Concrete service life calculation method considering protection and repair effects in plateau environment

By simulating the multi-factor coupling physics in the plateau environment, the concrete geometric model is constructed and the steel bar corrosion is calculated, the inaccurate calculation of concrete life in the plateau environment is solved, effective protection and repair measures are provided, and the concrete service is extended life.

WO2024239355A1PCT designated stage expired Publication Date: 2024-11-28SOUTHEAST UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097012
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2023-05-30
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing research methods cannot accurately calculate the life of concrete in plateau environments, especially the protection and restoration effects cannot be considered, resulting in inaccurate calculation of concrete life in complex plateau environments.

Method used

By simulating the temperature, humidity, salt concentration and load conditions in the plateau environment, establishing the multi-factor coupling physical field equation, constructing a concrete geometric model, determining material properties, solving the temperature, humidity, salt concentration and stress distribution, and calculating the corrosion situation of steel bars. Determine the service life of concrete.

Benefits of technology

This method can simulate the effects of protection and restoration materials in different environments, provide a basis for concrete structure design and construction in plateau environments, and extend the service life of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097012_28112024_PF_FP_ABST
    Figure CN2023097012_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A concrete service life calculation method considering protection and repair effects in a plateau environment, comprising: establishing a mapping relationship among the plateau environment, a load parameter and time; constructing a concrete geometric model, and determining material attributes of each phase in the geometric model; establishing a multi-factor coupling action physical field equation, and setting boundary conditions and an initial condition on the basis of the concrete geometric model; solving for the internal temperature, humidity, salt concentration, and stress distribution of concrete, and the change conditions of the internal temperature, humidity, salt concentration, and stress distribution of the concrete along with time; and calculating the time when reinforcing steel bars in the concrete reach a critical corrosion concentration to generate a depassivation state, and determining the service life of the concrete. The present invention simulates the internal temperature, humidity, stress response and service life of the concrete after a single surface protection coating, a crack repairing material, and a reinforcing steel bar corrosion repairing material are used or several types of protection and repairing materials are simultaneously used in different plateau environments, thereby providing a basis for design and construction of a concrete structure in a plateau environment.
Need to check novelty before this filing date? Find Prior Art

Description

A method for calculating concrete lifespan in plateau environments considering protection and repair effects Technical Field

[0001] The present invention belongs to the field of concrete service life calculation, and in particular relates to a concrete service life calculation method taking protection and repair effects into consideration in a plateau environment. Background Art

[0002] Major national transportation projects such as the Sichuan-Tibet Railway and the Qinghai-Tibet Expressway are being advanced in plateau regions. These projects are characterized by extreme environmental conditions, including a maximum diurnal temperature swing of 28°C, relative humidity of 30%-50%, freezing temperatures as low as -32°C, frequent freeze-thaw cycles of positive and negative temperatures exceeding 180 days, and hypersaline soils with salt concentrations several times higher than the upper limit. The combination of large temperature swings, extreme dryness, unsaturated freeze-thaw cycles, and saline soils leads to rapid deterioration of concrete properties, making construction and maintenance difficult. This poses a significant challenge to the safe service life and durability of major transportation projects, primarily bridges and tunnels. Surface protection, matrix damage repair, and rebar corrosion repair are crucial measures to ensure the durability of reinforced concrete in plateau environments characterized by frequent freeze-thaw cycles, large temperature swings, and hypersaline soils.

[0003] Currently, researchers at home and abroad have conducted numerous experiments on concrete corrosion degradation under freeze-thaw, salt erosion, and alternating wet-dry conditions, collecting concentration distributions of ions such as chloride and sulfate to predict concrete service life. However, the plateau environment is complex, with a wide variety of protective and repair materials and varying performance. Existing research methods are inaccurate for calculating concrete life in a single plateau environment and are not applicable to the multi-factor coupled plateau environment, let alone calculating concrete service life that takes into account protective and repair effects.

[0004] Summary of the Invention

[0005] The purpose of the present invention is to provide a method for calculating the service life of concrete in a plateau environment taking into account the protection and repair effects, so as to solve the problem that the existing method cannot calculate the service life of concrete in a plateau environment taking into account the protection and repair effects.

[0006] To achieve the above object, the present invention provides a method for calculating the life of concrete in a plateau environment taking into account protection and repair effects, comprising the following steps:

[0007] S1. Determine the temperature, humidity, salt concentration, and internal and external load conditions of the simulated plateau environment, and establish a mapping relationship between the plateau environment, load parameters, and time;

[0008] S2. Construct a geometric model of concrete that takes into account protection and repair in a plateau environment, and determine the material properties of each phase in the geometric model;

[0009] S3. Establishing the physical field equations for the temperature-humidity-salt concentration-load multi-factor coupling effect, setting internal and external boundary conditions and initial conditions based on the concrete geometric model, wherein the external boundary conditions are the mapping relationship between the plateau environment, load parameters, and time;

[0010] S4. Determine the internal temperature, humidity, salt concentration, stress distribution of concrete and their temporal changes under high altitude environment and load, taking into account protection and repair functions;

[0011] S5. Calculate the time it takes for the steel bars inside the concrete to reach the critical corrosion concentration and become depassivated, taking into account the protection and repair functions, and determine the service life of the concrete.

[0012] Optionally, in S1, the mapping relationship between the plateau environment, load parameters and time is fixed or arbitrarily changing temperature, humidity, salt concentration and internal and external force loads; salt is the corrosive medium, including: sodium chloride, calcium chloride, cesium chloride, sodium sulfate, magnesium sulfate; internal and external force loads include: gravity, internal pore expansion force, external load.

[0013] Optionally, in S2, the construction process of the concrete geometric model is: randomly generating the concrete microstructure using the Monte Carlo method, adding a protective coating geometric model of arbitrary thickness to the concrete surface, wherein the protective coating geometric model is a line segment connected to the concrete in a one-dimensional structure, a tetrahedron fitted with the concrete in a two-dimensional model, and a hexahedron fitted with the concrete in a three-dimensional structure model, and the damage repair material is a lattice or spatial domain uniformly distributed inside the cement paste;

[0014] Optionally, in S2, the concrete geometric model includes coarse aggregate, fine aggregate and cement paste, the coarse and fine aggregate grading type can be freely set, the aggregate volume fraction is between 0% and 80%, the concrete surface protective coating is a continuous coating adhered to the concrete surface, and the concrete repair material is evenly distributed in the cement paste in the form of a field, and automatically triggers the repair effect after damage occurs, reducing the transmission rate of the erosion medium and restoring the mechanical properties of the concrete.

[0015] Optionally, in S2, the material phase includes: aggregate, slurry, and coating;

[0016] The material properties of the slurry include: elastic modulus, Poisson's ratio, density, tensile strength, fracture energy, phase transition temperature, phase transition temperature interval, phase transition latent heat, thermal conductivity, constant pressure heat capacity, ion diffusion coefficient, porosity, and pore size distribution;

[0017] The material properties of the coating include: thermal conductivity, constant pressure heat capacity, and ion diffusion coefficient;

[0018] The relevant experimental parameters of the aggregate and the coating are obtained through experimental testing; the slurry is composed of sand and cement slurry, and the parameters of the slurry are calculated by micromechanics equivalent medium theory.

[0019] Optionally, in S3, the multi-factor coupling physical field equations include: a temperature conduction equation, a moisture transfer equation, a salt transfer equation, and a force action equation;

[0020] Optionally, the temperature conduction equation is:

[0021] Where ρ is density, C is specific heat capacity, T is temperature, t is time, λ is thermal conductivity, L is latent heat of phase change, θ L is the moisture content; the internal initial temperature is set to be consistent with the initial temperature of the plateau environment, and the boundary condition uses the Dirichlet boundary condition, which is consistent with the plateau environment temperature parameter determined in S1;

[0022] The water transport equation takes into account the transport effects of gaseous water and liquid water and is expressed as follows:

[0023] Among them, P c is the moisture characteristic curve, K sl is the permeability coefficient of water in the material under saturated state, is the porosity, η is the viscosity of water, K rl is the relative permeability coefficient of the liquid phase, M w is the molar mass of water, R is the relative gas constant, ρ l is the density of water, D g0 is the free diffusion coefficient of water vapor in air; P gs is the saturated vapor pressure;

[0024] The internal initial moisture content is set according to the actual concrete, ranging from 0 to 100 RH%, and the boundary condition uses the Dirichlet boundary condition, which is consistent with the plateau environment moisture parameters determined in S1;

[0025] When salt ion transport only considers convection and diffusion and does not consider chemical reactions, the salt transport equation is as follows:

[0026] Where c is the salt ion concentration, D0 is the reference ion diffusion coefficient in the slurry, t0 is the time of reference ion diffusion coefficient measurement, m is the time dependence coefficient, θ c is the critical saturation of pores, U is the ion activation energy in concrete, T ref is the temperature when the reference ion diffusion coefficient is measured, d is the damage factor, which is obtained by the damage mechanics energy method, and f ris the repair rate of the repair material to the damage, D f is the diffusion coefficient of ions in water, R b is the factor affecting the binding of concrete to ions; the internal initial ion concentration is set to 0, and the boundary condition uses the Dirichlet boundary condition, which is consistent with the plateau environment ion parameters determined in S1;

[0027] The force equation is as follows:

[0028] Where σ is stress, b is Biot coefficient, p * The equivalent load of environmental action includes the equivalent load of internal expansion caused by freeze-thaw and sulfate factors;

[0029] Among them, p FT * is the internal expansion load caused by freeze-thaw, r max and r min are the maximum and minimum pore diameters in the matrix, K and K L , K C are the matrix moduli of slurry, water and ice respectively, ∈ is the strain of slurry, b L 、b C are the Biot coefficients of water and ice, α s is the thermal expansion coefficient of the slurry, p atm is the plateau ambient pressure, p atm0 is the ambient pressure during slurry pouring, S C 、S L 、S G are the volume fractions of ice, water and pores at the corresponding temperatures, respectively, and p s * is the equivalent load of internal expansion caused by sulfate attack, v AFt is the volume fraction of expanded ettringite, ω i is the corresponding environmental impact factor, p i * Represent the equivalent loads of freeze-thaw, sulfate, and magnesium salt environments, respectively.

[0030] Optionally, S5 is specifically as follows: taking the life of the concrete when the steel bar begins to corrode as the final service life, solving the ion concentration at different depths through steps S1-S4, and comparing the critical concentration to determine the service life of the concrete. The steel bar corrosion repair material will increase the critical ion concentration of the steel bar, so the concrete service life is calculated as follows:

[0031] Among them, t cis the service life of concrete, x d is the embedded depth of steel bars, f rr is the action factor of steel corrosion repair material, and ccr is the inherent critical concentration of steel corrosion.

[0032] The technical effects of the present invention are:

[0033] The present invention can simulate the internal temperature, humidity, stress response and service life of concrete after using a single surface protective coating, crack repair material and steel bar rust-proof material, or using several types of protective and repair materials simultaneously in different plateau environments, thereby providing a basis for the design and construction of concrete structures in plateau environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings, which constitute part of this application, are intended to provide a further understanding of this application. The exemplary embodiments and descriptions of this application are intended to explain this application and do not constitute an improper limitation on this application. In the accompanying drawings:

[0035] FIG1 is a schematic diagram of a geometric model for considering protection and repair materials in a two-dimensional form in an embodiment of the present invention;

[0036] FIG2 is a schematic diagram showing the distribution of the concentration of the corrosive medium at 0-5 mm on the concrete surface after using different types of protective coatings in an embodiment of the present invention;

[0037] FIG3 is a schematic diagram showing the distribution of corrosive medium concentration at the embedded depth of steel bars after using different types of protective coatings in an embodiment of the present invention;

[0038] FIG4 is a schematic diagram showing the distribution of the concentration of the corrosive medium inside the concrete after applying protective coatings of different thicknesses according to an embodiment of the present invention;

[0039] FIG5 is a schematic diagram showing the distribution of corrosive medium concentration inside concrete after using protective coatings of different lifespans in an embodiment of the present invention;

[0040] FIG6 is a schematic diagram showing the distribution of the concentration of the corrosive medium inside the concrete after using the crack repair material with a repair rate of 50% in an embodiment of the present invention;

[0041] FIG7 is a schematic diagram showing the distribution of the concentration of the corrosive medium inside the concrete after using the crack repair material with a repair rate of 70% in an embodiment of the present invention;

[0042] FIG8 is a schematic diagram showing the distribution of the concentration of the corrosive medium inside the concrete after using the crack repair material with a repair rate of 90% in an embodiment of the present invention;

[0043] FIG9 is a schematic diagram showing a comparison between the concentration of a concrete corrosive medium and a critical concentration at the depth of the steel bars after applying a protective coating according to an embodiment of the present invention;

[0044] FIG10 is a schematic diagram showing a comparison of the concentration of the concrete corrosive medium and the critical concentration at the depth of the steel bar after the damage repair material and the steel bar corrosion repair in an embodiment of the present invention. DETAILED DESCRIPTION

[0045] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments in this application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0046] The purpose of the present invention is to provide a method for calculating the service life of concrete in a plateau environment taking into account the protection and repair effects, so as to solve the problem that the existing method cannot calculate the service life of concrete in a plateau environment taking into account the protection and repair effects.

[0047] A method for calculating the life of concrete in a plateau environment taking into account protection and repair effects includes the following steps:

[0048] (1) Determine the temperature, humidity, salt concentration, and internal and external load conditions of the simulated plateau environment, and establish a mapping relationship between the above environmental and load parameters and time;

[0049] (2) Construct a concrete mesostructure geometric model that takes into account protection and repair functions, and determine the material properties of each phase in the geometric model;

[0050] (3) Establishing the physical field equations of temperature-humidity-salt concentration-load multi-factor coupling, setting internal and external boundary conditions and initial conditions based on the concrete geometric model established in step (2), wherein the external boundary conditions are the mapping relationship between the plateau environment and load parameters and time determined in step (1);

[0051] (4) Determine the internal temperature, humidity, salt concentration, stress distribution of concrete and their changes over time under plateau environment and load, taking into account protection and repair functions;

[0052] (5) Calculate the time it takes for the steel bars inside the concrete to reach the critical corrosion concentration and become depassivated, taking into account the protection and repair functions, and determine the service life of the concrete.

[0053] The mapping relationship between the environment and load parameters and time in step (1) can be fixed or arbitrarily changing temperature, humidity and external load effects.

[0054] In step (2), the concrete geometric model considering both protection and repair functions is randomly generated using the Monte Carlo method. A protective coating geometric model of arbitrary thickness is added to the concrete surface. The protective coating geometric model is a line segment connected to the concrete in a one-dimensional structure, a tetrahedron conforming to the concrete in a two-dimensional model, and a hexahedron conforming to the concrete in a three-dimensional structure model. The damage repair material is a lattice or spatial domain uniformly distributed within the cement paste.

[0055] The concrete geometric model considering the protection and repair effects in step (2) contains physical phases such as aggregate, slurry, and coating. The slurry needs to provide parameters including elastic modulus, Poisson's ratio, density, tensile strength, fracture energy, phase change temperature, phase change temperature interval, phase change latent heat, thermal conductivity, constant pressure heat capacity, ion diffusion coefficient, porosity, pore size distribution, etc. The coating needs to provide thermal conductivity, constant pressure heat capacity, and ion diffusion coefficient.

[0056] The relevant experimental parameters of the aggregate and coating were obtained through experimental testing. Since the slurry is composed of sand and cement slurry, it is a composite material. The slurry parameters were calculated using the micromechanical equivalent medium theory.

[0057] When considering the protection and repair effects in step (3), the multi-factor coupling physical field equations in concrete include the temperature conduction equation, the moisture transfer equation, the salt transfer equation, and the force action equation. The temperature conduction equation is as follows:

[0058] Where ρ is density, C is specific heat capacity, T is temperature, t is time, λ is thermal conductivity, L is latent heat of phase change, θ L is the moisture content.

[0059] The internal initial temperature is set to be consistent with the initial temperature of the plateau environment, and the boundary conditions are Dirichlet boundary conditions, which are consistent with the plateau environment temperature parameters determined in step (1).

[0060] The water transport equation takes into account the transport effects of gaseous water and liquid water, as shown below:

[0061] The specific P c is the moisture characteristic curve, K sl is the permeability coefficient of water in the material under saturated conditions. is the porosity, η is the viscosity of water, K rl is the relative permeability coefficient of the liquid phase, M w is the molar mass of water, R is the relative gas constant, ρ l is the density of water, D g0 is the free diffusion coefficient of water vapor in air; Pgs is the saturated vapor pressure.

[0062] The internal initial moisture content is set according to the actual concrete, ranging from 0 to 100 RH%. The boundary conditions are Dirichlet boundary conditions, which are consistent with the plateau environment moisture parameters determined in step (1).

[0063] The salt ion transport only considers convection and diffusion, and does not consider chemical reactions. The governing equation is as follows:

[0064] Where c is the salt ion concentration, D0 is the reference ion diffusion coefficient in the slurry, t0 is the time for measuring the reference ion diffusion coefficient, m is the time dependence coefficient, θ c is the critical saturation of pores, U is the ion activation energy in concrete, T ref is the temperature when the reference ion diffusion coefficient is measured, d is the damage factor, which is obtained by the damage mechanics energy method, and f r is the repair rate of the repair material to the damage, D f is the diffusion coefficient of ions in water, R b is the factor affecting the binding of concrete to ions.

[0065] The internal initial ion concentration is set to 0, and the boundary condition is the Dirichlet boundary condition, which is consistent with the plateau environment ion parameters determined in step (1).

[0066] The force equation is as follows:

[0067] Where σ is stress, b is Biot coefficient, and p is * It is the equivalent load of environmental action. In plateau environment, it mainly includes the equivalent load of internal expansion caused by factors such as freeze-thaw and sulfate.

[0068] The equivalent internal expansion load caused by freeze-thaw in plateau environments is solved according to the following steps: ① first determine the content of gas, liquid, and ice crystals in the pores of the slurry at a specific temperature; ② calculate the internal expansion load based on the content of gas, liquid, and ice crystals.

[0069] ① Step calculation is carried out as follows:

[0070] The specific r c is the critical freezing aperture at the corresponding temperature, γ CL is the water-ice interfacial energy, Σ mis the water ice phase transition entropy, ΔT is the temperature difference between the actual temperature under the plateau environment and the freezing point of the solution under the corresponding plateau pressure environment, which is affected by the plateau pressure, pores, etc., δ is the thickness of the water film at the pore wall, which is obtained by molecular dynamics simulation of the water distribution in the pores of unsaturated CSH gel, and S l0 (r), S C (r), S L (r) are the initial liquid water saturation function, ice crystal saturation function and liquid water saturation function at the corresponding pore size, respectively. S G is the gas saturation in the pores of the slurry, r sc The critical saturated pores are also obtained from molecular dynamics simulations. The aperture is smaller than r sc porosity.

[0071] ②The calculation is carried out as follows:

[0072] The specific p FT * is the internal expansion load caused by freeze-thaw, r max and r min are the maximum and minimum pore diameters in the matrix, K and K L , K C are the matrix moduli of slurry, water and ice respectively, ∈ is the strain of slurry, b L 、b C are the Biot coefficients of water and ice, α s is the thermal expansion coefficient of the slurry, p atm is the plateau ambient pressure, p atm0 is the ambient pressure when pouring slurry, M is the calculation coefficient, S C 、S L 、S G are the volume fractions of ice, water and pores at the corresponding temperatures, respectively.

[0073] Among them, the internal expansion force generated by the expansion medium generated in the pores of the slurry due to the invasion and chemical reaction of corrosive ions such as sulfate in the plateau environment is solved according to the following steps: ① Considering the effect of chemical reaction, solve the concentration distribution of different ions in the slurry; ② Calculate the volume expansion force of the chemical reaction based on the ion concentration distribution.

[0074] ① The calculation of sulfate attack step is carried out as follows:

[0075] The specific c CA 、cgpy 、 are the concentrations of sulfate ion, calcium ion, calcium hydroxide, gypsum and calcium ion respectively, k, k1 and k2 are the chemical reaction coefficients, is the diffusion coefficient of sulfate ions and calcium ions, q is the concrete corrosion coefficient, is the calcium ion activity.

[0076] ②The calculation is carried out as follows:

[0077] The specific p s * is the equivalent load of internal expansion caused by sulfate attack, v AFt is the volume fraction of expanded ettringite, which is determined by the concentration calculated in step ① combined with the chemical reaction equation.

[0078] The internal expansion force of other corrosive products such as magnesium salts in the slurry can be calculated according to their chemical reaction equations in combination with step ①.

[0079] When freeze-thaw and sulfate corrosion media are present in the plateau environment, the final internal expansion load on the slurry is calculated as follows:

[0080] The specific ω i is the corresponding environmental impact factor, p i * They represent the environmental equivalent loads such as freeze-thaw, sulfate, and magnesium salt respectively.

[0081] The step (4) solves the numerical model of concrete considering the protection and repair functions of the plateau environment, which can be solved by using the finite element method.

[0082] In step (5), the life span of the concrete is calculated as the life span when the steel bar begins to corrode. The ion concentration at different depths is solved through steps (1-4) and the critical concentration is compared to determine the service life of the concrete. The steel bar corrosion repair material will increase the critical ion concentration of the steel bar, so the service life of the concrete is calculated as follows:

[0083] The specific t c is the service life of concrete, x d is the embedded depth of steel bars, f rr is the action factor of steel corrosion repair material, and ccr is the inherent critical concentration of steel corrosion.

[0084] Example 1

[0085] As shown in Figures 1-10, this embodiment provides a method for calculating the life of concrete in a plateau environment taking into account protection and repair effects. The specific process is as follows:

[0086] A concrete pier serving in a plateau environment in my country was selected. The pier is in contact with water in the temperature range of -8 to 20°C, with a chloride concentration of 20,000 mg / L. It contains no sulfate and is not subjected to additional external loads. Different types of protective coatings (green polyethylene coating CPE / chloroprene emulsion coating CR / chloroprene emulsion coating PVDC / chlorinated polyvinyl chloride coating CPVC) were used, as well as different crack damage repair materials (repair rate 50% / 70% / 90%) and different steel bar corrosion repair materials (critical concentration increased by 10% / 30%).

[0087] According to steps (1-4), a numerical model considering the protective effect in plateau environment is constructed (Figure 1), and the distribution of various parameters in concrete is obtained, taking the chloride ion concentration that is most likely to cause steel corrosion as an example (Figure 2-8).

[0088] As shown in Figure 2, neither moisture nor ions penetrated the protective coating within two years. At the fifth year, small amounts of moisture and chloride ions appeared in localized areas of the concrete's surface with less aggregate. However, within the 10 years of the protective coating's effectiveness, no significant amounts of moisture or chloride ions were present within the concrete. This demonstrates that the protective coating effectively isolates water and ions throughout its service life, directly improving the concrete's erosion resistance. Following the failure of the protective coating, moisture and chloride ions directly contacted the concrete surface, leading to a significant increase in moisture and chloride ion content within the concrete. Because chloride ion transport primarily occurs via water level and due to adsorption and binding within the concrete, the water transport rate far exceeds that of the concrete. At 30 years, the overall saturation within the concrete was close to 1, but chloride ions were confined to the surface. For a surface protective coating with a 10-year service life, the chloride ion transmission depths were 8 mm, 37 mm, 34 mm, 40 mm, and 48 mm at 15, 30, 50, and 100 years, respectively.

[0089] As shown in Figure 3, the chloride ion concentration in concrete increases over time, with the growth trend shifting from a sharp rise to a gradual improvement. The use of protective coatings delays the onset of chloride ion attack in concrete and slows the diffusion rate of chloride ions in concrete. The chloride ion concentration in concrete is closely related to the lifespan of the protective coating. As the lifespan of the protective coating increases, the onset of chloride ion intrusion in concrete is gradually delayed, and the chloride ion concentration in concrete also decreases linearly. This indicates that increasing the lifespan of the protective coating effectively reduces the chloride ion concentration in concrete throughout its entire lifespan. Improving the lifespan of the protective coating is an effective means of preventing and delaying chloride ion attack and extending the service life of concrete.

[0090] As shown in Figure 4, increasing the thickness of the protective coating effectively reduces the final chloride ion concentration on the concrete surface and within the concrete, with the reduction in chloride ion concentration within the concrete being more pronounced than on the concrete surface. When the protective coating thickness is less than 1 mm, the time at which chloride ions begin to appear on the concrete surface is not delayed; however, when the protective coating thickness exceeds 1 mm, the chloride ion concentration on the concrete surface begins to gradually increase. This indicates that a protective coating thickness of at least 1 mm is required to effectively prevent media from invading the concrete within the coating's expected lifespan. However, even if the protective coating thickness is gradually increased to 3 mm, chloride ions will still intrude on the concrete surface.

[0091] As shown in Figure 5, compared to no protective coating, the application of chlorinated polyethylene (CPE), chloroprene emulsion (CR), chloroprene dichloromethane (PVDC), and chlorinated polyvinyl chloride (CPVC) coatings reduced the final chloride ion concentration of concrete by 86%, 40%, 70%, and 84%, respectively. CPE, CR, PVDC, and CPVC all effectively delayed chloride ion intrusion into concrete, reducing the chloride ion concentration within the concrete and thus extending its service life.

[0092] Figures 6-8 show that when the damage repair material has a 70% repair rate, the chloride ion content at 30 mm after 100 years is 73% of the unrepaired level. When the damage repair material has a 90% repair rate, the chloride ion content can be reduced to 35% of the unrepaired level. However, the change in damage repair rate from 70% to 90% has little effect on the transmission of corrosive media within 5 mm, because the damage is not completely repaired. Due to the suction effect of the solution in the surface cracks, the corrosive media has already quickly penetrated into the concrete through the channel. The repair material's repair rate significantly reduces the concentration of corrosive media within the 10-30 mm range.

[0093] Considering the effects of protective coating, damage repair materials and steel corrosion repair materials respectively, the service life of concrete is solved according to step (5) (Figures 9-10).

[0094] As shown in Figure 9, the service life of concrete damaged by environmental factors is 50 years. If a 0.3 mm protective coating is used, the service life can be increased to only 56 years. If a 3 mm protective coating is used, the service life can be increased to 70 years.

[0095] As shown in Figure 10, for concrete without protective materials, considering both the damage repair effect and the corrosion repair effect, a service life of 78 years can be achieved using a repair material with an 80% damage repair rate. If a steel corrosion repair material that can increase the critical concentration by 10% is used, the service life can reach 63 years. If both types of repair materials are used simultaneously, the concrete can be guaranteed to have a service life of 100 years.

[0096] Therefore, this method can effectively calculate the service life of concrete considering protection and repair functions in plateau environments, providing important guidance for engineering practice.

[0097] The above description is merely a preferred embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by a person skilled in the art within the technical scope disclosed in the present application should be included in the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of protection of the claims.

Claims

1. A method for calculating the concrete life in a plateau environment taking into account the protection and repair effects, characterized in that: The following steps are involved: S1. Determine the temperature, humidity, salt concentration and internal and external load conditions of the simulated plateau environment, and establish the mapping relationship between the plateau environment, load parameters and time; S2. Construct a concrete geometric model considering protection and repair functions under plateau environment, and determine the material properties of each phase in the geometric model; S3. Establishing the physical field equation of temperature-humidity-salt concentration-load multi-factor coupling, setting internal and external boundary conditions and initial conditions based on the concrete geometric model, wherein the external boundary condition is the mapping relationship between the plateau environment, load parameters and time; S4. Solve the temperature, humidity, salt concentration, stress distribution inside the concrete and their changes over time under the plateau environment and load, considering the protection and repair functions; S5. Calculate the time it takes for the steel bars inside the concrete to reach the critical corrosion concentration and become depassivated, taking into account the protection and repair functions, and determine the service life of the concrete.

2. The method for calculating the concrete lifespan in plateau environment considering protection and repair effects according to claim 1 is characterized in that: In S1, the mapping relationship between the plateau environment, load parameters and time is fixed or arbitrarily changing temperature, humidity, salt concentration and internal and external force loads; Salt is the corrosive medium, including: sodium chloride, calcium chloride, cesium chloride, sodium sulfate, magnesium sulfate; internal and external force loads include: gravity, internal pore expansion force, and external load.

3. The method for calculating the concrete lifespan in plateau environment considering protection and repair effects according to claim 1 is characterized in that: In S2, the construction process of the concrete geometric model is: using the Monte Carlo method to randomly generate the concrete microstructure, adding a protective coating geometric model of arbitrary thickness to the surface of the concrete, the protective coating geometric model is a line segment connected to the concrete in the 1D structure, a tetrahedron fitted to the concrete in the 2D model, and a hexahedron fitted to the concrete in the 3D structure model, and the damage repair material is a lattice or space domain evenly distributed inside the cement paste.

4. The method for calculating the concrete lifespan in plateau environment considering protection and repair effects according to claim 1 is characterized in that: In S2, the concrete geometric model includes coarse aggregate, fine aggregate and cement paste, the coarse and fine aggregate grading type can be freely set, the aggregate volume fraction is between 0% and 80%, the concrete surface protective coating is a continuous coating adhered to the concrete surface, and the concrete repair material is evenly distributed inside the cement paste in the form of a field.

5. The method for calculating the concrete lifespan in plateau environment considering protection and repair effects according to claim 1 is characterized in that: In said S2, said phases include: aggregate, slurry, and coating; The material properties of the slurry include: elastic modulus, Poisson's ratio, density, tensile strength, fracture energy, phase change temperature, phase change temperature interval, phase change latent heat, thermal conductivity, constant pressure heat capacity, ion diffusion coefficient, porosity, pore size distribution; The material properties of the coating include: thermal conductivity, constant pressure heat capacity, and ion diffusion coefficient; The parameters of the aggregate and the coating are obtained through experimental tests; the slurry is composed of sand and cement slurry, and the parameters of the slurry are calculated by micromechanics equivalent medium theory.

6. The method for calculating the concrete lifespan in consideration of protection and repair effects in plateau environment according to claim 1 is characterized in that: In S3, the multi-factor coupling physical field equations include: temperature conduction equation, Water transport equation, salt transport equation and force equation.

7. The method for calculating the concrete lifespan in consideration of protection and repair effects in plateau environment according to claim 6 is characterized in that: The temperature conduction equation is: Where ρ is density, C is specific heat, T is temperature, t is time, λ is thermal conductivity, L is latent heat of phase change, θ L is the moisture content; The internal initial temperature is set to be consistent with the initial temperature of the plateau environment, and the boundary conditions are Dirichlet boundary conditions, which are consistent with the plateau environment temperature parameters determined in S1; The water transport equation takes into account the two transport effects of gaseous water and liquid water and is expressed as follows: Among them, P c is the moisture characteristic curve, K sl is the permeability coefficient of water in the material under saturated state, is the porosity, η is the viscosity of water, K rl is the relative permeability coefficient of the liquid phase, M w is the molar mass of water, R is the relative gas constant, ρ l is the density of water, D g0 is the free diffusion coefficient of water vapor in air; P gs is the saturated vapor pressure; The internal initial moisture content is set according to the actual concrete, ranging from 0 to 100 RH%, and the boundary condition uses the Dirichlet boundary condition, which is consistent with the plateau environmental moisture parameters determined in S1; When salt ion transport only considers convection and diffusion and does not consider chemical reactions, the salt transport equation is as follows: Where c is the salt ion concentration, D0 is the reference ion diffusion coefficient in the slurry, t0 is the time of reference ion diffusion coefficient measurement, m is the time dependence coefficient, θ c is the critical saturation of pores, U is the ion activation energy in concrete, T ref is the temperature when the reference ion diffusion coefficient is measured, d is the damage factor, which is obtained by the damage mechanics energy method, and f r is the repair rate of the repair material to the damage, D f is the diffusion coefficient of ions in water, R b is the factor affecting the binding of concrete to ions; The internal initial ion concentration was set to 0, and the boundary condition was the Dirichlet boundary condition, which was consistent with the plateau environmental ion parameters determined in S1; The force equation is as follows: Where σ is stress, b is Biot coefficient, p * It is the equivalent load of environmental action, which includes: the equivalent load of internal expansion caused by freeze-thaw and sulfate factors; Among them, p FT * is the internal expansion load caused by freeze-thaw, r max and r min are the maximum and minimum pore sizes in the matrix, K and K L , K C are the matrix moduli of slurry, water and ice respectively, ∈ is the strain of slurry, b L , b C are the Biot coefficients of water and ice, α s is the thermal expansion coefficient of the slurry, p atm is the plateau ambient pressure, p atm0 is the ambient air pressure during slurry pouring, S C , S L , S G are the volume fractions of ice, water and pores at the corresponding temperature, respectively, s * is the equivalent load of internal expansion caused by sulfate attack, v AFt is the volume fraction of expanded ettringite, ω i is the corresponding environmental impact factor, p i * They represent the equivalent loads of freeze-thaw, sulfate and magnesium salt environments respectively.

8. The method for calculating the concrete lifespan in plateau environment considering protection and repair effects according to claim 1 is characterized in that: Specifically, S5 is: the service life of the concrete is the life when the steel bar begins to corrode, and the ion concentration at different depths is solved by S1-S4, and the service life of the concrete is determined by comparing the critical concentration. The service life of the concrete is calculated as follows: Among them, t c is the service life of concrete, x d is the buried depth of steel bars, f rr is the action factor of steel corrosion repair material, and ccr is the inherent critical concentration of steel corrosion.

Citation Information

Patent Citations

  • Method for evaluating chloride ion transmission in concrete by considering sulfate chemical damage effect

    CN112414902A

  • Concrete microstructure chloride ion erosion model based on natural environment effect of cold region

    CN114861496A

  • Method and system for estimating degradation and durability of concrete structures and asset management system making use of same

    US20140249788A1

  • Life-cycle performance intelligent-sensing and degradation warning system and method for concrete structures

    US20210356451A1