Air-stable solid electrolyte, preparation method therefor, and use thereof
By converting garnet electrolyte into water garnet electrolyte layer under high temperature conditions, the stability problem of garnet electrolyte in the air is solved, the high energy density and safety of lithium-ion batteries and lithium-air batteries are achieved, and the preparation process is simplified. , reduces costs.
Patent Information
- Application Number
- PCT/CN2024/090768
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-21
AI Technical Summary
After exposure to the air, existing garnet electrolytes form impurity layers such as lithium carbonate, hindering ion transport and restricting their application. Conventional doping and coating methods cannot effectively improve stability, making preparation difficult.
Li-H ion exchange is carried out by exposing the garnet electrolyte to a high-temperature proton-containing solution to form a water garnet electrolyte layer, which is stable to air, does not react with carbon dioxide, and blocks hydrogen ion conduction to protect the internal garnet electrolyte. The method includes high-temperature oxygen-rich sintering and hydrothermal treatment to form an air-stable solid electrolyte with a composite structure.
The long-term stability of garnet electrolyte in an open air environment is achieved, impurities are avoided, the stability of lithium metal and the electrochemical performance of electrolytes are improved, and the preparation cost and difficulty are reduced.
Smart Images

Figure CN2024090768_21112024_PF_FP_ABST
Abstract
Description
An air-stable solid electrolyte and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of all-solid-state lithium batteries, and in particular to an air-stable solid electrolyte and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are currently widely used in portable electronic devices, power batteries, and other fields due to their high energy density and low self-discharge effect. However, because commercial lithium-ion batteries use organic electrolytes, they are increasingly facing problems such as poor safety, flammability and explosiveness, poor high-voltage stability, and incompatibility with lithium metal anodes. At the same time, to further increase the energy density of lithium batteries, it is imperative to develop new systems based on ultra-high energy density cathodes, such as lithium-air batteries. Organic electrolytes are unable to effectively block pollutants such as moisture in the air, which seriously reduces the operating life of lithium-air batteries and hinders further improvements in lithium battery safety and energy density.
[0003] Inorganic solid electrolytes such as garnet-type electrolytes (LLZO), NASICON-type electrolytes (LAGP), and perovskite-type electrolytes (LLTO) often have high Young's modulus, good high-voltage stability, and intrinsic non-combustion properties, thus achieving higher safety and energy density. Among them, garnet-type electrolytes (LLZO) have attracted much attention for their high ionic conductivity and high stability to lithium metal. However, when garnet electrolytes are exposed to air, they will form impurity layers such as lithium carbonate, which hinder ion transport and hinder their practical application. Although researchers have optimized garnet electrolytes through doping and coating methods, conventional doping cannot effectively improve the stability of garnet electrolytes; the interface layer introduced by the coating method is often less stable. At the same time, the techniques used, such as magnetron sputtering and atomic layer deposition, greatly increase the difficulty of preparation.
[0004] Summary of the Invention
[0005] Garnet electrolytes, when exposed to air, form impurity layers such as lithium carbonate, hindering ion transport. Existing techniques such as doping, coating, magnetron sputtering, and atomic layer deposition (ALD) are not effective in addressing this issue. In light of these limitations, the present invention aims to provide an air-stable solid electrolyte, its preparation method, and its applications. Furthermore, a lithium-ion battery and a lithium-air battery are provided as applications.
[0006] The solid electrolyte provided by the present invention can be stable in the air for a long time.
[0007] To achieve the objectives of the present invention, the inventors, after extensive research, discovered that when a garnet electrolyte is exposed to a proton-containing solution at a relatively high temperature, it undergoes a vigorous Li-H ion exchange. Simultaneously, under the high temperature and accompanying high pressure, the protonated electrolyte transforms from a garnet structure to a hydrogarnet structure. This hydrogarnet electrolyte layer is inherently stable to air and no longer reacts with carbon dioxide to form lithium carbonate. Furthermore, the hydrogarnet protective layer blocks the conduction of hydrogen ions into the interior, inhibiting the continued penetration of the Li-H ion exchange reaction into the garnet electrolyte, effectively protecting the internal garnet electrolyte.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] In a first aspect, the present invention provides an air-stable solid electrolyte having a composite structure, wherein the solid electrolyte is composed of an outer hydrogarnet electrolyte and an inner garnet electrolyte.
[0010] In one embodiment of the present invention, the garnet electrolyte is obtained by high-temperature oxygen-rich atmospheric pressure sintering, spark plasma sintering or hot pressing sintering, and has a morphology of any one of block, sheet, rod, or spherical structures or a combination of at least two thereof, and has a density of more than 90%.
[0011] In one embodiment of the present invention, the chemical composition of the garnet electrolyte is Li 7-a La3Zr 2-a M a O 12 , where M refers to one or more of the doping metal ions Ta, Nb, W, and Mo, and 0.25 <a<1。
[0012] In one embodiment of the present invention, the hydrogarnet electrolyte of the outer layer has The crystal structure of the space group; the chemical composition is Li x La6Zr 4-2a M 2a O 24-z (OH) z , where x+2a+z=14, the type and concentration of the doped metal ion M are consistent with those of the inner garnet electrolyte, and the ratio of lithium ion to hydrogen ion concentration is 0.2 <x / z<1。
[0013] In one embodiment of the present invention, the outer layer hydrogarnet electrolyte is formed by converting the garnet electrolyte through an in-situ Li-H ion exchange reaction.
[0014] In one embodiment of the present invention, the thickness of the outer layer of hydrogarnet electrolyte is 50 nm to 50 μm.
[0015] In one embodiment of the present invention, the air-stable solid electrolyte, also known as a multilayer garnet-type electrolyte, can be placed in the open atmosphere for one year without producing significant lithium carbonate or lithium hydroxide impurities on the surface. On the one hand, the hydrogarnet electrolyte on its surface is intrinsically stable to air and will not decompose or react with carbon dioxide, water, etc. to produce impurities such as lithium carbonate and lithium hydroxide; on the other hand, the migration rate of hydrogen ions in the surface hydrogarnet electrolyte is extremely low, blocking the penetration of hydrogen ions into the internal garnet electrolyte, thereby inhibiting the lithium-hydrogen exchange reaction between the internal garnet electrolyte and moisture in the air. These two aspects work together to achieve long-term stability in an open air environment.
[0016] A second aspect of the present invention provides a method for preparing the air-stable solid electrolyte, comprising the following steps:
[0017] Step 1: Grind the garnet electrolyte block to be treated to remove surface impurities and place it in a reactor. Add treatment liquid until the electrolyte block is completely immersed and shaken to remove bubbles.
[0018] Step 2: placing the reactor in step 1 in an oven, heating it to the target temperature and keeping it warm, cooling it after the insulation is completed, and washing it to obtain a multilayer garnet electrolyte, which is the air-stable solid electrolyte.
[0019] In one embodiment of the present invention, in step 1, the treatment liquid is deionized water, or an aqueous solution of an alkali metal weak acid salt; the alkali metal weak acid salt is one or more inorganic salts of metals Li, Na, and K, such as sulfites, phosphates, carbonates, or organic salts such as acetates, formates, citrates, and ethylenediaminetetraacetates.
[0020] In one embodiment of the present invention, in step 2, the heating rate is 1-10°C / min; the target temperature is 120-220°C; and the holding time is 1 to 48 hours.
[0021] The third aspect of the present invention provides the use of the air-stable solid electrolyte in the preparation of a solid-state lithium-ion battery.
[0022] A fourth aspect of the present invention provides a solid-state lithium-ion battery comprising the air-stable solid electrolyte.
[0023] A fifth aspect of the present invention provides a solid-state lithium-air battery comprising the air-stable solid electrolyte.
[0024] The solid-state lithium-air battery assembled based on the solid-state electrolyte provided by the present invention, which is stable to air and lithium metal, can operate in an open atmospheric environment and has an extremely high positive electrode specific capacity.
[0025] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0026] In the present invention, the hydrogarnet electrolyte in the air-stable solid electrolyte is generated by converting the original garnet electrolyte through an ion exchange reaction, and has no obvious phase interface. At the same time, because the lattice constants of the two electrolytes are very close and the topological structures of the heavy elements are exactly the same, a very close quasi-isotropic contact is formed, ensuring good bonding strength and low interfacial impedance. Thanks to the uniform infiltration of the original garnet electrolyte by the liquid medium, the hydrogarnet electrolyte layer generated in situ is continuously distributed and has a uniform thickness, achieving complete protection of the original garnet electrolyte. At the same time, the hydrogarnet layer formed by ion exchange inherits the good stability of the garnet electrolyte to lithium metal and the good wettability to lithium metal, and has low interfacial impedance to lithium metal.
[0027] The present invention uses a hydrothermal treatment method to construct the air-stable solid electrolyte. This hydrothermal treatment method avoids the use of expensive thin film preparation equipment. At the same time, it uses inexpensive, environmentally friendly deionized water or an aqueous solution of a weak alkali metal salt as the treatment medium, avoiding the use of toxic and hazardous reagents. It is low-cost and environmentally friendly, suitable for large-scale production. At the same time, by adjusting the hydrothermal reaction temperature and time, the depth of the Li-H exchange reaction can be affected. Therefore, a hydrogarnet electrolyte layer with adjustable thickness can be converted on the garnet electrolyte surface, thereby taking into account both the electrolyte ion conductivity and the protective effect of the protective layer.
[0028] The solid electrolyte provided by the present invention can still stably operate more than 50 times after being placed in the air for one year, showing high air stability and maintaining good electrochemical performance. The solid-state lithium-air battery assembled using the solid electrolyte can operate normally in the open air at 60°C without applying additional protective layers on the positive and negative electrode sides, and has a capacity of 6000mAh·g -1 cathode High discharge capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] FIG1 is a scanning electron microscope image of the surface of the air-stable solid electrolyte described in preferred Example 1 of the present invention and the garnet electrolyte described in Comparative Example 1.
[0030] FIG2 is a scanning electron microscope image of a cross section of the air-stable solid electrolyte described in Example 1 of the present invention and the garnet electrolyte described in Comparative Example 1.
[0031] FIG3 is a Raman spectrum of the solid electrolyte described in the preferred embodiment 1 of the present invention.
[0032] Figure 4a is a scanning electron microscope image of the surface of the solid electrolyte described in the preferred Embodiment 1 of the present invention after aging in air for one year, and Figure 4b is a scanning electron microscope image of the surface of the garnet solid electrolyte in Comparative Example 1 after aging in air for one year.
[0033] Figure 5 is a Raman spectrum of the solid electrolyte described in the preferred Embodiment 1 of the present invention and the garnet solid electrolyte in Comparative Example 1 after aging in air for one year.
[0034] Figure 6 is a scanning electron microscope image of the cross-section of a lithium metal symmetric battery assembled using the solid electrolyte described in the preferred Embodiment 1 of the present invention.
[0035] Figure 7 is a cycling curve of a lithium metal symmetric battery assembled using the solid electrolyte described in the preferred Embodiment 1 of the present invention.
[0036] Figure 8 is a charge-discharge curve of a lithium metal lithium iron phosphate battery assembled using the solid electrolyte described in the preferred Embodiment 1 of the present invention.
[0037] Figure 9 is a cycling curve of a lithium symmetric battery assembled using the solid electrolyte described in the preferred Embodiment 1 of the present invention after aging in air for one year.
[0038] Figure 10 is a cycling curve of a lithium metal lithium iron phosphate battery assembled using the solid electrolyte described in the preferred Embodiment 1 of the present invention after aging in air for one year.
[0039] Figure 11 is a charge-discharge curve of the lithium-air battery described in the preferred Embodiment 1 of the present invention at 60 °C. Detailed Embodiments
[0040] In one embodiment of the present invention, an air-stable solid electrolyte is provided. The solid electrolyte is composed of an outer hydrogarnet electrolyte and an inner garnet electrolyte. The garnet electrolyte is obtained by high-temperature oxygen-rich atmospheric sintering, spark plasma sintering or hot pressing sintering, and has a morphology of any one or at least two combinations of block, sheet, rod, and spherical structures, and the density is above 90%. The chemical composition of the garnet electrolyte is Li 7-a La3Zr 2-a M a O 12 , where the doped metal ion represented by M is one or more of Ta, Nb, W, and Mo, and 0.25 < a < 1. The outer hydrogarnet electrolyte has a crystal structure belonging to space group; the chemical composition is Li x La6Zr 4-2a M 2a O 24-z (OH) z, where x + 2a + z = 14, the type and concentration a of the doped metal ion M are the same as those of the inner garnet electrolyte, and at the same time, the ratio of the concentration of lithium ions to hydrogen ions is 0.2 < x / z < 1. The outer hydrogarnet electrolyte is formed by in-situ Li-H ion exchange reaction of the garnet electrolyte. The thickness of the outer hydrogarnet electrolyte is 50 nm to 50 μm.
[0041] The air-stable solid electrolyte can also be called a multi-layer garnet-type electrolyte, which can be placed in open air for one year without obvious lithium carbonate and lithium hydroxide impurities on the surface.
[0042] In another embodiment of the present invention, a preparation method of the air-stable solid electrolyte is provided, including the following steps:
[0043] Step 1: Grind the garnet electrolyte block to be processed to remove surface impurities, then place it in a reaction kettle, add a treatment solution to completely immerse the electrolyte block, and shake to remove bubbles;
[0044] Step 2: Place the reaction kettle in step 1 in an oven, heat it to the target temperature and keep it warm, and after the heat preservation is over, cool it and wash it to obtain a multi-layer garnet electrolyte, that is, the air-stable solid electrolyte.
[0045] Among them, in step 1, the treatment solution is deionized water or an aqueous solution of a weak alkali metal salt; the weak alkali metal salt is one or more of inorganic salts of metals Li, Na, K such as sulfite, phosphate, carbonate or organic salts such as acetate, formate, citrate, ethylenediaminetetraacetate. In step 2, the heating rate is 1 - 10 °C / min; the target temperature is 120 - 220 °C; the heat preservation time is 1 - 48 hours.
[0046] In another embodiment of the present invention, a solid-state lithium-ion battery or a solid-state lithium-air battery containing the air-stable solid electrolyte is provided. [[ID=Step 1: Take a hot-pressed sintered garnet-type LLZTO (Li 6.5 La3Zr 1.5 Ta 0.5 O 12 The electrolyte sheet was polished with 1000-grit sandpaper to remove impurities on its surface and then set aside. The electrolyte sheet was then placed in a 25 mL polytetrafluoroethylene reactor, 10 g of deionized water was added, and the reactor was sealed after shaking.
[0051] Step 2: Place the polytetrafluoroethylene reactor in step 1 in an oven and heat it to 140°C. After keeping it warm for 6 hours, cool it down, wash the surface with deionized water, and air dry it naturally to obtain an air-stable solid electrolyte (multilayer garnet electrolyte).
[0052] Natural aging of electrolytes:
[0053] The electrolyte obtained in this example was placed in an open container and kept in a ventilated and cool place. After one year, it was taken out and the surface dust was cleaned with deionized water for subsequent testing and battery assembly.
[0054] Combination of lithium metal anode and solid electrolyte:
[0055] 0.2g of lithium metal is placed on a platinum plate. The plate is heated on a heating platform to above the melting point of lithium metal. The pure lithium metal spreads out on the surface of the plate into a thin film tens of microns thick. One side of the naturally aged solid electrolyte sheet from this example is then applied to the spread lithium metal film and scraped. After removal and cooling, a lithium metal anode tightly bonded to the solid electrolyte sheet is obtained.
[0056] Comparative Example 1
[0057] This comparative example provides a solid electrolyte different from that of Example 1, which is a raw garnet electrolyte. The preparation method is as follows: a hot-pressed sintered garnet-type LLZTO (Li 6.5 La3Zr 1.5 Ta 0.5 O 12 ) Electrolyte sheet, use 1000 grit sandpaper to remove impurities on its surface and set aside.
[0058] The natural aging of the electrolyte and the combination of the lithium metal negative electrode and the solid electrolyte in this comparative example 1 are the same as those in Example 1.
[0059] Performance test case
[0060] (1) Lithium-lithium iron phosphate battery assembly and performance testing
[0061] The performance test was conducted in a homemade soft pack battery in the laboratory. The battery assembly method is as follows: take out the electrolyte sheet with lithium metal negative electrode attached on one side, and drip 10μL / cm 2 The ionic liquid electrolyte improves the interface contact and then the coating loading is 2mg / cm 2 The lithium iron phosphate negative electrode was transferred between the stainless steel tabs of the soft pack battery and vacuum sealed. The ionic liquid electrolyte was Pyr14TFSI ionic liquid dissolved with 0.1g / ml LiTFSI. The test current density was 35mA / g LFP , the voltage control range is 2.7~3.8V.
[0062] (2) Solid-state lithium-air battery assembly and performance testing:
[0063] The assembly of the solid electrolyte and the lithium metal anode is described in the previous section. To ensure stable operation of the lithium metal in the open atmosphere, the lithium metal anode is encapsulated with stainless steel and epoxy resin.
[0064] Preparation method of the composite positive electrode: 60 mg of lithium bis(trifluoromethylsulfonyl)imide, 80 mg of poly(vinylidene fluoride-hexafluoropropylene) and 120 mg of Ketjen black were ultrasonically dissolved and dispersed in 12 mL of N-methylformamide to prepare a positive electrode slurry.
[0065] Assembly of solid-state lithium-air battery: Take 200 μL of composite positive electrode slurry and evenly apply it to the positive electrode side of the electrolyte sheet that has been encapsulated with a lithium negative electrode. Then, carbon paper is gently pressed on the droplet as a current collector. Then, it is dried at normal pressure at 60°C for 2 hours, and then vacuum dried at 80°C for 6 hours to obtain a solid-state lithium-air battery.
[0066] The battery test was carried out in an electric oven to maintain a constant temperature of 60°C and a current of 30 μA / cm 2 , the charge and discharge cut-off voltage is 2.5-4V.
[0067] Figure 1 shows scanning electron micrographs of the surfaces of the air-stable solid electrolyte described in preferred Example 1 of the present invention and the garnet electrolyte described in Comparative Example 1. It can be observed that after ion exchange treatment, the hydrogarnet layer on the surface of the air-stable solid electrolyte sheet exhibits no apparent cracks or holes, and exhibits virtually no morphological changes compared to the original garnet electrolyte.
[0068] Figure 2 is a scanning electron microscope image of the cross section of the air-stable solid electrolyte described in the preferred embodiment 1 of the present invention and the garnet electrolyte described in the comparative example 1. It can be observed that there is no obvious hydrogarnet-garnet interface in the cross section of the air-stable solid electrolyte, showing good interfacial contact.
[0069] Figure 3 is a Raman spectrum of the air-stable solid electrolyte described in the preferred embodiment 1 of the present invention. The spectrum is superimposed with Raman signals of two materials, hydrogarnet electrolyte and garnet electrolyte, which proves the formation of surface hydrogarnet electrolyte and the multilayer structure of hydrogarnet-garnet.
[0070] Figure 4 shows scanning electron micrographs of the surfaces of the air-stable solid electrolyte described in preferred Example 1 of the present invention and the garnet solid electrolyte of Comparative Example 1 after one year of aging in air. It can be seen that after one year of aging, the surface of the original garnet electrolyte changes from smooth to rough, while the air-stable solid electrolyte retains its previously smooth surface morphology.
[0071] Figure 5 shows the Raman spectra of the air-stable solid electrolyte described in preferred Example 1 of the present invention and the garnet solid electrolyte of Comparative Example 1 after one year of aging in air. After one year of aging, the surface of the original garnet electrolyte exhibits a strong Raman peak characteristic of lithium carbonate, while the surface of the air-stable solid electrolyte exhibits a relatively low Raman peak characteristic of lithium carbonate.
[0072] Figure 6 is a scanning electron microscope image of a cross-section of a symmetrical lithium metal battery assembled using the air-stable solid electrolyte described in Example 1 of the present invention. The electrolyte exhibits a tight bond with the lithium metal, with no apparent cracking or pores, demonstrating its excellent stability for lithium metal.
[0073] FIG7 is a cycle curve of a lithium metal symmetrical battery assembled using the air-stable solid electrolyte described in Example 1 of the present invention, at 0.2 mA / cm 2 The symmetrical battery can be stably cycled for more than 1000 hours at a current density of , demonstrating the excellent stability of the solid-state electrolyte to lithium metal.
[0074] FIG8 is a charge and discharge curve of a lithium metal to lithium iron phosphate battery assembled using the air-stable solid electrolyte described in the preferred embodiment 1 of the present invention, which can be stably cycled for more than 150 times at room temperature and 0.2C rate.
[0075] FIG9 is a cycle curve of a lithium symmetrical battery assembled using the air-stable solid electrolyte described in the preferred embodiment 1 of the present invention after aging in air for one year. 2 The symmetrical battery can be stably cycled for more than 200 hours at a current density of 1.5 GHz, indicating that the solid-state electrolyte maintains excellent stability to lithium metal even after aging.
[0076] Figure 10 shows the cycle curve of a lithium metal to lithium iron phosphate battery assembled after aging in air for one year using the air-stable solid electrolyte described in the preferred embodiment 1 of the present invention. At 60°C, the battery can still operate stably for more than 300 hours (30 cycles at a current density of 0.2C), indicating that the aged electrolyte has good stability to positive electrode materials such as lithium iron phosphate and still maintains good electrochemical properties.
[0077] FIG11 is a charge and discharge curve of the solid-state lithium-air battery described in the preferred embodiment 1 of the present invention at 60° C., with a discharge capacity of up to 6000 mAh g cathode -1 , showing the excellent prospects of the air-stable solid electrolyte as an electrolyte for solid-state air batteries.
[0078] Example 2
[0079] This embodiment provides a method for preparing an air-stable solid electrolyte, namely a multilayer garnet electrolyte, comprising the following steps:
[0080] Step 1: Take some hot-pressed sintered garnet-type LLZTO (Li 6.5 La3Zr 1.5 Ta 0.5 O 12 The electrolyte sheet was manually polished with 5000-mesh abrasive paste to remove surface impurities and then set aside. The electrolyte sheet was then placed in a 500-mL polytetrafluoroethylene reactor, 250 g of deionized water was added, and the reactor was sealed after shaking.
[0081] Step 2: Place the polytetrafluoroethylene reactor in step 1 in an oven and heat it to 120° C., keep it warm for 18 hours, then cool it down, wash the surface with deionized water, and air-dry it to obtain the multilayer garnet electrolyte.
[0082] The assembly of lithium-lithium iron phosphate battery and solid-state lithium-air battery is the same as that in Example 1.
[0083] Example 3
[0084] This embodiment provides a method for preparing an air-stable solid electrolyte, namely a multilayer garnet electrolyte, comprising the following steps:
[0085] Step 1: Take a hot-pressed sintered garnet-type LLZTO (Li 6.5 La3Zr 1.5 Ta 0.5 O 12The electrolyte column was manually polished with 1000-grit sandpaper to remove any impurities on its surface and then set aside. The electrolyte column was then placed in a 50-mL polytetrafluoroethylene reactor, 20 g of deionized water was added, and the reactor was sealed after shaking.
[0086] Step 2: Place the polytetrafluoroethylene reactor in step 1 in an oven and heat it to 180° C., keep it warm for 2 hours, then cool it down, wash the surface with deionized water, and air-dry it to obtain the multilayer garnet electrolyte.
[0087] Example 4
[0088] This embodiment provides a method for preparing an air-stable solid electrolyte, namely a multilayer garnet electrolyte, comprising the following steps:
[0089] Step 1: Take the hot-pressed sintered garnet-type LLZTO (Li 6.5 La3Zr 1.5 Ta 0.5 O 12 The electrolyte balls were manually polished with 3000-grit sandpaper to remove surface impurities and then set aside. The electrolyte balls were then placed in a 50 mL polytetrafluoroethylene reactor, 10 g of deionized water was added, and the reactor was sealed after shaking.
[0090] Step 2: Place the polytetrafluoroethylene reactor in step 1 in an oven and heat it to 140° C., keep it warm for 48 hours, then cool it down, wash the surface with deionized water, and air-dry it to obtain the multilayer garnet electrolyte.
[0091] The above description of the embodiments is intended to facilitate understanding and use of the invention by those skilled in the art. It will be apparent that those skilled in the art can readily make various modifications to these embodiments and apply the general principles described herein to other embodiments without requiring inventive effort. Therefore, the present invention is not limited to the above-described embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention, without departing from the scope of the present invention, should be within the scope of protection of the present invention.
Claims
1. An air-stable solid electrolyte, characterized in that The solid electrolyte is composed of an outer layer of hydrogarnet electrolyte and an inner layer of garnet electrolyte; The chemical composition of the garnet electrolyte is Li 7-a LqCy 2-a M a O 12 , where M refers to one or more of the doping metal ions Ta, Nb, W, and Mo, and 0.25 <a<1; The hydrogarnet electrolyte of the outer layer has The crystal structure of the space group; the chemical composition is Li x Ln6 4-2a M 2a O 24-z (OH) z , where x+2a+z=14, the type and concentration of the doped metal ion M are consistent with the inner garnet electrolyte, and the ratio of lithium ion to hydrogen ion concentration is 0.2 <x / z<1。 2. An air-stable solid electrolyte according to claim 1, characterized in that: The garnet electrolyte is obtained by high-temperature oxygen-rich atmospheric pressure sintering, spark plasma sintering or hot pressing sintering, and has a shape of any one of block, sheet, rod, and spherical structures or a combination of at least two thereof, and has a density of more than 90%.
3. An air-stable solid electrolyte according to claim 1, characterized in that: The outer layer hydrogarnet electrolyte is formed by converting the garnet electrolyte through an in-situ Li-H ion exchange reaction.
4. An air-stable solid electrolyte according to claim 1, characterized in that: The thickness of the hydrogarnet electrolyte in the outer layer is 50 nm to 50 μm.
5. The method for preparing the air-stable solid electrolyte according to any one of claims 1 to 4, characterized in that: The steps include: Step 1: Grind the garnet electrolyte block to be treated to remove surface impurities and place it in a reactor, add treatment liquid until the electrolyte block is completely immersed, and shake to remove bubbles; Step 2: heating the reactor in step 1 to the target temperature and keeping it warm, cooling it after the insulation is completed, and washing it to obtain a multilayer garnet electrolyte, which is the air-stable solid electrolyte.
6. The method for preparing the air-stable solid electrolyte according to claim 5, characterized in that: In step 1, the treatment liquid is deionized water or an aqueous solution of an alkali metal weak acid salt; the alkali metal weak acid salt is one or more inorganic or organic salts of metals Li, Na, and K.
7. The method for preparing the air-stable solid electrolyte according to claim 5, characterized in that: In step 2, the heating rate is 1-10°C / min; the target temperature is 120-220°C; and the insulation time is 1 to 48 hours.
8. Use of the air-stable solid electrolyte according to any one of claims 1 to 4 in the preparation of a solid-state lithium-ion battery.
9. A solid-state lithium-ion battery, characterized in that: Containing the air-stable solid electrolyte according to any one of claims 1 to 4.
10. A solid-state lithium-air battery, characterized in that: Containing the air-stable solid electrolyte according to any one of claims 1 to 4.
Citation Information
Patent Citations
Surface treatment method for garnet type solid electrolyte
CN112290082A
Stabilized solid garnet electrolyte and methods thereof
CN112563566A
Heterovalent difunctional co-doped garnet type solid electrolyte and preparation method thereof
CN115763957A
Garnet type lithium ion solid electrolyte and preparation method thereof
CN115911523A