Artificial stone and a method for manufacturing artificial stone

The method of manufacturing artificial stone by intermixing finely ground recycled materials with an alkaline activator and foaming addresses the challenge of creating lightweight, energy-efficient, and carbon-reducing construction materials, enabling the production of lightweight artificial stone for construction applications.

WO2024236230A2PCT designated stage expired Publication Date: 2024-11-21ECOUP OY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/FI2024/050236
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing artificial stone manufacturing methods face limitations in utilizing recycled materials efficiently, particularly in achieving a lightweight product that reduces energy consumption and carbon emissions, as alkaline-activated materials have specific weight restrictions and processes like expanded clay require significant energy and cannot incorporate recycled materials.

Method used

A method involving the intermixing of finely ground recycled materials like rockwool, glass wool, glass, brick, and blast-furnace slag with an alkaline activator solution, followed by foaming to achieve a specific weight of no more than 1200 kg/cubic meter, utilizing alkalis like sodium aluminate and caustic soda, and optionally incorporating expanded polystyrene to reduce weight further.

Benefits of technology

The method enables the production of lightweight artificial stone that efficiently utilizes recycled materials, reducing energy consumption and carbon emissions, while allowing for the creation of construction elements with targeted specific weights, thus addressing the limitations of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The invention concerns artificial stone and a method for manufacturing it. In the method, alkaline-activated material is foamed to achieve the desired specific weight. Demolition waste, such as mineral wool, brick, and demolished concrete, can be used as material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] ARTIFICIAL STONE AND A METHOD FOR MANUFACTURING ARTIFICIAL STONE

[0002] FIELD OF THE INVENTION

[0003] The invention is related to artificial stone that comprises recycled material and can be used in construction and earthwork construction. The invention is also related to a method for manufacturing artificial stone and to construction elements made out of artificial stone.

[0004] PRIOR ART

[0005] One of the most essential objectives of circular economy is to save natural resources by utilizing materials efficiently and sustainably. Utilization of waste materials, material side streams, and demolition materials is key for an effective circular economy.

[0006] Artificial stones can be made in many ways. One area that has been studied extensively over recent years is alkaline-activated materials that can replace concrete. Alkaline-activated materials can partly be made out of industrial waste materials and material side streams, which reduces carbon dioxide emissions compared with Portland cement. However, these alkaline- activated materials correspond to concrete in terms of their specific weight, which restricts their applications. There are also other artificial stone materials, such as expanded clay, which is clearly lighter and is typically made by expanding and firing clay. But that process cannot make use of recycled materials, and firing clay requires a lot of energy.

[0007] OBJECT OF THE INVENTION

[0008] The object of the invention is artificial stone in whose manufacturing recycled materials can be utilized, a manufacturing method for artificial stone, and / or a product made of artificial stone.

[0009] SHORT DESCRIPTION OF THE INVENTION

[0010] The object of the invention can be achieved, e.g., with a method for manufacturing artificial stone. The method involves intermixing the dry materials, comprising finely ground rockwool, glass wool, glass, brick, concrete or their mixture as well as ground blast-furnace slag and cement. An alkaline activator solution consisting of an alkali, i.e. an alkaline activator, and water is mixed separately. The alkaline activator solution is mixed into the dry materials, resulting in a paste whose consistency can be semi-dry or runny. The paste is foamed, until the desired targeted specific weight is achieved or at least until the specific weight is no more than 1200 kg / cubic meter. Finally, the foamed paste is allowed to set. The object of the invention can also be achieved with artificial stone made using the method described above.

[0011] DETAILED DESCRIPTION OF THE INVENTION

[0012] An embodiment of the first aspect of the invention is a method for manufacturing artificial stone. The method comprises the steps where the dry materials are intermixed into a homogenous mixture, the liquid materials are intermixed into a solution, said mixture created from the dry materials and said solution created from the liquid materials are intermixed into a paste, the paste is foamed so that the specific weight of the foamed paste is no more than 1200 kg / cubic meter, and finally the foamed paste is allowed to set.

[0013] The liquid materials stated in the method comprise water and an alkali, such as sodium aluminate, caustic soda, sodium hydroxide, magnesium hydroxide, water glass, or two or more of the aforementioned alkalis. In the context of this publication, “alkalis” refer to a chemical activator, i.e. alkaline activator, which is used to facilitate the setting process. Regularly used alkaline activators are alkaline compounds, such as carbonates, hydroxides and silicates that can be added in liquid form. Alkaline activators in dry form can also be used, whereby even mere water can be used as liquid material. In a preferable embodiment, the liquid materials comprise sodium aluminate and water. In a preferable embodiment, the liquid materials consist of sodium aluminate, caustic soda and water. In some embodiments, lime and sodium hydroxide can be used to replace caustic soda and / or sodium aluminate. In some embodiments, magnesium hydroxide can be used to replace caustic soda and / or sodium aluminate. In a preferable embodiment, the liquid materials comprise sodium aluminate representing at least 10% of the mass of the dry materials and no more than 20% of the mass of the dry materials.

[0014] In the method, said dry materials comprise blast-furnace slag and cement and at least one of the following materials ground into a grain size of 0- 400 micrometers, preferably into a grain size of 0-200 micrometers and very preferably into a grain size of 0-100 micrometers: rockwool, glass wool, glass, brick, and concrete. The grain sizes stated in this publication can be D90 grain sizes, wherein at least 90% of the particles fall within said grain size range. Said rockwool, glass wool, glass, brick, and concrete are preferably materials demolished from buildings, materials at the end of their useful life, or materials otherwise recycled. Preferably, mineral wool, i.e. rockwool or glass wool, represents the largest share in the dry materials, whereby mineral wool represents at least 40%, preferably at least 50% and very preferably at least 55% of the mass of the dry materials. In a preferable embodiment, cement represents no more than 20%, preferably no more than 15% and very preferably no more than 10% of the mass of the dry materials. Preferably, all the dry materials have been ground to a grain size of 0-400 micrometers, preferably to a grain size of 0- 200 micrometers, and very preferably to a grain size of 0-100 micrometers before the dry materials are intermixed. In a preferable embodiment, the dry materials also comprise sodium carbonate, e.g., no more than 5%, preferably no more than 4% and very preferably no more than 2% of the mass of the dry materials.

[0015] In the method’s foaming step, the foaming can be done by applying methods familiar from similar industrial processes. For example, a foam based on animal proteins or synthetic proteins can be used, or an air-entraining agent applied as concrete additive can be used, or a combination of the two. For example, a foam with a specific weight of 85 kg / m3can be used at a ratio of 10- 20 grams per one liter of paste. Correspondingly, when using an air-entraining agent, the share of the air-entraining agent is preferably 0.5-1.0% of the total mass of the paste. In a preferable embodiment, the method comprises, prior to the foaming step, a step wherein expanded polystyrene is added into the paste, mixing continuously. Expanded polystyrene is added into the paste preferably in a steady stream, mixing continuously. Expanded polystyrene reduces the specific weight of the paste and either lightens the specific weight of the created artificial stone or reduces the need for foaming to achieve the desired specific weight.

[0016] An embodiment of the second aspect of the invention is artificial stone that can comprise finely ground recycled materials. In the entire context of this publication, “finely ground material” means such material that has been ground into a grain size of 0-400 micrometers, preferably into a grain size of 0-200 micrometers and very preferably into a grain size of 0-100 micrometers. Finely grinding the material enables it to be chemically activated.

[0017] In a preferable embodiment, artificial stone comprises blast-furnace slag and cement and additionally rockwool, glass wool, glass, brick, or concrete ground into a grain size of 0-400 micrometers, preferably into a grain size of 0- 200 micrometers and very preferably into a grain size of 0-100 micrometers. The artificial stone has been created by alkaline activation and foaming so that the specific weight of the artificial stone is no more than 1200 kg / cubic meter. The alkaline activation and foaming can be implemented, e.g., using a method according to the first aspect of the invention. In an embodiment, the artificial stone is made using a method according to the first aspect of the invention. The substances, materials and work stages described in the methods according to the first aspect of the invention can be utilized correspondingly also in connection with artificial stone according to the second aspect of the invention.

[0018] Preferably, the rockwool, glass wool, glass, brick, and concrete are materials demolished from buildings, materials at the end of their useful life, or materials otherwise recycled. Preferably, the largest share of the mass of the artificial stone is represented by mineral wool, i.e. rockwool or glass wool, whereby mineral wool represents at least 40%, preferably at least 50% and very preferably at least 55% of the mass of the artificial stone. In a preferable embodiment, cement represents no more than 20%, preferably no more than 15% and very preferably no more than 10% of the mass of the artificial stone.

[0019] In a preferable embodiment, the artificial stone also comprises sodium carbonate. In a preferable embodiment, the artificial stone also comprises expanded polystyrene, which inherently reduces the specific weight of the artificial stone. In an embodiment, the artificial stone also comprises sodium aluminate, which catalyzes alkaline activation.

[0020] A third aspect of the invention is the use of the artificial stone according to an embodiment of the second aspect of the invention as lightweight aggregate. Lightweight aggregates can be used in the manufacture of stone-based products to lighten the manufactured product or as such in earthwork construction, for example.

[0021] A fourth aspect of the invention is a construction element comprising artificial stone according to an embodiment of the second aspect of the invention. The construction element can be, e.g., a brick, block, wall element, floor element, roof element, slab, hollow-core slab, or another construction element.

[0022] To demonstrate the invention, presented hereunder are examples of utilizing the invention according to its various aspects.

[0023] Example 1

[0024] The dry materials as mass percentages of the total mass of the dry materials:

[0025] 57.7% rockwool powder

[0026] 5.6% cement

[0027] 28.9% slag

[0028] 5.6% hardening mixture

[0029] 2.2% sodium carbonate

[0030] The liquid materials as weight percentages calculated from the total mass of the dry materials: 17.8% sodium aluminate solution

[0031] 1.1% caustic soda solution

[0032] 13.3% water

[0033] Foaming agents proportioned to the volume of the paste 10-20 g of foam per liter (foam weight 85g / liter)

[0034] Additionally as option, calculated from the total mass of the dry materials:

[0035] 0.89% expanded polystyrene

[0036] In Example 1, the hardening mixture comprises 11-17% gypsum, 45- 59% blast-furnace slag, 19-25% mineral wool, glass, or brick, and 5-10% slaked lime. All the materials have been ground to a grain size of 0-200 micrometers and intermixed.

[0037] Artificial stone is made advantageously by first intermixing the dry materials. Then the sodium carbonate is added and mixed in. Alternatively, the sodium carbonate can be simultaneously intermixed with the other dry materials. All the liquid materials are first intermixed and then mixed into the dry materials. At this phase, the consistency of the mixture can be semi-dry, for example. The expanded polystyrene is added gradually in a steady stream, mixing continuously. Finally, foam is added, until the desired specific weight of the paste is achieved. The targeted weight is 600-1100 g / liter.

[0038] Example 2

[0039] The dry materials as mass percentages of the total mass of the dry materials: 66.4% rockwool powder 5.6% cement 28% blast-furnace slag

[0040] Additionally, 100-250 g of sodium carbonate for every 5.2 kg of dry materials.

[0041] The liquid materials as weight percentages calculated from the total mass of the dry materials:

[0042] 22% sodium aluminate solution

[0043] 1.1% caustic soda solution

[0044] 16.7% water Additionally as option, calculated from the total mass of the dry materials:

[0045] 0.7% expanded polystyrene

[0046] 20-30% of the rockwool powder can be replaced with glass powder, brick powder, demolished concrete powder, or by using various ashes.

[0047] Artificial stone is made advantageously by first intermixing the dry materials. Then the sodium carbonate is added and mixed in. Alternatively, the sodium carbonate can be simultaneously intermixed with the other dry materials. All the liquid materials are first intermixed and then mixed into the dry materials. At this phase, the consistency of the mixture can be semi-dry, for example. The expanded polystyrene is added gradually in a steady stream, mixing continuously. Finally, foam is added, until the desired specific weight of the paste is achieved. The targeted weight is 600-1100 g / liter.

[0048] Example 3

[0049] The materials as grams per 1000 g of total mass:

[0050] 200-495 g of ground rockwool, ground demolished concrete or their combination

[0051] 200-495 g of ground blast-furnace slag

[0052] 10 g of cement

[0053] 68 g of sodium carbonate

[0054] 100-500 g of water

[0055] As an option, 10-30 g of 50% caustic soda solution

[0056] Additionally, either a foaming agent or recycled expanded polystyrene, or both, until the desired specific weight is achieved, however, no more than 1200 kg / cubic meter.

[0057] Artificial stone is made advantageously by first intermixing the dry materials. The blast-furnace slag as well as the rockwool, demolished concrete, or a combination of the two has been ground to a grain size of at least 0-400 micrometers, preferably to a grain size of 0-200 micrometers and even more preferably to a grain size of 0-100 micrometers. The water and the caustic soda solution, if the latter is used, are intermixed and then mixed into the dry materials. Use of caustic soda solution facilitates the development of strength. The expanded polystyrene, if used, is added gradually in a steady stream, mixing continuously. Foam, if used, is added last, until the desired specific weight of the paste is achieved.

[0058] To a skilled person in the art, it is obvious that the basic idea of the invention can be implemented in various ways, as technology and materials develop. The invention and its embodiments are therefore not limited to only the examples presented above; rather they may vary within the scope of the claims.

Claims

CLAIMS1. A method for manufacturing artificial stone, which method comprises the steps where: the dry materials are intermixed into a homogenous mixture, the liquid materials are intermixed into a solution, wherein said liquid materials comprise water and an alkaline activator, the mixture created from the dry materials and the solution created from the liquid materials are intermixed into a paste, the paste is foamed so that the specific weight of the foamed paste is no more than 1200 kg / cubic meter, and the foamed paste is allowed to set, which method is characterized in that the dry materials comprise blast-furnace slag and cement and at least one of the following materials ground into a grain size of 0-400 micrometers: rockwool, glass wool, glass, brick, and concrete.

2. The method according to claim 1, comprising, prior to the foaming step, a step where expanded polystyrene is added into the paste, mixing continuously.

3. The method according to claim 1 or 2, wherein the liquid materials comprise sodium aluminate and water.

4. The method according to any of claims 1-3, wherein the dry materials also comprise sodium carbonate.

5. The method according to any of claims 1-4, wherein at least 50% of the mass of the dry materials is represented by rockwool, glass wool, glass, brick, or concrete ground into a grain size of 0-400 micrometers and no more than 10% of the mass of the dry materials is represented by cement.

6. The method according to any of claims 1-5, wherein the liquid materials comprise sodium aluminate that represents at least 10% of the mass of the dry materials and no more than 20% of the mass of the dry materials.

7. The method according to any of claims 1-6, wherein said mineral wool is recycled mineral wool.

8. The method according to any of claims 1-7, wherein the dry materials also comprise demolished concrete ground into a grain size of 0-400 micrometers.

9. Artificial stone that comprises blast-furnace slag and cement and is characterized in that the artificial stone also comprises rockwool, glass wool, glass, brick, or concrete ground into a grain size of 0-400micrometers, and which artificial stone has been created by alkaline activation and foaming so that the specific weight of the artificial stone is no more than 1200 kg / cubic meter.

10. Artificial stone according to claim 9, also comprising demolished concrete ground into a grain size of 0-400 micrometers.

11. Artificial stone according to claim 9 or 10, also comprising expanded polystyrene.

12. Artificial stone according to any of claims 9-11, also comprising sodium aluminate.

13. Artificial stone manufactured with the method according to claim 1.

14. Use of artificial stone according to claim 9 or 13 as lightweight aggregate material.

15. A construction element which is characterized in that it comprises artificial stone according to claim 9 or 13.