Composition and method for cationic frontal polymerization
The introduction of a reducing agent in cationic frontal polymerization compositions addresses the issues of incomplete curing and decarboxylation by controlling Bronsted acid formation and maintaining low temperatures, enhancing curing depth and crosslink-density while reducing energy consumption.
Patent Information
- Application Number
- PCT/AT2023/060158
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
Radical induced cationic frontal polymerization compositions face challenges with incomplete curing of thick composites or high filler content due to heat loss, leading to decarboxylation and bubble formation, which requires high temperatures that can decompose monomers and initiators, resulting in inefficient energy use and poor material properties.
Incorporating a reducing agent that interacts with the onium salt to control Bronsted acid formation and react with thermally generated radicals, maintaining low polymerization temperatures and reducing decarboxylation, thereby sustaining the polymerization front and minimizing bubble formation.
This approach increases curing depth and reduces curing time for high filler content composites, prevents bubble formation, and improves crosslink-density of the polymer, allowing for polymerization at milder conditions with lower energy input.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] Composition and Method for Cationic Frontal Polymerization
[0002] The invention relates to a composition as well as a method for cationic frontal polymerization, the composition containing a cationically polymerizable monomer, a photoinitiator, and a thermally inducible radical forming agent.
[0003] Frontal polymerization is a technique for producing a polymer from a composition containing a plurality of monomer molecules, which is known in the art. The reaction principle involves a polymerization reaction, in which a propagating and self-sustaining polymerization front is produced typically via a one-time energy input. One type of frontal polymerization is radical induced cationic frontal polymerization. It allows autocatalytic curing of functional groups such as vinyl esters and cyclic ether monomers in the form of a hot propagating front. The reaction may be induced via an initiator, which is exposed to electromagnetic radiation and / or high temperatures. The amount of input energy needs to be sufficient to at least temporarily generate radicals from the initiator. After induction of the reaction, no external energy input is necessary and the reaction proceeds in a self-sustained manner.
[0004] Compositions suitable for cationic frontal polymerization induced by exposure to electromagnetic radiation typically contain a monomer with cationically polymerizable functional groups; a photoinitiator, for example an onium salt; and a thermal radical initiator such as an organic peroxide or a pinacol derivative.
[0005] In case of onium salts being used as photoinitiator, the reaction mechanism is understood to be as follows: Radicals and cations generated from the photo-excited state of an onium salt lead to the formation of a strong Bronsted acid, further leading to the protonation of the monomer. The highly reactive cations, which are thereby formed, attack adjacent polymerizable groups. The generated heat of polymerization is then utilized to homolytically cleave the thermal radical initiator. The front propagates by the thermally generated radicals. Thus, the curing follows a radical cationic mechanism and the remaining unreacted monomers are consumed in the absence of UV light or an external heat source.
[0006] Several problems arise within state-of-the-art radical induced cationic frontal polymerization compositions as described above. For example, composite polymerization compositions comprising monomers with cyclic ether functional groups such as epoxy groups and higher amounts of filler material (typically >40 vol.-% of total composition volume) do not reach in-depth curing for thicknesses above 10 mm. The front can be triggered after short duration oven curing at temperatures 130-150°C since the radical thermal initiator can disassociate at these temperatures. However, mainly due to heat losses, the front cannot be sustained, resulting in incomplete curing of thick composites or composites with high filler content.
[0007] To cure such high filler content composite compositions, high temperatures of up to 300°C are usually required over an extended period of time until the entire resin throughout the composite thickness achieves a self-sustaining front. Exposing the composite to 300°C for a prolonged period, however, boils off or decomposes the epoxy monomers as well as the initiators, leading to loss of material properties of the resulting polymer and damage to the composite. Additionally, the necessity of these high temperatures does render the polymerization to be not very energy-efficient. Another problem arising within existing compositions and methods for radical induced cationic frontal polymerization is decarboxylation, which in particular has been observed for monomers with cyclic ether functionalities such as epoxy groups or oxetanes.
[0008] It has been discovered, that within a typical and above described cationic frontal polymerization, the formed Bronsted acid attacks the ester bonds present either in the polymerizable monomer or in the thermal initiator (e.g. in benzoyl peroxide) during frontal polymerization, resulting in decarboxylation and release of carbon dioxide at high temperatures. If an organic peroxide is used as thermal initiator, the situation aggravates since oxygen radicals also contribute to extensive bubble formation within the cured material, resulting in a foamed and cracked polymer. Using radical thermal initiators such as benzopinacol instead of organic peroxides could not solve the problem of decarboxylation to this day.
[0009] One objective of the present invention may thus be to at least partially overcome one or more of the above-described drawbacks of known compositions and methods for radical induced frontal polymerization.
[0010] A particular objective of the present invention may be seen in increasing the curing depth of composite compositions with high filler contents curable via radical cationic frontal polymerization. Another objective may be seen in decreasing curing times of cationically polymerizable monomer compositions. One further objective of the present invention may be seen in obtaining a polymer with reduced or no bubble formation from cationic frontal polymerization. An even further objective of the present invention may be seen in improving crosslink-density of the polymer produced from cationic frontal polymerization. Another objective of the present invention may be seen in providing compositions, which are polymerizable at milder conditions or with lower energy input.
[0011] One or more of the aforementioned objectives are solved in particular by the composition and the method according to the independent patent claims.
[0012] The current invention therefore particularly relates to a composition for cationic frontal polymerization, containing: a cationically polymerizable monomer M; a photoinitiator, the photoinitiator being an aromatic onium salt having the general formula [AnB]+[XYm]'; a thermally inducible radical forming agent.
[0013] It has been surprisingly and unexpectedly found by the present inventors that the addition of a reducing agent may provide beneficial results if used in such compositions. In this context, the reducing agent is typically capable of reducing and / or lowering the charge of B, which is the central atom of the cation, in the onium salt.
[0014] The present inventors have discovered that the interaction of the reducing agent with the onium salt, in particular in its singlet state, provides desirable effects to the composition and the method of the present invention.
[0015] Without wishing to be bound to this theory, the inventors have found that the reducing agent may control the above-described formation of the Bronsted acid from the onium salt, and also react with the onium salt after oxidation of the thermally generated radicals, which are oxidized to cations in the presence of the onium salt. The reducing agent may therefore also aid in the continuation of the reaction after the oxidation of the radicals of the thermally inducible radical forming agent to cations via the onium salt.
[0016] It has been revealed that these mechanisms can aid in sustaining relatively low polymerization temperatures during frontal curing of the composition, thus preventing boiling off or decomposition of composition compounds. Furthermore, bubble formation can be minimized due to reduced or completely prevented decarboxylation and CO2formation.
[0017] As already mentioned, the onium salt may have the general formula [AnB]+[XYm]'. In particular, at least one of the substituents A of the cationic portion of the onium salt is an aryl functional group, such that the onium salt may also be referred to as aryl onium salt.
[0018] The number n of substituents A included in the onium salt cation is an integer number, depending on the charge of the central atom B of the cation. Such onium cations are generally well known in the art. The substituents A of the central atom B can be the same or different. In addition, a number of substituents A may be the same, while some substituents A may be different. For example, if n is 3, two substituents Ai and A2may be the same and one substituent A3may be different from the two substituents A! and A2.
[0019] In the above general formula, B is an element, which is typically selected from N, P, As, Sb, Bi, S, Se, Te, F, Cl, Br or I.
[0020] If B is selected from N, P, As, Sb, and Bi, n is 4. If B is selected from S, Se, and Te, n is 3. If B is selected from F, Cl, Br, and I, n is 2.
[0021] The aryl group of the onium salt is typically derived from an aromatic hydrocarbon ring such as a phenyl or naphthyl, and is covalently bound to B. The aryl group may also be a phenyl or naphthyl functional group without further substituents. The substituents A may also solely comprise aryl groups, which may be the same or different from each other. “Different” in this context may refer to the aryl having different substituents or having the same substituents but in a different position.
[0022] Other substituents A may for example be selected from alkyl or alkoxy groups.
[0023] The anionic portion [XYm]' of the onium salt may generally be selected from those anions that are known to be suitable for the intended purpose.
[0024] Typically, it may be provided that X is selected from Sb, As, P, Al or B (boron). If X is selected from Sb, As, P, m is 6. If X is selected from Al or B, m is 4. Y typically is a halogen, in particular F, when X is Sb, As, P or B. Y may also be a perfluorinated aryl group, in particular perfluorophenyl, when X is B. Y typically is a perfluorinated alkoxide group, when X is Al. X generally forms the core atom of the anion, with Y being covalently bound to X. The substituents Y may be the same or different from each other.
[0025] The anion [XYm]' determines the strength of the acid formed upon photoinitiator excitation. In general, low nucleophilicity of the anion is desired to form an acid, which readily donates protons.
[0026] Preferably, it may be provided that the cationic component of the onium salt is selected from diaryliodonium cations and triarylsulfonium cations, and / or the anionic component of the onium salt is selected from SbF6‘, AsF6‘, PF6‘, BF4', tetrakis(pentafluorophenyl)borate ([C24BF20]') and tetrakis(perfluoro-tert- butoxy)alum inate ([Ci6F36AIO4]').
[0027] Perfluorinated aluminates may also be selected from AI[OC(Ph)(CF3)2]4', AI[OCH(CF3)2]4’, AI[OC(CH3)(CF3)2]4’ or AI[OC(CF3)3]4’.
[0028] Specific examples of onium salts for use in the present invention are diaryliodonium salts. Those include: diphenyliodonium hexafluorophosphate, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroarsenate, diphenyliodonium tetrakis(perfluoro-tert-butoxy)aluminate, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, bis(4-tert-butylphenyl)iodonium tetrafluoroborate, , bis(4-tert- butylphenyl)iodonium tetrakis(perfluoro-tert-butoxy)alum inate, (4-lsobutylphenyl)(p- tolyl)iodonium, hexafluorophosphate, [4-(2-hydroxytetradecyl)oxy]phenyliodonium hexafluoroantimonate, (4-(octyloxy) phenyl) (phenyl) iodonium hexafluoroantimonate, (4-(1 -methylethyl)phenyl)-(4-methylphenyl)iodonium tetrakis(pentafluorophenyl)borate.
[0029] Also triarylsulfonium salts may be used. Those include: (4-hydroxyphenyl)- dimethylsulfonium hexfluoroantimonate, dimethylphenacylsulfonium tetrafluoroborate, triphenylsulfonium tetrafluoroborate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrakis(perfluoro-tert- butoxy)alum inate, tri-p-toylsulfonium hexafluorophosphate, diphenyl [4- (phenylthio)phenyl]sulfonium hexafluoroantimonate, diphenyl [4- (phenylthio)phenyl]sulfonium hexafluorophosphate.
[0030] Generally, it may be provided that the photoinitiator has an absorption maximum at a wavelength of between 200 nm and 450 nm.
[0031] Commonly used wavelengths for curing, are 365 nm, 385 nm, 395 nm and 405 nm. Therefore, a maximum absorption of the photoinitiator is preferably between 350 nm and 410 nm.
[0032] It may be provided that the reducing agent is capable of reducing and / or lowering the charge of B when the cationic component of the onium salt is present in its basic state with the general formula [AnB]+and / or when the cationic component of the onium salt is present as a radical species with the general formula [An.iB*]+. Typically, radicals and cations generated from the photo-excited singlet state with [An.1B*]+or triplet state with [AB] of an onium salt lead to the formation of a strong Bronsted acid starting the cationic polymerization. The following cationic polymerization pathway, for example a ring-opening cationic polymerization, is highly exothermic. The exothermic nature of the reaction thus enables cleavage of the thermally inducible radical forming agent, which in turn produces a radical species. The carbon-centered radicals may then be oxidized to carbocations in the presence of the onium salt, which then continue the cationic polymerization.
[0033] A person skilled in the art will be capable of selecting a reducing agent, which is suitable for the intended purpose. In particular, the selection of the reducing agent will depend on the specific onium salt and / or the used monomer. The reduction potential of the reducing agent will be a guidance for the selection.
[0034] It may be provided that the reducing agent is selected from:
[0035] - thiophenol compounds,
[0036] - ascorbic acid and suitable ascorbic acid derivatives,
[0037] - citric acid and suitable citric acid derivatives,
[0038] - metallocene compounds,
[0039] - Cu(l) halides,
[0040] - organic Co(ll) salts,
[0041] - Sn(ll) salts, preferably organic Sn(ll) salts.
[0042] These compounds are known to form redox couples with at least some of the above- mentioned onium salts. The presence of the reducing agent accelerates the curing reaction and lowers the temperature required for starting the reaction.
[0043] Preferably, it may be provided that
[0044] - the thiophenol compound is selected from thiophenol, pentachlorothiophenol or thiosalicylic acid,
[0045] - the ascorbic acid derivative is a carboxylic acid ester of ascorbic acid, such as ascorbyl palmitate, ascorbyl oleate or ascorbyl acetate,
[0046] - the metallocene is selected from ferrocene and t-butyl ferrocene,
[0047] - the Cu(l) halide is selected from CuCI, CuBr, and Cui, - the organic Co(ll) salt is selected from Co2(CO)6[(C6H5)3P]2, Co(CO)6[(C6H5)2P- CH3C6H4]2, (C7HI5CO2)2CO,
[0048] - the Sn(ll) salt is selected from Sn(ll) 2-ethylhexanoate, Sn(ll) stearate, Sn(ll) laurate, Sn(ll) citrate, Sn(ll) oxalate and Sn(ll) benzoate.
[0049] More preferably, it may be provided that the reducing agent is Sn(ll)-2-ethylhexanoate. Sn(ll)-2-ethylhexanoate is registered in the REACH repository and will therefore provide the possibility to obtain compositions with low health hazards.
[0050] In further specific embodiments of the invention, the reducing agent may be an organic Sn(ll)-salt.
[0051] In the composition, the thermally inducible radical forming agent is typically different from the photoinitiator, i.e., these two substances are distinct or different substances.
[0052] The thermally inducible radical forming agent is capable of forming a reactive species upon exposure to heat. Such compounds are generally known to a person skilled in the art.
[0053] The reactive species of the thermally inducible radical forming agent is typically capable of being oxidized to form a reactive species capable of reacting with the polymerizable monomer present within the composition. The thermally inducible radical forming agent forms a radical or radicals upon exposure to heat, for example via homolytic cleavage of a peroxide bond. This heat may particularly be generated during the polymerization reaction.
[0054] It may be provided that the thermally inducible radical forming agent is an organic peroxide, such as benzoyl peroxide or a pinacol-type compound, in particular benzopinacol and a suitable benzopinacol derivative.
[0055] The thermally inducible radical forming agent may be capable of forming radicals at a temperature of below 300°C.
[0056] Organic peroxides may specifically be selected from compounds such as te / t-butyl hydroperoxide, cumene hydroperoxide, di-te / Y-butyl peroxide, dicumyl peroxide, benzoyl peroxide, 2-butanone peroxide and 4-hydroxy-4-methyl-2-pentanone and N-methyl-2- pyrrolidone.
[0057] In particular, benzopinacol has shown to be a suitable thermally inducible radical forming agent in radical induced cationic frontal polymerization as benzopinacol can cause the decomposition of cationic photoinitiators and radical polymerization of a respective monomer.
[0058] The thermally inducible radical forming agent may be capable of forming radicals, in particular thermally generated radicals, below 150°C.
[0059] Cationically polymerizable monomers M, which may be employed in the context of the present invention, contain at least two functional groups being selected from a cyclic ether group and a vinyl ether group.
[0060] The cyclic ether group may be an epoxide group, an oxetane group, or a lactide group.
[0061] Generally, these functional groups may be referred to as polymerizable functional groups. Two or more different polymerizable functional groups may be present in the monomer. However, the at least two polymerizable functional groups contained in one monomer molecule are usually the same.
[0062] Suitable epoxide-based monomers may be selected from bisphenol A diglyceride ether (2,2-bis(4-glycidyloxyphenyl)propane) and derivatives thereof and / or bisphenol F diglycidyl ether (bis-[4-(glycidyloxy)-phenyl]-methane) and derivatives thereof. Other epoxide-based monomers may be selected from cycloaliphatic epoxides such as 3,4- epoxycyclohexylmethyl-3',4'-epoxycyclohexane carboxylate or bis((3,4- epoxycyclohexyl)methyl) adipate.
[0063] Suitable oxetanes may be selected from 4,4-bis[3-ethyl-3-oxetanyl)methoxymethyl] bisphenyl or 1 ,4-bis[3-ethyl-3-oxetanyl)methoxymethyl]benzene. A lactide may be selected from (R,R)-lactide, (S,S)-lactide and meso-lactide or mixtures of all three isomers. Vinyl ethers may be selected from vinyl ethers capable of undergoing a cationic living polymerization. Preferably, it may be provided that the cationically polymerizable monomer M is a diepoxy compound.
[0064] Di-epoxy compounds have shown to be particularly advantageous in practice. For example, cycloaliphatic epoxy monomers are commonly used for photopolymerization processes due to their low molecular weight allowing tunable processing viscosity. They are also characterized by their higher cyclic ether ring strain making them an ideal choice for thermal frontal polymerization processes.
[0065] As a general remark concerning the composition of the present invention, it shall be mentioned that the expression “containing” is to be understood as encompassing the meanings “comprising” and “consisting of”. This means that a composition containing a cationically polymerizable monomer M; a photoinitiator; a thermally inducible radical forming agent; and a reducing agent may also contain further components or no further components.
[0066] Any component mentioned herein may be one single chemical compound or a mixture of two or more chemical compounds from the respective group. For example, the cationically polymerizable monomer of the invention may be a substance which essentially contains only one type of cationically polymerizable monomer molecules, or which contains two or more different types of cationically polymerizable monomer molecules.
[0067] The cationically polymerizable monomer generally is to be understood as comprising functional groups capable of forming a polymer via a cationic polymerization pathway.
[0068] The photoinitiator in the present disclosure generally is a chemical compound capable of forming a reactive species upon exposure to electromagnetic radiation, such as UV or visible light of a certain wavelength, X-rays, electron beam, and / or heat. The reactive species of the photoinitiator is capable of reacting with the polymerizable monomer present within the composition initiating the polymerization reaction.
[0069] A specific composition according to the present invention may contain the following components: A diglycidyl ether as monomer; (4-(octyloxy)phenyl))(phenyl)iodonium hexafluoroantimonate as photoinitiator; benzopinacol as thermally inducible radical forming agent; and Sn(ll)-octoate as reducing agent. The diglycidyl ether may be a mixture of different diglycidyl ethers.
[0070] A specific composition according to the present invention may contain the following components: A cycloaliphatic epoxide as monomer; (4- (octyloxy)phenyl))(phenyl)iodonium hexafluoroantimonate as photoinitiator; benzoyl peroxide as thermally inducible radical forming agent; and Sn(ll)-octoate as reducing agent. The monomer may comprise a mixture of a cycloaliphatic epoxide and another cyclic ether.
[0071] It may be provided that the composition comprises 0.1 to 5.0 wt.-% photoinitiator in relation to the total weight of cationically polymerizable monomer M. Depending on the reactivity of cyclic ether or vinyl monomer used, the amount of used photoinitiator lies in the upper range for slowly reacting monomers such as bisphenol A diglycidylether. For highly reactive monomers such as oxetanes or cycloaliphatic epoxy, lower amounts of photoinitiator may be sufficient.
[0072] It may be provided that the composition comprises 0.1 to 5.0 wt.-% thermally inducible radical forming agent in relation to the total weight of cationically polymerizable monomer M. Depending on the reactivity of cyclic ether or vinyl monomer used, the amount of used thermally inducible radical forming agent lies in the upper range for slowly reacting monomers such as bisphenol A diglycidylether. For highly reactive monomers such as oxetanes or cycloaliphatic epoxy, lower amounts of thermally inducible radical forming agent may be sufficient.
[0073] It may be provided that the composition comprises 0.1 to 5.0 wt.-% reducing agent in relation to the total weight of cationically polymerizable monomer M. Depending on the reactivity of cyclic ether or vinyl monomer used, the amount of used reducing agent lies in the upper range for slowly reacting monomers such as bisphenol A diglycidylether. For highly reactive monomers such as oxetanes or cycloaliphatic epoxy, lower amounts of reducing agent may be sufficient.
[0074] It may be provided that the total weight of the cationically polymerizable monomer M amounts to more than 30 wt.-% of the total weight of the composition. Besides monomer, photoinitiator, thermally inducible radical forming agent, and reducing agent, further substances or additives may be contained in the composition such as sensitizers or filler materials like carbon fiber or glass fiber. Especially filler materials may be added in relatively high quantities to obtain composite polymers. The beneficial effects of the present invention may be employed particularly well in compositions with high filler contents. However, in order to ensure a strong composite material, a minimum amount of monomer M is required.
[0075] An additive may be selected from one or more of the following: pigments; fibers, such as carbon or glass fibers; filler particles; stabilizers; dyes; sensitizers.
[0076] The composition may comprise a number of different additives in suitable quantities.
[0077] The additives include commonly used and well-known compounds. Additives may aid in the polymerization reaction, but they may also not be involved in the reaction process. The latter is typically the case for fillers.
[0078] Pigments, fibers and dyes may influence the material properties of the resulting (composite) polymer.
[0079] Stabilizers are compounds used to increase stability of the composition and may include radical scavengers such as butylated hydroxy toluene or light-absorbers.
[0080] Sensitizers generally absorb electromagnetic radiation and transfer the absorbed energy into neighboring molecules. Among suitable sensitizers is the compound 1- chloro-4-propoxythioxanthone, which is well known in the art.
[0081] It may be provided that the additive or at least one additive, if multiple additives are contained in the composition, is an opaque material. Such a material may for instance be a pigment or fibers, such as carbon fibers, or other organic or inorganic filler particles.
[0082] It may be provided that the at least one additive are fibers and / or filler particles, wherein the fibers and / or filler particles are contained in the composition in an amount of at least 20 vol. -% , in particular at least 40 vol.-%, in relation to the total volume of the composition. A maximum of 70 vol.-%, or preferably a maximum of 60 vol.-%, of fibers and / or filler particles may be contained in the composition.
[0083] Fiber-reinforced composite polymers, in particular containing glass or carbon fiber, resulting from the polymerization reaction of the composition of the present invention generally result in tack-free and lightweight materials with good material strength. Such composite polymers for instance find application in the automotive, aerospace or construction industry.
[0084] The present invention may also relate to a use of the composition described herein for frontal polymerization of a cationically polymerizable monomer.
[0085] The present invention also relates to a method for frontal polymerization of a cationically polymerizable monomer M, using the previously described composition. The method may comprise an initiation step, in which the polymerization reaction is initiated by irradiation of the composition with electromagnetic radiation and / or by exposure of the composition to a temperature of at least 100°C, in particular of between 100°C and 300°C. A further step of the method may be a polymerization reaction propagation step.
[0086] In the polymerization reaction propagation step, no or substantially no external energy may be input in order to sustain the polymerization reaction.
[0087] The initiation step may be performed for a predetermined time period. The exposure of the composition to an external energy source such as electromagnetic radiation or heat may start the polymerization reaction. The propagation step involves the self-sustained growth of the polymer chains or polymer network via a cationic polymerization mechanism until the monomer M is essentially completely consumed.
[0088] It may be provided that the electromagnetic radiation used in the initiation step has a wavelength suitable for generating a radical species of the cationic component of the onium salt, wherein the radical species has the general formula [An.1B*]+.
[0089] It may be provided that the irradiation during the initiation step is performed for less than 1 min, preferably for less than 30 s, wherein the power flux density of the electromagnetic radiation applied to the composition is at least 50 mW / m2, in particular at least 100 mW / m2
[0090] A one-time energy input via electromagnetic irradiation may enable energy efficient curing. The power flux should be chosen so that a sufficient amount of photoinitiator molecules is excited to start a polymerization reaction throughout the depth of the entire composition.
[0091] It may be provided that the electromagnetic radiation used for irradiation has a wavelength of between 200 nm and 450 nm.
[0092] The wavelength of the electromagnetic irradiation is selected according to the absorption maximum of the photoinitiator contained in the composition. Typical absorption wavelengths are between 300 nm and 400 nm but may also lie below 300 nm or above 400 nm, depending on the specific photoinitiator.
[0093] It may be provided that during the polymerization reaction propagation step, the polymerization reaction proceeds via thermal generation of radicals from the thermally inducible radical forming agent, wherein the temperature in every part of the composition is below 300°C.
[0094] This is advantageous as high temperatures over an extended period of time can lead to decomposition or boiling off the monomer or other components present in the composition. The presence of the reducing agent in the composition enables keeping the temperature during the polymerization reaction low enough to prevent decomposition or boiling off.
[0095] During the propagation step, a thermal front may travel through the composition. The material which lies behind this front is typically cured polymer, whereas the material, which has not yet been reached by the front is uncured, i.e., contains essentially unreacted monomer.
[0096] Further features of the invention can be derived from the patent claims and the following description of exemplary embodiments of the invention. The following section discloses exemplary embodiments of the present invention. These embodiments are intended to demonstrate particularly advantageous effects of the invention, but they are not intended to limit the scope of the patent claims.
[0097] Examples
[0098] Example 1
[0099] A frontally curable epoxy composition according to the invention was prepared, comprising a resin with the monomers bisphenol A diglycidyl ether and 1 ,4-butanediol diglycidyl ether (commercially available under the brand name Litestone 2130E). (4- (octyloxy) phenyl))(phenyl) iodonium hexafluoroantimonate was used as photoinitiator, benzopinacol as thermally inducible radical forming agent, and Sn(ll)-2-ethylhexanoate as the reducing agent. The components were contained in the following amounts: 96.6 wt.-% monomer, 1.93 wt.-% photoinitiator, 0.47 wt.-% thermally inducible radical forming agent, and 0.97 wt.-% reducing agent, all relative to the total weight of the composition.
[0100] The photoinitiator and the reducing agent were admixed to the monomer without any further treatment. Benzopinacol was ground to a fine powder before mixing to the composition in a speed mixer.
[0101] The resin composition was cast into a silicon mold and was then cured by exposing the mixture to a temperature of approx. 150°C for less than 10 min.
[0102] Example 2 (comparative)
[0103] A frontally curable epoxy composition according to the prior art was prepared in analogy to Example 1 described above, with the difference that no reducing agent was included in the reaction mixture.
[0104] The amounts of the components contained in the composition were as follows: 97.0 wt.- % monomer, 1.5 wt.-% photoinitiator, and 1.5 wt.-% thermally inducible radical forming agent, all relative to the total weight of the composition. Example 3
[0105] The composition was prepared using the epoxy resin 3,4-epoxycyclohexylmethyl-3',4'- epoxycyclohexane carboxylate as monomer, photoinitiator (4-(octyloxy) phenyl))(phenyl) iodonium hexafluoroantimonate, thermally inducible radical forming agent benzoyl peroxide, reducing agent Sn(ll)-2 -ethylhexanoate, and sensitizer 1- chloro-4-propoxythioxanthone. The mixture was speed mixed for 5 minutes until homogenous.
[0106] The amounts of the components contained in the composition were as follows: 98.0 wt.- % monomer, 0.49 wt.-% photoinitiator, 0.40 wt.-% thermally inducible radical forming agent, 0.42 wt.-% reducing agent, and 0.61 wt.-% sensitizer, all relative to the total weight of the composition.
[0107] The composition was poured into an aluminium cup and then irradiated for 15 seconds with an LED lamp at 405 nm (150 mWcm’2) to initiate the curing front at room temperature. Then, the mixture was left until the reaction was completed without exposure to an external radiation or heat source.
[0108] The resulting polymer was clear, without visible bubbles, tack free and could be removed easily from the mold.
[0109] Example 4 (comparative)
[0110] The composition was prepared in the same way as example 2 but without addition of the reducing agent Sn(ll)-2-ethylhexanoate.
[0111] Upon irradiation, instant fuming followed by rapid bubble formation began, resulting in a foamed and cracked polymer.
[0112] A comparison with the polymer of Example 3 demonstrates that the inventive composition is superior, as in Example 4, a polymer material with undesirable properties was obtained. The polymer of Example 4 is not suitable for actual use. Example 5
[0113] The frontally polymerizable composition was prepared in the same way as in Example 1.
[0114] However, before curing, a carbon fiber plate comprised of Non Crimp-Fabric carbon fiber and carbon fiber weave with 30 mm thickness was prepared and impregnated with this mixture. Thus, the composition according to this Example contained the mixture described in Example 1 along with the carbon fiber weave. The carbon fiber weave was contained in the composition in an amount of approx. 55 vol.-%.
[0115] The composite composition was cured in the same way as described in Example 1. During curing, the temperature in the middle of the composite composition reached a maximum temperature of 238 °C. The cured composite material was tack free and intact with no visible sign of degradation.
[0116] Characterization of the prepared polymers
[0117] The polymers were characterized using the below-described methods.
[0118] Differential Scanning Calorimetry (DSC)
[0119] Non-isothermal DSC was performed using Perkin Elmer 4000 on specimens (15-20 mg) cut from samples that were cured in the silicon mold or in aluminium cups, depending on what has been described above. The DSC was performed for two heating runs at 20°C / min with the first run from 20°C-160°C followed by cooling to 20°C, and the second heating from 20°C-210°C, as per DIN EN ISO 11357. Each measurement was replicated twice and the best curves used for mid-point glass transition temperature measurement.
[0120] Dynamic mechanical analysis (DMA) and tensile tests
[0121] The DMA was performed on a Mettler Toledo DMA 861 in three-point bending mode according to DIN EN ISO 6721-5. The specimens were cured on silicon molds with dimensions measuring 70 x 10 x 3 mm or in the dimension of multi-purpose test specimens according to DIN EN ISO 527-2 and the samples for DMA were cut away from the shoulder part to obtain 70x10x3 mm dimensions. DMA was performed for a temperature range of 0 between 220°C at 2 °C / min with an oscillation of 1 Hz and 200% offset. The force and displacement were set to 40 N and 100 microns respectively.
[0122] The tensile tests were performed on a Zwick Z250 machine with a pre-load of 0.25 MPa and test speed of 2 mm min'1.
[0123] Glass transition temperature and cross-linking density
[0124] The mid-point glass transition temperature (Tg) of the resin frontally cured without Sn(ll) 2-ethylhexanoate (Example 2, not inventive) was 53°C whereas, the Tgof the frontally cured resin containing Sn(ll) 2-ethylhexanoate (Example 1 , inventive) was 90°C.
[0125] To further verify the changes in Tgof the frontally cured resin with and without Sn( 11)-2- ethylhexanoate, a cross-linking density calculation was done using the approximation, that the modulus of elasticity in the rubbery region at temperature T, is equal to 3 times the shear modulus at that temperature T.
[0126] The calculated cross-link density of the polymers from Examples 1 and 2 were 5345 mol / m3for Example 1 and 2200 mol / m3for Example 2.
[0127] The results show an approx, two-fold increase in the cross-linking density with the addition of Sn(ll)-2 -ethylhexanoate, which demonstrates the improvement in polymer formation using the composition of the invention.
[0128] For Example 3, the results showed a glass transition temperature of 61 °C and additionally, a large post curing effect, wherein the glass transition temperature from the first to the second heating run in DSC increased to 110°C. While the composition of Example 3, containing Sn(ll) 2-ethylhexanoate, gave a high glass transition temperature of 109°C in the first heating run and only a slight increase in Tgto 120°C after the second heating run. The glass transition temperature of the material produced in Example 3 was further verified with DMA analysis with a Tgof 108°C. Comparative DMA samples of Example 4 could not be prepared due to the poor material properties of the resulting polymer.
[0129] The tensile strength of the material obtained in Example 3 was determined to evaluate the mechanical performance of the resin. The average tensile strength of Example 3 was 30.0 ± 6.1 MPa, the tensile modulus 2.8 ± 0.12 GPa and the strain at break 1 .1 ± 0.30% (n=5 for all measurements).
[0130] It was not possible to prepare tensile test specimens of Example 4 to compare material properties, since the material properties of the polymer resulting from Example 4 were too poor.
[0131] Further examples
[0132] The following specific compositions can be prepared in a similar way as described above:
[0133] Pentachlorothiophenol or thiosalicyclic acid as reducing agent and sulfonium salts as photoinitiator with bisphenol A (BPA) and all types of substituted BPA and also cycloaliphatic epoxy (CE) as monomer.
[0134] Ferrocene as reducing agent in combination with diaryliodonium antimonate or arsenate as photoinitiator can cure both BPA and CE.
[0135] Cobalt salts as reducing agent and iodonium salt as photoinitiator also successfully cured CE and BPA.
[0136] Ascorbic acid as reducing agent and diaryliodonium salt as photoinitiator in combination with CE and BPA.
[0137] Copper (I) bromide as reducing agent and diaryliodonium salts as photoinitiator have shown a redox couple capable of curing at least CE.
Claims
Claims1 . A composition for cationic frontal polymerization, containing:- a cationically polymerizable monomer M,- a photoinitiator, the photoinitiator being an aromatic onium salt having the general formula [AnB]+[XYm]', wherein at least one of the substituents A is an aryl functional group, o wherein B is selected from N, P, As, Sb, and Bi, and wherein n is 4, or o wherein B is selected from S, Se, and Te, and wherein n is 3, or o wherein B is selected from F, Cl, Br, and I, and wherein n is 2,- a thermally inducible radical forming agent, the radical forming agent being different from the photoinitiator, characterized in that the composition further contains a reducing agent, wherein the reducing agent is capable of reducing and / or lowering the charge of B in the onium salt.
2. The composition according to claim 1 , characterized in that the reducing agent is capable of reducing and / or lowering the charge of B when the cationic component of the onium salt is present in its basic state with the general formula [AnB]+and / or when the cationic component of the onium salt is present as a radical species with the general formula [An.iB*]+.
3. The composition according to claim 1 or 2, characterized in that X is selected from i) Sb, As, P, wherein m is 6, ii) Al, B, wherein m is 4, and wherein Y is a halogen, in particular F, when X is Sb, As, P, wherein Y is F or a perfluorinated aryl group, when X is B, wherein Y is a perfluorinated alkoxide group, when X is Al.
4. The composition according to any of claims 1 to 3,- wherein the cationic component [AnB]+of the onium salt is selected from diaryliodonium cations and triarylsulfonium cations, and / or- wherein the anionic component [XYm]' of the onium salt is selected from SbF6‘ , ASF6‘, PF6‘, BF4', tetrakis(pentafluorophenyl)borate ([C24BF20]') and tetrakis(perfluoro-tert-butoxy)alum inate ([Ci6F36AIO4]').
5. The composition according to any of claims 1 to 4, characterized in that the photoinitiator has an absorption maximum at a wavelength of between 200 nm and 450 nm.
6. The composition according to any of claims 1 to 5, characterized in that the cationically polymerizable monomer M contains at least two functional groups, being selected from one or more of the following:- a cyclic ether group, in particular selected from one or more of an epoxide group, an oxetane group, and a lactide group, and / or- a vinyl ether group.
7. The composition according to claim 6, characterized in that the cationically polymerizable monomer M is a di-epoxy compound.
8. The composition according to any of claims 1 to 7, characterized in that the thermally inducible radical forming agent is i) an organic peroxide, such as benzoyl peroxide, ii) a pinacol-type compound, in particular benzopinacol and a suitable benzopinacol derivative, wherein the thermally inducible radical forming agent preferably is capable of forming radicals at a temperature of below 300°C.
9. The composition according to any of claims 1 to 8, characterized in that the reducing agent is selected from:- thiophenol compounds,- ascorbic acid and suitable ascorbic acid derivatives,- citric acid and suitable citric acid derivatives,- metallocene compounds,- Cu(l) halides,- organic Co(ll) salts,- Sn(ll) salts, preferably organic Sn(ll) salts.
10. The composition according to claim 9, wherein- the thiophenol compound is selected from thiophenol, pentachlorothiophenol or thiosalicylic acid,- the ascorbic acid derivative is a carboxylic acid ester of ascorbic acid, such as ascorbyl palmitate, ascorbyl oleate or ascorbyl acetate,- the metallocene is selected from ferrocene and t-butyl ferrocene,- the Cu(l) halide is selected from CuCI, CuBr, and Cui,- the organic Co(ll) salt is selected from Co2(CO)6[(C6H5)3P]2, Co(CO)6[(C6H5)2P- CH3C6H4]2, (C7HI5CO2)2CO,- the Sn(ll) salt is selected from Sn(ll) 2-ethylhexanoate, Sn(ll) stearate, Sn(ll) laurate, Sn(ll) citrate, Sn(ll) oxalate and Sn(ll) benzoate.11 . The composition according to claim 9 or 10, wherein the reducing agent is Sn(ll)- 2-ethylhexanoate.
12. The composition according to any of claims 1 to 11 , characterized in that the composition comprises 0.1 to 5.0 wt.-% photoinitiator in relation to the total weight of cationically polymerizable monomer M.
13. The composition according to any of claims 1 to 12, characterized in that the composition comprises 0.1 to 5.0 wt.-% thermally inducible radical forming agent in relation to the total weight of cationically polymerizable monomer M.
14. The composition according to any of claims 1 to 13, characterized in that the composition comprises 0.1 to 5.0 wt.-% reducing agent in relation to the total weight of cationically polymerizable monomer M.
15. The composition according to any of claims 1 to 14, characterized in that the total weight of the cationically polymerizable monomer M amounts to more than 30 wt.- % of the total weight of the composition.
16. The composition according to any of claims 1 to 15, characterized in that the composition additionally comprises at least one additive, the additive being selected from one or more of the following: pigments; fibers, such as carbon or glass fibers; filler particles; stabilizers; dyes; sensitizers.
17. The composition according to claim 16, characterized in that the additive or at least one additive, if multiple additives are contained in the composition, is an opaque material.
18. The composition according to any of claims 1 to 17, characterized in that the at least one additive of the composition are fibers and / or filler particles, wherein the fibers and / or filler particles are contained in the composition in an amount of at least 20 vol.-%, in particular at least 40 vol.-%, in relation to the total volume of the composition.
19. The composition according to any of claims 1 to 18, characterized in that the photoinitiator has a diaryliodonium; in that the thermally inducible radical forming agent is pinacol and / or an organic peroxide; and in that the reducing agent is an organic Sn(ll) salt, in particular Sn(ll)-2-ethylhexanoate.
20. A use of a composition according to any of claims 1 to 19 for frontal polymerization of a cationically polymerizable monomer.21 . A method for frontal polymerization of a cationically polymerizable monomer M, using a composition according to any of claims 1 - 19, the method comprising:- an initiation step, in which the polymerization reaction is initiated by irradiating of the composition by electromagnetic radiation and / or by heating the composition to a temperature of at least 100°C, in particular of between 100°C and 300°C, and- a polymerization reaction propagation step.
22. The method according to claim 21 , characterized in that in the polymerization reaction propagation step no irradiating and / or heating, in particular no heating by external means, of the composition is performed.
23. The method according to claim 21 or 22, characterized in that the electromagnetic radiation used for initiation has a wavelength suitable for generating a radical species of the cationic component of the onium salt having the general formula [An.iB-]+.
24. The method according to any of claims 21 to 23, characterized in that irradiating during the initiation step is performed for less than 1 min, preferably for less than 30 s, wherein the power flux density of the electromagnetic radiation applied to the composition is at least 50 mW / m2, in particular at least 100 mW / m2.
25. The method according to any of claims 21 to 24, characterized in that the electromagnetic radiation used for irradiating the composition has a wavelength of between 200 nm and 450 nm.
26. The method according to any of claims 21 to 25, characterized in that during the polymerization reaction propagation step, the polymerization reaction proceeds via thermal generation of radicals from the thermally inducible radical forming agent, wherein the temperature in every part of the composition is below 300°C.
Citation Information
Patent Citations
Polymerizing composition, method of manufacture thereof and articles comprising the same
CA3198838A1
Power facility measurement phase verification device and method
KR1020230156591A
Process for frontal polymerization of cationically polymerizable monomers
US10738146B2