Printing ink for washing-free cold-transfer printing process
By developing printing ink for free washing and cold transfer printing process, combined with water-based polyurethane thickener, the printing and dyeing wastewater problems caused by water washing in the prior art are solved, and an efficient printing process without water washing is achieved, and color fastness and friction are improved. Fastness has huge economic and social benefits.
Patent Information
- Application Number
- PCT/CN2023/126790
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2023-10-26
- Publication Date
- 2024-11-28
Smart Images

Figure CN2023126790_28112024_PF_FP_ABST
Abstract
Description
Printing ink for water-free cold transfer printing process Technical Field
[0001] The present invention relates to a printing ink for a wash-free cold transfer printing process and a method for printing polyester fabric using the printing ink. The printing ink and printing method can achieve an enhanced fixation effect of disperse dyes on polyester fabrics, thereby eliminating the washing process after printing and fixing, and thus achieving wash-free cold transfer printing of disperse dyes. Background Art
[0002] Textile printing is a method of printing patterns of various colors on textiles. Common printing processes can be divided into direct printing, anti-dye printing and transfer printing.
[0003] Transfer printing is, in a sense, an extension of printing technology applied to textiles. However, the uneven and porous surface of fabrics, unlike the dense, flat surface of paper targeted by the printing industry, makes it difficult to achieve highly detailed patterns. Therefore, in the textile printing process, transfer printing involves first using printing technology to print ink containing dye onto a carrier such as paper to create a decal. The fabric is then subjected to heavy pressure to temporarily render the surface quasi-flat. The pattern on the decal is then transferred to the fabric using the dye's migration properties under certain conditions. The advantages of the transfer printing process include artistically designed patterns, the ability to produce rich, lifelike patterns, and a short processing time, allowing factories to quickly accept orders and process them, leading to its rapid development.
[0004] Common transfer printing processes include heat transfer printing and cold transfer printing. Heat transfer printing primarily utilizes the sublimation properties of disperse dyes to transfer dyes from paper to fabric. Because disperse dyes have a high affinity for polyester fibers, heat transfer printing is primarily used for printing polyester fabrics. For example, Chinese patent CN201210055121.7 discloses a heat-sublimation water-based gravure printing ink and its preparation method. However, the heat transfer printing process consumes a lot of energy, requires high equipment, and can easily damage other fibers in polyester blends that are sensitive to high temperatures. Furthermore, the poor heat transfer fastness of heat transfer printed products is difficult to overcome.
[0005] Cold transfer printing primarily utilizes the properties of water-based disperse dyes in a wet environment, such as migration, osmotic reaction crosslinking, and capillary effect, to achieve transfer printing. For example, Chinese patent CN201210365576.9 discloses a disperse dye ink for cold transfer printing and its application method. However, current cold transfer printing still requires washing to remove surface floating color to improve color fastness. Specifically, floating color refers to dye molecules that remain on the fiber surface without entering the fiber wells and bonding. In the prior art, washing is the only method to remove floating color and improve color fastness. This is because, under dyeing conditions, if the dye source is cut off, the monomolecular dye already adsorbed on the fiber surface and even remaining in the dye bath will continue to migrate into the fiber interior. The polar water environment is the source of the huge driving force that drives these dye molecules into the non-polar fiber interior. This method of driving the dye into the fiber interior and removing floating color is simple and easy, so washing is the most commonly used method to remove floating color in the prior art. However, the washing process is the main source of printing and dyeing wastewater. As the country implements a strict wastewater discharge system, the production capacity of printing and dyeing enterprises is limited, costs increase, and they lose market competitiveness.
[0006] The present invention aims to develop a printing ink for a water-free cold transfer printing process and a method for printing polyester fabric using the printing ink, based on the existing disperse dye cold transfer printing process. The printing ink and the printing method can omit the washing process after printing fixation, thereby avoiding the generation of printing wastewater, reducing printing wastewater or even achieving zero wastewater discharge, and having huge economic and social benefits.
[0007] BRIEF DESCRIPTION OF THE DRAWINGS
[0008] FIG1 is an infrared spectrum of the waterborne polyurethane thickener used in Example 1.
[0009] Summary of the Invention
[0010] In one aspect, the present invention provides a printing ink for a water-free cold transfer printing process, comprising a disperse dye, a binder, a surfactant, a dispersant, a thickener, and water, wherein the thickener is an aqueous polyurethane thickener having a solid content of about 20-40%, preferably about 25-35%, and the aqueous polyurethane thickener has the following structure:
[0011] Wherein, m is 8-20, preferably 8-15, n is 15-25, preferably 17-20, and k is 1-8, preferably 2-6.
[0012] In one embodiment, for gravure printing equipment, in the aqueous polyurethane thickener, m is preferably 8-10, n is preferably 17-18, and k is preferably 3-4; for flexographic printing equipment, m is preferably 10-13, n is preferably 18-19, and k is preferably 2-3; for rotary screen printing equipment, m is preferably 13-15, n is preferably 19-20, and k is preferably 5-6.
[0013] In one embodiment, the printing ink comprises about 1.0-10.0% of a disperse dye, about 2.0-6.0% of a binder, about 0.5-2.0% of a surfactant, about 0.5-2.0% of a dispersant, about 3.0-15.0%, preferably about 5.0-10.0% of a thickener, and the balance water, based on the total weight of the printing ink.
[0014] The disperse dye is a disperse dye commonly used in the field of printing, including medium-temperature SE type disperse dyes or high-temperature S type disperse dyes. The disperse dyes are all commercially available. Examples thereof include medium-temperature SE type series disperse dyes or high-temperature S type series disperse dyes produced by Zhejiang Longsheng Group Co., Ltd., Zhejiang Runtu Co., Ltd., Huntsman, and Dystar.
[0015] The binder is a commonly used binder in the field of printing, including, for example, a multifunctional aziridine binder. The binder is commercially available, and examples thereof include, for example, 9122 binder purchased from Hangzhou Yinsheng Chemical Factory, TF-320 binder and F-321A binder purchased from Zhejiang Chuanhua Co., Ltd.
[0016] The surfactant is a surfactant commonly used in the field of printing, including, for example, an organosilicon surfactant, examples of which include, for example, BYK-378 purchased from BYK Chemicals, or SF-678 purchased from Shanmu Chemical Co., Ltd.
[0017] The dispersant is a commonly used dispersant in the printing field, including, for example, a series of naphthalenesulfonic acid derivatives, examples of which include, for example, formaldehyde condensates of naphthalenesulfonic acid, such as sodium methylene bis-naphthalenesulfonate (CAS No. 36290-04-7) or polynaphthalene formaldehyde sulfonic acid sodium salt (CAS No. 9084-06-4). These dispersants are commercially available, such as INVALON DAM dispersant (polynaphthalene formaldehyde sulfonic acid sodium salt) purchased from Huntsman, and dispersant NNO (sodium methylene bis-naphthalenesulfonate) purchased from Hai'an Petrochemical Plant in Jiangsu Province.
[0018] The thickener is an aqueous polyurethane thickener having a solid content of about 20-40%, preferably about 25-35%, and the aqueous polyurethane thickener has the following structure:
[0019] Wherein, m is 8-20, preferably 8-15, n is 15-25, preferably 17-20, and k is 1-8, preferably 2-6.
[0020] The aqueous polyurethane thickener can be prepared by, for example, a prepolymer dispersion method.
[0021] In one embodiment, the method for preparing the waterborne polyurethane thickener comprises the following sequential steps:
[0022] In a reaction vessel, stirring a mixture of about 24-30 parts by weight of dry polycaprolactone diol solid powder and about 10-15 parts by weight of dry polyethylene glycol solid powder at a temperature of about 50-60° C. for about 15-20 minutes to obtain a uniform mixture;
[0023] Add about 10-14 parts by weight of isophorone diisocyanate to a reaction vessel, heat the system to about 80-95°C at a stirring rate of about 250-300 rpm, keep the temperature for about 40-45 minutes, and then reduce the system temperature to about 75-85°C;
[0024] Add about 1.3-1.5 parts by weight of dimethylolpropionic acid to the reaction vessel, continue the reaction for about 15-25 minutes, and then reduce the system temperature to about 45-55°C;
[0025] Add about 0.8-1.2 parts by weight of triethylamine into the reaction vessel and continue the reaction for about 25-35 minutes to obtain a waterborne polyurethane prepolymer, and then reduce the system temperature to about 35-45°C;
[0026] While slowly increasing the stirring speed from about 250-300 rpm to about 1400-1600 rpm, about 169.5-183.5 parts by weight of water are gradually added to the waterborne polyurethane prepolymer, and at the same time, an aqueous solution containing about 1.6-2.3 parts by weight of N-acetylethylenediamine at a concentration of about 20-30% by mass is continuously dripped therein, thereby obtaining a waterborne polyurethane thickener having a solid content of about 20-40%.
[0027] In a specific embodiment, the method for preparing the waterborne polyurethane thickener comprises the following steps in sequence:
[0028] In a reaction vessel, a mixture of 27 parts by weight of dry polycaprolactone diol solid powder and 12 parts by weight of dry polyethylene glycol solid powder was stirred at a temperature of about 55±3° C. for 15 minutes to obtain a uniform mixture;
[0029] Add 10-14 parts by weight of isophorone diisocyanate to a reaction vessel, heat the system to 88±3°C at a stirring rate of 250-300 rpm, keep the temperature for reaction for 40 minutes, and then reduce the system temperature to 80°C;
[0030] 1.3-1.5 parts by weight of dimethylolpropionic acid was added to the reaction vessel, and the reaction was continued for 20 minutes, and then the system temperature was lowered to 50°C;
[0031] 1 part by weight of triethylamine was added to the reaction vessel and the reaction was continued for 30 minutes to obtain a waterborne polyurethane prepolymer, and then the system temperature was lowered to 40±2°C;
[0032] While slowly increasing the stirring speed from 250-300 rpm to 1500 rpm, 169.5-183.5 parts by weight of water are gradually added to the aqueous polyurethane prepolymer, and at the same time, a 20% mass concentration aqueous solution containing 2 parts by weight of N-acetylethylenediamine is continuously dripped therein to obtain an aqueous polyurethane thickener with a solid content of 30%.
[0033] The purity grades of the aforementioned isophorone diisocyanate, dimethylolpropionic acid, triethylamine, and N-acetylethylenediamine are all ≥ industrial purity. The average molecular weight of polycaprolactone diol is approximately 2000-2400 g / mol, and the average molecular weight of polyethylene glycol is approximately 400-1000 g / mol, both of which are ≥ industrial purity. These raw materials are commercially available.
[0034] The specific reaction process in the above preparation is as follows:
[0035] The water can be distilled water or deionized water.
[0036] The method for preparing the printing ink for the water-free cold transfer printing process is known in the art, for example, the preparation method may include:
[0037] Add about 3.0-15.0% of a water-based polyurethane thickener having a solid content of 20-40% into a container, add about 40-60% of water, and stir thoroughly for about 2 hours to prepare a thickener paste for later use;
[0038] Adding about 0.5-2.0% of a dispersant to an appropriate amount of water and stirring thoroughly, and then adding about 1.0-10.0% of a disperse dye, about 2.0-6.0% of a binder, and about 0.5-2.0% of a surfactant thereto and stirring thoroughly to dissolve to obtain a mixed paste; and
[0039] The mixed paste is mixed with the thickener original paste, adjusted to 100% with water and fully stirred, thereby obtaining the printing ink for the water-free cold transfer printing process.
[0040] The viscosity of the printing ink is usually about 100-6000 mPa·s, preferably 150-5000 mPa·s.
[0041] In another aspect, the present invention provides a method for performing water-free cold transfer printing on polyester fabric, comprising using the printing ink described above. The method does not require a water-washing and color-fixing step.
[0042] The polyester fabric is a polyester fabric known in the art that can be printed and dyed with disperse dyes, including, for example, Lotaffeta fabric, taffeta fabric, polyester plain fabric, polyester silk fabric, polyester Oxford cloth, polyester brushed cloth, and the like.
[0043] The method of using the printing ink in cold transfer printing is known in the art, for example, by gravure, flexographic or rotary screen printing, the pattern of the printing ink is printed on a transfer carrier to make a flower paper, wherein the transfer carrier is known in the art, including, for example, a printing film, printing paper, a transfer blanket or a transfer rubber roller; then, the polyester fabric is superimposed on the transfer carrier and pressure-transferred, so that the pattern is transferred to the polyester fabric; then, the transferred polyester fabric is subjected to a color fixing step, for example, by a high-temperature and high-pressure steaming or baking process known in the art, wherein the high-temperature and high-pressure steaming is usually carried out at a high temperature of about 125-135°C and a saturated vapor pressure (2.3-3.1 MPa) for about 20-40 minutes, and the baking process is usually carried out at a temperature of about 180-220°C for 30-90 seconds.
[0044] The water-free cold transfer printing method of the present invention does not require a water washing step for color fixation, thereby avoiding the generation of printing wastewater, reducing printing wastewater or even achieving zero wastewater discharge, and has huge economic and social benefits.
[0045] Moreover, even though the cold transfer printing method of the present invention omits the washing and color fixing step, the washing color fastness of the obtained printed product can still reach ≥ level 4, the wet rubbing fastness reaches level 4, and the dry rubbing fastness reaches level 4-5. The washing color fastness is tested according to the standard method of GB / T 5713-2013 or AATCC 61-2013, and the wet rubbing fastness and dry rubbing fastness are tested according to the standard method of GB / T 3920-1997 or AATCC 8-2016.
[0046] In another aspect, the present invention provides a thickener for a printing ink for a water-free cold transfer printing process, which is an aqueous polyurethane thickener having a solid content of about 20-40%, preferably about 25-35%, and the aqueous polyurethane thickener has the following structure:
[0047] Wherein, m is 8-20, preferably 8-15, n is 15-25, preferably 17-20, and k is 1-8, preferably 2-6.
[0048] Above-mentioned aqueous polyurethane thickener is prepared by the above method.Described aqueous polyurethane thickener is the novel aqueous polyurethane thickener obtained by carrying out prepolymer chain extension modification to polyurethane main body, it does not contain the easily color-changing groups such as halogen and sulfonic acid group, ensures the controllability of the color of disperse dye, and its thermal stability, cohesiveness and storage stability are all excellent, is very suitable for the disperse dye free washing printing ink of the present invention.By using described aqueous polyurethane thickener, when disperse dye contacts terylene fiber in transfer printing, the adsorption of disperse dye by terylene fiber is enhanced, and under the effect of pressure transfer printing and chemical potential afterwards, the dye molecules of adsorption layer diffuse dyeing to fiber interior by free volume, and the dye carried by synthetic paste continues to supplement, adsorb to fiber surface, and whole system maintains a kind of dynamic balance, thus significantly improving the dyeing effect and color fastness of dye, finally making cold transfer printing process without adopting the washing process of removing floating color and fixing color. Example
[0049] The present invention is further illustrated by the following non-limiting examples. It should be noted that these examples should not be considered as limiting the present invention.
[0050] Example 1
[0051] In this embodiment, a pattern of a dark printing ink used in a water-free cold transfer printing process is transferred onto a polyester taffeta textile by gravure printing using printed paper as a transfer carrier.
[0052] The formula of the dark printing ink is:
[0053] The disperse dye is a medium-temperature SE type disperse dye purchased from Huntsman Co., Ltd. The binder is TF-320 adhesive purchased from Zhejiang Chuanhua Co., Ltd. The surfactant is BYK-378 purchased from BYK Chemical. The dispersing aid is Huntsman INVALONDAM. The waterborne polyurethane is:
[0054] Wherein m=8, n=17, k=4.
[0055] The waterborne polyurethane is prepared as follows:
[0056] In a reaction vessel, a mixture of 27 parts by weight of dry polycaprolactone diol (having an average molecular weight of 2000 g / mol) solid powder and 12 parts by weight of dry polyethylene glycol (having an average molecular weight of 400 g / mol) solid powder was stirred at a temperature of 55±3° C. for 15 minutes to obtain a uniform mixture;
[0057] 10 parts by weight of isophorone diisocyanate was added to the reaction vessel, and the system temperature was heated to 88±3°C at a stirring rate of 250 rpm. The temperature was kept to react for 40 minutes, and then the system temperature was lowered to 80°C.
[0058] 1.3 parts by weight of dimethylolpropionic acid was added to the reaction vessel, and the reaction was continued for 20 minutes, and then the system temperature was lowered to 50° C.; 1 part by weight of triethylamine was added to the reaction vessel, and the reaction was continued for 30 minutes to obtain a waterborne polyurethane prepolymer, and then the system temperature was lowered to 40° C.;
[0059] While slowly increasing the stirring speed from 250 rpm to 1500 rpm, 183.5 parts by weight of deionized water were gradually added to the aqueous polyurethane prepolymer, and at the same time, a 20% mass concentration aqueous solution containing 2 parts by weight of N-acetylethylenediamine was continuously dripped therein to obtain an aqueous polyurethane thickener with a solid content of 30%.
[0060] The infrared spectrum of the obtained waterborne polyurethane thickener is shown in Figure 1.
[0061] The printing ink is prepared as follows:
[0062] Add 5% of the above-mentioned 30% solid content water-based polyurethane thickener into a container, add 50% of distilled water, and stir thoroughly for 2 hours to dissolve and prepare a thickener paste;
[0063] 2.0% of a dispersing aid is added to an appropriate amount of distilled water and stirred thoroughly, and then 10.0% of a disperse dye, 6.0% of a binder, and 1.0% of a surfactant are added thereto and stirred thoroughly to dissolve to obtain a mixed paste; and
[0064] The mixed paste is mixed with the thickener original paste, adjusted to 100% with water and stirred thoroughly to prepare printing ink with a viscosity of 800 mPa·s.
[0065] The pattern of the printing ink was printed on transfer printing paper by gravure printing, and a polyester taffeta textile (specifications: 63D x 63D / 160T) was superimposed on the transfer printing paper and pressure-transferred to transfer the pattern to the textile. The transferred textile was then subjected to high-temperature and high-pressure steaming at a temperature of 125° C. and a saturated vapor pressure of 2.3 MPa for about 35 minutes to fix the color, thereby obtaining a printed product.
[0066] The color fastness to washing, wet rubbing, and dry rubbing of the printed products were then tested using AATCC 61-2013 and AATCC 8-2016 standard methods.
[0067] The results showed that the washing color fastness of the printed product was ≥ grade 4, the wet rubbing fastness reached grade 4, and the dry rubbing fastness reached grade 4-5.
[0068] Example 2
[0069] In this embodiment, a transfer printing film is used as a transfer carrier, and a pattern of light-colored printing ink used in a water-free cold transfer printing process is transferred onto a polyester Oxford cloth through a flexographic printing device.
[0070] The formula of the light-colored printing ink is:
[0071] The disperse dye is a high-temperature S-type disperse dye purchased from Zhejiang Longsheng Group Co., Ltd. The binder is 9122 adhesive purchased from Hangzhou Yinsheng Chemical Plant. The surfactant is SF-678 purchased from Shanmu Chemical Co., Ltd. The dispersing aid is Huntsman INVALON DAM dispersant. The waterborne polyurethane is:
[0072] Wherein m=13, n=18, k=2.
[0073] The waterborne polyurethane is prepared as follows:
[0074] In a reaction vessel, a mixture of 27 parts by weight of dry polycaprolactone diol (having an average molecular weight of 2000 g / mol) solid powder and 12 parts by weight of dry polyethylene glycol (having an average molecular weight of 1000 g / mol) solid powder was stirred at 55±3° C. for 15 minutes to obtain a uniform mixture;
[0075] 14 parts by weight of isophorone diisocyanate was added to the reaction vessel, and the system temperature was heated to 88±3°C at a stirring rate of 250 pm, and the temperature was kept to react for 40 minutes, and then the system temperature was lowered to 80°C;
[0076] 1.5 parts by weight of dimethylolpropionic acid was added to the reaction vessel, and the reaction was continued for 20 minutes, and then the system temperature was lowered to 50°C;
[0077] 1 part by weight of triethylamine was added to the reaction vessel and the reaction was continued for 30 minutes to obtain a waterborne polyurethane prepolymer, and then the system temperature was lowered to 40±2°C;
[0078] While slowly increasing the stirring speed from 250 rpm to 1500 rpm, 169.5 parts by weight of deionized water were gradually added to the aqueous polyurethane prepolymer, and at the same time, a 20% mass concentration aqueous solution containing 2 parts by weight of N-acetylethylenediamine was continuously dripped therein to obtain an aqueous polyurethane thickener with a solid content of 30%.
[0079] The printing ink is prepared as follows:
[0080] Add 3% of the above-mentioned 30% solid content water-based polyurethane thickener into a container, add 50% distilled water, and stir thoroughly for 2 hours to dissolve and prepare a thickener paste;
[0081] 0.5% of a dispersing aid is added to an appropriate amount of distilled water and stirred thoroughly, and then 2.0% of a disperse dye, 2.0% of a binder, and 0.5% of a surfactant are added thereto and stirred thoroughly to dissolve to obtain a mixed paste; and
[0082] The mixed paste is mixed with the thickener original paste, adjusted to 100% with water and stirred thoroughly to prepare a printing ink for a water-free cold transfer printing process, the viscosity of which is 150 mPa.s.
[0083] The pattern of the printing ink was printed on a transfer printing film by flexographic printing, and a polyester Oxford cloth (specifications: 300D x 600D / 90T) was laminated with the transfer printing film and pressure-transferred to transfer the pattern to the textile. The transferred textile was then baked at 200°C for about 60 seconds to obtain a printed product.
[0084] Then, the color fastness to washing, wet rubbing fastness and dry rubbing fastness of the obtained printed product were tested by the experimental method described in Example 1.
[0085] The results showed that the washing color fastness of the printed product was ≥ grade 4, the wet rubbing fastness reached grade 4, and the dry rubbing fastness reached grade 4-5.
[0086] Example 3
[0087] In this embodiment, a transfer rubber roller is used as a transfer carrier, and a rotary screen transfer printing device is used to transfer a pattern of a medium-dark color printing ink used in a water-free cold transfer printing process onto a polyester brushed cloth.
[0088] The formula of the medium to dark printing ink is:
[0089] The disperse dye is a medium-temperature SE type disperse dye purchased from Zhejiang Runtu Co., Ltd. The binder is TF-320 adhesive purchased from Zhejiang Chuanhua Co., Ltd. The surfactant is BYK-378 purchased from BYK Chemical. The dispersing aid is dispersant NNO purchased from Hai'an Petrochemical Plant in Jiangsu Province. The waterborne polyurethane is:
[0090] Wherein m=18, n=22, k=6.
[0091] The waterborne polyurethane is prepared as follows:
[0092] In a reaction vessel, a mixture of 27 parts by weight of dry polycaprolactone diol (average molecular weight 2400 g / mol) solid powder and 12 parts by weight of dry polyethylene glycol (average molecular weight 400 g / mol) solid powder was stirred at 55±3° C. for 15 minutes to obtain a uniform mixture;
[0093] 12 parts by weight of isophorone diisocyanate was added to the reaction vessel, and the system temperature was heated to 88±3°C at a stirring rate of 300 rpm. The temperature was kept to react for 40 minutes, and then the system temperature was lowered to 80°C.
[0094] 1.5 parts by weight of dimethylolpropionic acid was added to the reaction vessel, and the reaction was continued for 20 minutes, and then the system temperature was lowered to 50°C;
[0095] 1 part by weight of triethylamine was added to the reaction vessel and the reaction was continued for 30 minutes to obtain a waterborne polyurethane prepolymer, and then the system temperature was lowered to 40±2°C;
[0096] While slowly increasing the stirring speed from 300 rpm to 1500 rpm, 177 parts by weight of deionized water were gradually added to the prepolymer, and at the same time, a 20% mass concentration aqueous solution containing 2 parts by weight of N-acetylethylenediamine was continuously dripped therein to obtain a water-based polyurethane thickener with a solid content of 30%.
[0097] The printing ink is prepared as follows:
[0098] Add 15% of a 30% solid content water-based polyurethane thickener into a container, add 50% deionized water, and stir thoroughly for 2 hours to dissolve and prepare a thickener paste;
[0099] 1.0% of a dispersing aid is added to an appropriate amount of distilled water and stirred thoroughly, and then 6.0% of a disperse dye, 5.0% of a binder, and 1.5% of a surfactant are added thereto and stirred thoroughly to dissolve to obtain a mixed paste; and
[0100] The mixed paste is mixed with the thickener original paste, adjusted to 100% with water and stirred thoroughly to prepare a printing ink for a water-free cold transfer printing process, the viscosity of which is 6000 mPa.s.
[0101] The pattern of the printing ink is printed on a transfer roller using a rotary screen transfer printing device, and the transfer roller is superimposed on a polyester brushed cloth (specifications: 75D x 150D / 150T) and pressure-transferred to transfer the pattern onto the textile. The transferred textile is then subjected to high-temperature and high-pressure steaming at a temperature of 130° C. and a saturated steam pressure of 2.7 MPa for about 20 minutes to fix the color, thereby obtaining a printed product.
[0102] Then, the color fastness to washing, wet rubbing fastness and dry rubbing fastness of the obtained printed product were tested by the experimental method described in Example 1.
[0103] The results showed that the washing color fastness of the printed product was ≥ grade 4, the wet rubbing fastness reached grade 4, and the dry rubbing fastness reached grade 4-5.
Claims
1. A printing ink for a water-free cold transfer printing process, comprising a thickener, a disperse dye, a binder, a surfactant, a dispersant and water, The thickener is an aqueous polyurethane thickener having a solid content of 20-40%, and the aqueous polyurethane thickener has the following structure: in, m is 8-20, n is 15-25, and k is 1-8.
2. The printing ink according to claim 1, wherein the thickener is an aqueous polyurethane thickener having a solid content of 25-35%.
3. The printing ink according to claim 1, wherein m is 8-15, n is 17-20, and k is 2-6.
4. The printing ink according to any one of claims 1 to 3, wherein the printing ink comprises 3.0 to 15.0% of a thickener.
5. The printing ink according to claim 4, wherein the printing ink comprises 5.0-10.0% of a thickener.
6. The printing ink according to any one of claims 1 to 3, wherein the printing ink comprises 3.0-15.0% of a thickener, 1.0-10.0% of a disperse dye, 2.0-6.0% of a binder, 0.5-2.0% of a surfactant, 0.5-2.0% of a dispersant, and the balance of water, based on the total weight of the printing ink.
7. A method for water-free cold transfer printing on polyester fabric, comprising using the printing ink according to any one of claims 1 to 6, wherein the method does not include a washing and color fixing step.
8. The method according to claim 7, wherein the polyester fabric comprises Lotaffeta fabric, taffeta fabric, polyester plain fabric, polyester silk fabric, polyester Oxford fabric and polyester brushed fabric.
9. A thickener for printing ink in a water-free cold transfer printing process, which is an aqueous polyurethane thickener having a solid content of 20-40%, preferably 25-35%, and the aqueous polyurethane thickener has the following structure: in, m is 8-20, preferably 8-15, n is 15-25, preferably 17-20, and k is 1-8, preferably 2-6.
10. A method for preparing the thickener according to claim 9, comprising: In a reaction vessel, at a temperature of 50-60° C., a mixture of 24-30 parts by weight of dry polycaprolactone diol solid powder and 10-15 parts by weight of dry polyethylene glycol solid powder is stirred for 15-20 minutes to obtain a uniform mixture; Add 10-14 parts by weight of isophorone diisocyanate into a reaction vessel, heat the system to 80-95°C at a stirring rate of 250-300 rpm, keep the temperature for reaction for 40-45 minutes, and then reduce the system temperature to about 75-85°C; Add 1.3-1.5 parts by weight of dimethylol propionic acid into the reaction vessel, continue the reaction for 15-25 minutes, and then reduce the system temperature to about 45-55°C; Add 0.8-1.2 parts by weight of triethylamine into the reaction container, continue the reaction for 25-35 minutes to obtain a waterborne polyurethane prepolymer, and then reduce the system temperature to 35-45° C.; and While slowly increasing the stirring speed from 250-300 rpm to 1400-1600 rpm, 169.5-183.5 parts by weight of water are gradually added to the aqueous polyurethane prepolymer, and at the same time, a 20-30% mass concentration aqueous solution containing 1.6-2.3 parts by weight of N-acetylethylenediamine is continuously dripped therein to obtain the thickener.
Citation Information
Patent Citations
Disperse dye ink for cold transfer printing and application method thereof
CN102838897A
Waterborne polyurethane adhesive cement emulsion for swimwear printing and preparation method thereof
CN110922563A
Polyester washing-free dye composition and preparation process and dyeing process thereof
CN111925667A
Washing-free or less-washing printing method
CN112301761A
Washing-free foam printing paste and printing method
CN112626885A