Yellow fluorescent material, preparation method and application thereof, high-color-rendering inorganic yellow fluorescent pigment and preparation thereof
The combination of yellow fluorescent materials through Ce-Eu energy transmission with inorganic yellow pigments solves the problem of difficult industrialization and poor weather resistance of new yellow phosphors, and significantly improves the color development performance and application range of inorganic yellow pigments.
Patent Information
- Application Number
- CN202411075852.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The existing new yellow phosphor is difficult to achieve industrialization, and it has poor heat, light and weather resistance after mixing with organic pigments, which affects the application of inorganic yellow pigments.
The yellow fluorescent material of Sr2-x-y-zBaxSiO4:yCe3+, zEu2+ is used to enhance the yellow luminescence of the emission spectrum through Ce-Eu energy transfer, and a highly color-developed inorganic yellow fluorescent pigment is prepared in combination with traditional inorganic yellow pigments.
It significantly improves the color development performance of inorganic yellow pigments, enhances the luminous intensity of phosphors and the diffuse reflection effect of pigments, improves the brightness and yellowness value, and expands the application range.
Smart Images

Figure CN118995204A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a yellow fluorescent material and a preparation method and application thereof, and a high color rendering inorganic yellow fluorescent pigment and a preparation thereof. Background Art
[0002] In recent years, new yellow phosphors have been reported one after another. Among them, the most widely studied matrices include nitrogen oxides, silicates and aluminates, and they have attracted more and more attention. Among them, phosphors based on silicates have many attractive advantages, such as Sr2SiO4:Eu 2+ It can emit bright orange-yellow light, with an excitation spectrum covering the near-ultraviolet (380-410nm) and blue (450-480nm) ranges, and an emission band centered at 562nm, while exhibiting good thermal stability. Yellow silicate phosphor Sr2SiO4:Eu 2+ The luminescence properties are the key to improving the color rendering properties of inorganic yellow pigments.
[0003] Yellow pigment is a very eye-catching type of pigment, which is widely used in road signs, signboards, etc. Traditional inorganic yellow pigments include iron yellow, cadmium chrome yellow, titanium yellow, bismuth yellow, etc. Among them, color is one of the important indicators to measure the performance of inorganic pigments, so improving the color performance of inorganic yellow pigments is the goal of researchers. However, the new yellow pigments developed in recent years are difficult to achieve industrialization. Although mixing with organic pigments can help improve the color performance of yellow pigments, the disadvantages of organic pigments such as poor heat resistance, light resistance and weather resistance also indirectly affect the application of inorganic yellow pigments. Summary of the invention
[0004] The purpose of the present invention is to provide a yellow fluorescent material and a preparation method and application thereof, a high color rendering inorganic yellow fluorescent pigment and its preparation, wherein the yellow fluorescent material can significantly improve the color rendering performance of the inorganic yellow pigment.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a yellow fluorescent material, the chemical composition of which is Sr 2-x-y-z Ba x SiO4:yCe 3+ ,zEu 2+ , where 0.2≤x<1, 0.01 <y≤0.08,0<z<0.1。
[0007] Preferably, x=0.4, y=0.04 and z=0.01.
[0008] The present invention provides a method for preparing the yellow fluorescent material described in the above technical solution, comprising the following steps:
[0009] mixing a strontium compound, a barium compound, a silicon compound, a cerium compound and a europium compound with a grinding medium and grinding the mixture to obtain a mixed raw material;
[0010] The mixed raw material is pre-fired and then calcined under a protective atmosphere to obtain a yellow fluorescent material.
[0011] Preferably, the strontium compound includes SrCO3; the barium compound includes BaCO3; the silicon compound includes SiO2; the cerium compound includes Ce2(CO3)3 or CeO2; the europium compound includes Eu2O3;
[0012] The grinding time is 10 to 30 minutes; the pre-calcination temperature is 950 to 1050°C and the time is 0.5 to 1 hour;
[0013] The calcination temperature is 1250-1350°C and the calcination time is 4-5h;
[0014] In terms of volume percentage, the protective atmosphere is composed of 90-95% nitrogen and 5-10% hydrogen.
[0015] Preferably, the average particle size of the yellow fluorescent material is 5 to 15 μm.
[0016] The present invention provides the use of the yellow fluorescent material described in the above technical solution or the yellow fluorescent material prepared by the preparation method described in the above technical solution in improving the color rendering performance of inorganic yellow pigments.
[0017] The present invention provides an inorganic yellow fluorescent pigment with high color rendering property, comprising yellow fluorescent powder and an inorganic yellow pigment without yellow light emission;
[0018] The yellow fluorescent powder is the yellow fluorescent material described in the above technical solution or the yellow fluorescent material prepared by the preparation method described in the above technical solution; the inorganic yellow pigment without yellow light emission includes SrCrO4, BiVO4 or PbCrO4.
[0019] Preferably, the mass of the yellow fluorescent powder is 3-35% of the total mass of the yellow fluorescent powder and the inorganic yellow pigment.
[0020] The present invention provides a method for preparing the inorganic yellow fluorescent pigment with high color rendering property described in the above technical solution, comprising the following steps: mixing the inorganic yellow pigment with yellow fluorescent powder and water, and then drying and grinding the mixture in sequence to obtain the inorganic yellow fluorescent pigment with high color rendering property.
[0021] Preferably, the mixing is carried out under ultrasonic vibration, the frequency of the ultrasonic vibration is 28 - 40 KHz, and the time is 5 - 15 min; the drying temperature is 50 - 90 °C, and the time is 1 - 3 h; the fineness of the grinding is ≤15 μm.
[0022] The present invention provides a yellow fluorescent material with a chemical composition of Sr 2-x-y-z Ba x SiO4:yCe 3+ ,zEu 2+ , where 0.2 ≤ x < 1, 0.01 < y ≤ 0.08, 0 < z < 0.1. In the Ce and Eu co-doped yellow fluorescent material provided by the present invention, there is Ce-Eu energy transfer: Sr 2-x Ba x SiO4:Ce 3+ emits blue light under the excitation of near-ultraviolet light, while Sr 2-x Ba x SiO4:Eu 2+ emits yellow light under the excitation of near-ultraviolet light and blue light. There is a certain overlapping region between the emission of Ce 3+ and the excitation of Eu 2+ , which enables energy transfer between the two. In the present invention, Ce ions and Eu ions are simultaneously doped in the Sr 2-x Ba x SiO4 system, and Ce-Eu energy transfer will occur, so that the emission spectrum has a stronger emission intensity, the yellow light emission in the spectrum is significantly increased, and the luminescence intensity of the phosphor is enhanced. Therefore, the yellow fluorescent material of the present invention has a very wide excitation band, can be effectively excited by near-ultraviolet light and blue light, has strong absorption in the 300 - 450 nm band, emits yellow light with a main peak of about 550 nm, and has a relatively high emission intensity.
[0023] The yellow fluorescent material of the present invention is prepared by the traditional high-temperature solid-phase method, and the preparation process is simple and easy, with low cost and no pollution.
[0024] The yellow fluorescent material provided by the present invention can be combined with traditional inorganic pigments to exert its potential value: the above-mentioned yellow fluorescent material (which can strongly emit visible yellow light after stimulated radiation) is combined with an inorganic yellow pigment (both of which have the characteristics of high absorption of blue light and high reflection of yellow light) to prepare an inorganic yellow fluorescent pigment, and the addition of the yellow fluorescent material can enhance the reflection of yellow by the traditional inorganic pigment, and compared with the substantial increase in the reflection of yellow, the addition of the new yellow fluorescent material does not increase the reflection of blue (the complementary color of yellow) by the traditional inorganic pigment, and the prepared inorganic yellow fluorescent pigment has the superposition effect of fluorescent pigment absorption-reflection light and phosphor excitation-emission light in the long-wave region of visible light, thereby significantly enhancing the diffuse reflection effect of the inorganic fluorescent pigment on yellow under sunlight, and effectively improving the color rendering performance of the inorganic pigment.
[0025] The inorganic yellow fluorescent pigment product prepared by the present invention has significantly improved color rendering performance parameters such as brightness value L*, yellowness value b*, and yellow light region reflectivity compared with simple reflective pigments. The inorganic yellow fluorescent pigment in the present invention has a wide range of raw materials, which can expand the scope of application, and when the yellow fluorescent material of the present invention improves the performance of other yellow inorganic pigments, the doping ratio will vary due to the different performances of the pigment and the fluorescent powder itself. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is the XRD pattern of the yellow phosphor in Example 1;
[0027] Figure 2 The excitation and emission spectra of the yellow phosphor in Example 1;
[0028] Figure 3 is the XRD pattern of the yellow phosphor in Example 2;
[0029] Figure 4 The excitation and emission spectra of the yellow phosphor in Example 2;
[0030] Figure 5 is the XRD pattern of the yellow phosphor in Example 3;
[0031] Figure 6 The excitation and emission spectra of the yellow phosphor in Example 3;
[0032] Figure 7 Graphs showing emission spectra of the yellow phosphors in Examples 1 to 3;
[0033] Figure 8 The excitation and emission spectra of the yellow phosphor in Example 3 and Comparative Example 1;
[0034] Fig. 9 The excitation and emission spectra of the phosphors in Example 3 and Comparative Examples 1-2 are shown;
[0035] Fig.10 Excitation and emission spectra of the phosphors prepared in Examples 3-6 and Comparative Examples 3-4;
[0036] Fig.11 Reflection spectra of the yellow phosphor in Example 3 doped with yellow pigment at different ratios. Detailed implementation mode
[0037] The present invention provides a yellow fluorescent material with a chemical composition of Sr 2-x-y-z Ba x SiO4:yCe 3+ ,zEu 2+ , where 0.2 ≤ x < 1, 0.01 < y ≤ 0.08, 0 < z < 0.1.
[0038] In the present invention, preferably 0.2 ≤ x < 1, more preferably 0.3-0.8, and further preferably 0.4-0.6; preferably 0.01 < y ≤ 0.08, more preferably 0.02-0.06, and further preferably 0.04-0.06; preferably 0 < z < 0.1, more preferably 0.002-0.01, and further preferably 0.003-0.006.
[0039] In the present invention, x is the molar percentage of Ba relative to the substituting atom Sr, and y and z are the molar percentages of Ce 3+ and Eu 2+ relative to Sr, respectively.
[0040] As a preferred embodiment of the present invention, x = 0.4, y = 0.04 and z = 0.01, and the chemical composition of the corresponding yellow fluorescent material is Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ .
[0041] Introducing an appropriate amount of Ba into Sr2SiO4 2+ can obtain a stable α'-Sr2SiO4 phase structure, and changing the doping amount of Ba 2+ will shift the strongest emission wavelength within a certain wavelength range; the present invention studies and finds that (Sr,Ba)2SiO4:Ce 3+ emits blue light under near-ultraviolet excitation, while (Sr,Ba)2SiO4:Eu 2+ emits yellow light under near-ultraviolet and blue light excitation, and the emission of Ce 3+ and Eu 2+There is a certain overlapping area in the excitation of Ce-Eu, which makes it possible for energy transfer to occur between the two. The present invention utilizes the energy transfer of Ce-Eu to obtain a yellow phosphor with better performance.
[0042] The present invention provides a method for preparing the yellow fluorescent material described in the above technical solution, comprising the following steps:
[0043] mixing a strontium compound, a barium compound, a silicon compound, a cerium compound and a europium compound with a grinding medium and grinding the mixture to obtain a mixed raw material;
[0044] The mixed raw material is pre-fired and then calcined under a protective atmosphere to obtain a yellow fluorescent material.
[0045] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0046] In the present invention, the strontium compound preferably includes SrCO3; the barium compound preferably includes BaCO3; the silicon compound preferably includes SiO2; the cerium compound preferably includes Ce2(CO3)3 or CeO2; the europium compound preferably includes Eu2O3;
[0047] In the present invention, the grinding medium is preferably ethanol or acetone, and the grinding time is preferably 10 to 30 minutes, more preferably 20 minutes; the present invention has no special limitation on the amount of the grinding medium, and uniform mixing can be ensured according to actual needs; in an embodiment of the present invention, the volume ratio of the total mass of the strontium compound, the barium compound, the silicon compound, the cerium compound and the europium compound to the grinding medium is 1.5g:20mL.
[0048] In the present invention, the pre-calcination temperature is preferably 950-1050°C, more preferably 1000°C, and the time is preferably 0.5-1h, more preferably 1h; the present invention decomposes the carbonate in the raw material through pre-calcination, increases the shrinkage rate of the raw material, and makes the contact between the raw materials closer, so that the solid phase reaction is more sufficient.
[0049] In the present invention, the calcination temperature is preferably 1250-1350° C., more preferably 1300° C., and the calcination time is preferably 4-5 hours; in terms of volume percentage, the protective atmosphere is preferably composed of 90-95% nitrogen and 5-10% hydrogen.
[0050] After the calcination is completed, the present invention preferably cools the obtained product in air, grinds the obtained calcined product to obtain a yellow fluorescent material; the present invention has no special limitation on the grinding, as long as the desired particle size is achieved.
[0051] In the present invention, the average particle size of the yellow fluorescent material is preferably 5 to 15 μm, more preferably 10 μm.
[0052] The present invention provides the use of the yellow fluorescent material described in the above technical solution or the yellow fluorescent material prepared by the preparation method described in the above technical solution in improving the color rendering performance of inorganic yellow pigments.
[0053] The inorganic yellow pigment of the present invention is a pigment used in coatings and spray paints.
[0054] The present invention provides an inorganic yellow fluorescent pigment with high color rendering property, comprising yellow fluorescent powder and an inorganic yellow pigment without yellow light emission;
[0055] The yellow fluorescent powder is the yellow fluorescent material described in the above technical solution or the yellow fluorescent material prepared by the preparation method described in the above technical solution; the inorganic yellow pigment without yellow light emission includes SrCrO4, BiVO4 or PbCrO4.
[0056] In the present invention, the mass of the yellow phosphor is preferably 3-35% of the total mass of the yellow phosphor and the inorganic yellow pigment, and more preferably 15-25%.
[0057] In the present invention, the average particle size of the inorganic yellow pigment is preferably ≤1 μm.
[0058] The present invention provides a method for preparing the inorganic yellow fluorescent pigment with high color rendering property described in the above technical solution, comprising the following steps: mixing the inorganic yellow pigment with yellow fluorescent powder and water, and then drying and grinding the mixture in sequence to obtain the inorganic yellow fluorescent pigment with high color rendering property.
[0059] In the present invention, the mixing is preferably carried out under the condition of ultrasonic vibration, the frequency of the ultrasonic vibration is preferably 28-40KHz, more preferably 32-35KHz, the time is preferably 5-15min, more preferably 10min; the present invention has no special limitation on the amount of water, as long as the materials are mixed evenly; the drying temperature is preferably 50-90°C, more preferably 60°C, the time is preferably 1-3h, more preferably 2-3h; the grinding fineness is preferably ≤15μm, more preferably 1-5μm.
[0060] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0061] Example 1
[0062] This embodiment provides Sr 1.558 Ba 0.4 SiO4:0.04Ce 3+ ,0.002Eu 2+ The yellow phosphor powder, the preparation method thereof comprises the following steps:
[0063] (1) According to the chemical formula Sr 1.558 Ba 0.4 SiO4:0.04Ce 3+ ,0.002Eu 2+ 0.7830 g SrCO3 (99.0%), 0.2758 g BaCO3 (99.0%), 0.2099 g SiO2 (99.0%), 0.0012 g Eu2O3 (99.99%) and 0.0322 g Ce2(CO3)3 (99.9%) were weighed as raw materials;
[0064] (2) mixing all the above raw materials with ethanol at a mass to volume ratio of 1.5 g:20 mL and grinding for 20 min to obtain a mixed raw material;
[0065] (3) placing the mixed raw materials into an alumina crucible, and then placing it into a tube furnace, pre-calcining at 1000° C. for 1 h, and then heating to 1300° C. and calcining for 4 h in a reducing atmosphere (composed of 95% by volume nitrogen and 5% by volume hydrogen). After the calcination, the heating furnace body is removed and cooled in air to obtain a calcined product;
[0066] (4) The calcined product was ground to an average particle size of 10 μm to obtain a yellow phosphor.
[0067] Example 2
[0068] This embodiment provides Sr 1.554 Ba 0.4 SiO4:0.04Ce 3+ ,0.006Eu 2+ The yellow phosphor powder, the preparation method thereof comprises the following steps:
[0069] (1) According to the chemical formula Sr 1.554 Ba 0.4 SiO4:0.04Ce 3+ ,0.006Eu 2+ 0.7802 g SrCO3 (99.0%), 0.2756 g BaCO3 (99.0%), 0.2097 g SiO2 (99.0%), 0.0037 g Eu2O3 (99.99%) and 0.0321 g Ce2(CO3)3 (99.9%) were weighed as raw materials in a stoichiometric ratio;
[0070] (2) mixing all the above raw materials with acetone at a mass to volume ratio of 1.5 g:20 mL and grinding for 20 min to obtain a mixed raw material;
[0071] (3) placing the mixed raw materials into an alumina crucible, and then placing it into a tube furnace, pre-calcining at 1000° C. for 1 h, and then heating to 1300° C. and calcining for 4 h in a reducing atmosphere (composed of 95% by volume nitrogen and 5% by volume hydrogen). After the calcination, the heating furnace body is removed and cooled in air to obtain a calcined product;
[0072] (4) The calcined product was ground to an average particle size of 5 μm to obtain a yellow phosphor.
[0073] Example 3
[0074] This embodiment provides Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ The yellow phosphor powder, the preparation method thereof comprises the following steps:
[0075] (1) According to the chemical formula Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ 0.7775 g SrCO3 (99.0%), 0.2753 g BaCO3 (99.0%), 0.2096 g SiO2 (99.0%), 0.0061 g Eu2O3 (99.99%) and 0.0321 g Ce2(CO3)3 (99.9%) were weighed as raw materials in a stoichiometric ratio;
[0076] (2) mixing all the above raw materials with acetone at a mass to volume ratio of 1.5 g:20 mL and grinding for 20 min to obtain a mixed raw material;
[0077] (3) placing the mixed raw materials into an alumina crucible, and then placing it into a tube furnace, pre-calcining at 1000° C. for 1 h, and then heating to 1300° C. and calcining for 4 h in a reducing atmosphere (composed of 95% by volume nitrogen and 5% by volume hydrogen). After the calcination, the heating furnace body is removed and cooled in air to obtain a calcined product;
[0078] (4) The calcined product was ground to an average particle size of 15 μm to obtain a yellow phosphor.
[0079] Comparative Example 1
[0080] This comparative example provides Sr 1.59 Ba 0.4 SiO4:0.01Eu 2+ The yellow phosphor powder, the preparation method thereof comprises the following steps:
[0081] (1) According to the chemical formula Sr 1.59 Ba 0.4SiO4:0.01Eu 2+ 0.8155 g SrCO3 (99.0%), 0.2742 g BaCO3 (99.0%), 0.2087 g SiO2 (99.0%), and 0.0061 g Eu2O3 (99.99%) were weighed as raw materials in a stoichiometric ratio;
[0082] (2) mixing all the above raw materials with acetone at a mass to volume ratio of 1.5 g:20 mL and grinding for 20 min to obtain a mixed raw material;
[0083] (3) placing the mixed raw materials into an alumina crucible, and then placing it into a tube furnace, pre-calcining at 1000° C. for 1 h, and then heating to 1300° C. and calcining for 4 h in a reducing atmosphere (composed of 95% by volume nitrogen and 5% by volume hydrogen). After the calcination, the heating furnace body is removed and cooled in air to obtain a calcined product;
[0084] (4) The calcined product was ground to an average particle size of 15 μm to obtain a yellow phosphor.
[0085] Comparative Example 2
[0086] This comparative example provides Sr 1.56 Ba 0.4 SiO4:0.04Ce 3+ The preparation method of the blue phosphor comprises the following steps:
[0087] (1) According to the chemical formula Sr 1.56 Ba 0.4 SiO4:0.04Ce 3+ 0.7960 g SrCO3 (99.0%), 0.2728 g BaCO3 (99.0%), 0.2077 g SiO2 (99.0%), and 0.0318 g Ce2(CO3)3 (99.9%) were weighed as raw materials in a stoichiometric ratio;
[0088] (2) mixing all the above raw materials with acetone at a mass to volume ratio of 1.5 g:20 mL and grinding for 20 min to obtain a mixed raw material;
[0089] (3) placing the mixed raw materials into an alumina crucible, and then placing it into a tube furnace, pre-calcining at 1000° C. for 1 h, and then heating to 1300° C. and calcining for 4 h in a reducing atmosphere (composed of 95% by volume nitrogen and 5% by volume hydrogen). After the calcination, the heating furnace body is removed and cooled in air to obtain a calcined product;
[0090] (4) The calcined product was ground to an average particle size of 15 μm to obtain a blue phosphor.
[0091] Examples 4 to 6 and Comparative Examples 3 to 4
[0092] According to the ratios in Table 1 and the preparation conditions in Example 3, phosphors of different compositions were prepared.
[0093] Table 1 Raw material ratios of Examples 3 to 6 and Comparative Examples 3 to 4
[0094]
[0095]
[0096] Characterization and performance testing
[0097] Figure 1 is the XRD pattern of the yellow phosphor in Example 1; Figure 3 is the XRD pattern of the yellow phosphor in Example 2; Figure 5 is the XRD diagram of the yellow phosphor in Example 3; Figure 1 , Figure 3 and Figure 5 It can be seen that the diffraction peak positions of the yellow luminescent materials prepared in Examples 1 to 3 are consistent with the standard card and are good single-phase samples.
[0098] The yellow phosphors prepared in Example 1, Example 2 and Example 3 were tested for excitation and emission using a fluorescence spectrophotometer. The spectra were as follows: Figure 2 , Figure 4 and Figure 6 As shown. Figure 2 , Figure 4 and Figure 6 It can be seen that the excitation peak range of the prepared luminescent material is 300-400nm, and the strongest excitation peak is located at 350nm, which can effectively absorb excitation in the near-ultraviolet range. Figure 2 It can be seen that the yellow phosphor prepared in Example 1 has two emission peaks, namely Ce at around 410nm and 3+ The emission peak of Eu at around 540nm 2+ The emission peak, and the emission intensity Ce 3+ Greater than Eu 2+ That is, the characteristic emission peaks of Eu and Ce exist simultaneously in the yellow phosphor, proving that Eu and Ce are doped successfully; Figure 4 and Figure 6 It can be seen that the yellow phosphor Eu obtained in Example 2 2+ The emission intensity is greater than Ce 3+ The strongest emission wavelength range is 500-600nm, and the strongest emission peak is located in the yellow light region of 550nm.
[0099] In addition, from Figure 6 It can be seen that in Example 3, Sr 1.55 Ba0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ The emission spectrum includes the yellow band of visible light, and the excitation peak is located in the near-ultraviolet region, which can effectively prevent the phosphor and pigment from absorbing blue light at the same time. 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Therefore, the present invention uses Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Fluorescent pigments made from fluorescent powder can be excited by sunlight outdoors, emitting yellow light to enhance the color rendering of the pigment.
[0100] Comparing the emission spectra of the yellow phosphors prepared in Example 1, Example 2 and Example 3, the spectra are shown in FIG. Figure 7 As shown. Figure 7 It can be seen that the yellow phosphors prepared in Examples 2 and 3 are Ce higher than that prepared in Example 1. 3+ The emission peak decreases, while Eu 2+ The emission peak of α increases, which confirms that the system enhances the Eu through the Ce-Eu energy transfer process. 2+ of launch.
[0101] The yellow phosphors of Example 3 and Comparative Example 1 and the blue phosphors of Comparative Example 2 were tested for excitation and emission spectra. The results are as follows: Figures 8-9 As shown. Figures 8-9 It can be seen that the excitation spectrum of the yellow phosphor in Comparative Example 1 and the emission spectrum of the blue phosphor in Comparative Example 2 have obvious overlaps. Compared with the excitation and emission spectra of the yellow phosphor in Comparative Example 1, there is also obvious Ce in the excitation spectrum of Example 3. 3+ The characteristic excitation peak of Ce 3+ Doping was successful, Ce was doped in Example 3 3 + The emission intensity of the yellow phosphor obtained was significantly enhanced. This confirmed that the Ce-Eu energy transfer enhanced the Eu 2+ of launch.
[0102] Fig.10 The excitation and emission spectra of the phosphors prepared in Examples 3 to 6 and Comparative Examples 3 to 4 are shown in FIG. Fig.10 It can be seen that as the Ba ion doping amount changes from x = 0 to x = 1.0, the emission peak wavelength of the phosphor blue shifts from 570nm to about 520nm. When x = 0.4, the phosphor Sr 1.55 Ba0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ The yellow light emission and luminescence intensity can effectively adapt to its application in yellow pigments, showing the most excellent luminescence performance of this phosphor.
[0103] Application Examples
[0104] The Sr prepared in Example 3 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ The yellow phosphor is added to the inorganic yellow pigment SrCrO4, and the specific steps are as follows:
[0105] According to the mass ratio shown in Table 2, the Sr prepared in Example 3 was weighed 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Yellow phosphor and inorganic yellow pigment SrCrO4 are used to obtain inorganic yellow fluorescent pigments with different mass ratios. The specific data are shown in Table 2.
[0106] Table 2 Theoretical mass ratio of inorganic yellow fluorescent pigment (Note: the ratio is based on a total amount of 1g)
[0107] <![CDATA[Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ (the amount of addition is set to m)]]> <![CDATA[SrCrO4]]> 0% 100% 15% 85% 20% 80% 25% 75% 30 70%
[0108] The preparation method of the above-mentioned inorganic yellow fluorescent pigment is:
[0109] Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Yellow fluorescent powder and SrCrO4 pigment (average particle size ≤ 1 μm) were mixed, dissolved in 5 mL of distilled water, and uniformly mixed by 32 kHz ultrasonic vibration for 10 min, then dried at 60° C. for 3 h, and then ground in a mortar to obtain an inorganic yellow fluorescent pigment with a fineness of 1 to 5 μm.
[0110] Test Case
[0111] The inorganic yellow fluorescent pigment samples with different mass ratios in the corresponding use case were tested using a desktop colorimeter. The measured samples were pressed into powder cakes in a cuvette. Ultraviolet and visible light were used as the light source and the reflection mode was used to directly measure the samples. The parameter values of the undoped phosphor and the mixed powder were compared using the comparative measurement mode to determine the value of the Sr doped 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu2+ The effect of powder on SrCrO4 yellow inorganic pigment, the results are shown in Table 3.
[0112] Table 3 Different amounts of Sr added 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Chromaticity data of powdered inorganic yellow fluorescent pigment
[0113] <![CDATA[Sr 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ :SrCrO4]]> L* b* 0%:100% 87.20 29.97 15%:75% 88.38 30.15 20%:80% 91.20 31.82 25%:75% 89.79 31.26 30%:70% 89.52 30.55
[0114] It can be seen from Table 3 that compared with the SrCrO4 pigment without phosphor, when Sr 1.55 Ba 0.4 SiO4:0.04Ce 3 + ,0.01Eu 2+ When the mixing ratio of powder and SrCrO4 pigment is 20%:80%, the brightness value L* increases by 4.0%, which has the greatest impact on the color performance parameters of the pigment. 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ The addition of the powder greatly improves the brightness of the SrCrO4 pigment, making it look brighter; the yellowness value b* increases by 1.85%, indicating that the color of the inorganic pigment becomes more yellow under simulated sunlight after the addition of the phosphor. Based on the changes in the above data, it is concluded that: SrCrO4 pigment has a yellowish color when exposed to sunlight. 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ After the powder is added, its coloring ability is significantly improved, and the effect is most significant when the addition ratio is 20%.
[0115] Fig.11 is Sr in Example 3 1.55 Ba 0.4 SiO4:0.04Ce 3+ ,0.01Eu 2+ Reflection spectra of phosphors doped with SrCrO4 pigments at different ratios. Fig.11 It can be seen that the addition of phosphor significantly improves the reflectivity of the pigment in the yellow light band, and compared with pure SrCrO4 pigment, the reflectivity of the pigment after adding 20% phosphor is increased by 6.8%, which effectively shows that the addition of phosphor can effectively improve the color rendering performance of the pigment.
[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A yellow fluorescent material, characterized in that: The chemical composition is Sr 2-x-y-z Ba x SiO4:yCe 3+ ,zEu 2+ , where 0.2≤x<1, 0.01 <y≤0.08,0<z<0.1。 2. The yellow fluorescent material according to claim 1, characterized in that: x=0.4, y=0.04 and z=0.
01.
3. The method for preparing the yellow fluorescent material according to claim 1 or 2, characterized in that: The following steps are involved: mixing a strontium compound, a barium compound, a silicon compound, a cerium compound and a europium compound with a grinding medium and grinding the mixture to obtain a mixed raw material; The mixed raw material is pre-fired and then calcined under a protective atmosphere to obtain a yellow fluorescent material.
4. The preparation method according to claim 3, characterized in that: The strontium compound includes SrCO3; the barium compound includes BaCO3; the silicon compound includes SiO2; the cerium compound includes Ce2(CO3)3 or CeO2; the europium compound includes Eu2O3; The grinding time is 10 to 30 minutes; the pre-calcination temperature is 950 to 1050°C and the time is 0.5 to 1 hour; The calcination temperature is 1250-1350°C and the calcination time is 4-5h; In terms of volume percentage, the protective atmosphere is composed of 90-95% nitrogen and 5-10% hydrogen.
5. The preparation method according to claim 3 or 4, characterized in that: The average particle size of the yellow fluorescent material is 5 to 15 μm.
6. Use of the yellow fluorescent material according to claims 1 to 2 or the yellow fluorescent material prepared by the preparation method according to any one of claims 3 to 5 in improving the color rendering performance of inorganic yellow pigments.
7. A high color rendering inorganic yellow fluorescent pigment, characterized in that: Including yellow phosphors and inorganic yellow pigments without yellow light emission; The yellow fluorescent powder is the yellow fluorescent material described in claims 1 to 2 or the yellow fluorescent material prepared by the preparation method described in any one of claims 3 to 5; the inorganic yellow pigment without yellow light emission includes SrCrO4, BiVO4 or PbCrO4.
8. The high color rendering inorganic yellow fluorescent pigment according to claim 7, characterized in that: The mass of the yellow fluorescent powder is 3-35% of the total mass of the yellow fluorescent powder and the inorganic yellow pigment.
9. The method for preparing the high color rendering inorganic yellow fluorescent pigment according to claim 7 or 8, characterized in that: The following steps are involved: The inorganic yellow pigment is mixed with yellow fluorescent powder and water, and then dried and ground in sequence to obtain an inorganic yellow fluorescent pigment with high color rendering property.
10. The preparation method according to claim 9, characterized in that: The mixing is carried out under the condition of ultrasonic vibration, the frequency of the ultrasonic vibration is 28-40KHz, and the time is 5-15min; the drying temperature is 50-90°C, and the time is 1-3h; the grinding fineness is ≤15μm.
Citation Information
Patent Citations
High-color-rendering inorganic yellow pigment, preparation method thereof and application of fluorescent powder in improving color rendering performance of inorganic yellow pigment
CN116640463A
Phosphor for Producing White Light Under Excitation of UV Light and Method for making the same
US20090001318A1
Cited By
Yellow overglaze color fluorescent pigment as well as preparation method and application thereof
CN120059495A
Ion absorption type silicate coloring pigment
CN121471914A