Spherical silica powder and method for producing spherical silica powder
The production of spherical silica powder with a controlled silanol group ratio and processing in a reducing atmosphere addresses the challenge of achieving low dielectric loss and excellent adhesion to resin, enhancing its performance in electronic applications.
Patent Information
- Application Number
- PCT/JP2024/016817
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-01
- Publication Date
- 2024-11-21
AI Technical Summary
Spherical silica powders with low dielectric loss and excellent adhesion to resin are needed for electronic applications, as existing methods to reduce silanol groups in silica powders often result in poor compatibility and low adhesion with resin.
The spherical silica powder is produced with a specific ratio of internal to isolated silanol groups, characterized by IR peak intensities within certain ranges, and processed to achieve a median diameter of 0.5 to 20.0 μm and a specific surface area of 0.1 to 4.0 m²/g, while being fired in a reducing atmosphere to optimize dielectric properties and adhesion.
The resulting silica powder exhibits low dielectric loss tangent and improved adhesion to resin, ensuring sufficient peel strength and high-frequency characteristics for electronic applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Spherical silica powder and method for producing spherical silica powder
[0001] The present invention relates to a spherical silica powder and a method for producing the spherical silica powder.
[0002] Silica (SiO 2 Silica particles containing methyl methacrylate as a main component have conventionally been used in a variety of applications, including electronic materials such as printed wiring boards and package wiring boards, optical materials such as lenses and optical films, functional materials such as catalysts and catalyst carriers, and pigments for paints and cosmetics.
[0003] In recent years, with the increase in the volume of information communication in the communications field, the use of high-frequency signals has become widespread in electronic devices and communications equipment, and materials with a low dielectric loss tangent are required for use in high-frequency devices. Silica has a low dielectric constant (3.9) and a low thermal expansion coefficient (3 to 7.9 ppm / °C), making it a promising filler material with both a low dielectric constant and a low thermal expansion coefficient, and it is expected to be used in high-frequency dielectric devices, etc.
[0004] Since silanol (Si—OH) groups contained in silica cause an increase in dielectric loss, reducing the silanol groups contained in silica is effective in improving dielectric properties. For example, Patent Document 1 discusses reducing the amount of silanol groups by baking silica containing silanol groups in a hydrogen gas flow at a temperature of 1100° C. or higher.
[0005] Japanese Patent Publication No. 3-228817
[0006] However, reducing the number of silanol groups to improve dielectric properties leads to a problem that the compatibility between the spherical silica powder and the resin deteriorates, resulting in poor adhesion to the resin. If the adhesion between the spherical silica and the resin is poor, a resin composition containing the spherical silica powder mixed with the resin may not have sufficient peel strength when used in electronic applications.
[0007] Therefore, an object of the present invention is to provide a spherical silica powder that has low dielectric loss and excellent adhesion to resin when mixed with resin for use in electronic applications.
[0008] As a result of extensive research, the inventors have discovered that the above-mentioned problems can be solved by ensuring that the ratio of the amount of internal silanol groups to the amount of isolated silanol groups on the surface of the spherical silica powder is within a specific range, and have thus completed the present invention.
[0009] The present invention relates to the following: [1] A spherical silica powder having a silanol group-derived internal silanol group of 3600 to 3700 cm -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 [2] A spherical silica powder having a maximum IR peak intensity B ratio (B / A) of 0.5 to 1.5. -1 Super 3800cm -1 [3] The spherical silica powder according to [1], wherein the maximum IR peak intensity B in the range of 3600 to 3700 cm originating from the internal silanol groups of the spherical silica powder is 0.1 or less. -1 and the maximum IR peak intensity A at 3700 cm originating from isolated silanol groups on the surface. -1 Super 3800cm -1 The spherical silica powder according to [1], wherein the sum of the maximum IR peak intensities B below (A + B) is less than 0.2. [4] The spherical silica powder according to [1], wherein the sum of the maximum IR peak intensities B below (A + B) is less than 0.2. -1 [5] The spherical silica powder according to [1], wherein the maximum IR peak intensity at 0.2 or less. [6] The spherical silica powder according to [1], wherein the median diameter d50 is 0.5 to 20.0 μm. [7] The spherical silica powder according to [1], wherein the specific surface area is 0.1 to 4.0 m 2 / g. [7] The spherical silica powder according to [1], wherein the dielectric dissipation factor of the spherical silica powder is 0.0020 or less at a frequency of 1 GHz. [8] The spherical silica powder according to [1], wherein the spherical silica powder contains 30 to 1500 ppm by mass of Ti. [9] A method for producing the spherical silica powder according to any one of [1] to [8], comprising calcining a spherical silica precursor under a reducing atmosphere.
[10] A method for producing the spherical silica powder according to [9], comprising forming the spherical silica precursor by a wet method.
[11] A resin composition comprising the spherical silica powder according to any one of [1] to [8], and a resin.
[0010] According to the present invention, it is possible to provide a spherical silica powder that has low dielectric loss and excellent adhesion to resin when mixed with resin for use in electronic applications.
[0011] The present invention will be described below, but the present invention is not limited to the examples in the following description. In this specification, the term "to" indicating a range of values means that the values before and after it are included as the lower and upper limits. In this specification, "mass" is synonymous with "weight."
[0012] <Spherical Silica Powder> The spherical silica powder of the present invention has a silanol group density of 3600 to 3700 cm originating from the internal silanol groups of the spherical silica powder. -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 The ratio (B / A) of the maximum IR peak intensity B below is 0.5 to 1.5.
[0013] Generally, silanol groups (Si—OH) of silica particles are classified into internal silanol groups present within the Si—O network inside the particles, isolated silanol groups present on the particle surface that are not bonded to water adsorbed on the silica particles, and bonded silanol groups that are bonded to water adsorbed on the silica particles or silanols on the silica surface. Silanol groups are polar functional groups that increase dielectric loss, so from the perspective of reducing dielectric loss, it is preferable to have a small amount of silanol groups. However, the present inventors have found that the fewer isolated silanol groups present on the particle surface, the more inactive the surface of the spherical silica powder becomes, resulting in poor compatibility when mixed with a resin and reduced adhesion to the resin. The 3600 to 3700 cm peaks derived from the internal silanol groups of the spherical silica powder. -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 When the ratio (B / A) of the maximum IR peak intensity B below is 0.5 to 1.5, a spherical silica powder can be provided that has low dielectric loss and excellent adhesion to resin when mixed with resin for use in electronic applications.
[0014] In the spherical silica powder of the present invention, the silanol groups of 3600 to 3700 cm originating from the internal silanol groups -1 The maximum IR peak intensity A at 3600 to 3700 cm originating from the internal silanol groups of the spherical silica powder is preferably less than 0.2. When the internal silanol groups are large, the dielectric loss tends to increase when a resin composition obtained by mixing the spherical silica powder with a resin is used for electronic applications. -1 When the maximum IR peak intensity A in the range of 3600 to 3700 cm originating from the internal silanol group is less than 0.2, the dielectric loss can be reduced. -1 The maximum IR peak intensity A at is more preferably 0.10 or less, even more preferably 0.08 or less, and most preferably 0.05 or less. The internal silanol groups do not interact with the resin and deteriorate the dielectric loss tangent, so the fewer the number the better. Therefore, there is no particular lower limit.
[0015] In the spherical silica powder of the present invention, the 3700 cm-1 Super 3800cm -1 The maximum IR peak intensity B below is preferably 0.1 or less. When there are many isolated silanol groups on the surface, the dielectric loss tends to increase when a resin composition in which spherical silica powder is mixed with a resin is used for electronic applications. However, the 3700 cm IR peak intensity derived from the isolated silanol groups on the surface of the spherical silica powder is -1 Super 3800cm -1 When the maximum IR peak intensity B below 3700 cm originating from isolated silanol groups on the surface is 0.1 or less, the dielectric loss can be reduced. -1 Super 3800cm -1 The maximum IR peak intensity B below is more preferably 0.05 or less, and even more preferably 0.03 or less. In addition, from the viewpoint of improving the adhesion to the resin when the spherical silica powder is mixed with the resin, the 3700 cm IR peak intensity derived from the isolated silanol groups on the surface of the spherical silica powder is -1 Super 3800cm -1 The maximum IR peak intensity B below is preferably 0.005 or more, more preferably 0.010 or more, even more preferably 0.013 or more, and particularly preferably 0.015 or more. That is, the 3700 cm -1 Super 3800cm -1 The maximum IR peak intensity B below is preferably in the range of 0.005 to 0.1.
[0016] The spherical silica powder of the present invention has a silanol group-derived 3600 to 3700 cm -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1The ratio (B / A) of the maximum IR peak intensity B below is 0.5 to 1.5. A B / A of 1.5 or less leaves isolated silanol groups that function to enhance adhesion at the interface between the resin and silica, while sufficiently reducing the amount of internal silanol groups that do not interact with the resin and deteriorate the dielectric tangent, thereby achieving both adhesion to the resin and a reduced dielectric tangent. Furthermore, a B / A of 0.5 or more reduces the amount of internal silanol groups, thereby sufficiently reducing the dielectric tangent. This allows for excellent peel strength when the spherical silica powder is mixed with a resin and a resin composition is formed on a substrate such as a metal. B / A is preferably 1.3 or less, more preferably 1.1 or less, and preferably 0.6 or more, more preferably 0.7 or more.
[0017] 3600-3700 cm due to internal silanol groups -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 The ratio (B / A) of the maximum IR peak intensity B below can be adjusted by the firing conditions during production of the spherical silica powder, the particle size of the silica precursor, etc.
[0018] In addition, the spherical silica powder of the present invention has a molecular weight of 3600 to 3700 cm originating from internal silanol groups. -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 It is preferable that the sum of the maximum IR peak intensities B below (A + B) is less than 0.2. -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1When the sum (A+B) of the maximum IR peak intensities B below is less than 0.2, the dielectric loss can be further reduced when a resin composition containing spherical silica powder mixed with a resin is used in electronic applications. A+B is more preferably 0.19 or less, even more preferably 0.15 or less, particularly preferably 0.10 or less, and most preferably 0.05 or less. Furthermore, from the viewpoint of improving the adhesion at the interface between the isolated silanol groups on the silica surface and the resin, A+B is preferably 0.02 or more, more preferably 0.03 or more.
[0019] In addition, the silanol groups of the spherical silica powder have a wavelength of 3300 to 3800 cm -1 The maximum IR peak intensity at 3300 to 3800 cm is preferably 0.2 or less, more preferably 0.1 or less, even more preferably 0.05 or less, particularly preferably 0.02 or less, and most preferably 0.017 or less. -1 When the maximum IR peak intensity at 3300 to 3800 cm originating from the silanol groups of the spherical silica powder is 0.2 or less, the dielectric loss can be reduced when a resin composition obtained by mixing the spherical silica powder with a resin is used for electronic applications. -1 The maximum IR peak intensity at is preferably 0.010 or more.
[0020] The IR spectrum of the silanol groups of the spherical silica powder can be measured by the following procedure. (Measurement Method) Using an infrared spectrometer (for example, IR Prestige-21 (manufactured by Shimadzu Corporation)), spherical silica powder is dispersed in diamond and measured by the diffuse reflectance method. The measurement range is 400 to 4000 cm. -1 , resolution is 4cm -1 The number of times of accumulation is 128. The dilution to the diamond powder is defined as [mass dilution ratio] = ([sample mass]) / ([diamond mass] + [sample mass]), and [mass dilution ratio] = 85 - 2.5 × [BET specific surface area]. The spherical silica powder used is vacuum dried at 180 °C for 1 hour. The IR spectrum is measured at 800 cm -1 Normalized to 3800 cm -1 After adjusting the baseline, 3600-3700 cm-1 The maximum IR peak at 3700 cm -1 Super 3800cm -1 The maximum IR peaks below and 3300-3800 cm -1 The maximum IR peak in the range is obtained.
[0021] The spherical silica powder preferably has a median diameter d50, which is the particle diameter at the point where the cumulative volume is 50% on a volume-based particle size distribution curve, of 0.5 to 20.0 μm. When the median diameter d50 of the spherical silica powder is 0.5 μm or more, the dielectric loss tangent can be significantly reduced. Furthermore, when the median diameter d50 of the spherical silica powder is 20.0 μm or less, the particle gauge value can be prevented from increasing, thereby achieving excellent peel strength when a resin composition containing the spherical silica powder is used in electronic applications. Therefore, in the present invention, the median diameter d50 of the spherical silica powder is preferably 0.5 to 20.0 μm, more preferably 0.5 to 10.0 μm, and even more preferably 1 to 5.0 μm.
[0022] The 10% particle size d10, which is the particle size at which the cumulative volume becomes 10% in the volume-based particle size distribution curve of the spherical silica powder, is preferably 0.5 to 5.0 μm, more preferably 1.0 to 3.0 μm, from the viewpoints of improving the uniform dispersibility when the spherical silica powder is mixed into a resin and enhancing the interaction between the spherical silica powder and the resin.
[0023] The ratio of the median diameter d50 to the 10% particle diameter d10 (d50 / d10) is preferably greater than 1.0 and not greater than 5.0, more preferably 1.3 to 4.0, and even more preferably 1.5 to 3.0, from the viewpoints of improving the uniform dispersibility when the spherical silica powder is mixed into a resin and enhancing the interaction between the spherical silica powder and the resin.
[0024] The maximum particle diameter (Dmax) of the spherical silica powder is preferably 150 times or less, more preferably 100 times or less, even more preferably 50 times or less, and particularly preferably 10 times or less, the median diameter d50. If the maximum particle diameter (Dmax) is 150 times or less the median diameter d50, defects are less likely to occur when the sheet is processed. Furthermore, the maximum particle diameter (Dmax) is preferably 1.2 times or more, more preferably 1.5 times or more, and even more preferably 2 times or more, the median diameter d50.
[0025] The median diameter d50 is the volume-based cumulative 50% diameter determined using a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by Microtrac-Bell Co., Ltd.). That is, the particle size distribution is measured using a laser diffraction / scattering method, a cumulative curve is calculated with the total volume of the spherical silica powder set to 100%, and the particle diameter is the point on the cumulative curve where the cumulative volume is 50%. The 10% particle diameter d10 is the volume-based cumulative 10% diameter determined using a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by Microtrac-Bell Co., Ltd.). That is, the particle size distribution is measured using a laser diffraction / scattering method, a cumulative curve is calculated with the total volume of the spherical silica powder set to 100%, and the particle diameter is the point on the cumulative curve where the cumulative volume is 10%. The maximum particle diameter can also be obtained by the same measurement as the median diameter d50 and the 10% particle diameter d10.
[0026] The specific surface area Y of the spherical silica powder of the present invention is 0.1 to 4.0 m 2 It is preferable that the specific surface area Y is in the range of 0.1 m / g. 2 When the spherical silica powder has a particle size of 4.0 m / g or more, there is sufficient contact with the resin when the spherical silica powder is contained in the resin composition, so that the spherical silica powder is well-suited to the resin. 2 When the specific surface area Y is 4.0 m / g or less, the dielectric loss tangent can be reduced, so that the powder can exhibit an excellent low dielectric loss tangent even in a resin composition, and the dispersion in the resin composition is improved. 2 / g or less, and 3.5m 2 / g or less is more preferable, and 3.0m 2 / g or less is particularly preferred, and 2 / g or more, and2 / g or more is more preferable, and 0.5m 2 / g or more is particularly preferred. 2 It is practically difficult to obtain a value less than 1 / g.
[0027] The specific surface area is determined by the BET method based on the nitrogen adsorption method using a specific surface area / pore distribution measuring device (for example, "BELSORP-mini II" manufactured by Microtrac-Bell, or "Tristar II" manufactured by Micromeritics).
[0028] The specific surface area Y (m 2 / g) and the median diameter d50 (μm), Y×d50 is 2.7 to 5.0 μm 2 It is preferable that Y×d50 is 5.0 μm·m 2 / g or less, the specific surface area per particle size can be sufficiently reduced, and the dielectric loss tangent can be reduced. 2 / g is more preferable, and 2.7 to 4.0 μm m 2 The theoretical value of Y×d50 is 2.7 [specific surface area=6 / (true density of silica 2.2 (g / cm 3 ) × median diameter d50 (μm)], and values below this are practically unattainable.
[0029] The average circularity of the spherical silica powder is preferably 0.75 to 1.0. As the average circularity decreases, the specific surface area increases, which tends to increase the dielectric loss tangent, so the average circularity is preferably 0.75 or more. The average circularity is more preferably 0.85 or more, even more preferably 0.90 or more, and particularly preferably 0.93 or more, and the closer to 1.0 the better.
[0030] The average circularity can be obtained by measuring the maximum diameter (DL) and the minor diameter (DS) perpendicular to the maximum diameter (DL) of each of 100 particles in a photographic projection obtained by photographing with a scanning electron microscope (SEM), and calculating the average value of the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL).
[0031] The spherical silica powder of the present invention preferably has a dielectric dissipation factor of 0.0020 or less at a frequency of 1 GHz, more preferably 0.0010 or less, and even more preferably 0.0008 or less. In particular, when measuring the dielectric dissipation factor and dielectric constant of the powder, the sample space becomes small at frequencies of 10 GHz or higher, resulting in poor measurement accuracy. Therefore, in the present invention, measurements at a frequency of 1 GHz are used. When the spherical silica powder has a dielectric dissipation factor of 0.0020 or less at a frequency of 1 GHz, excellent dielectric loss suppression effects are achieved, resulting in substrates and sheets with improved high-frequency characteristics. The smaller the dielectric dissipation factor, the more the circuit transmission loss is suppressed, so the lower limit is not particularly limited. From the same perspective, the dielectric constant of the spherical silica powder is preferably 5.0 or less at a frequency of 1 GHz, more preferably 4.5 or less, and even more preferably 4.1 or less.
[0032] The dielectric loss tangent and dielectric constant can be measured by a perturbation resonator method using a dedicated device (for example, "Vector Network Analyzer E5063A" manufactured by Keycom Corporation).
[0033] The spherical silica powder of the present invention is preferably one that has a viscosity of 5000 mPa·s or less when measured by the following measurement method: (Measurement method) 6 parts by mass of boiled linseed oil specified in JIS K 5421:2000 and 8 parts by mass of spherical silica powder are mixed, kneaded at 2000 rpm for 3 minutes, and the kneaded product is subjected to a shear rate of 1 s using a rotational rheometer. -1 The measurement is carried out for 30 seconds, and the viscosity at the time of 30 seconds is determined.
[0034] The shear rate of the kneaded material obtained by the above measurement method is 1 s -1When the viscosity at 1000 mPa·s is 5000 mPa·s or less, the amount of solvent added during molding and film formation of a resin composition containing spherical silica powder can be reduced, the drying speed can be increased, and productivity can be improved. Furthermore, if the specific surface area according to the particle size of the silica powder is large, the viscosity tends to increase when added to a resin composition, so in order to suppress the increase in viscosity of the resin composition, it is preferable to reduce the specific surface area of the spherical silica powder of the present invention, for example. The viscosity of the kneaded product is more preferably 4000 mPa·s or less, and even more preferably 3500 mPa·s or less. At a shear rate of 1 s of the kneaded product, -1 The lower the viscosity at 200°C, the better the coatability of the resin composition and the higher the productivity, so there is no particular restriction on the lower limit.
[0035] The spherical silica powder is preferably non-porous particles. Porous particles tend to increase the oil absorption, leading to an increase in viscosity in the resin, an increase in surface area, and an increase in the number of silanol (Si—OH) groups on the silica particle surface, resulting in a deterioration in the dielectric loss tangent. Specifically, the oil absorption is preferably 100 ml / 100 g or less, more preferably 70 ml / 100 g or less, and most preferably 50 ml / 100 g or less. There is no particular restriction on the lower limit, but it is practically difficult to achieve an oil absorption of 20 ml / 100 g or less.
[0036] The spherical silica powder of the present invention preferably contains titanium (Ti) in the range of 30 to 1500 ppm by mass. The Ti content is more preferably 80 ppm by mass or more, even more preferably 100 ppm by mass or more, and more preferably 1000 ppm by mass or less, even more preferably 500 ppm by mass or less. The Ti content can be measured by inductively coupled plasma (ICP) emission spectrometry after adding perchloric acid and hydrofluoric acid to the silica powder and igniting the mixture to remove the main component silicon.
[0037] Ti is an optional component that can be included in the production of spherical silica powder. If fine powder is generated due to cracking of silica particles during the production of spherical silica powder, the fine powder will adhere to the surface of the base particles, increasing the specific surface area of the particles. By including Ti during the production of spherical silica powder, densification during firing is facilitated. This makes the particles less likely to crack during post-treatment after firing, thereby suppressing the generation of fine powder and reducing the number of particles adhering to the surface of the silica base particles, thereby suppressing an increase in the specific surface area. By including 30 ppm by mass or more of Ti, densification during firing is facilitated, thereby suppressing the generation of fine powder due to cracking. When the Ti content is 1500 ppm by mass or less, the above effects can be achieved, and an increase in the amount of silanol groups can be suppressed, thereby suppressing a deterioration in the dielectric loss tangent.
[0038] The spherical silica powder of the present invention may contain impurity elements other than titanium (Ti) as long as the effects of the present invention are not impaired. Examples of impurity elements other than Ti include Na, K, Mg, Ca, Al, and Fe. The total content of alkali metals and alkaline earth metals among the impurity elements is preferably 2000 mass ppm or less, more preferably 1000 mass ppm or less, and even more preferably 200 mass ppm or less.
[0039] <Method for Producing Spherical Silica Powder> The method for producing spherical silica powder according to the present invention includes calcining a spherical silica precursor in a reducing atmosphere.
[0040] (Silica precursor) It is preferable to use a porous silica precursor. The silica precursor being porous means that pores are uniformly distributed in the silica precursor. By using porous silica particles as the silica precursor, it is easier to obtain particles with controlled particle shape, particle size distribution, etc., compared to particles produced by pulverizing a non-porous raw material and then calcining it.
[0041] The pore volume of the silica precursor is preferably in the range of 0.1 to 2.0 ml / g. If the pore volume is 0.1 ml / g or more, the apparent volume of the particles decreases when the silica is rendered non-porous during firing, resulting in sparse particles that are difficult to sinter, or a powder with weak sintering strength is obtained. If the pore volume is 2.0 ml / g or less, the bulk density of the silica particles before firing is prevented from becoming too large, improving productivity, and the silica particles shrink sufficiently during firing, allowing the specific surface area to be sufficiently small. The pore volume is more preferably 0.3 ml / g or more, even more preferably 0.6 ml / g or more, particularly preferably 0.7 ml / g or more, and more preferably 1.8 ml / g or less, even more preferably 1.5 ml / g or less, and particularly preferably 1.2 ml / g or less.
[0042] The specific surface area of the silica precursor is 200 to 1000 m 2 / g. 2 / g or more, the surface area after firing can be reduced while suppressing sintering of the particles. 2 When the specific surface area is 400 m / g or less, the strength of the silica precursor particles is sufficiently high. 2 / g or more is more preferable, and 500m 2 / g or more is more preferable, and 700m 2 / g or more is particularly preferred, and 2 / g or less is more preferable, and 2 / g or less is more preferable.
[0043] The pore volume and specific surface area can be determined by the BET method based on the nitrogen adsorption method using a specific surface area / pore distribution measuring device (for example, "BELSORP-mini II" manufactured by Microtrac-Bell, or "Tristar II" manufactured by Micromeritics).
[0044] The average pore diameter of the silica precursor is preferably 1.0 to 50.0 nm. When the average pore diameter is 1.0 nm or more, the particles can be made uniformly non-porous throughout, leaving no bubbles inside, and the dielectric loss tangent can be reduced. When the average pore diameter is 50.0 nm or less, the silica particles can be densified (reduced specific surface area) by firing without leaving any pores, and the dielectric loss tangent can be reduced. The average pore diameter is more preferably 2.0 nm or more, even more preferably 3.0 nm or more, and particularly preferably 4.0 nm or more, and more preferably 40.0 nm or less, even more preferably 30.0 nm or less, and particularly preferably 20.0 nm or less.
[0045] The average pore diameter can be determined by the BET method based on the nitrogen adsorption method using a specific surface area / pore distribution measuring device (for example, "BELSORP-mini II" manufactured by Microtrac-Bell, or "Tristar II" manufactured by Micromeritics).
[0046] The silica precursor used in the manufacturing method of the present invention is spherical, and its average circularity is preferably 0.90 or more. When the average circularity is 0.90 or more, the particle is substantially spherical, so the surface area of the particle can be reduced, and the active surface is not exposed because the protrusions are not broken by vibration of the particle, so the silica particles can have a low dielectric constant. The average circularity is more preferably 0.92 or more, and particularly preferably 0.95 or more. Furthermore, the closer to a perfect sphere, the more desirable it is, so 1.00 is the most preferable.
[0047] The average circularity can be calculated by the same method as described above.
[0048] The median diameter d50 of the silica precursor, which is the particle diameter at the point where the cumulative volume is 50% on the volume-based particle size distribution curve, is preferably 1 to 500 μm. If the median diameter d50 of the silica precursor is 1 μm or more, it can be made into spherical particles even after calcination to reduce the surface area, and if it is 500 μm or less, it can be easily used as a filler for resins that are easy to mold. The median diameter d50 is more preferably 1.2 μm or more, even more preferably 1.5 μm or more, more preferably 100 μm or less, even more preferably 50 μm or less, particularly preferably 20 μm or less, even more preferably 10 μm or less, and most preferably 5 μm or less.
[0049] Furthermore, the silica precursor preferably has a weight loss rate of 10% or less when dried at 230°C for 12 hours. If the weight loss rate is 10% or less, sintering of the particles is unlikely to occur when the silica precursor is fired in a state where the particles are in contact with each other, making it easier to obtain spherical silica powder. The weight loss rate is more preferably 9% or less, even more preferably 8% or less, and particularly preferably 6% or less. Furthermore, since it is desirable that the weight does not change even after drying at 230°C for 12 hours, the lower limit is not particularly limited. If the obtained silica precursor has a high water content and the weight loss rate when dried at 230°C for 12 hours exceeds 10%, it is preferable to dry it until the weight loss rate is 10% or less. Examples of drying methods include a spray dryer, static drying in a dryer, and ventilation with dry air.
[0050] The ignition loss of the silica precursor is preferably 5.0 to 15.0% by mass. The ignition loss is the sum of the water adhering to the silica precursor and the water generated by condensation of silanol groups contained in the silica precursor. When the silica precursor has an appropriate number of silanol groups, condensation proceeds during calcination, making it easier for the silanol groups to be reduced. If the ignition loss is too high, the yield during calcination decreases and productivity deteriorates. Therefore, the ignition loss of the silica precursor is preferably 15.0% by mass or less, more preferably 13.0% by mass or less, and most preferably 12.0% by mass or less. If the ignition loss is too low, silanol groups are more likely to remain during calcination. Therefore, the ignition loss of the silica precursor is preferably 5.0% by mass or more, more preferably 6.0% by mass or more, and most preferably 7.0% by mass or more.
[0051] Here, the ignition loss is determined in accordance with JIS K0067 (1992) as the mass loss when 1 g of silica precursor is heated and dried at 850° C. for 0.5 hours.
[0052] The silica precursor may be obtained by manufacturing or may be a commercially available product, such as H-11, H-31, or H-201 manufactured by AGC Si-Tech Co., Ltd.
[0053] When a silica precursor is obtained by manufacturing, it can be obtained by methods such as a wet method or a granulation method. Among these, it is preferable to form a silica precursor using a wet method. The wet method refers to a method that includes a process of using a liquid silica source and gelling it to obtain a raw material for spherical silica powder. By forming a silica precursor using a wet method, spherical silica particles can be formed, eliminating the need to adjust the particle shape by pulverization or the like, and as a result, particles with a small specific surface area can be obtained. In addition, the wet method is less likely to produce particles that are significantly smaller than the average particle size, and the specific surface area tends to be small after firing. In addition, in the wet method, the amount of impurity elements such as titanium can be adjusted by adjusting the impurities in the silica source, and the aforementioned impurity elements can be uniformly dispersed in the particles.
[0054] Examples of wet methods include spraying and emulsion gelation. Examples of emulsion gelation methods include emulsifying a dispersed phase containing a silica precursor with a continuous phase, and gelling the resulting emulsion to obtain a spherical silica precursor. A preferred emulsification method is to feed a dispersed phase containing a silica precursor into a continuous phase through micropores or a porous membrane to produce an emulsion. This produces an emulsion with uniform droplet sizes, resulting in spherical silica with uniform particle sizes. Examples of such emulsification methods include a micromixer method and a membrane emulsification method. For example, the micromixer method is disclosed in International Publication No. 2013 / 062105. The spherical silica powder obtained by the above method is amorphous solid silica.
[0055] The spherical silica powder of the present invention is obtained by calcining the spherical silica precursor described above under a reducing atmosphere. It is believed that calcination in a reducing atmosphere promotes the condensation of silanol groups and the reduction of OH groups. This reduces the amount of isolated silanol groups on the surface of the spherical silica powder and internal silanol groups, and in particular, significantly reduces internal silanol groups, thereby improving dielectric properties while maintaining adhesion to resin. In this specification, "reducing atmosphere" refers to an atmosphere containing hydrogen. From the viewpoint of reaction equilibrium, the hydrogen concentration is preferably 1% by volume or more, more preferably 3% by volume or more, even more preferably 5% by volume or more, and particularly preferably 8% by volume or more. The upper limit of the hydrogen concentration is 100% by volume.
[0056] The calcination method is not particularly limited, but examples include static heat treatment, heat treatment in a rotary furnace, etc. For static heat treatment, a static electric furnace, a roller hearth kiln, a continuous furnace classified as a tunnel furnace, etc. can be used. For heat treatment in a rotary furnace, a horizontal rotary furnace (rotary kiln), a rotary tubular furnace, etc. can be used.
[0057] The baking temperature is preferably 700° C. or higher, more preferably 800° C. or higher, even more preferably 900° C. or higher, and particularly preferably 1000° C. or higher. From the viewpoint of suppressing strong sintering of the particles and reducing the particle gauge in the resin composition, the baking temperature is preferably 1600° C. or lower, more preferably 1500° C. or lower, and even more preferably 1400° C. or lower.
[0058] The firing time may be adjusted as appropriate depending on the firing apparatus and firing time used, but is preferably 0.5 to 50 hours, more preferably 1 to 10 hours, for example.
[0059] Examples of methods for forming a reducing atmosphere include methods using reducing gases such as hydrogen gas and carbon monoxide. Examples of devices for forming a reducing atmosphere include atmospheric furnaces that can use the reducing gas, and these devices may include, within the furnace, a heating device, a chamber filled with an inert gas (nitrogen, argon, etc.), a mechanism for evacuating the chamber, and the like, which makes it easier to control the reducing gas.
[0060] The spherical silica powder may be weakly sintered after firing, in which case it may be crushed. Crushing is preferably carried out so that the average circularity of the particles does not fall below 0.90 in order to maintain the surface area and not impair the effects of the present invention. It is also preferable that the surface area does not increase as a result of the crushing treatment. A significant increase in surface area due to the crushing treatment means that some spherical particles have been pulverized or that fine damage has occurred on the surface, resulting in the generation of fine powder. An increase in surface area is undesirable because it leads to an increase in viscosity when the spherical silica powder is dispersed in a resin and a deterioration in the dielectric loss tangent.
[0061] The crushing can be carried out using a crushing device such as a cyclone mill, a jet mill, or an impact mill, and crushing can also be carried out using an agate mortar or a vibrating sieve.
[0062] The spherical silica powder obtained by calcination may be surface-treated with a silane coupling agent. This process causes the silanol groups present on the surface of the spherical silica powder to react with the silane coupling agent, reducing the number of silanol groups on the surface and improving the dielectric loss tangent. Furthermore, the surface becomes hydrophobic, improving the affinity for resins and improving dispersibility in resins.
[0063] The conditions for the surface treatment are not particularly limited, and general surface treatment conditions may be used, and a wet treatment method or a dry treatment method may be used. From the viewpoint of performing a uniform treatment, the wet treatment method is preferred.
[0064] Examples of the silane coupling agent used in the surface treatment include aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, fluorine-containing silane coupling agents, organosilazane compounds, etc. These may be used alone or in combination of two or more.
[0065] Specific examples of the surface treatment agent (silane coupling agent) include aminosilane-based coupling agents such as aminopropyl methoxysilane, aminopropyl triethoxysilane, ureidopropyl triethoxysilane, N-phenylaminopropyl trimethoxysilane, and N-2(aminoethyl)aminopropyl trimethoxysilane; epoxysilane-based coupling agents such as glycidoxypropyl trimethoxysilane, glycidoxypropyl triethoxysilane, glycidoxypropyl methyldiethoxysilane, glycidyl butyl trimethoxysilane, and (3,4-epoxycyclohexyl)ethyl trimethoxysilane; mercaptosilane-based coupling agents such as mercaptopropyl trimethoxysilane and mercaptopropyl triethoxysilane; silane-based coupling agents such as methyltrimethoxysilane, vinyltrimethoxysilane, octadecyltrimethoxysilane, phenyltrimethoxysilane, metachloroxypropyl trimethoxysilane, imidazole silane, and triazine silane; and CF 3 (CF 2 ) 7 CH 2 CH 2 Si(OCH 3 ) 3 , C.F. 3 (CF 2 ) 7 CH 2 CH 2 SiCl 3 , C.F. 3 (CF 2 ) 7 CH 2 CH 2 Si(CH 3 ) (OCH 3 ) 2 , C.F. 3 (CF 2 ) 7 CH 2 CH 2 Si(CH 3 ) C1 2 , C.F. 3 (CF 2 ) 5 CH 2 CH 2 SiCl 3 , C.F. 3 (CF 2 )5 CH 2 CH 2 Si(OCH 3 ) 3 , C.F. 3 CH 2 CH 2 SiCl 3 , C.F. 3 CH 2 CH 2 Si(OCH 3 ) 3 , C 8 F 17 SO 2 N (C 3 H 7 ) CH 2 CH 2 CH 2 Si(OCH 3 ) 3 , C 7 F 15 CONHCH 2 CH 2 CH 2 Si(OCH 3 ) 3 , C 8 F 17 CO 2 CH 2 CH 2 CH 2 Si(OCH 3 ) 3 , C 8 F 17 -O-CF(CF 3 )CF 2 -O-C 3 H 6 SiCl 3 , C 3 F 7 -O-(CF(CF 3 )CF 2 -O) 2 -CF (CF 3 )CONH-(CH 2 ) 3 Si(OCH 3 ) 3 and organosilazane compounds such as hexamethyldisilazane, hexaphenyldisilazane, trisilazane, cyclotrisilazane, and 1,1,3,3,5,5-hexamethylcyclotrisilazane.
[0066] The amount of the silane coupling agent used for treatment is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, and even more preferably 0.10 parts by mass or more, per 100 parts by mass of the spherical silica powder, and is preferably 5 parts by mass or less, and more preferably 2 parts by mass or less.
[0067] Examples of methods for treating with a silane coupling agent include a dry method in which the silane coupling agent is sprayed onto spherical silica powder, and a wet method in which the spherical silica powder is dispersed in a solvent and then a silane coupling agent is added to cause a reaction.
[0068] The fact that the surface of the spherical silica powder has been treated with a silane coupling agent can be confirmed by detecting a peak due to a substituent of the silane coupling agent by IR. The amount of the silane coupling agent attached can be measured by the carbon content.
[0069] <Resin Composition> The spherical silica powder of the present invention has excellent adhesion to resins, and therefore excellent mixability into resin compositions. The resin composition according to this embodiment contains the spherical silica powder of the present invention and a resin. The content of the spherical silica powder in the resin composition is preferably 5 to 90% by mass, more preferably 10 to 85% by mass, even more preferably 10 to 80% by mass, particularly preferably 10 to 75% by mass, especially preferably 10 to 70% by mass, and most preferably 15 to 70% by mass. A spherical silica powder content of 5% by mass or more provides sufficient peel strength, while a spherical silica powder content of 90% by mass or less prevents the viscosity of the resin composition from increasing excessively, making it easy to handle. The content of the spherical silica powder in the resin composition is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, especially preferably 75% by mass or less, and most preferably 70% by mass or less.
[0070] Examples of the resin include epoxy resin, silicone resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, fluororesin, polyamide resin such as polyimide resin, polyamideimide resin, and polyetherimide; polyester resin such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene ether resin, polyphenylene sulfide resin, orthodivinylbenzene resin, aromatic polyester resin, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile butadiene styrene) resin, AAS (acrylonitrile-acrylic rubber styrene) resin, AES (acrylonitrile ethylene propylene diene rubber styrene) resin, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-ethylene copolymer (ETFE). One or more of these may be used. The dielectric loss tangent of a resin composition also depends on the properties of the resin, so the resin to be used should be selected taking these into consideration.
[0071] The resin preferably contains a thermosetting resin. One type of thermosetting resin may be used, or two or more types may be used. Examples of the thermosetting resin include epoxy resin, polyphenylene ether resin, polyimide resin, phenol resin, and orthodivinylbenzene resin. From the viewpoints of adhesion, heat resistance, and the like, the thermosetting resin is preferably an epoxy resin, polyphenylene ether resin, or orthodivinylbenzene resin.
[0072] From the viewpoint of adhesion, dielectric properties, etc., the weight average molecular weight of the thermosetting resin is preferably 1000 to 7000, more preferably 1000 to 5000, and even more preferably 1000 to 3000. The weight average molecular weight is determined using gel permeation chromatography (GPC) in terms of polystyrene.
[0073] From the viewpoints of suppressing uneven distribution of silica particles, reducing water absorption, low dielectric tangent, adhesion, etc., the content of the spherical silica powder relative to 100 parts by mass of the thermosetting resin is preferably 10 to 400 parts by mass, more preferably 50 to 300 parts by mass, and even more preferably 70 to 250 parts by mass. In particular, when a high loading of silica particles is desired, the content of the silica particles is preferably 80 parts by mass or more, and more preferably 90 parts by mass or more.
[0074] The silica particles contained in the resin composition preferably have a unimodal particle size distribution, which can be confirmed by a single peak in the particle size distribution measured by a laser diffraction / scattering method.
[0075] The resin composition may contain any component other than the resin and medium (e.g., toluene, methyl ethyl ketone, etc.) Examples of the optional component include a dispersing aid, a surfactant, and a filler other than silica.
[0076] When a resin film is produced using a resin composition containing the spherical silica powder of the present invention, the dielectric loss tangent is preferably 0.012 or less at a frequency of 10 GHz, more preferably 0.010 or less, and even more preferably 0.009 or less. If the dielectric loss tangent at a frequency of 10 GHz is 0.012 or less, the resin film has excellent electrical properties and can be expected to be used in electronic devices, communication devices, etc. The smaller the dielectric loss tangent, the more the circuit transmission loss can be suppressed, so the lower limit is not particularly limited.
[0077] Furthermore, when a resin film is produced using a resin composition containing the spherical silica powder of the present invention, the relative dielectric constant thereof is preferably 2.0 to 3.5 at a frequency of 10 GHz, with the lower limit being more preferably 2.2 or more, and even more preferably 2.3 or more, and the upper limit being more preferably 3.2 or less, and even more preferably 3.0 or less. When the relative dielectric constant of the resin film at a frequency of 10 GHz is within this range, the resin film has excellent electrical properties and is therefore expected to be used in electronic devices, communication devices, etc.
[0078] The relative dielectric constant can be measured by a perturbation resonator method using a dedicated device (for example, a "Vector Network Analyzer E5063A" manufactured by Keycom Co., Ltd.). The dielectric loss tangent of the resin film can be measured using a split post dielectric resonator (SPDR) (for example, manufactured by Agilent Technologies).
[0079] The resin film preferably has an average linear expansion coefficient of 10 to 50 ppm / °C. When the average linear expansion coefficient is within this range, it is close to the thermal expansion coefficient of copper foil, which is widely used as a substrate, and therefore has excellent electrical properties. The average linear expansion coefficient is more preferably 12 ppm / °C or higher, and even more preferably 15 ppm / °C or higher, and more preferably 40 ppm / °C or lower, and even more preferably 30 ppm / °C or lower.
[0080] The average linear expansion coefficient can be determined by using a thermomechanical analyzer (for example, "TMA-60" manufactured by Shimadzu Corporation) to heat the resin film under a load of 5 N at a temperature increase rate of 2°C / min, measuring the dimensional change of the sample from 30°C to 150°C, and calculating the average.
[0081] The spherical silica powder of the present invention can also be used as a variety of fillers, and is particularly suitable as a filler for resin compositions used in the production of electronic substrates for use in electronic devices such as personal computers, laptop computers, and digital cameras, and communication devices such as smartphones and game consoles. Specifically, the silica powder of the present invention is expected to be applied to resin compositions, prepregs, metal foil-clad laminates, printed wiring boards, resin sheets, adhesive layers, adhesive films, solder resists, bump reflow materials, rewiring insulating layers, die bond materials, encapsulants, underfills, mold underfills, and laminated inductors, among other applications, due to its low dielectric loss tangent, low transmission loss, low moisture absorption, and improved peel strength.
[0082] As described above, the present specification discloses the following configurations: <1> A spherical silica powder having a silanol group-derived internal silanol group of 3600 to 3700 cm -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1<2> A spherical silica powder having a maximum IR peak intensity B of 3700 cm originating from isolated silanol groups on the surface, the ratio (B / A) of which is 0.5 to 1.5. -1 Super 3800cm -1 The spherical silica powder according to <1>, wherein the maximum IR peak intensity B in the range of 3600 to 3700 cm originating from the internal silanol groups of the spherical silica powder is 0.1 or less. -1 and the maximum IR peak intensity A at 3700 cm originating from isolated silanol groups on the surface. -1 Super 3800cm -1 The spherical silica powder according to <1> or <2>, wherein the sum of the maximum IR peak intensities B below (A+B) is less than 0.2. <4> The spherical silica powder according to <1> or <2>, wherein the sum of the maximum IR peak intensities B below (A+B) is less than 0.2. -1 <5> The spherical silica powder according to any one of <1> to <4>, having a median diameter d50 of 0.5 to 20.0 μm. <6> The spherical silica powder according to any one of <1> to <4>, having a specific surface area of 0.1 to 4.0 m. 2 / g. <7> The spherical silica powder according to any one of <1> to <5>, wherein the dielectric dissipation factor of the spherical silica powder is 0.0020 or less at a frequency of 1 GHz. <8> The spherical silica powder according to any one of <1> to <7>, wherein the spherical silica powder contains 30 to 1500 ppm by mass of Ti. <9> A method for producing the spherical silica powder according to any one of <1> to <8>, comprising calcining a spherical silica precursor under a reducing atmosphere. <10> A method for producing the spherical silica powder according to <9>, comprising forming the spherical silica precursor by a wet method. <11> A resin composition comprising the spherical silica powder according to any one of <1> to <8>, and a resin.
[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the same components are used. Examples 1 and 2 are comparative examples, and Examples 3 to 7 are working examples.
[0084] Example 1 Silica powder (SO-C2 manufactured by Admatechs Co., Ltd.) was prepared as a silica precursor. 15 g of the silica precursor was washed with 150 ml of distilled water, dried at 200°C for 12 hours, and then loaded into an alumina crucible and heat-treated (fired) at 1200°C in an air atmosphere for 1 hour. After the heat treatment (fired), the mixture was cooled to 25°C and crushed in an agate mortar to obtain the silica powder of Example 1.
[0085] Example 2 The same operation as in Example 1 was carried out, except that silica powder produced by a wet method (AGC Si-Tech Co., Ltd.: H-31, d50: 3.5 μm) was used as the silica precursor, to obtain silica powder of Example 2.
[0086] Example 3 The same procedure as in Example 2 was carried out, except that the silica precursor was calcined under a hydrogen atmosphere, to obtain silica powder of Example 3.
[0087] Example 4 The same procedure as in Example 3 was carried out, except that the calcination time of the silica precursor was changed to 3 hours, to obtain silica powder of Example 4.
[0088] Example 5 The same procedure as in Example 2 was carried out, except that the silica precursor was calcined in a nitrogen atmosphere containing hydrogen, to obtain silica powder of Example 5. The volume ratio of hydrogen to nitrogen was 1:9.
[0089] (Example 6) A silica powder produced by a wet process (AGC Si-Tech Co., Ltd.: H-11, d50: 2.0 μm) was prepared as a silica precursor, and the same operation as in Example 2 was carried out except that the silica precursor was calcined in a nitrogen atmosphere containing hydrogen, to obtain the silica powder of Example 6. The volume ratio of hydrogen to nitrogen was 1:9.
[0090] (Example 7) A silica powder produced by a wet process (AGC Si-Tech Co., Ltd.: H-201, d50: 20.0 μm) was prepared as a silica precursor, and the same operation as in Example 2 was carried out except that the silica precursor was calcined in a nitrogen atmosphere containing hydrogen, to obtain silica powder of Example 7. The volume ratio of hydrogen to nitrogen was 1:9.
[0091] The following measurements were carried out on the silica powders of Examples 1 to 7. The results are shown in Table 1.
[0092] <Silanol Groups> The amount of silanol groups on the surface of the spherical silica powder was measured by infrared spectroscopy. The infrared spectroscopy was measured by a diffuse reflectance method using an IR Prestige-21 (manufactured by Shimadzu Corporation) by dispersing the spherical silica powder in diamond. The measurement range was 400 to 4000 cm -1 , resolution is 4cm -1 The number of times of accumulation was 128. The dilution to the diamond powder was defined as [mass dilution ratio] = ([sample mass]) / ([diamond mass] + [sample mass]), and [mass dilution ratio] = 85 - 2.5 × [BET specific surface area]. The spherical silica powder used was vacuum dried at 180 °C for 1 hour. The IR spectrum was measured at 800 cm -1 Normalized to 3800 cm -1 After adjusting the baseline, 3600-3700 cm -1 The maximum IR peak intensity A is 3700 cm -1 Super 3800cm -1 The maximum IR peak intensity B and 3300 to 3800 cm -1 The maximum IR peak intensity among those in the range was determined.
[0093] <Median diameter> Measurement was performed using a laser diffraction particle size distribution analyzer (MT3300EXII manufactured by Microtrac-Bell). Measurement was performed after dispersing the spherical silica powder by irradiating it with ultrasonic waves three times for 60 seconds inside the device. Measurement was performed twice for 60 seconds each, and the average value was calculated.
[0094] <Specific Surface Area> The spherical silica powder was dried under reduced pressure at 230°C to completely remove moisture, and used as a sample. The specific surface area of this sample was determined by the multipoint BET method using nitrogen gas with an automatic specific surface area and pore distribution measuring device "Tristar II" manufactured by Micromeritics.
[0095] <Dielectric Loss Tangent> 5 g of spherical silica powder, 20 ml of toluene, and 0.5 g of hexamethyldisilazane were placed in a 30 ml PE bottle, stirred, and filtered. The resulting powder was vacuum dried at 120°C for 1 hour to obtain a surface-treated silica powder. The resulting surface-treated silica powder was measured using a dedicated device (Vector Network Analyzer E5063A, Keycom Corporation) using a perturbation resonator method at a test frequency of 1 GHz, a test temperature of approximately 24°C, and a humidity of approximately 45%, with three measurements. Specifically, the spherical silica powder was vacuum dried at 150°C, and then thoroughly filled into a polytetrafluoroethylene (PTFE) cylinder while tapping. The dielectric constant of the container was measured, and then converted to a dielectric loss tangent using the powder filling rate in the container.
[0096] <Ti Content> Perchloric acid and hydrofluoric acid were added to the spherical silica powder, and the mixture was ignited to remove the silicon, which is the main component. Then, the Ti content was measured by ICP-AES (inductively coupled plasma atomic emission spectroscopy) using an ICPE-9000 (manufactured by Shimadzu Corporation).
[0097] <Average Circularity> The average circularity was determined by measuring the maximum diameter (DL) and the minor diameter (DS) perpendicular to the maximum diameter (DL) of each of 100 particles in a photographic projection obtained by photographing with a scanning electron microscope (SEM), and calculating the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL) to obtain an average value.
[0098] <Peel Strength> 55 parts by weight of the spherical silica powder obtained above, 59 parts by weight of polyphenylene ether resin, 16 parts by weight of butadiene-styrene random copolymer (Ricon 100 manufactured by Cray Valley), 25 parts by weight of triallyl isocyanurate (curing accelerator, TAIC manufactured by Mitsubishi Chemical Corporation), 1 part by weight of α,α'-di(t-butylperoxy)diisopropylbenzene (curing agent, Perbutyl P manufactured by NOF Corporation), and 80 parts by weight of toluene were placed in a polyvinyl alcohol bottle, and φ20 mm alumina balls were added and mixed at 30 rpm for 12 hours. The alumina balls were then removed to obtain a liquid composition. The liquid composition was impregnated into an IPC Spec 2116 glass cloth and heated and dried at 160°C for 4 minutes to obtain a prepreg. Copper foil (thickness: 18 μm, maximum height roughness Rz: 2 μm, manufactured by Mitsui Kinzoku Co., Ltd., MT18E) was laminated on both sides of the prepreg, and the laminate was then subjected to a temperature of 230°C and a pressure of 30 kg / cm. 2 The resin-coated metal substrate was subjected to measurement of the peel strength between the prepreg and the carrier-attached copper foil in accordance with IPC-TM650-2.4.8.
[0099]
[0100] The spherical silica powders of Examples 3 to 7, which are working examples, all had lower dielectric loss tangents than the comparative examples 1 and 2. In addition, the peel strength was high, demonstrating excellent adhesion to resin. On the other hand, the spherical silica powders of Comparative Examples 1 and 2 had a dielectric loss of 3600 to 3700 cm originating from the internal silanol groups. -1 The maximum IR peak intensity A is at 3700 cm , which is derived from isolated silanol groups on the surface. -1 Super 3800cm -1 The ratio (B / A) of the maximum IR peak intensity B shown below was greater than 1.5, and compared with the examples, the dielectric tangent was high and the peel strength was low, indicating poor adhesion to resin.
[0101] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-080276) filed on May 15, 2023, the entire contents of which are incorporated by reference.
Claims
1. 3600-3700 cm originating from the internal silanol groups of spherical silica powder -1 The maximum IR peak intensity A at 3700 cm originates from the isolated silanol groups on the surface. -1 Super 3800cm -1 A spherical silica powder having a ratio (B / A) of the maximum IR peak intensity B below of 0.5 to 1.
5.
2. 3700 cm originating from isolated silanol groups on the surface -1 Super 3800cm -1 The spherical silica powder according to claim 1, wherein the maximum IR peak intensity B below is 0.1 or less.
3. 3600 to 3700 cm originating from the internal silanol groups of the spherical silica powder -1 and the maximum IR peak intensity A at 3700 cm originating from isolated silanol groups on the surface. -1 Super 3800cm -1 The spherical silica powder according to claim 1, wherein the sum (A+B) of the maximum IR peak intensities B below is less than 0.
2.
4. 3300 to 3800 cm originating from the silanol groups of the spherical silica powder -1 2. The spherical silica powder according to claim 1, wherein the maximum IR peak intensity at is 0.2 or less.
5. The spherical silica powder according to claim 1, having a median diameter d50 of 0.5 to 20.0 μm.
6. Specific surface area is 0.1 to 4.0 m 2 The spherical silica powder according to claim 1, wherein the molecular weight is 1 / g.
7. The spherical silica powder according to claim 1, wherein the dielectric tangent of the spherical silica powder is 0.0020 or less at a frequency of 1 GHz.
8. The spherical silica powder according to claim 1, wherein the spherical silica powder contains 30 to 1,500 ppm by mass of Ti.
9. A method for producing a spherical silica powder according to any one of claims 1 to 8, comprising calcining a spherical silica precursor in a reducing atmosphere.
10. A method for producing the spherical silica powder according to claim 9, comprising forming the spherical silica precursor by a wet process.
11. A resin composition comprising the spherical silica powder according to any one of claims 1 to 8 and a resin.
Citation Information
Patent Citations
Modified sql-gel process silica particle and method for producing the same
JP2002255535A
Alkali-resistant chemically modified silica gel
JP2004250247A
Surface-modified spherical silica, method of manufacturing the same and resin composition for sealing
JP2005022915A
Amorphous silica and process for producing same
WO2011049121A1
Hollow silica particles and method for producing same
WO2021172294A1