Brilliant pigment, pigment-containing composition, and pigment-containing coated body
By coating a flake-like substrate with an optical interference film and using composite particles that include oxide particles to prevent agglomeration, the glittering pigment achieves enhanced color development and stability, addressing the issue of pigment particle aggregation and fall-off in existing technologies.
Patent Information
- Application Number
- PCT/JP2024/017832
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-21
AI Technical Summary
Existing glittering pigments that adhere pigment particles to a light interference film fail to produce the desired reflected light color, as the pigment particles tend to aggregate and fall off, reducing the effectiveness of the light interference effect.
A flake-like substrate coated with an optical interference film and composite particles comprising pigment particles and oxide particles, where the oxide particles prevent agglomeration and ensure the pigment particles remain attached, enhancing the light interference effect and color vividness.
The solution provides a bright, stable glittering pigment with improved color development and vividness by maintaining the pigment particles on the interference film, ensuring consistent and vibrant light reflection.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Luster pigment, pigment-containing composition, and pigment-containing coated body
[0001] The present invention relates to a bright pigment, more specifically to a bright pigment having a flake substrate and an optical interference film on the flake substrate.The present invention also relates to a pigment-containing composition and a pigment-containing coated article that contain the bright pigment.
[0002] Photoluminescent pigments produce a pearlescent luster due to the light interference effect of an optical interference film. Photoluminescent pigments are added to products such as paints and cosmetics to give these products a vivid, particulate light reflection. A typical optical interference film is a titanium oxide film. Photoluminescent pigments that use a dye in combination with an optical interference film are also known. For example, Patent Document 1 discloses a cosmetic additive in which mica coated with a titanium oxide film (titanium oxide-coated mica) is further coated with a red organic dye.
[0003] Japanese Patent Application Laid-Open No. 2004-315426
[0004] The use of a pigment is useful as a method for adjusting the color tone of light reflected from a bright pigment. However, according to the inventors' investigations, a bright pigment in which pigment particles are attached to an optical interference film as a pigment may not always provide the desired reflected light. An object of the present invention is to provide a new bright pigment that contains pigment particles together with an optical interference film.
[0005] The present invention provides a bright pigment comprising: a flake-shaped substrate; an optical interference film on the flake-shaped substrate; and composite particles containing pigment particles and oxide particles adhered to the optical interference film.
[0006] According to the present invention, a new bright pigment is provided that contains pigment particles together with an optical interference film.
[0007] The present invention will be described in detail below, but the following description is not intended to limit the present invention to a specific embodiment. In this specification, the term "major component" refers to the component with the highest content by mass. The average particle size can be determined based on the observation results of 20 or more, preferably 50, objects using a scanning electron microscope (SEM) or the like. The average particle size is, for example, the arithmetic mean of the particle sizes of individual objects, determined by averaging the longest diameter and the diameter at the midpoint of the longest diameter in a direction perpendicular to the longest diameter.
[0008] (Flake-like substrate) The flaky substrate is a minute plate-like flake, also called a scale-like substrate. The flaky substrate is, for example, flaky glass, flaky alumina, mica, talc, or sericite. The flaky substrate is preferably flaky glass, flaky alumina, or mica. The mica may be natural mica or synthetic mica.
[0009] The average thickness of the flaky substrate is preferably 5 μm or less, particularly 2 μm or less, for example, 0.1 to 5 μm, and furthermore, 0.15 to 2 μm. The average thickness of the flaky substrate is determined by averaging the thicknesses of 20 or more, preferably 50, flaky substrates. The thickness of each flaky substrate can be measured by observation using a scanning electron microscope (SEM). The average particle size of the flaky substrate is preferably 3 to 600 μm, particularly 4 to 500 μm, for example, 5 to 200 μm.
[0010] A particularly preferred flake substrate is flake glass. The main surfaces of flake glass are smoother than crystalline particles such as mica, and are suitable for producing vivid interference light through the interference of incident light. The glass composition constituting the flake glass is not particularly limited, but for example, a glass composition containing silicon oxide as a main component and further containing other metal oxide components such as aluminum oxide, calcium oxide, and sodium oxide can be used. Specific examples of glass compositions include soda-lime glass, A-glass, C-glass, E-glass, ECR glass, borosilicate glass, and aluminosilicate glass.
[0011] (Optical interference film) The optical interference film may contain, for example, at least one selected from the group consisting of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zinc oxide, iron oxide, tin oxide, niobium oxide, cerium oxide, nickel oxide, chromium oxide, and vanadium oxide. The optical interference film may be composed of a single layer or multiple layers. Each layer constituting the optical interference film contains, for example, at least one of the oxides described above, and preferably contains one of the oxides described above as a main component. The optical interference film may contain titanium oxide, or may include a layer containing titanium oxide as a main component.
[0012] Optical interference films produce a variety of interference colors depending on the number and arrangement of layers and the materials that make up each layer. For example, a single-layer titanium oxide film produces interference colors such as yellow at a thickness of about 100 nm, red at a thickness of about 130 nm, blue at a thickness of about 160 nm, and green at a thickness of about 175 nm. However, depending on the film formation conditions and other factors, the color tone may vary slightly even if the titanium oxide film has the same thickness.
[0013] Titanium oxide has a high refractive index and is suitable for forming films with excellent color development. Titanium oxide has three crystalline forms: anatase, brookite, and rutile, of which anatase and rutile are industrially mass-produced. The preferred crystalline form of titanium oxide is rutile. Rutile titanium oxide has low photocatalytic activity, making it less likely to affect matrix materials such as paints to which photoluminescent pigments are added, and has the highest refractive index.
[0014] Formation of a rutile-type titanium oxide film on a flake-shaped substrate can be carried out with reference to the methods disclosed in, for example, Japanese Patent Application Laid-Open Nos. 2001-31421 and 2003-12962. In the methods disclosed in these publications, rutile-type titanium oxide is precipitated on glass flakes in a solution containing a titanium compound such as titanium tetrachloride, forming a coating. Rutile-type titanium oxide can be precipitated on glass flakes by adding an alkaline compound or alkaline solution to a solution containing a titanium compound at a temperature of 55 to 85°C and a pH of 1.3 or less. Precipitation of rutile-type titanium oxide is promoted by prior tin treatment, in which tin or a tin compound is attached to the glass flakes. This method allows for the formation of a rutile-type titanium oxide film without the need for heating for crystal transformation. However, the production method for titanium oxide films and other films is not limited to liquid-phase deposition methods; vapor-phase deposition methods, such as sputtering, may also be used.
[0015] An even more diverse range of interference light can be obtained from an optical interference film, which is a multilayer film. Here, only the layered structures of optical interference films, which are multilayer films, are exemplified below. - Flake-shaped substrate / silicon oxide / titanium oxide - Flake-shaped substrate / silicon oxide / iron oxide - Flake-shaped substrate / silicon oxide / titanium oxide / iron oxide - Flake-shaped substrate / silicon oxide / titanium oxide / aluminum oxide - Flake-shaped substrate / silicon oxide / titanium oxide / silicon oxide / titanium oxide - Flake-shaped substrate / titanium oxide / iron oxide - Flake-shaped substrate / titanium oxide / aluminum oxide - Flake-shaped substrate / titanium oxide / silicon oxide / titanium oxide - Flake-shaped substrate / tin oxide / titanium oxide - Flake-shaped substrate / aluminum oxide / titanium oxide - Flake-shaped substrate / iron oxide / titanium oxide
[0016] In the above laminated structure, " / " indicates the boundary between layers. Each layer may be a layer whose main component is the indicated oxide, or may be a layer composed of the indicated oxide. Note that the optical interference film is preferably formed so as to cover the entire surface of the flaky substrate, but for convenience, the above description shows only the multilayer film on one main surface of the flaky substrate.
[0017] (Composite particles) Composite particles contain pigment particles and oxide particles. Composite particles may contain one pigment particle and multiple oxide particles, or multiple pigment particles and multiple oxide particles. Composite particles may contain 5 or more, 10 or more, 30 or more, 50 or more, or in some cases 100 or more oxide particles. The number of pigment particles that can be contained in a composite particle may also be equal to or greater than the lower limit exemplified above. The upper limits of the number of pigment particles and the number of oxide particles that can be contained in a composite particle are not particularly limited, but are, for example, 10,000 or less, 5,000 or less, 3,000 or less, 1,000 or less, or even 500 or less, respectively.
[0018] (Pigment Particles) The pigment may contain an inorganic pigment and / or an organic pigment, or may contain an organic pigment. The pigment may be composed of a non-metallic material. Examples of inorganic pigments include yellow pigments such as yellow iron oxide, composite oxide yellow, and bismuth yellow; red pigments such as molybdenum red and red iron oxide (iron oxide red); green pigments such as chromium oxide green, chromium hydroxide green, and composite oxide green; blue pigments such as Prussian blue, ultramarine blue, and composite oxide blue (e.g., cobalt blue); and purple pigments such as manganese violet. Examples of organic pigments include azo pigments, isoindoline / isoindolinone pigments, metal complex pigments, phthalocyanine pigments, quinacridone pigments, dioxazine pigments, diketopyrrolopyrrole pigments, quinophthalone pigments, perylene pigments, thioindigo pigments, anthraquinone pigments, and triarylmethane pigments.
[0019] The azo pigment may be either a soluble azo pigment or an insoluble azo pigment. Soluble azo pigments are usually produced by insolubilizing (laking) the azo pigment with barium or other metal salts after a coupling reaction, and are therefore also called azo lake pigments. Examples of azo lake pigments include β-naphthol-based, β-oxynaphthoic acid-based, naphthol AS-based, arylide acetoacetate-based, and naphthalenesulfonic acid-based pigments. Many azo lake pigments exhibit a color tone ranging from yellow to red. Azo pigments, typified by azo lake pigments, have high coloring power and excellent clarity, and are suitable for enhancing the effects of the bright pigment of this embodiment.
[0020] There are no particular limitations on the size of the pigment particles, and they may have a size suitable for functioning as a pigment. The average particle size of the pigment particles is, for example, 50 nm or more and 1 μm or less. The lower limit of this average particle size may be 70 nm or more, 80 nm or more, 100 nm or more, or even 150 nm or more. The upper limit of this average particle size may be 800 nm or less, 700 nm or less, 600 nm or less, or even 500 nm or less.
[0021] (Oxide Particles) The oxide particles may contain at least one oxide selected from the group consisting of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zinc oxide, tin oxide, niobium oxide, cerium oxide, nickel oxide, chromium oxide, vanadium oxide, and iron oxide. The oxide particles may contain at least one oxide selected from the group consisting of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and zinc oxide. The oxide particles may contain silicon oxide or may contain silicon oxide as a main component. Silicon oxide has high light transmittance and is essentially colorless, making it particularly suitable for use in combination with pigments.
[0022] There are no particular limitations on the size of the oxide particles, but the average particle size is, for example, 5 nm or more and 500 nm or less. The lower limit of this average particle size may be 10 nm or more, 30 nm or more, or even 50 nm or more. The upper limit of this average particle size may be 500 nm or less, 200 nm or less, or even 150 nm or less. The average particle size of the oxide particles may be smaller than the average particle size of the pigment particles.
[0023] The oxide particles prevent multiple pigment particles from agglomerating in a state of direct contact on the optical interference film. The aggregation of pigment particles alone increases the apparent particle size of the pigment particles, which can lead to their detachment from the optical interference film. The detachment of pigment particles inhibits the development of the reflected color resulting from the combination of the optical interference film and the pigment particles. The oxide particles may also act to hold the pigment particles on the optical interference film by virtue of the hydroxyl groups present on their surfaces.
[0024] Surprisingly, it was also found that oxide particles themselves can improve the vividness of the color produced by the combination of an optical interference film and pigment particles. The oxide particles, interposed between pigment particles, may prevent a large area of the surface of the optical interference film from being covered solely by pigment particles, making the reflected light from the optical interference film more visible.
[0025] (Oxide particles / pigment particles) The ratio of the amount of oxide particles to the amount of pigment particles is not particularly limited, but may be, for example, 0.25 or more and 1.8 or less by mass. The lower limit of this ratio may be, for example, 0.3 or more, 0.4 or more, 0.5 or more, 0.7 or more, or even 0.8 or more, and in some cases 1.0 or more. The upper limit of this ratio may be, for example, 1.8 or less, 1.75 or less, or even 1.7 or less, and in some cases 1.6 or less. By appropriately adjusting the ratio of oxide particles to pigment particles, the shedding of pigment particles can be reliably suppressed, and the vividness of the color of the bright pigment may be further improved.
[0026] (Composite particles / shiny pigment) The ratio of the amount of composite particles to the amount of shiny pigment (total amount of pigment) is not particularly limited, but may be, for example, 0.05% or more and 70% or less by mass. The lower limit of this ratio may be, for example, 0.1% or more, 0.5% or more, or even 1% or more. The upper limit of this ratio may be, for example, 50% or less, 20% or less, or even 10% or less.
[0027] (Attachment of Composite Particles) It is desirable that the composite particles be attached so that at least a portion of the surface of the optical interference film is exposed, in other words, so as not to cover the optical interference film, as this is suitable for improving the vividness of the color development of the bright pigment.
[0028] (Additional Film) The bright pigment of this embodiment may further include a film that covers the composite particles. This embodiment is desirable in order to reliably prevent the composite particles from falling off. The additional film may contain the oxides exemplified as oxides that constitute the optical interference film. However, the additional film may affect the color development of the bright pigment. In the bright pigment, at least the composite particles, and in some cases, a portion of the surface of the optical interference film and the composite particles may be exposed.
[0029] (Hue) L * C * In the h color system, h represents the hue angle. * a * b * a in the color system * and b * and h = tan -1 (b * / a * ) relationship. In the bright pigment of this embodiment, the difference in h between the light reflected from the optical interference film and the light reflected from the pigment particles may be 100 degrees or less, 80 degrees or less, or even 60 degrees or less. The optical interference film and pigment used in the examples have a difference in h of 60 degrees or less. Specifically, the h of the light reflected from the optical interference film can be measured as the h of the flaky substrate with the optical interference film. h can be measured by the (color evaluation) described in the Examples section. When the difference in h is greater than 180 degrees, the difference is expressed by subtracting the difference from 360 degrees. Therefore, the difference between h1 = 340 degrees and h2 = 20 degrees is 40 degrees, not 320 degrees. In the bright pigment of this embodiment, c * is not particularly limited, but may be 30 or more, 40 or more, further 45 or more, and in some cases 50 or more. * is an index of the vividness of a color and is called saturation, and c * = ((a * ) 2 +(b * ) 2 ) 1 / 2 The following relationship is established.
[0030] (Pigment-containing composition and pigment-containing coated body) The bright pigment according to this embodiment can be used, for example, by blending it into various compositions. In another aspect, the present invention provides a pigment-containing composition containing the bright pigment according to the present invention. Examples of the pigment-containing composition include at least one selected from paints, inks, cosmetics, and resin compositions. Examples of the resin composition include artificial marble moldings.
[0031] In yet another aspect, the present invention provides a pigment-containing coated body comprising a coating film containing the luster pigment of the present invention and a substrate supporting the coating film. The pigment-containing coated body may be coated paper. In this case, the substrate is paper, but the substrate is not limited to paper and may be metal, resin, ceramic, or the like. The coating film may be composed of the pigment-containing composition of the present invention, or may be formed by applying the pigment-containing composition of the present invention to the substrate.
[0032] Specific examples of the pigment-containing composition itself and the pigment-containing coated body itself are well known, and therefore, description thereof will be omitted here, except for the following description regarding cosmetics.
[0033] Examples of the cosmetic include facial cosmetics, makeup cosmetics, and hair cosmetics. The glitter pigment of this embodiment is particularly suitable for use in makeup cosmetics such as eye shadow, nail enamel, eyeliner, mascara, lipstick, and fancy powder. The form of the cosmetic is not particularly limited, and examples include powder, cake, pencil, stick, ointment, liquid, emulsion, and cream.
[0034] The present invention will be described in more detail below with reference to examples.
[0035] (Color Evaluation) The bright pigment powders obtained from the above Examples and Comparative Examples and the base pigment powder (titanium oxide-coated flake glass) used were subjected to color measurement using a spectrophotometer "CM-5" (manufactured by Konica Minolta). The powders to be measured were filled into a small Petri dish (φ3 mm) and subjected to measurement. The light source used was D65, and color measurement was performed under the SCE (specularly reflected light excluded) method at a viewing angle of 2°.
[0036] (Dropping test) 0.1 g of the bright pigment powder and 20 mL of water were placed in a beaker and stirred at about 200 rpm for 24 hours using a stirrer and a stirrer. After stirring, the color of the supernatant was visually observed to confirm whether the pigment particles had shed from the bright pigment.
[0037] (Amount of Pigment Particles Adhered) The concentration of organic matter contained in the bright pigment was measured using a thermogravimetric differential thermal analyzer (TG-DTA). The amount of adhered pigment particles was determined by dividing this value by the concentration (50% by mass) of organic matter in the pigment constituting the pigment particles.
[0038] (Amount of Oxide Particles Adhered) The resulting bright pigment was dissolved by heating with sodium carbonate and boric acid, and then further dissolved by adding hydrochloric acid. This was thoroughly washed with hydrochloric acid and hot water and subjected to solid-liquid separation using filter paper. The amount of silica contained in the filtrate was determined by molybdenum blue absorptiometry. The amount of silica in the solid was determined by the weight difference before and after washing with hydrofluoric acid. Thermogravimetric analysis was performed on the solid obtained by solid-liquid separation and on a solid obtained by dissolving and washing silica with hydrofluoric acid, and the amount of silica was determined from the difference. The silica concentration in the bright pigment was determined by the sum of the silica amounts in the filtrate and the solid. Furthermore, the silica concentration of the titanium oxide-coated flake glass used as the substrate was determined using the same method, and the amount of silica (silicon oxide) constituting the attached oxide particles was determined from the difference between the silica in the bright pigment and the substrate.
[0039] <Preparation of Luster Pigment> (Example 1) Ethanol and a pigment were mixed to a pigment concentration of 3% by mass, and the mixture was dispersed in a bead mill using 0.3 mm zirconia balls to obtain a pigment dispersion. Red 202, a type of azo pigment, was used as the pigment. The average particle size of the obtained pigment was between 100 nm and 200 nm. Meanwhile, 51.3 g of tetramethyl orthosilicate (TMOS) was weighed into a flask, and 623.7 g of pure water was added while stirring, followed by further stirring for 1 hour to obtain a TMOS hydrolyzed solution with a silica concentration of 3% by mass. Next, the amount of pigment dispersion shown in Table 1 was added to this hydrolyzed solution to obtain a TMOS hydrolyzed solution in which the pigment was dispersed.
[0040] Separately from the above, 891 g of pure water and 0.1 g of 1 N TMAH (tetramethyl orthosilicate) were added to a flask, and 100 g of titanium oxide-coated flake glass ("Metashine (registered trademark) MT1080RR" manufactured by Nippon Sheet Glass Co., Ltd.; average particle size 80 μm, thickness 1.3 μm) was added and stirred to obtain a flake glass dispersion. While stirring the flake glass dispersion, the TMOS hydrolyzed liquid having the pigment dispersed therein was added dropwise at a rate of 3.3 mL / min so that the mass of silica (silicon oxide) added reached the value shown in Table 1. During the addition of the TMOS hydrolyzed liquid, 1 N TMAH was also added dropwise so that the pH was maintained in the range of 8 to 9. The resulting dispersion was then spray-dried to remove the solvent, and the resulting powder was dried at 150°C to obtain a bright pigment powder in which the pigment and silicon oxide particles were composited and attached to a titanium oxide film.
[0041] Examples 2 to 5 and Comparative Example 1 A bright pigment was obtained in the same manner as in Example 1, except that the amount of pigment dispersion added and the amount of the TMOS hydrolyzed liquid containing the pigment dispersed therein, calculated as silica, added were changed to the values shown in Table 1. However, in Comparative Example 1, TMOS was not used.
[0042]
[0043] The ratio of the amount of oxide to the amount of pigment, "amount of oxide / amount of pigment," calculated from each of the raw materials added, was 0 for Comparative Example 1, 0.42 for Example 1, 0.70 for Example 2, 1.17 for Example 3, 1.56 for Example 4, and 0.68 for Example 5.
[0044] Observation using an SEM revealed that composite particles containing pigment particles and oxide particles were attached to the surface of the optical interference film in each example, although a portion of the surface of the optical interference film was exposed.
[0045] <Preparation of Pigment-Containing Composition> (Eye Shadow) The extender pigment and spherical powder of Category A shown in Table 2 were placed in a disposable cup and mixed with a spatula. The mixture was then placed in a mixer and mixed for 1 minute. The color pigment and luster pigment were then added and mixed in the mixer for an additional 30 seconds. Subsequently, the raw materials of Category B were added to the mixer and mixed for an additional 1 minute. The resulting powder was removed, and an appropriate amount was placed in a mold and pressed to obtain an eye shadow.
[0046]
[0047] A vivid red color was observed from the obtained eye shadow. When applied to the back of the hand and observed, a clear red color without dullness was visible regardless of the angle. In particular, a brilliant red color was visible from the direction of specular reflection.
[0048] (Lip gloss) The ingredients of category A shown in Table 3 were weighed into a disposable cup and mixed while melting in a hot water bath at 80 to 90° C. The bright pigment of category B was then added and mixed, and the mixture was poured into a transparent container.
[0049]
[0050] The lip gloss of Formula 1 had a striking bright pink pearly appearance. Formula 2 had excellent transparency and brilliance, but some red pigment was observed to have fallen off and aggregated. When applied to the lips, Formula 1 imparted a glossy appearance as well as a healthy glow. Formula 2 imparted a glossy appearance but not a healthy glow.
[0051] (Examples of embodiments of the present invention) As described above, the present invention provides, in a first form, a bright pigment comprising: a flaky substrate; an optical interference film on the flaky substrate; and composite particles containing pigment particles and oxide particles adhered to the optical interference film.
[0052] In a second aspect, the present invention provides the bright pigment according to the first aspect, in which the pigment particles include an organic pigment.
[0053] The present invention provides, as a third aspect, the bright pigment of the first or second aspect, in which the oxide particles include at least one selected from the group consisting of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zinc oxide, iron oxide, tin oxide, niobium oxide, and cerium oxide.
[0054] The present invention provides, in a fourth aspect, the bright pigment of the third aspect, in which the oxide particles contain silicon oxide.
[0055] The present invention provides, in a fifth aspect, the bright pigment according to any one of the first to fourth aspects, wherein the optical interference film contains titanium oxide.
[0056] The present invention provides, as a sixth aspect, the bright pigment according to any one of the first to fifth aspects, wherein the flaky substrate is glass flake.
[0057] The present invention provides, as a seventh aspect, the bright pigment according to any one of the first to sixth aspects, in which the ratio of the amount of the oxide particles to the amount of the pigment particles is 0.25 or more on a mass basis.
[0058] The present invention provides, as an eighth aspect, the bright pigment according to any one of the first to seventh aspects, in which the ratio of the amount of the oxide particles to the amount of the pigment particles is 1.8 or less on a mass basis.
[0059] The present invention provides, in a ninth aspect, a pigment-containing composition comprising the bright pigment of any one of the first to eighth aspects.
[0060] In a tenth aspect, the present invention provides a pigment-containing coated body comprising a coating film containing the luster pigment of any one of the first to eighth aspects and a substrate supporting the coating film.
Claims
1. A bright pigment comprising: a flake-shaped substrate; an optical interference film on the flake-shaped substrate; and composite particles containing pigment particles and oxide particles and attached to the optical interference film.
2. The photoluminescent pigment according to claim 1, wherein the pigment particles include an organic pigment.
3. The bright pigment according to claim 1, wherein the oxide particles comprise at least one selected from the group consisting of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, zinc oxide, iron oxide, tin oxide, niobium oxide, and cerium oxide.
4. The bright pigment according to claim 3, wherein the oxide particles include silicon oxide.
5. The bright pigment according to claim 1, wherein the optical interference film contains titanium oxide.
6. The bright pigment according to claim 1, wherein the flake-shaped substrate is glass flake.
7. The bright pigment according to claim 1, wherein the ratio of the amount of said oxide particles to the amount of said pigment particles is 0.25 or more on a mass basis.
8. The bright pigment according to claim 1, wherein the ratio of the amount of said oxide particles to the amount of said pigment particles is 1.8 or less on a mass basis.
9. A pigment-containing composition comprising the bright pigment according to any one of claims 1 to 8.
10. A pigment-containing coated body comprising a coating film containing the luster pigment according to any one of claims 1 to 8 and a substrate supporting said coating film.
Citation Information
Patent Citations
Deposition of rutile-type titanium dioxide, and base material and glass flake each set therewith
JP2001031421A
Clear bright pigment, and coating material, resin composition, ink composition, molded artificial marble, coated paper, and cosmetics using the same
JP2003012962A
Additive for cosmetic
JP2004315426A
Flaky powder, its production, and cosmetic formulated therewith
JP1996239310A
Make-up cosmetic
JP1998087433A