpendicular to the axial direction at the axially opposite ends of the electrode assembly (20).

[0112] As shown in FIGS. 5 and 6, the first collector plate (31) and the second collector plate (32) can be joined to a substantially flat surface provided by bending the notched tabs (27) exposed at both axial ends of the electrode assembly (20).

[0113] In the embodiment, the first collector plate (31) is exemplified as a positive collector plate and the second collector plate (32) is exemplified as a negative collector plate. The first collector plate (31) may be made of aluminum, and the second collector plate (32) may be made of copper.

[0114] The above-mentioned collector plate (31, 32) can be manufactured by punching, trimming, piercing, and bending a metal sheet.

[0115] Referring to Fig. 5, the first collector plate (31) has a terminal connection portion (312) extending radially from the center, a ring portion (313) connecting the centrifugal edge of the terminal connection portion (312) in a circumferential direction, and an electrode connection portion (314) extending centripetally from the ring portion (313) but not connected to the terminal connection portion (312). The center portion of the terminal connection portion (312) covers at least a portion of the core hollow portion of the electrode assembly (20).

[0116] The above electrode connection part (314) is joined to the notched tab (27) of the first electrode (21) of the electrode assembly (20) by laser welding or the like before the electrode assembly (20) is placed in the can (10). The welding line of the laser may extend radially.

[0117] Referring to FIG. 6, the second collector plate (32) includes an inner ring (321) that defines a hole (322) corresponding to the core hollow portion of the electrode assembly (20) and is provided in a form that surrounds the core hollow portion, and an electrode tab connection portion (323) that extends radially from the inner ring (321). The electrode tab connection portion (323) may be in the form of a plurality of spokes that extend radially outward from the inner ring portion. Here, at least one of the spokes may have a radially outer end that is connected to the periphery of the second collector plate (32), referred to as a can connection portion (324). In addition, at least one of the spokes of the electrode tab connection portion (323) may have a radially outer end that does not reach the can connection portion (324). The can connection portion (324) has an outer ring shape surrounding the electrode tab connection portion (323), and the can connection portion (324) may include a step that extends away from the electrode assembly (20) in the axial direction. Accordingly, at least the outermost periphery of the can connection portion (324) may be arranged to be spaced further away from the electrode assembly (20) than the electrode tab connection portion (323), the inner ring portion (321), and other portions of the can connection portion (324).

[0118] The above electrode tab connection portion (323) can be joined to the notched tab (27) of the second electrode (22) of the electrode assembly (20) by laser welding or the like before placing the electrode assembly (20) into the can (10). The welding line of the laser can extend radially.

[0119] As illustrated in FIGS. 7 and 8, the electrode assembly (20) is accommodated in the can (10) in a state where the first collector plate (31) is aligned toward the bottom member (12) of the can (10). At this time, an insulator (19) is interposed between the first collector plate (31) and the bottom member (12) of the can (10) so that the first collector plate (31) is electrically insulated from the bottom member (12).

[0120] And, the terminal connection part (312) of the first collector plate (31) is joined to the first electrode terminal (13) fixed to the can (10) by resistance welding, ultrasonic welding, laser welding, or the like. The welding device for welding the first collector plate (31) and the first electrode terminal (13) can approach the back surface (the surface facing the electrode assembly (20)) of the center of the terminal connection part (312) of the first collector plate (31) through the core hollow portion of the electrode assembly (20) from the open end of the can (10) and perform welding. Of course, in addition to this, the first collector plate (31) and the first electrode terminal (13) can also be joined by brazing or soldering. In other words, various methods can be applied to the first collector plate (31) and the first electrode terminal (13) as long as they can be electrically connected and fixed to each other.

[0121] In a state where the electrode assembly (20) is accommodated inside the can (10), the electrode tab (27) of the second electrode (22) and the second current collector (32) can be arranged to face the open end of the side wall member (11).

[0122] After the first collector plate (31) and the first electrode terminal (13) are joined, an electrolyte can be injected into the can (10). After the electrolyte is injected, the open end of the side wall member (11) can be covered and finished with a cap (16) as shown in Fig. 9.

[0123] Of course, the welding method of the present invention can also be applied to a method of first covering the cap (16), then injecting the electrolyte through the injection port of the cap (16), and then closing the injection port of the cap (16).

[0124] The edge of the cap (16) is joined by laser seam welding with the edge of the side wall member (11) as shown in Fig. 10, and thus the can (10) can be sealed.

[0125] Referring to FIGS. 10 and 11, an inner diameter expansion portion (113) may be provided on the open end side of the side wall member (11). The inner diameter expansion portion (113) may be in the shape of a lateral step that extends across the central longitudinal axis and is arranged along the radially inner surface of the side wall member (11).

[0126] Accordingly, the radially inner side surface of the side wall member (11) may include a first inner side surface (111) that is positioned axially inner than the inner diameter expansion portion (113), that is, further from the opening of the open end of the side wall member (11), and a second inner side surface (115) that is positioned axially outer than the inner diameter expansion portion (113), that is, closer to the opening of the open end of the side wall member (11).

[0127] The second inner side surface (115) may have an inner diameter larger than that of the first inner side surface (111). Accordingly, the side wall member (11) may have a second thickness (t2) measured in the radial direction at a portion where the second inner side surface (115) is provided that is thinner than a first thickness (t1) measured in the radial direction at a portion where the first inner side surface (111) is provided.

[0128] The can connection portion (324) provided at the edge of the second collector plate (32) and electrically connected to the can (10) includes a first portion that is in contact with the second inner surface (115) of the side wall member (11). The first portion is provided with a mating outer surface (325) that faces and is in contact with the second inner surface (115) of the side wall member (11) in the radial direction.

[0129] The above can connection portion (324) includes a second portion that comes into contact with the cap (16). The second portion is provided with a cap mating surface (326) that faces and comes into contact with the inner surface of the cap (16) in the axial direction, i.e., the bottom surface of the cap (16).

[0130] The outer diameter of the mating outer surface (325) of the can connection portion (324) is set to be larger than the inner diameter of the first inner surface (111). Accordingly, the can connection portion (324) includes a third portion that contacts the inner diameter expansion portion (113). The third portion is provided on the opposite side of the cap mating surface (326) in the axial direction. The third portion contacts the inner diameter expansion portion (113) and regulates the insertion depth of the second collector plate (32) with respect to the can (10).

[0131] The second collector plate (32) further includes a first bend portion (327) and a second bend portion (328), whereby the second collector plate (32) is provided with an axial step. The first bend portion (327) provides a shape for bending the second collector plate (32), which extends radially outward, axially outward. And the second bend portion (328) provides a shape for bending the second collector plate (32), which extends axially outward, radially outward. Due to the axial step between the first bend portion (327) and the second bend portion (328), the peripheral portion or can connection portion (324) of the second collector plate (32) is axially offset toward the open end of the can (10) with respect to the central portion of the second collector plate (32).

[0132] The above can connection part (324) is connected to the electrode tab connection part (323) through the first bend part (327) and the second bend part (328) and through the inner ring part (321) described above.

[0133] The above can connection portion (324) is connected to the radially outer side of the second bend portion (328) and has a shape that extends radially from the second bend portion (328). Accordingly, the area of ​​the cap mating surface (326) of the second collector plate (32) can be further secured.

[0134] Preferably, the material of the second collector plate (32) may be softer than the material of the side wall member (11). Therefore, in the process of inserting the second collector plate (32) into the open end of the side wall member (11), the first bent portion (327) and the second bent portion (328) are elastically deformed. Accordingly, when the outer diameter of the abutting outer circumferential surface (325) is set to be slightly larger than the inner diameter of the second inner side surface (115), the abutting outer circumferential surface (325) is press-fitted into the second inner side surface (115).

[0135] The cap (16) is provided, in order from the radial center to the outside, with a cap body (160), a thickness reduction portion (161) in which the thickness of the cap changes, and a joint portion (17). That is, the cap body (160) is centered in the central region of the cap (16), and the thickness reduction portion (161) is provided on the radial outside of the cap body (160). The joint portion (17) is provided on the radial outside of the thickness reduction portion (161) to define an annular region of the cap (16) having a relatively reduced thickness with respect to the cap body (160). That is, the third thickness (t3) of the joint portion (17) measured in the axial direction is smaller than the fourth thickness (t4) of the cap body (160) measured in the axial direction.

[0136] Along the radially outer surface of the cap (16), specifically, along the radially outer surface of the joint portion (17), a joint outer surface (171) is provided that radially faces and comes into contact with the second inner surface (115) of the side wall member (11). In addition, along the joint portion (17), a bottom surface of the cap (16) is provided with a collector plate abutment surface (173) that faces axially inward so as to come into contact with the cap abutment surface (326) of the can connection portion (324) of the second collector plate (32).

[0137] By appropriately selecting the position where the thickness reduction portion (161) is provided, at least a portion of the thickness reduction portion (161) can be brought into contact with the second collector plate (32). Then, in the process of inserting the cap (16) into the open end of the side wall member (11), the thickness reduction portion (161) of the cap (16) comes into contact with the second collector plate (32), and the center of the cap (16) is aligned with the longitudinal axis of the center of the second collector plate (32).

[0138] In the embodiment, the thickness reduction portion (161) is positioned at a position corresponding to the position where the second bend portion (328) of the second collector plate (32) is formed in the radial direction, so as to enjoy this alignment effect.

[0139] Preferably, in order to enhance the alignment effect, the embodiment implements the thickness reduction portion (161) in the form of a slope that extends axially outward as it goes radially outward.

[0140] Also, preferably, in order to enhance the alignment effect, the embodiment also provides a sloped surface shape to the second collector plate (32) through the surface shape of the second bending portion (328) of the second collector plate (32).

[0141] In the radial direction, the joint outer surface (171) of the cap (16) and the mating outer surface (325) of the second collector plate (32) are each in contact with the second inner surface (115) of the side wall member (11).

[0142] And in the axial direction, at least a portion of the lower portion along the periphery of the second collector plate (32) is in contact with the inner diameter expansion portion (113) of the side wall member (11). In the axial direction, the cap mating surface (326) provided on the upper portion of the second collector plate (32) is in contact with the collector plate mating surface (173) provided on the lower portion of the joint portion (17) of the cap (16).

[0143] In this state where the second collector plate (32) and the cap (16) are inserted, an overhang (117) that protrudes further axially outward than the cap (16) can be provided at the open end of the side wall member (11).

[0144] The first height (h1) of the section provided axially outside the inner diameter expansion portion (113) of the side wall member (11) is greater than the sum of the third thickness (t3) of the joint portion (17) of the cap (16) and the fifth thickness (t5) of the can connection portion (324) of the second collector plate (32). The second height (h2) of the overhang portion (117) may be the length obtained by subtracting the third thickness (t3) and the fifth thickness (t5) from the first height (h1). For example, the first height (h1) may be 1 mm, the second height (h2) may be 0.2 mm, the third thickness (t3) may be 0.5 mm, and the fifth thickness (t5) may be 0.3 mm.

[0145] In the above battery cell, at the abutment portion of the side wall member (11), the cap (16), and the second collector plate (32), a weld portion (W) is formed by welding together the second inner surface (115) portion of the side wall member (11), the joint outer surface (171) portion of the cap (16), and the can connection portion (324) portion of the second collector plate (32).

[0146] In the embodiment, it is exemplified that the weld (W) is formed substantially over the entire circumferential section of the cap (16). Accordingly, the weld (W) can also function as a sealing portion (S) that seals the abutting portion of the can (10) and the cap (16).

[0147] However, unlike the embodiment, the welded portion (W) may be formed only in some sections that are discontinuously spaced apart from each other in the circumferential direction. Accordingly, the welded portion (W) may constitute some sections of the sealing portion (S) that seals the abutting portion of the can (10) and the cap (16).

[0148] The above welding part (W) can be formed by laser welding that examines the abutting part of the can (10) and the cap (16) along the circumferential direction, and at this time, welds together the can connection part (324) of the second collector plate (32).

[0149] The above sealing portion (S) can also be formed by laser welding by continuously irradiating the abutting portion of the can (10) and cap (16) along the circumferential direction.

[0150] In one example, the weld (W) may be formed during a preliminary welding process or during a subsequent main welding process.

[0151] The above sealing portion (S) can be formed during this welding process.

[0152] The above welding part (W) and sealing part (S) can be formed together during this welding process.

[0153] In the embodiment, a structure is exemplified in which a laser is continuously irradiated along the circumferential direction to the mating portion of the can (10) and the cap (16) during the welding process, and the energy density and scan speed of the laser are kept constant, and the can connection portion (324) of the second collector plate (32) is welded together, so that a welded portion (W) is formed along the entire circumferential direction and a sealing portion (S) is also formed.

[0154] However, unlike this, in the present welding process, the abutting portion of the can (10) and the cap (16) is continuously irradiated with a laser along the circumferential direction, but at this time, the energy density of the laser is increased or the scan speed is decreased only in a specific discontinuous section so that the laser penetrates deeper and welds the can (10) together with the can connection portion (324) of the second collector plate (32), so that a sealing portion (S) is formed over the entire section of the side wall member in the circumferential direction, and of course, a structure in which a welding portion (W) is formed in the specific section can be implemented.

[0155] The discontinuous portion where the weld (W) is formed between the second collector plate (32) and the can (10) is similar to a 'tack weld' that secures the two components together, whereas the continuous seal (S) forms a seal along substantially the entire exposed area between the can (10) and the cap (16).

[0156] In practice, similar to tack welding, the welding method may first comprise the step of forming a plurality of discontinuous welds (W) between the second collector plate (32) and the can (10) and between the cap (16) and the can (10) (e.g., using laser irradiation at discrete individual locations along the circumference at a slower speed and / or a higher energy density). Thereafter, the laser irradiation may be performed continuously along the entire exposed joint between the can (10) and the cap (16). This approach has the advantage that the discontinuous welds may at least temporarily fix the positions of the second collector plate (32) and the cap (16) with respect to the can (10) while the subsequent process of forming and sealing a continuous seal (S) is performed.

[0157] As shown, the axial upper portion of the inner surface of the side wall member (11) and the outer surface of the cap (16) that are radially opposed to each other are exposed to the outside of the battery cell.

[0158] The above welding part (W) is formed by a laser irradiated from the axial outer side of the battery cell toward the joint outer surface (171) of the cap (16) and the axial end of the second inner surface (115) of the side wall member (11).

[0159] At this time, since the outer surface (325) of the second collector plate (32) positioned axially lower than the cap (16) faces and comes into contact with the radially inner surface of the side wall member (11), the laser is prevented from entering the internal volume space of the can through a gap that may exist between the side wall member (11) and the cap (16).

[0160] In addition, the inner diameter expansion portion (113) of the side wall member (11) also prevents the internal penetration of a laser that may enter through the gap between the side wall member (11) and the cap (16) or the side wall member (11) and the second collector plate (32).

[0161] The second collector plate (32) may be made of a material having a higher thermal conductivity than the side wall member (11). In addition, the second collector plate (32) is in contact with the side wall member (11). Therefore, when the welding heat generated in the side wall member (11) by the laser is conducted along the axial direction of the side wall member (11), it is distributed across the upper portion of the electrode assembly (20) through the second collector plate (32), thereby preventing the phenomenon of the welding heat being transmitted to the separator portion of the electrode assembly (20) and damaging the separator.

[0162] The second collector plate (32) is also in contact with the cap (16). Accordingly, heat generated in the cap (16) by the laser is distributed and transmitted through the second collector plate (32). Then, when the abutting portion of the cap (16) and the side wall member (11) is heated by the laser, the side wall member (11) may be heated first and melted.

[0163] Therefore, if the side wall member (11) is too thin, the side wall member (11) may melt before the cap (16), and welding may not be performed smoothly. Preferably, the second thickness (t2) of the side wall member (11) may be 0.25 mm or more. For example, the second thickness (t2) may be 0.35 mm.

[0164] On the other hand, when the pressure inside the can (10) increases, it is also important that the cap (16) has the strength to support it. If the cap (16) is too thin, excessive bulging occurs, in which the cap (16) swells in the shape of a spherical surface profile when the internal pressure inside the can (10) increases, which deteriorates the durability of the battery cell. To resist such bulging deformation, it is important that the cap (16) secure a certain thickness.

[0165] On the other hand, if the thickness of the cap (16) is excessively thick compared to the side wall member (11), only the side wall member (11) is melted first during laser welding, significantly reducing the welding processability. In addition, as the thickness of the cap (16) increases, the axial length of the joint outer circumferential surface (171) of the cap (16) where welding is to be performed also increases.

[0166] In Fig. 15, (a) is a diagram showing the results of a stress analysis when the internal pressure of the can (10) increases when the joint outer circumferential surface (171) of the cap (16) is welded in the full axial direction to form a sealing portion (S) and / or a welded portion (W), (b) is a diagram showing the results when the joint outer circumferential surface (171) of the cap (16) is welded in the axial direction by 75% of the section to form a sealing portion (S) and / or a welded portion (W), and (c) is a diagram showing the results when the joint outer circumferential surface (171) of the cap (16) is welded in the axial direction by 25% of the section to form a sealing portion (S) and / or a welded portion (W). Referring to Fig. 15, it can be confirmed that a weak point exists in the welding area of ​​the side wall member (11) and the cap (16) when the joint outer circumferential surface (171) of the cap (16) is not welded in the full axial direction.

[0167] Accordingly, the embodiment discloses a cap (16) having a structure in which the third thickness (t3) of the joint (17) where welding is performed with the side wall member (11) and the fourth thickness (t4) of the cap body (160) are different. The thicker the fourth thickness (t4), the higher the resistance to bulging, but the larger the space it occupies inside the can. In order to increase the resistance to bulging while minimizing the space occupied and weight, it is preferable that the fourth thickness (t4) be as small as possible within the required bulging resistance range.

[0168] Ultimately, the fourth thickness (t4) of the cap body (160), which occupies most of the cap (16), is preferably larger than the third thickness (t3) in order to minimize deformation of the cap (16) due to the internal pressure of the can (10). On the other hand, the thickness dimension of the welded portion along the axial direction is also minimized so that the sealing portion (S) and / or the welded portion (W) is reliably formed over the entire axial direction of the joint outer circumference (171). Accordingly, the strength of the cap (16) itself is increased, and also the bonding strength of the cap (16) to the side wall member (11) is increased.

[0169] The ratio of the third thickness (t3) to the fourth thickness (t4) may preferably be 0.4 to 0.8, more preferably 0.5 to 0.75. If the ratio is less than the above range, there is a concern that the cap body (160) may become excessively thick without increasing the bulging resistance and / or the strength of the weld may be insufficient. If the ratio exceeds the above range, the bulging resistance of the cap body (160) may be insufficient and / or it may be difficult to weld the outer circumferential joint surface (171) of the cap (16) along the entire axial direction.

[0170] Accordingly, by increasing the fourth thickness (t4) of the cap body (160) that occupies the overall shape of the cap (16), deformation of the cap (16) due to the internal pressure of the can (10) is minimized, while suppressing the axial dimension of the welding portion for the side wall member (11), i.e., the joint outer circumference (171), so that the sealing portion (S) and / or the welding portion (W) is formed over the entire axial direction of the joint outer circumference (171), thereby increasing both the strength of the cap (16) itself and the bonding strength of the cap (16) to the side wall member (11).

[0171] According to the cap (16) of the embodiment, the radial position of the thickness reduction portion (161) can be positioned as close as possible to the welding area, thereby maximizing the area of ​​the cap body (160) that resists bulging. In addition, by selecting the position of the thickness reduction portion (161), a guide function that aligns the center of the cap (16) while making contact with the second collector plate (32) can also be provided.

[0172] The third thickness (t3) of the joint (17) of the cap (16) may be set to be greater than the second thickness (t2) of the side wall member (11). The third thickness (t3) may be at least one time and at most two times the second thickness (t2). For example, when the second thickness (t2) is 0.35 mm, the third thickness (t3) may be 0.5 mm or in the range of 0.5 to 0.7 mm.

[0173] If the third thickness (t3) exceeds twice the second thickness (t2), there is a risk that the side wall member (11) may melt excessively before the cap (16) melts during the process of forming the sealing portion and / or the welding portion. In addition, if the third thickness (t3) exceeds twice the second thickness (t2), there is a risk that the sealing portion and / or the welding portion may not be formed over the entire axial direction of the joint outer surface (171) of the cap (16).

[0174] If the third thickness (t3) is less than one time the second thickness (t2), that is, if the second thickness (t2) is greater than the third thickness (t3), it is difficult to secure strength at the edge portion of the cap (16), and it is also difficult to secure sufficient dimensions of the lateral step of the inner diameter expansion portion (113) of the side wall member (11) without increasing the overall thickness (t1) of the side wall member (11).

[0175] Next, the overhang portion (117) can delay the melting point of the relatively thin side wall member (11) to reduce the difference in the melting point of the side wall member (11) and the cap (16), and can be welded to the welding area of ​​the radially inner surface of the side wall member (11) and the joint outer circumferential surface (171) of the cap (16) during the welding process.

[0176] Accordingly, the diameter of the joint outer circumference (171) of the cap (16) can be made slightly smaller than the diameter of the second inner surface (115) of the side wall member (11) adjacent to the joint outer circumference (171). Here, the concept that two objects are 'adjacent' means that the two objects are spaced closely together compared to their outer dimensions, and that there is no separate intervening object between the two objects within the relevant plane (i.e., the radial plane perpendicular to the central longitudinal axis). Since the diameter of the joint outer circumference (171) of the cap (16) is slightly smaller than the diameter of the second inner surface (115) of the side wall member (11), a small gap is defined between these two components.

[0177] This gap can serve as a passage through which the welding laser can be directly irradiated to the second collector plate (32).

[0178] Preferably, such a gap can have an overall uniform radial width along the circumference of the cap (16) due to the alignment of the center of the cap (16) by the interaction between at least the thickness-reduced portion (161) of the cap (16) and the second collector plate (32), as described above.

[0179] In addition, during the welding process, it is preferable that the material of the overhang (117) penetrates into the gap between the joint outer surface (171) of the cap (16) and the second inner surface (115) of the side wall member (11) to join the cap (16) and the side wall member (11).

[0180] In one example, the height (h2) of the overhang (117) is 0.2 mm, while the thickness (t3) of the joint (17) of the cap (16) is 0.5 mm. When the thickness (t2) of the overhang (117) is 0.35 mm, sufficient molten material is provided during the welding process, so that a strong joint can be formed between the cap (16) and the side wall member (11). For example, the ratio of the height (h2) of the overhang to the thickness (t3) of the joint (17) may preferably be in the range of 0.2 to 1.

[0181] The overhang (117) of FIG. 11 may be melted as shown in FIGS. 12 and 13 during the process of forming the sealing portion (S) and / or the welding portion (W). Accordingly, the height of the battery cell may be determined by the outer surface of the cap (16). That is, according to the embodiment, since the sealing portion (S) and / or the welding portion (W) do not regulate the height of the battery cell, the height dimension of the battery cell may be managed to be constant.

[0182] Hereinafter, with reference to FIG. 14, a modified example of a welding structure according to the present invention will be described. In describing the modified example, differences from the previous embodiment will be primarily explained to avoid redundant explanation. Therefore, it is self-evident that matters not described in the modified example can be sufficiently understood through the description of the previous embodiment, and it is self-evident that each component of the previous embodiment and the following modified example can be substituted or omitted as long as it does not go against the spirit of the invention.

[0183] The side wall member (11) has an inner diameter expansion portion (113) on the open end side. The inner diameter expansion portion (113) has an inclined or slanted surface shape provided on the inner surface of the side wall member (11) so as to expand the inner diameter of the side wall member (11) as it goes outward in the axial direction. That is, the inner diameter expansion portion (113) is provided on the inner surface of the side wall member (11) and includes an inclined surface shape that is relatively slanted with respect to the central longitudinal axis and extends radially outward as it goes toward the axial upper end of the side wall member (11).

[0184] The second collector plate (32) includes a first bend portion (327). The first bend portion (327) provides a shape that extends axially by bending the second collector plate (32), which extends radially outward, axially outward. Therefore, the peripheral portion (i.e., the can connection portion (324)) of the second collector plate does not extend radially as in the previously described embodiments, but extends axially. As a result, the abutting outer peripheral surface (325) that contacts the second inner surface (115) of the side wall member (11) extends along the longitudinal dimension of the peripheral portion, rather than being defined by the end portion of the peripheral portion. Instead, the end portion of the peripheral portion in the embodiment of FIG. 14 becomes the cap abutting surface (326) that abuts against the collector abutting surface (173) at the bottom of the cap (16) along the joint portion (17).

[0185] The can connection part (324) of the second collector plate (32) is connected to the electrode tab connection part (323) through the first bending part (327) and the inner ring part (321) described above.

[0186] Since the material of the second collector plate (32) is softer than the material of the side wall member (11), the first bent portion (327) is elastically deformed in the process of inserting the second collector plate (32) into the open end of the side wall member (11). Accordingly, when the outer diameter of the abutting outer circumferential surface (325) is set to be slightly larger than the inner diameter of the second inner surface (115), the abutting outer circumferential surface (325) is pressed into the second inner surface (115), so that the abutting outer circumferential surface (325) and the second inner surface (115) are in close contact in the radial direction.

[0187] Dimensionally, the outer circumferential surface of the first bent portion (327) of the second collector plate (32) partially overlaps with the inner diameter expansion portion (113) of the side wall member (11). Accordingly, even if a tolerance occurs in the dimensions of the second collector plate (32) or the side wall member (11), the outer circumferential surface of the second collector plate (32) can be in strong contact with the radially inner surface of the side wall member (11).

[0188] Accordingly, according to the structure of the second collector plate (32) of the modified example, the cap-fitting surface (326) provided on the axial outer end of the can connection portion (324) of the second collector plate (32) has a radial width corresponding to approximately the fifth thickness (t5). That is, the area of ​​the portion where the second collector plate (32) comes into contact with the side wall member (11) may be wider than the area of ​​the portion where the second collector plate (32) comes into contact with the cap (16).

[0189] Then, compared to the previous embodiment, the heat generated in the side wall member (11) by the laser can be more quickly dispersed and conducted through the second collector plate (32), and the heat generated in the cap (16) by the laser can be somewhat more slowly dispersed and conducted through the second collector plate (32). Accordingly, the melting point of the side wall member (11), which is relatively thinner than the joint (17) of the cap (16), can be further delayed.

[0190] In addition, since most of the welding heat transmitted through the side wall member (11) is distributed through the second collector plate (32), the phenomenon of heat being transmitted toward the separator (28) of the electrode assembly (20) in contact with the first inner surface (111) of the side wall member (11) can be further reduced.

[0191] Next, the thickness reduction portion (161) of the cap (16) of the modified example is positioned radially further outward than the thickness reduction portion (161) of the cap (16) of the previous embodiment. Accordingly, the area of ​​the cap body (160) can be further secured. In addition, the thickness reduction portion (161) is also provided in the form of an inclined surface, so that it can contact the second collector plate (32) during the insertion process of the cap (16) and guide the center alignment of the cap (16).

[0192] According to the embodiments and modifications described above, even though the range of the welding process is wide, the weldability can be improved by securing a sealing force without leakage of the perforation, and the process stability can be improved by preventing thermal damage to the components of the cell or the separator due to the welding heat, and the durability can also be improved by securing dimensional stability or bulging resistance by suppressing dimensional deformation according to the internal pressure.

[0193] Referring to FIGS. 7 to 10 and FIG. 16 below, a method for manufacturing the above-described battery cell will be described.

[0194] According to the manufacturing method of the above battery cell, first, a can (10) with a first electrode terminal (13) fixed to a bottom member (12) is prepared, and an electrode assembly (20) with a first collector plate (31) and a second collector plate (32) bonded to each of the axial ends is prepared.

[0195] Then, the electrode assembly (20) is inserted and accommodated in the can (10) with the first collector plate (31) facing the bottom member (12). Then, the second collector plate (32) is positioned toward the open end of the can (10). In the process of accommodating the electrode assembly (20) in the can (10), the mating outer surface (325) of the can connecting portion (324) provided at the radially outer edge of the second collector plate (32) is brought into contact with the second inner surface (115) of the side wall member (11).

[0196] At this time, by bringing the can connection part (324) of the second collector plate (32) into contact with the inner diameter expansion part (113) of the side wall member (11), the adhesion of the second collector plate (32) to the inner surface of the side wall member (11) can be secured, and the insertion depth of the second collector plate (32) can be regulated.

[0197] Next, the first collector plate (31) and the first electrode terminal (13) are joined.

[0198] Then, the electrolyte is injected into the can (10).

[0199] After the electrolyte injection is completed, the open end of the side wall member (11) is covered with a cap (16), and the bonding outer surface (171) and the collector plate mating surface (173) provided on the edge of the cap (16) are brought into contact with the second inner surface (115) of the side wall member (11) and the cap mating surface (326) of the second collector plate (32), respectively. At this time, the thickness reduction portion (161) in the form of an inclined surface provided on the axial inner surface of the cap (16) is brought into contact with the second collector plate (32), thereby aligning the center of the cap (16).

[0200] Next, a laser is irradiated from the axial outer side to the abutting portion of the second inner side (115) of the side wall member (11) and the joint outer surface (171) of the cap (16), thereby welding the inner surface of the side wall member (11), the joint outer surface (171) of the cap (16), and the can connection portion (324) of the second collector plate (32) together. Accordingly, the welding portion (W) joins the side wall member (11), the cap (16), and the second collector plate (32) together.

[0201] At this time, the overhang portion (117) of the side wall member (11) that protrudes further axially outward than the cap (16) can be welded to the welding area of ​​the inner surface of the side wall member (11) and the joint outer surface (171) of the cap (16).

[0202] The battery cell (72) manufactured through the welding structure and welding process described above can be accommodated in the housing (71) of the battery pack (70) as illustrated in FIG. 17. The battery pack (70) may be configured using a battery module, which is an intermediate form of assembly, or the battery pack (70) may be configured directly without a battery module as illustrated.

[0203] Since the battery cell (72) described above has a large volume in itself, there is no particular difficulty in implementing a battery pack (70) even without using an intermediate structure called a battery module. Furthermore, the battery cell (72) has low internal resistance and a higher energy density. Accordingly, the energy density of a battery pack (70) equipped with the battery cell (72) can be implemented even higher.

[0204] A battery pack (70) with such a high energy density can store the same amount of energy while reducing its volume and weight. Therefore, when a battery pack (70) equipped with such battery cells (72) is installed in a vehicle, such as an automobile (80) that uses electricity as its energy source, as illustrated in FIG. 18, the vehicle's mileage per unit of energy can be further increased.

[0205] While the above seam welding structures and methods have been disclosed in the context of cylindrical battery cans, it should be understood that, within the scope of the present disclosure, these techniques can be similarly applied to other battery form factors. For example, the associated battery cells need not have a circular cross-sectional profile orthogonal to a central longitudinal axis, but rather can utilize other cross-sectional shapes, including oval, square, rectangular, and partially circular. Moreover, the central longitudinal axis need not be oriented orthogonally to the bottom member and / or cap at each opposing end. For example, the side wall members of the can (together with the internal components of the can) can form a tube extending along an axis oriented obliquely with respect to a plane defined by the bottom member and / or cap. Furthermore, the welding techniques disclosed herein can also be utilized outside the scope of cylindrical battery cans, and can also be applied to batteries having, for example, prismatic and pouch-shaped form factors.

[0206] It should be understood that the above-described embodiments are illustrative in all respects and not restrictive, and the scope of the present invention will be determined by the claims that follow, rather than by the detailed description set forth above. Furthermore, the meaning and scope of the claims that follow, as well as all possible modifications and variations derived from their equivalent concepts, should be construed as encompassing the scope of the present invention.

[0207] Although the present invention has been described with reference to the drawings exemplified above, it is to be understood that the present invention is not limited to the embodiments and drawings disclosed herein, and that various modifications may be made by those skilled in the art within the scope of the technical idea of ​​the present invention. Furthermore, even if the operational effects according to the configuration of the present invention have not been explicitly described while describing the embodiments of the present invention, it is natural that the effects predictable by the corresponding configuration should also be acknowledged.

Claims

1. A can having a side wall enclosing an internal volume and defining an opening in said internal volume at a first end along a longitudinal axis of the center; An electrode assembly accommodated within the internal volume of the can; a current collector electrically connected to the electrode assembly; and A cap covering the opening of the can so as to surround the internal volume; The above current collector plate includes a central portion and a peripheral portion, the central portion being electrically connected to the electrode tab of the electrode assembly, the peripheral portion being arranged around the central portion and being arranged farther from the central longitudinal axis than the central portion, the peripheral portion contacting a radially inner surface of the side wall so as to be electrically connected to the can, and the peripheral portion contacting a lower portion of the cap facing the internal volume along an axial direction extending parallel to the central longitudinal axis. A battery cell wherein the side wall, the radial outer surface of the cap, and the periphery of the current collector are welded to each other.

2. In claim 1, The radially inner side surface of the side wall includes a lateral step extending across the central longitudinal axis, a first inner side surface of the side wall axially disposed on a first side of the lateral step has a first diameter, a second inner side surface of the side wall axially disposed on a second side of the lateral step has a second diameter, the second side of the lateral step is disposed closer to the opening than the first side, and the second diameter is larger than the first diameter. A battery cell, wherein the radial outer surface of the cap and the peripheral portion of the current collector plate are in contact with the second inner surface.

3. In claim 2, A battery cell, wherein the outer diameter of the periphery of the above-mentioned collector plate is larger than the first diameter of the above-mentioned first inner surface.

4. In claim 2, A battery cell in which the peripheral portion of the above-mentioned current collector plate is in contact with the above-mentioned lateral step.

5. In claim 2, A battery cell, wherein the lateral step extends obliquely from a first diameter of the first inner side to a second diameter of the second inner side.

6. In claim 2, A battery cell, wherein a first thickness of the cap in the axial direction along the radial outer surface is greater than a second thickness of the side wall in the radial direction along the second inner surface, wherein the radial direction is perpendicular to the central longitudinal axis.

7. In claim 6, A battery cell wherein the first thickness is 1 to 2 times thicker than the second thickness.

8. In any one of claims 1 to 7, The diameter of the radially outer surface of the cap is smaller than the diameter of the adjacent portion of the radially inner surface of the side wall, A battery cell, wherein the welding area extends from the adjacent portion of the radially inner surface of the side wall to the radially outer surface of the cap.

9. In any one of claims 1 to 7, The cap comprises an annular region extending along the radially outer surface, A battery cell, wherein the thickness of the annular region of the cap along the axial direction is smaller than the thickness of the central region of the cap arranged along the central longitudinal axis.

10. In claim 9, A battery cell, wherein a slope along the lower portion of the cap connects the annular region and the central region.

11. In claim 10, The above inclined surface is in contact with the above current collector plate, the battery cell.

12. In any one of claims 1 to 7, A battery cell wherein the collector plate includes an axial step between the central portion and the peripheral portion, such that the peripheral portion is offset relative to the central portion toward the opening of the can.

13. In any one of claims 1 to 7, The longitudinal dimension of the central portion of the above collector plate extends across the axial direction, A battery cell, wherein the longitudinal dimension of the peripheral portion of the above-mentioned current collector extends parallel to the axial direction, and the peripheral portion extends along the radially inner surface of the side wall of the can to the tip of the peripheral portion that abuts against the lower portion of the cap.

14. Positioning the cap and the collector plate in an assembly position within the opening of the can, such that, at the assembly position, the collector plate is electrically connected to the electrode assembly accommodated within the internal volume of the can, the periphery of the collector plate contacts the radially inner surface of the side wall of the can surrounding the opening, and the cap is positioned on the collector plate along the central longitudinal axis of the can, such that the cap is positioned further from the electrode assembly than the collector plate; and A method for manufacturing a battery cell, comprising: welding the radially inner surface of the side wall, the radially outer surface of the cap, and the peripheral portion of the current collector to each other.

15. In claim 14, A method for manufacturing a battery cell, wherein placing the cap and the collector plate at the assembly position includes contacting a peripheral portion of the collector plate with a lateral step defined on the radially inner surface of the side wall of the can.

16. In claim 14, A method for manufacturing a battery cell, wherein placing the cap and the collector plate at the assembly position includes contacting an inclined surface disposed along the lower portion of the cap with an annular area of ​​the collector plate extending along the circumference.

17. In any one of claims 14 to 16, A method for manufacturing a battery cell, wherein welding the radially inner surface of the side wall of the can comprises melting a material of an extension portion of the side wall that protrudes above the cap along an axial direction extending parallel to the central longitudinal axis, and thereby causing the material of the extension portion to flow between the radially inner surface of the side wall and the radially outer surface of the cap to join them together.

18. In any one of claims 14 to 16, A method for manufacturing a battery cell, wherein welding the radially inner surface of the side wall comprises performing tack welding at a plurality of discontinuous locations spaced apart from each other along the side wall in a circumferential direction about the central longitudinal axis, and then continuously performing welding along the side wall to form a weld that substantially surrounds the cap in the circumferential direction.

19. In any one of claims 14 to 16, A method for manufacturing a battery cell, wherein placing the cap and the collector plate at the assembly position includes inserting the electrode assembly to which the collector plate is joined into the internal volume of the can.

20. In claim 19, A method for manufacturing a battery cell, wherein placing the cap and the collector plate at the assembly position further includes inserting the electrode assembly to which the collector plate is joined, and then inserting the cap into the opening of the can so as to make contact with the collector plate.

Citation Information

Patent Citations

  • Bottom cover assembly and cylindrical battery

    CN115275464A

  • High rate battery

    CN209133626U

  • Battery module

    KR100814853B1

  • Secondary battery

    KR1020050094662A

  • Lamp for heating and heating apparatus including same

    KR1020230112057A