Production method for explosion-proof polyester needle punched felt
By using a hybrid fiber felt of anti-static microporous membrane and anti-static fibers in industrial needle felt, combined with steam hot pressing molding and flow rate control technology, the problem of explosive needle felt is solved, and higher anti-static and Explosion-proof effect improves safety and production simplicity.
Patent Information
- Application Number
- PCT/CN2023/094105
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-21
AI Technical Summary
During use, existing industrial needle felts are prone to explosion due to static electricity, which in turn causes fires and reduces safety factors.
The anti-static microporous membrane and anti-static fiber mixed fiber felt are formed by steam hot pressing to form a double anti-static layer, enhancing the anti-static and explosion-proof effects, and optimizing the hot pressing mold through the flow rate control mechanism and the membrane cutting structure to ensure the coating effect and structural simplicity.
It significantly improves the anti-static and explosion-proof performance of needle felt, enhances overall safety, simple structural design and stable coating effect, avoiding the complexity of subsequent processing.
Smart Images

Figure CN2023094105_21112024_PF_FP_ABST
Abstract
Description
A production method of explosion-proof polyester needle-punched felt Technical Field
[0001] The present invention relates to the technical field of needle-punched felt preparation, and more particularly to a method for producing explosion-proof polyester needle-punched felt. Background Art
[0002] Industrial needle felt is a dust removal device made by sewing industrial filter cloth. Industrial filter cloth is a filter medium woven from natural fibers and synthetic fibers. It is mainly used for solid-liquid separation and industrial dust removal. Bag dust collector is a high-efficiency dry dust collector. It relies on filter bags made of fiber filter materials. More importantly, it purifies the gas through the dust layer formed on the surface of the filter bag. For almost all dust in general industry, its dust removal efficiency can reach more than 99%. The core component of the belt dust collector is the needle felt.
[0003] The filter cloth materials of the existing industrial needle-punched felt used in belt dust collectors are gradually made of organic and inorganic artificial fiber fabrics such as nylon, Orlon, polyester, and glass fiber, or their blends. In actual use, especially when used for dust removal of metal powders such as magnesium powder, the needle-punched felt is prone to explosion due to the large static effect, which can easily lead to fire and reduce the safety factor. Summary of the Invention
[0004] In view of the shortcomings of the existing technology, the purpose of the present invention is to provide a production method for obtaining a needle-punched felt with good antistatic effect and explosion-proof effect after preparation, which has a simple preparation method and a high degree of molding integration.
[0005] To achieve the above-mentioned object, the present invention provides the following technical solution: A method for producing explosion-proof polyester needle-punched felt, comprising the following steps: S1, preparing an antistatic microporous membrane: adding an antistatic material to a polytetrafluoroethylene resin raw material, mixing the above-mentioned materials evenly, introducing them into an extruder, and obtaining an antistatic microporous membrane with a thickness of 15-30 μm, a porosity of 50%-85%, and a pore size distribution of 0.3-5 μm by extrusion, calendering, stretching, and heat setting. The obtained antistatic microporous membrane is used as a preparation, wherein the extrusion temperature is 200°C-300°C, the calendering pressure is between 200N-500N, the biaxial stretching is made into a thickness of 5-50 μm, and the heat setting temperature is between 150°C-180°C;
[0006] S2. Preparation of a mixed fiber felt: Polyester fiber and antistatic fiber are uniformly mixed in a weight ratio of 40-60:20-30 to obtain a mixed fiber; the mixed fiber is fed from a cotton feeder to a carding machine for carding to form a mixed fiber web; the mixed fiber web is fed to a cotton laying machine, and multiple layers of mixed limiting nets are laid to form a mixed fiber felt; the mixed fiber felt is needling-punched on a needle loom at a needling speed of 500-600 rpm to obtain a polyester needle-punched felt semi-finished product;
[0007] S3, placing the polyester needle felt semi-finished product after needle punching and reinforcement in step S2 in a hot pressing mold for hot pressing and laminating under vacuum, with the windward side of the polyester needle felt semi-finished product being the hot pressing and laminating side;
[0008] S4, placing the polyester needle felt semi-finished product treated in step S3 into a cooling fixture, and cooling and shaping it at room temperature for 60 to 70 seconds;
[0009] S5, cutting the polyester needle felt semi-finished product cooled in step S4 into desired dimensions to obtain the polyester needle felt finished product.
[0010] The present invention is further configured as follows: the specific method of hot pressing lamination in step S3 is as follows: S30, laminating the antistatic microporous film obtained in step S1 on the polyester needle-punched felt semi-finished product;
[0011] S32, vacuuming the upper mold of the hot pressing mold for 10 to 20 seconds at a pressure of 0.01 to 0.02 MPa, while introducing high-temperature steam;
[0012] S33, maintaining the vacuum degree, continuing to introduce high-temperature steam for heating and molding, the high-temperature steam pressure is 2.5-3 MPa, the inflation time is between 3 min and 5 min, the high-temperature steam temperature is 150-300°C, the mold pressing pressure is between 300N and 800N, and the molding time is 20-60 seconds, until the hot pressing is completed;
[0013] S34. After the hot pressing is completed, the laminating material is pulled by the traction equipment, and then the high-temperature steam in the upper mold is exhausted, and then the subsequent material that has not been hot pressed is hot pressed and laminated.
[0014] The present invention is further configured as follows: the hot pressing mold includes a steam channel and a flow rate control mechanism arranged in the steam channel, the flow rate control mechanism includes a regulating channel arranged in the steam channel, a regulator arranged in the regulating channel, and a lifting device for driving the regulator to rise and fall and adjust the air outlet volume of the regulating channel, the regulator is configured to form an annular flow channel with the inner wall of the regulator and the air outlet channel when it is lowered to the air outlet channel of the regulating channel; when it is separated from the air outlet channel under the drive of the lifting device, the air outlet channel restores the original ventilation volume.
[0015] The present invention is further configured as follows: a film cutting structure is also provided between the upper and lower molds of the hot pressing mold, and the film cutting structure includes a side cutting groove structure arranged on the lower mold, and a side cutting protrusion arranged on the upper mold and adapted to the side cutting groove structure. A shearing structure is formed between the side cutting groove structure and the side cutting protrusion. The shearing structure is used to form a timely shearing effect with the lower mold after the upper mold is pressed down, so as to shear and cut the excess part of the anti-static microporous membrane.
[0016] The present invention is further configured as follows: a flow regulating structure is provided between the regulator and the air outlet channel, and the flow regulating structure includes a plurality of step structures provided on the regulator, the outer diameter difference between two adjacent step structures is between 2cm-5cm, and the difference between two adjacent step structures is the same, and a primary channel, a secondary channel and a tertiary channel with ventilation volume from large to small are formed between the step structure and the air outlet channel.
[0017] The present invention is further configured as follows: the flow rate control mechanism also includes a control system, which includes an air pressure monitor for real-time monitoring of the steam pressure of the upper mold, a flow rate monitor arranged in the air outlet channel, an electromagnetic on-off valve arranged on the steam channel, and a controller for controlling the start and stop of the lifting device and the opening and closing of the electromagnetic on-off valve. The controller includes a receiving unit electrically connected to the air pressure detector and the flow rate monitor and for receiving electrical signals from the two monitors, a comparing unit for setting standard and warning steam pressure values of the upper mold and comparing them with the monitoring values, and a control unit for controlling the opening and closing of the electromagnetic on-off valve and the start and stop of the lifting device. The control method of the flow rate control mechanism in the steam channel specifically includes the following steps: S330, setting the warning pressure value of the upper mold steam pressure to P0, setting the standard value of the upper mold steam pressure to P, real-time monitoring of the upper mold steam pressure value to Pt, setting the flow rate warning value of the air outlet channel to S, and then introducing steam;
[0018] S331. During the first time period, the comparison unit compares P1 and PO. If P1 is less than P0, the steam flow continues. Conversely, if P1 is greater than P0, the regulator needs to be downgraded by the upgrading device to reduce the steam flow rate and adjust to the primary channel.
[0019] S332: During the second time period, the steam pressure of the upper mold is monitored in real time, P2. The difference between P2 and P is Δ. If Δ is within the reasonable pressure control range, ventilation continues through the primary channel. If Δ is outside the above range, the regulator is lowered by the upgrade device to reduce the steam flow rate and adjust to the secondary channel for ventilation within the time ts until the P value is reached.
[0020] S333. During the above time period, the flow velocity in the outlet channel is monitored in real time as S1. If S1 is greater than the S value, it is determined that the airflow disturbance is large and it is necessary to use the upgrading device to lower the regulator, reduce the steam flow rate, and adjust it to the third-level channel for a time of tp. Otherwise, ventilation is performed according to the currently required ventilation volume.
[0021] S334. During the tp time period, the flow velocity in the outlet channel is monitored in real time as Sp. If Sp is less than the S value, it is determined that the airflow disturbance is small, and ventilation is continued to be adjusted to the currently required ventilation volume; otherwise, ventilation is continued with the three-level channel.
[0022] An explosion-proof polyester needle punched felt suitable for the production method of the above-mentioned explosion-proof polyester needle punched felt, wherein the polyester needle punched felt has a four-layer structure, and the three layers of the polyester needle punched felt are each made by mixing polyester fibers and antistatic fibers, combing and mixing them into a web, and then needle-punching the three-layer mixed fiber web into a felt through a needle-punching process;
[0023] The polyester fiber and the antistatic fiber are evenly mixed in a weight ratio of 40-60:20-30, and the length of the antistatic fiber is between 2-3 cm, and the antistatic fiber is one or more of metal fiber or organic polymer-based metal complex antistatic fiber;
[0024] The antistatic microporous membrane and the mixed fiber felt are laminated on one side by steam hot pressing to obtain a laminated filter material, and the laminated surface of the antistatic microporous membrane is the windward surface of the polyester needle-punched felt; the antistatic material in the antistatic microporous membrane contains at least an antistatic organic polymer.
[0025] By adopting the above technical solution, the beneficial effects are as follows: 1. By adopting an antistatic microporous membrane and a mixed fiber felt mixed with antistatic fibers, and then forming the mixed fiber felt through steam hot pressing, the antistatic effect of the mixed fiber felt is greatly increased, thereby improving the overall explosion-proof effect. The antistatic microporous membrane is coated and the antistatic fibers are mixed to form a double antistatic fiber, which has strong practicality and simple structure.
[0026] 2. The hot pressing mold method is adopted instead of the roller pressing method in order to form a coating on the anti-static microporous membrane through the steam pressure and the pressure generated by the upper and lower molds themselves. The steam mold hot pressing method forms a double pressure effect, which makes the contact area between the anti-static microporous membrane and the filter material larger and the force is more uniform, so that the overall coating effect is better, the practicability is strong, and the structure is simple;
[0027] 3. Further, the hot pressing mold is configured to include a steam channel and a flow rate control mechanism provided in the steam channel, the flow rate control mechanism includes a regulating channel provided in the steam channel, a regulator provided in the regulating channel, and a lifting device for driving the regulator to lift and adjust the gas outlet of the regulating channel. The regulator is configured to form an annular flow channel with the inner wall of the regulator and the gas outlet channel when it is lowered to the gas outlet channel of the regulating channel; when it is separated from the gas outlet channel by the lifting device, the gas outlet channel restores the original ventilation volume. In order to better stabilize the steam pressure of the upper mold, the regulating channel, the regulator and the lifting device are arranged through the flow rate control mechanism, and the ventilation volume in the regulating channel is adjusted by the regulator to control the steam volume, thereby ensuring the stability of the steam pressure and achieving the stable effect of the subsequent steam pressure downward pressure. The pressure of the lower mold is at a standard value, thereby improving the overall film firmness and preventing damage to the anti-static microporous membrane.
[0028] 4. Furthermore, a membrane cutting structure is provided between the upper and lower molds of the hot pressing mold, and the membrane cutting structure is provided, so that the excess part of the antistatic microporous membrane can be cut in real time, which is convenient for the subsequent collection of the filter material and reduces the influence of the excess coating edge on the collection. The membrane cutting structure is provided to include a side cutting groove structure provided on the lower mold and a side cutting protrusion provided on the upper mold and adapted to the side cutting groove structure. A shearing structure is formed between the side cutting groove structure and the side cutting protrusion. The shearing structure is used to form a timely shearing effect with the lower mold after the upper mold is pressed down, so as to shear the excess part of the antistatic microporous membrane. The side cutting groove structure and the side cutting protrusion are provided, so that a shearing effect is formed between the side cutting groove structure and the side cutting protrusion. Because side cutting and pressing are carried out at the same time, the real-time cutting of the edge material after coating can be increased, thereby avoiding subsequent reprocessing. It has strong practicality and simple structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] FIG1 is a schematic diagram of a laminating structure of an embodiment of a method for producing explosion-proof polyester needle felt according to the present invention.
[0030] FIG2 is a schematic cross-sectional view of a hot pressing mold according to an embodiment of a method for producing explosion-proof polyester needle felt of the present invention.
[0031] The reference numerals in the figure are: 1, hot pressing mold; 10, steam channel; 2, regulating channel; 20, regulator; 21, lifting device; 201, annular flow channel; 220, side cutting groove structure; 221, side cutting protrusion; 202, step structure; 203, primary channel; 204, secondary channel; 205, tertiary channel; 3, controller; 30, air pressure monitor; 31, flow rate monitor; 32, electromagnetic on-off valve. Implementation Method
[0032] 1 and 2 , an embodiment of a method for producing explosion-proof polyester needle-punched felt according to the present invention will be further described.
[0033] For ease of explanation, spatial relative terms such as "upper", "lower", "left", and "right" are used in the embodiments to illustrate the relationship between one element or feature shown in the figures and another element or feature. It should be understood that, in addition to the orientation shown in the figures, spatial terms are intended to include different orientations of the device in use or operation. For example, if the device in the figure is inverted, the element described as being "under" other elements or features will be positioned "above" other elements or features. Therefore, the exemplary term "under" can include both upper and lower orientations. The device can be positioned in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here can be interpreted accordingly.
[0034] Moreover, relational terms such as “first” and “second” are merely used to distinguish one component from another having the same name, but do not necessarily require or imply any actual relationship or order between these components.
[0035] A method for producing an explosion-proof polyester needle-punched felt comprises the following steps: S1, preparing an antistatic microporous membrane: adding an antistatic material to a polytetrafluoroethylene resin raw material, mixing the materials uniformly, introducing the materials into an extruder, and obtaining an antistatic microporous membrane having a thickness of 15-30 μm, a porosity of 50%-85%, and a pore size distribution of 0.3-5 μm by extrusion, calendering, stretching, and heat setting. The obtained antistatic microporous membrane is used as a preparation, wherein the extrusion temperature is 200° C.-300° C., the calendering pressure is between 200 N and 500 N, the biaxial stretching is performed to obtain a thickness of 5-50 μm, and the heat setting temperature is between 150° C.-180° C.;
[0036] S2. Preparation of a mixed fiber felt: Polyester fiber and antistatic fiber are uniformly mixed in a weight ratio of 40-60:20-30 to obtain a mixed fiber; the mixed fiber is fed from a cotton feeder to a carding machine for carding to form a mixed fiber web; the mixed fiber web is fed to a cotton laying machine, and multiple layers of mixed limiting nets are laid to form a mixed fiber felt; the mixed fiber felt is needling-punched on a needle loom at a needling speed of 500-600 rpm to obtain a polyester needle-punched felt semi-finished product;
[0037] S3, placing the polyester needle felt semi-finished product after needle punching and reinforcement in step S2 in a hot pressing mold for hot pressing and laminating under vacuum, with the windward side of the polyester needle felt semi-finished product being the hot pressing and laminating side;
[0038] S4, placing the polyester needle felt semi-finished product treated in step S3 into a cooling fixture, and cooling and shaping it at room temperature for 60 to 70 seconds;
[0039] S5, cutting the polyester needle felt semi-finished product cooled in step S4 into desired dimensions to obtain the polyester needle felt finished product.
[0040] By adopting anti-static microporous membrane and mixed fiber felt mixed with anti-static fiber, and then forming through steam hot pressing, the anti-static effect of the mixed fiber felt is greatly increased, thereby improving the overall explosion-proof effect. The anti-static microporous membrane is coated and the anti-static fiber is mixed to form a double anti-static fiber, which has strong practicality and simple structure. By changing the steam mold hot pressing method to the roller coating method, the overall coating stability is good, the temperature is easy to control, the coating area is large, the overall coating pressure is more uniform, the practicality is strong, and the structure is simple.
[0041] The present invention is further configured such that the specific method of hot pressing lamination in step S3 is as follows: S30, laminating the antistatic microporous film obtained in step S1 on the polyester needle-punched felt semi-finished product;
[0042] S32, vacuuming the upper mold of the hot pressing mold for 10 to 20 seconds at a pressure of 0.01 to 0.02 MPa, while introducing high-temperature steam;
[0043] S33, maintaining the vacuum degree, continuing to introduce high-temperature steam for heating and molding, the high-temperature steam pressure is 2.5-3 MPa, the inflation time is between 3 min and 5 min, the high-temperature steam temperature is 150-300°C, the mold pressing pressure is between 300N and 800N, and the molding time is 20-60 seconds, until the hot pressing is completed;
[0044] S34. After the hot pressing is completed, the laminating material is pulled by the traction equipment, and then the high-temperature steam in the upper mold is exhausted, and then the subsequent material that has not been hot pressed is hot pressed and laminated.
[0045] The hot pressing mold method is adopted instead of the roller pressing method in order to form a coating on the anti-static microporous membrane through the steam pressure and the pressure value generated by the downward pressure of the upper and lower molds themselves. The steam mold hot pressing method forms a double pressure effect, which makes the contact area between the anti-static microporous membrane and the filter material larger and the force is more uniform, so that the overall coating effect is better, the practicability is strong, and the structure is simple.
[0046] The present invention is further configured as follows: the hot pressing mold 1 includes a steam channel 10 and a flow rate control mechanism arranged in the steam channel 10, the flow rate control mechanism includes a regulating channel 2 arranged in the steam channel 10, a regulator 20 arranged in the regulating channel 2, and a lifting device 21 for driving the regulator 20 to rise and fall and adjust the air outlet volume of the regulating channel 2, the regulator 20 is configured to form an annular flow channel 201 with the inner wall of the regulator 20 and the air outlet channel when it is lowered to the air outlet channel of the regulating channel 2; when it is driven by the lifting device 21 to separate from the air outlet channel, the air outlet channel restores its original ventilation volume, further by configuring the hot pressing mold 1 to include a steam channel 10 and a flow rate control mechanism arranged in the steam channel 10, the flow rate control mechanism includes a regulating channel 2 arranged in the steam channel 10, a regulator 20 arranged in the regulating channel 2, and a lifting device 21 for driving the regulator 20 to rise and fall and adjust the air outlet volume of the regulating channel 2. The regulator 20 in the regulating channel 2 and the lifting device 21 for driving the regulator 20 to rise and fall and adjust the air outlet volume of the regulating channel 2, the regulator 20 is configured to form an annular flow channel 201 with the inner wall of the regulator 20 and the air outlet channel when it is lowered to the air outlet channel of the regulating channel 2; when it is separated from the air outlet channel by the driving of the lifting device 21, the air outlet channel restores the original ventilation volume. In order to better stabilize the steam pressure of the upper mold, the regulating channel 2, the regulator 20 and the lifting device 21 are set through the flow rate control mechanism, and the ventilation volume in the regulating channel 2 is adjusted by the regulator 20, and the steam volume is controlled to ensure the stability of the steam pressure, so that the subsequent steam pressure is stabilized, the lower mold pressure is at the standard value, the overall coating is firm, and the damage of the anti-static microporous membrane is prevented.
[0047] It should be noted that the steam hot pressing adopted in this application and the control of the steam pressure at the corresponding pressure value are to improve the efficiency of hot pressing lamination, achieve the balance of the upper mold steam pressure, and the consistency of the upper mold surface temperature.
[0048] The present invention is further configured such that a film cutting structure is further provided between the upper and lower dies of the hot pressing die 1, and the film cutting structure includes a side cutting groove structure 220 provided on the lower die, and a side cutting protrusion 221 provided on the upper die and adapted to the side cutting groove structure 220, and a shearing structure is formed between the side cutting groove structure 220 and the side cutting protrusion 221, and the shearing structure is used to form a timely shearing effect with the lower die after the upper die is pressed down, so as to shear and cut the excess part of the antistatic microporous membrane. Furthermore, by providing a film cutting structure between the upper and lower dies of the hot pressing die 1, the excess part of the antistatic microporous membrane is cut in real time by the provided film cutting structure, which is convenient for the subsequent collection of the filter material and reduces the influence of the excess coating edge on the collection. In addition, by setting the film cutting structure to include a side cutting groove structure 220 provided on the lower mold and a side cutting protrusion 221 provided on the upper mold and adapted to the side cutting groove structure 220, a shearing structure is formed between the side cutting groove structure 220 and the side cutting protrusion 221. The shearing structure is used to form a timely shearing effect with the lower mold after the upper mold is pressed down, so as to shear and cut the excess part of the anti-static microporous membrane. By setting the side cutting groove structure 220 and the side cutting protrusion 221, a shearing effect is formed between the side cutting groove structure 220 and the side cutting protrusion 221. Because side cutting and pressing are carried out at the same time, the real-time cutting of the edge material after lamination can be increased, thereby avoiding subsequent reprocessing. It has strong practicality and simple structure.
[0049] The present invention is further configured such that a flow regulating structure is provided between the regulator 20 and the air outlet channel, and the flow regulating structure includes a step structure 202 provided on the regulator 20. A plurality of step structures 202, the outer diameter difference between two adjacent step structures 202 is between 2cm-5cm, and the difference between two adjacent step structures 202 is the same, and a primary channel 203, a secondary channel 204 and a tertiary channel 205 with ventilation volumes from large to small are formed between the step structure 202 and the air outlet channel. The above-mentioned structural setting is adopted, because the step structure 202 provided on the regulator 20 forms a primary channel 203, a secondary channel 204 and a tertiary channel 205 with ventilation volumes from large to small between the regulator 20 and the air outlet channel, thereby making the overall ventilation volume adjustable, having strong practicality and simple structure, and ensuring that the smoothness of steam circulation is increased.
[0050] The present invention is further configured such that the flow rate control mechanism also includes a control system, which includes an air pressure monitor 30 for real-time monitoring of the steam pressure of the upper mold, a flow rate monitor 31 provided in the air outlet channel, an electromagnetic on-off valve 32 provided on the steam channel 10, and a controller 3 for controlling the start and stop of the lifting device 21 and the opening and closing of the electromagnetic on-off valve 32. The controller 3 includes a receiving unit electrically connected to the air pressure detector and the flow rate monitor 31 and for receiving electrical signals from the two monitors, a comparing unit for setting standard and warning upper mold steam pressure values and comparing them with the monitoring values, and a control unit for controlling the opening and closing of the electromagnetic on-off valve 32 and the start and stop of the lifting device 21. The control method of the flow rate control mechanism in the steam channel 10 specifically includes the following steps: S330, setting the warning pressure value of the upper mold steam pressure to P0, setting the standard value of the upper mold steam pressure to P, real-time monitoring of the upper mold steam pressure value to Pt, setting the flow rate warning value of the air outlet channel to S, and then introducing steam;
[0051] S331. During the first time period, the comparison unit compares P1 and PO. If P1 is less than P0, the steam continues to flow. Conversely, if P1 is greater than P0, the regulator 20 needs to be downgraded by the upgrading device to reduce the steam flow rate and adjust it to the primary channel 203.
[0052] S332: During the second time period, the upper mold steam pressure value P2 is monitored in real time. The difference between P2 and P is Δ. If the value of Δ is within the reasonable pressure control range, ventilation continues through the primary channel 203. If the value of Δ is out of the above range, the regulator 20 needs to be lowered by the upgrade device to reduce the steam flow rate and adjust the steam flow rate to the secondary channel 204 for ventilation within the time ts until the value P is reached.
[0053] S333. During the above time period, the flow velocity in the outlet channel is monitored in real time as S1. If S1 is greater than the S value, it is determined that the airflow disturbance is large and it is necessary to perform a downgrade process on the regulator 20 through the upgrading device to reduce the steam flow rate and adjust it to the third-level channel 205 for a time period of tp. Otherwise, ventilation is performed according to the currently required ventilation volume.
[0054] S334. During the tp time period, the flow velocity in the outlet channel is monitored in real time as Sp. If Sp is less than the S value, it is determined that the air flow disturbance is small, and ventilation is continued to be adjusted to the currently required ventilation volume; otherwise, ventilation is continued with the third-level channel 205.
[0055] The above method is adopted to set up, and an air pressure monitor 30 is set in the steam cavity in the upper mold and a flow rate monitor 31 is set in the air outlet channel. The monitoring results of the two monitors are used as standards, and the air pressure in the steam cavity and the flow rate in the air outlet channel can be adjusted in real time, which increases the stability of the air pressure in the steam cavity and the flow rate in the air outlet channel, greatly increases the inflation effect, and thus improves the subsequent coating effect. It is highly practical and has a simple structure.
[0056] An explosion-proof polyester needle punched felt suitable for the production method of the above-mentioned explosion-proof polyester needle punched felt, wherein the polyester needle punched felt has a four-layer structure, and the three layers of the polyester needle punched felt are each made by mixing polyester fibers and antistatic fibers, combing and mixing them into a web, and then needle-punching the three-layer mixed fiber web into a felt through a needle-punching process;
[0057] The polyester fiber and the antistatic fiber are evenly mixed in a weight ratio of 40-60:20-30, and the length of the antistatic fiber is between 2-3 cm, and the antistatic fiber is one or more of metal fiber or organic polymer-based metal complex antistatic fiber;
[0058] The antistatic microporous membrane and the mixed fiber felt are laminated on one side by steam hot pressing to obtain a laminated filter material, and the laminated surface of the antistatic microporous membrane is the windward surface of the polyester needle-punched felt; the antistatic material in the antistatic microporous membrane contains at least an antistatic organic polymer.
[0059] The explosion-proof polyester needle-punched felt prepared by the above method is needle-punched through a four-layer structure and a three-layer mixed fiber mesh. The mixed fiber mesh is subjected to single-side hot pressing and lamination on the windward side, which greatly increases the anti-static and explosion-proof effects of the needle-punched felt. In addition, the weight ratio of polyester fiber and anti-static fiber is also to ensure the corresponding structural strength while greatly increasing the anti-static effect of the needle-punched felt. The practicality is strong and the anti-static range is also greatly improved.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Common changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing explosion-proof polyester needle felt, It is characterized in that The method comprises the following steps: S1, preparing an antistatic microporous membrane: adding an antistatic material to a polytetrafluoroethylene resin raw material, mixing the materials uniformly, introducing the materials into an extruder, and obtaining an antistatic microporous membrane having a thickness of 15-30 μm, a porosity of 50%-85%, and a pore size distribution of 0.3-5 μm by extrusion, calendering, stretching, and heat setting, and using the obtained antistatic microporous membrane as a preparation, wherein the extrusion temperature is 200° C.-300° C., the calendering pressure is between 200N-500N, the biaxial stretching is made into a thickness of 5-50 μm, and the heat setting temperature is between 150° C.-180° C.; S2, preparation of mixed fiber felt: polyester fiber and antistatic fiber are mixed uniformly in a weight ratio of 40-60:20-30 to obtain mixed fiber; the mixed fiber is fed from a cotton feeder to a carding machine for carding to form a mixed fiber web; the mixed fiber web is fed to a cotton laying machine, and multiple layers of mixed limiting nets are stacked to form a mixed fiber felt; the mixed fiber felt is needle-punched on a needle-punching machine for reinforcement at a needle-punching speed of 500-600 rpm to obtain a polyester needle-punched felt semi-finished product; S3, placing the polyester needle felt semi-finished product after needle punching reinforcement in step S2 in a hot pressing mold (1) for hot pressing and laminating under vacuum, with the windward side of the polyester needle felt semi-finished product being the hot pressing and laminating side; S4, placing the polyester needle felt semi-finished product treated in step S3 into a cooling fixture, and cooling and shaping it at room temperature, the cooling time being 60 to 70 seconds; S5, cutting the polyester needle felt semi-finished product cooled in step S4 into required dimensions to obtain the polyester needle felt finished product.
2. The method for producing explosion-proof polyester needle felt according to claim 1, It is characterized in that The specific method of hot pressing film coating in step S3 is as follows: S30, coating the antistatic microporous film obtained in step S1 on the polyester needle felt semi-finished product; S32, evacuating the upper mold of the hot pressing mold (1) for 10 to 20 seconds at a pressure of 0.01 to 0.02 MPa, and introducing high-temperature steam while evacuating; S33, maintaining the vacuum degree, continuing to introduce high-temperature steam for heating and molding, the high-temperature steam pressure is 2.5-3MPa, the inflation time is between 3min-5min, the high-temperature steam temperature is 150-300°C, the pressure of the mold pressing down is between 300N-800N, and the molding time is 20-60 seconds, until the hot pressing is completed; S34, after the hot pressing is completed, the laminating material is pulled by the pulling device, and then the high-temperature steam in the upper mold is exhausted, and then the subsequent material that has not been hot pressed is hot pressed and laminated.
3. A method for producing explosion-proof polyester needle felt according to claim 1 or 2, It is characterized in that The hot pressing mold (1) comprises a steam channel (10) and a flow rate control mechanism arranged in the steam channel (10), the flow rate control mechanism comprising a regulating channel (2) arranged in the steam channel (10), a regulator (20) arranged in the regulating channel (2), and a lifting device (21) for driving the regulator (20) to rise and fall and adjust the gas outlet volume of the regulating channel (2), the regulator (20) being configured such that when it is lowered to the gas outlet channel of the regulating channel (2), the regulator (20) and the inner wall of the gas outlet channel form an annular flow channel (201); when it is separated from the gas outlet channel under the drive of the lifting device (21), the gas outlet channel restores the original gas volume.
4. A method for producing explosion-proof polyester needle felt according to claim 1 or 2, It is characterized in that A film cutting structure is also provided between the upper and lower molds of the hot pressing mold (1), and the film cutting structure includes a side cutting groove structure (220) provided on the lower mold, and a side cutting protrusion (221) provided on the upper mold and adapted to the side cutting groove structure (220). A shearing structure is formed between the side cutting groove structure (220) and the side cutting protrusion (221). The shearing structure is used to form a timely shearing effect with the lower mold after the upper mold is pressed down, so as to shear and cut the excess part of the antistatic microporous film.
5. The method for producing explosion-proof polyester needle felt according to claim 3, It is characterized in that A flow regulating structure is also provided between the regulator (20) and the air outlet channel, the flow regulating structure comprising a step structure (202) provided on the regulator (20). A plurality of step structures (202) are provided, the difference in outer diameter between two adjacent step structures (202) is between 2 cm and 5 cm, and the difference between two adjacent step structures (202) is the same, and a primary channel (203), a secondary channel (204) and a tertiary channel (205) with ventilation volumes from large to small are formed between the step structure (202) and the air outlet channel.
6. The method for producing explosion-proof polyester needle felt according to claim 5, It is characterized in that The flow rate control mechanism also includes a control system, which includes an air pressure monitor (30) for real-time monitoring of the steam pressure of the upper mold, a flow rate monitor (31) arranged in the air outlet channel, an electromagnetic on-off valve (32) arranged on the steam channel (10), and a controller (3) for controlling the start and stop of the lifting device (21) and the opening and closing of the electromagnetic on-off valve (32), wherein the controller (3) includes a receiving unit electrically connected to the air pressure detector and the flow rate monitor (31) and used to receive electrical signals from the two monitors, a comparison unit for setting the standard and warning steam pressure values of the upper mold and comparing them with the monitoring value, and a control unit for controlling the opening and closing of the electromagnetic on-off valve (32) and the start and stop of the lifting device (21). The control method of the flow rate control mechanism in the steam channel (10) specifically includes the following steps: S330, setting the warning pressure value of the steam pressure of the upper mold to P0, setting the standard value of the steam pressure of the upper mold to P, real-time monitoring of the steam pressure value of the upper mold to Pt, setting the flow rate warning value of the air outlet channel to S, and then introducing steam; S331, within the first time period, compare P1 and PO through a comparison unit, if P1 is less than P0, continue to pass steam; on the contrary, if P1 is greater than P0, it is necessary to perform a down-processing on the regulator (20) through an upgrading device to reduce the steam flow rate and adjust it to the primary channel (203); S332, in the second time period, the steam pressure value of the upper mold is monitored in real time as P2, and the difference between P2 and P is △. If the value of △ is within the reasonable range of pressure control, ventilation is continued through the primary channel (203); if the value of △ is out of the above range, the regulator (20) needs to be lowered by the upgrading device to reduce the steam flow rate and adjust to the secondary channel (204) for ventilation within ts time until the P value is reached; S333, in the above time period, the flow velocity in the outlet channel is monitored in real time as S1. If S1 is greater than the S value, it is determined that the air flow disturbance is large, and it is necessary to perform a down-regulation process on the regulator (20) through the upgrading device to reduce the steam flow rate and adjust it to the third-level channel (205) for an adjustment time of tp; otherwise, ventilation is performed according to the currently required ventilation volume; S334. During the tp time period, the flow velocity in the outlet channel is monitored in real time as Sp. If Sp is less than the S value, it is determined that the air flow disturbance is small, and ventilation is continued to be adjusted to the currently required ventilation volume; otherwise, ventilation is continued with the third-level channel (205).
7. An explosion-proof polyester needle felt produced by the production method of the explosion-proof polyester needle felt according to any one of claims 1 to 6, It is characterized in that The polyester needle felt has a four-layer structure, and the three layers of the polyester needle felt are all made by mixing polyester fibers and antistatic fibers, combing and mixing them into a web, and then the three-layer mixed fiber web is needle-punched into a felt through a needle-punching process; The polyester fiber and the antistatic fiber are uniformly mixed in a weight ratio of 40-60:20-30, and the length of the antistatic fiber is between 2-3 cm, and the antistatic fiber is one or more of metal fiber or organic polymer-based metal complex antistatic fiber; The antistatic microporous membrane and the mixed fiber felt are coated on one side by steam hot pressing to obtain a coated filter material, and the coated surface of the antistatic microporous membrane is the windward surface of the polyester needle-punched felt; the antistatic material in the antistatic microporous membrane at least contains an antistatic organic polymer.
Citation Information
Patent Citations
Production technology of soft and hard layer sound insulating pad of automobile
CN102423945A
Modified polyester fiber needled felt filtration bag and preparation method thereof
CN104083947A
Manufacturing technology for fiber blanket
CN104665527A
High-temperature-resistant PTFE membrane filter material and production method thereof
CN112755653A
Production method of explosion-proof polyester needled felt
CN115726097A