Paste for current collector, and preparation method for carbon-coated aluminum foil current collector
By grinding low-melting point glass powder in lithium batteries to a small particle size and dispersing it into carbon coating slurry, the problem of large interface resistance of traditional current collectors is solved, the insulation effect of lithium batteries at high temperatures is achieved, and the battery is improved safety performance.
Patent Information
- Application Number
- PCT/CN2023/141124
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-28
AI Technical Summary
Traditional aluminum foil or copper foil current collectors have large interface resistance problems in lithium batteries, which affects the safety performance of the battery, and may lead to short circuits and temperature increases when they exceed the normal use range.
Using a slurry for current collector, including 70-90% pure water, 20-30% binder, 4-8% carbon powder and 0.05-1% crosslinker, by adding low-melting point glass powder and pelleting it The diameter is ground to D50≤2μm, dispersed into a carbon coated slurry, coated on the surface of the aluminum foil, and baked to prepare a carbon coated aluminum foil current collector.
This method changes the electrical properties of the carbon coating layer when the temperature of the lithium battery is abnormally increased, achieving insulation between the electrode sheet and the active material, preventing short-circuit reactions, improving the safety performance of the battery, and ensuring the safety of the lithium battery at high temperatures .
Smart Images

Figure PCTCN2023141124-FTAPPB-I100001
Abstract
Description
A slurry for current collector and a method for preparing the carbon-coated aluminum foil current collector Technical Field
[0001] The present application relates to the technical field of carbon-coated current collectors for lithium batteries, and specifically to a preparation method of a current collector slurry and a carbon-coated aluminum foil current collector. Background Art
[0002] Lithium-ion batteries are widely used in many fields such as automobiles and mobile phones due to their high energy density. The components of lithium batteries mainly include positive and negative electrode active materials, electrolytes, separators, and positive and negative electrode current collectors. At present, aluminum foil, copper foil, composite aluminum foil, composite copper foil, and carbon-coated aluminum foil, carbon-coated copper foil, composite carbon-coated aluminum foil, and composite carbon-coated copper foil with carbon coating on the surface are the main materials used to transmit electrons. However, traditional aluminum foil or copper foil current collectors have the problem of high interface resistance, while carbon-coated current collectors can improve the interface resistance and improve the charging and discharging of the battery. When the battery exceeds the normal operating range, it may experience phenomena such as short-circuit temperature increase. The existing carbon coating layer will affect the safety performance of the lithium battery during use.
[0003] In order to solve the above problems and improve the performance and safety of batteries, the present application provides a slurry for current collector and a method for preparing the carbon-coated aluminum foil current collector.
[0004] Summary of the Invention
[0005] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0006] The purpose of this application is to provide a slurry for a current collector and a method for preparing the carbon-coated aluminum foil current collector, so as to solve the problems raised in the above background technology.
[0007] In order to solve the above technical problems, this application provides the following technical solutions:
[0008] A slurry for a current collector is composed of the following raw materials, calculated by weight: 70-90 parts of pure water, 20-30 parts of a binder, 4-8 parts of carbon powder, 0.05-1 part of a cross-linking agent, and 0.5-3 parts of low-melting-point glass powder.
[0009] Optionally, the adhesive is any one or more of an acrylic adhesive, a polyacrylate adhesive, a styrene-butadiene emulsion adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, and a polyvinyl acetate adhesive.
[0010] Optionally, the carbon powder is any one or more of acetylene black, natural graphite, artificial graphite, and carbon nanotubes.
[0011] Optionally, the cross-linking agent is any one or more of sodium hydroxide, calcium hydroxide, and lithium hydroxide.
[0012] A method for preparing a carbon-coated aluminum foil current collector comprises the following steps:
[0013] Step 1: Take pure water and a binder, stir evenly to obtain a homogeneous solution; add carbon powder to the homogeneous solution, disperse it to obtain a premixed slurry; add a crosslinking agent to the premixed slurry, continue stirring to obtain a mixed slurry;
[0014] Step 2: Take pure water and low-melting-point glass powder, sand grind them to obtain a glass powder solution;
[0015] Step 3: Add the glass powder solution to the mixed slurry, disperse and sand grind to obtain the current collector slurry; apply the current collector slurry on the surface of the aluminum foil, bake, and obtain the carbon-coated aluminum foil current collector.
[0016] Optionally, in step 2, the number of sand grinding times is 1-7 times; after sand grinding, the particle size distribution of the low-melting-point glass powder is D50≤2μm.
[0017] Optionally, in step 1, the dispersion time is 0.5-1 h, and the dispersion speed is 500-3000 rpm.
[0018] Optionally, the preparation method of the low-melting-point glass powder is: take bismuth trioxide, boron oxide, phosphorus pentoxide, silicon dioxide, and titanium dioxide, dry them for 2-3 hours, and mix them evenly; sinter them at 900-920°C for 20-30 minutes, quench them with water, wash them, grind them at a speed of 500-600 rpm for 1-2 hours, sieve them, and dry them to obtain low-melting-point glass powder.
[0019] Optionally, the surface of the low-melting-point glass powder is modified by the following method: taking deionized water, adding acetic acid, stirring evenly, adding chitosan, and continuing to stir for 20-30 minutes to obtain a chitosan solution; taking ethyl orthosilicate, ethanol, and chitosan solution, ultrasonically oscillating for 50-70 minutes, and standing for 4-6 hours to obtain a mixed sol; taking the mixed sol and low-melting-point glass powder, mixing evenly, and drying to obtain a modified low-melting-point glass powder.
[0020] Optionally, the coating method is any one of gravure coating and slit coating.
[0021] Compared with the prior art, the beneficial effects achieved by this application are:
[0022] (1) The purpose of this application is to improve the safety performance of the battery on the basis of improving the battery performance. When the battery exceeds the normal use range, short circuit temperature rise and other phenomena may occur. The existing carbon coating layer cannot play a safety role in these situations, affecting the safety performance of the lithium battery during use. This application adds low-melting point glass powder and grinds the glass powder to a particle size of D50≤2μm, disperses the low-melting point glass powder containing small particles into the carbon coating slurry, and then coats it on the surface of the current collector, and bakes it to obtain a carbon-coated aluminum foil current collector. The addition of low-melting point glass powder material with D50≤2μm enables the carbon coating layer to undergo a transformation in electrical properties when the battery temperature abnormally rises to a specific temperature, thereby achieving insulation between the electrode and the active material, preventing further short-circuit reactions, and thus ensuring the safety performance of the battery. The carbon-coated aluminum foil current collector prepared by this process can achieve an insulating effect at high temperatures, ensuring the safety performance of the lithium battery when a short circuit occurs.
[0023] (2) This application uses bismuth trioxide, boron oxide, phosphorus pentoxide, silicon dioxide, and titanium dioxide to prepare a low-melting-point glass powder through high-temperature sintering and water quenching. This application also uses chitosan solution to add ethyl orthosilicate to prepare a mixed sol, which is mixed with the low-melting-point glass powder. The mixed sol contains a large number of amino and hydroxyl groups, which increases the surface tension of the low-melting-point glass powder, improves the dispersibility of the low-melting-point glass powder in pure water, improves the insulation effect, and ensures the safety performance of the lithium battery in the event of a short circuit.
[0024] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0025] The following is a clear and complete description of the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0026] Main materials and their sources in the examples:
[0027] Carbon nanotubes: OD: 1-2 nm, length: 20 μm.
[0028] Acrylic adhesive: There is no particular restriction on the manufacturer of this material, and an exemplary example includes: product number MA530, manufactured by Plexus.
[0029] Bismuth trioxide: There is no special restriction on the manufacturer of this substance, and an exemplary example includes: product number B802282, and the manufacturer is Macklin Reagent.
[0030] Boric acid: There is no particular restriction on the manufacturer of this substance, and examples thereof include: item number B802547, manufactured by Macklin Reagent.
[0031] Phosphorus pentoxide: There is no particular restriction on the manufacturer of this substance, and examples thereof include: product number P816727, and the manufacturer is Macklin Reagent.
[0032] Silicon dioxide: particle size is 5 μm. There is no special restriction on the manufacturer of this material. Examples include: product number S817558, manufacturer: Macklin Reagent.
[0033] Titanium dioxide: particle size is 2-3 μm. There is no special restriction on the manufacturer of this substance. Examples include: product number T832269, manufacturer: Macklin Reagent.
[0034] Ethyl orthosilicate: There is no special restriction on the manufacturer of this substance, and examples include: CAS78-10-4, manufacturer: Jinjinle (Hunan) Chemical Co., Ltd.
[0035] Example 1
[0036] Step 1: Preparation of mixed slurry:
[0037] Take 50 kg of pure water and 20 kg of acrylic adhesive, stir for 20 minutes to obtain a homogeneous solution; add 4 kg of carbon nanotubes to the homogeneous solution, disperse for 0.7 hours at a dispersion speed of 1000 rpm to uniformly disperse the carbon powder to obtain a premixed slurry; add 0.05 kg of sodium hydroxide and continue stirring to perform preliminary crosslinking on the premixed slurry to improve the stability of the slurry and obtain a mixed slurry.
[0038] Step 2: Preparation of low melting point glass powder:
[0039] Take 460g of bismuth trioxide, 300g of boron oxide, 100g of phosphorus pentoxide, 80g of silicon dioxide, and 60g of titanium dioxide, dry them for 2.5h, and mix them evenly; sinter them at 910℃ for 25min, quench them with water, wash them, grind them at 500rpm for 1h, pass them through a 500-mesh sieve, and dry them to obtain a low-melting-point glass powder.
[0040] Step 3: Preparation of current collector slurry:
[0041] Take 1 kg of low-melting-point glass powder, add 20 kg of pure water, and sand grind it 5 times at a speed of 1000 rpm to reduce the particle size distribution of the glass powder to D50 = 1.635 μm, D90 = 4.336 μm to obtain a glass powder solution; add the glass powder solution to the mixed slurry, disperse it at a speed of 3000 rpm, and sand grind it twice at a speed of 600 rpm. Discharge the material to obtain a slurry for the collector.
[0042] Step 4: Preparation of carbon-coated aluminum foil current collector:
[0043] The current collector slurry was coated on one side of an aluminum foil with a thickness of 13 μm using a gravure coating method and baked at 100° C. for 1 min to obtain a carbon-coated aluminum foil current collector with a total thickness of 13.5 μm.
[0044] Example 2
[0045] Step 1: Preparation of mixed slurry:
[0046] Take 50 kg of pure water and 20 kg of acrylic binder, stir for 10 minutes to obtain a homogeneous solution of the binder and water; add 4 kg of carbon nanotubes to the homogeneous solution, disperse for 0.5 hours at a dispersion speed of 500 rpm to uniformly disperse the carbon powder to obtain a premixed slurry; add 0.05 kg of sodium hydroxide to perform preliminary cross-linking on the premixed slurry to improve the stability of the slurry, and obtain a mixed slurry.
[0047] Step 2: Preparation of low melting point glass powder:
[0048] Take 460g of bismuth trioxide, 300g of boron oxide, 100g of phosphorus pentoxide, 80g of silicon dioxide, and 60g of titanium dioxide, dry them for 2h, and mix them evenly; sinter them at 900℃ for 20min, quench them with water, wash them, grind them at 500rpm for 1h, pass them through a 500-mesh sieve, and dry them to obtain a low-melting-point glass powder.
[0049] Step 3: Preparation of current collector slurry:
[0050] Take 1 kg of low-melting-point glass powder, add 20 kg of pure water, and sand grind it 5 times at a speed of 1000 rpm to reduce the particle size distribution of the glass powder to D50 = 1.753 μm, D90 = 5.096 μm to obtain a glass powder solution. Add the glass powder solution to the mixed slurry, disperse it at a speed of 3000 rpm, and sand grind it twice at a speed of 600 rpm. Discharge the material to obtain a slurry for the collector.
[0051] Step 4: Preparation of carbon-coated aluminum foil current collector:
[0052] The current collector slurry was coated on one side of an aluminum foil with a thickness of 13 μm using a gravure coating method and baked at 100° C. for 1 min to obtain a carbon-coated aluminum foil current collector with a total thickness of 13.5 μm.
[0053] Example 3
[0054] Step 1: Preparation of mixed slurry:
[0055] Take 50 kg of pure water and 20 kg of acrylic binder and stir for 30 minutes to obtain a homogeneous solution of the binder and water; add 4 kg of carbon nanotubes to the homogeneous solution and disperse for 1 hour at a dispersion speed of 3000 rpm to uniformly disperse the carbon powder to obtain a premixed slurry; add 0.05 kg of sodium hydroxide to perform preliminary cross-linking on the premixed slurry to improve the stability of the slurry to obtain a mixed slurry.
[0056] Step 2: Preparation of low melting point glass powder:
[0057] Take 460g of bismuth trioxide, 300g of boron oxide, 100g of phosphorus pentoxide, 80g of silicon dioxide, and 60g of titanium dioxide, dry them for 3h, and mix them evenly; sinter them at 920℃ for 30min, quench them with water, wash them, grind them at 500rpm for 1h, pass them through a 500-mesh sieve, and dry them to obtain a low-melting-point glass powder.
[0058] Step 3: Preparation of current collector slurry:
[0059] Take 1 kg of low-melting-point glass powder, add 20 kg of pure water, and sand grind it 5 times at a speed of 1000 rpm to reduce the particle size distribution of the glass powder to D50 = 1.225 μm, D90 = 4.772 μm to obtain a glass powder solution. Add the glass powder solution to the mixed slurry, disperse it at a speed of 3000 rpm, and sand grind it twice at a speed of 600 rpm. Discharge the material to obtain a slurry for the collector.
[0060] Step 4: Preparation of carbon-coated aluminum foil current collector:
[0061] The current collector slurry was coated on one side of an aluminum foil with a thickness of 13 μm using a gravure coating method and baked at 100° C. for 1 min to obtain a carbon-coated aluminum foil current collector with a total thickness of 13.5 μm.
[0062] Example 4: modified low-melting-point glass powder is used, and the rest is the same as Example 1.
[0063] Step 1: Preparation of mixed slurry:
[0064] Take 50kg of pure water and 20kg of acrylic binder and stir for 30 minutes to obtain a homogeneous solution; add 4kg of carbon nanotubes to the homogeneous solution and disperse for 1 hour at a dispersion speed of 3000rpm to uniformly disperse the carbon powder to obtain a premixed slurry; add 0.05kg of sodium hydroxide and continue stirring to perform preliminary crosslinking of the premixed slurry to improve the stability of the slurry and obtain a mixed slurry.
[0065] Step 2: Preparation of modified low-melting-point glass powder:
[0066] Take 460g of bismuth trioxide, 300g of boron oxide, 100g of phosphorus pentoxide, 80g of silicon dioxide, and 60g of titanium dioxide, dry them for 3h, and mix them evenly; sinter them at 920℃ for 30min, quench them with water, wash them, grind them at 500rpm for 1h, pass them through a 500-mesh sieve, and dry them to obtain a low-melting-point glass powder.
[0067] Take 1L of deionized water, add 40mL of acetic acid, stir evenly, add 20g of chitosan, and continue stirring for 30min to obtain a chitosan solution; take 25mL of ethyl orthosilicate, 100mL of ethanol, and 1L of chitosan solution, ultrasonically oscillate for 70min, and let it stand for 6h to obtain a mixed sol.
[0068] 1.5 kg of mixed sol and 1 kg of low-melting-point glass powder were mixed evenly and dried to obtain modified low-melting-point glass powder.
[0069] Step 3: Preparation of current collector slurry:
[0070] Take 1 kg of modified low-melting-point glass powder, add 20 kg of pure water, and sand grind it 5 times at a speed of 1000 rpm to reduce the particle size distribution of the glass powder to D50 = 1.635 μm, D90 = 4.336 μm to obtain a glass powder solution; add the glass powder solution to the mixed slurry, disperse it at a speed of 3000 rpm, and sand grind it twice at a speed of 600 rpm. Discharge the material to obtain a slurry for the collector.
[0071] Step 4: Preparation of carbon-coated aluminum foil current collector:
[0072] The current collector slurry was coated on one side of an aluminum foil with a thickness of 13 μm using a gravure coating method and baked at 100° C. for 1 min to obtain a carbon-coated aluminum foil current collector with a total thickness of 13.5 μm.
[0073] Comparative Example 1
[0074] Step 1: Preparation of mixed slurry:
[0075] Take 50 kg of pure water and 20 kg of acrylic binder and stir for 30 minutes to obtain a homogeneous solution of the binder and water; add 4 kg of carbon nanotubes to the homogeneous solution and disperse for 1 hour at a dispersion speed of 3000 rpm to uniformly disperse the carbon powder to obtain a premixed slurry; add 0.05 kg of sodium hydroxide to perform preliminary cross-linking on the premixed slurry to improve the stability of the slurry to obtain a mixed slurry.
[0076] Step 2: Preparation of current collector slurry:
[0077] The mixed slurry was dispersed at a rotation speed of 3000 rpm, sand-milled twice at a rotation speed of 600 rpm, and discharged to obtain a slurry for a current collector.
[0078] Step 3: Preparation of carbon-coated aluminum foil current collector:
[0079] The current collector slurry was coated on one side of an aluminum foil with a thickness of 13 μm using a gravure coating method and baked at 100° C. for 1 min to obtain a carbon-coated aluminum foil current collector with a total thickness of 13.5 μm.
[0080] experiment
[0081] The carbon-coated aluminum foil current collectors prepared in Examples 1 to 4 and Comparative Example 1 were baked in an oven at 300° C. The carbon-coated aluminum foil current collectors obtained in the aforementioned examples and the carbon-coated aluminum foil current collectors in the comparative examples were tested for room temperature penetration resistance and penetration resistance after baking at 300° C. (test instrument ACCFILM electrode sheet resistance meter, test conditions: total pressure 19.2 MPa, pressure increase rate 0.29 MPa / s, holding time 1 s). The data obtained are shown in the following table:
[0082] Conclusion: Examples 1 to 3 of this application add low-melting-point glass frit with a D50 of ≤ 2 μm to the slurry to prepare carbon-coated aluminum foil current collectors. This low-melting-point glass frit material with a D50 of ≤ 2 μm enables the carbon coating layer to undergo a transition in electrical properties when the battery temperature abnormally rises to a specific temperature, thereby achieving insulation between the electrode and the active material and preventing short circuits. At room temperature, the carbon-coated aluminum foil current collector exhibits no significant change in resistance. A penetration resistance test of the carbon-coated aluminum foil current collector doped with low-melting-point glass frit at 300°C reveals a short circuit, demonstrating excellent safety performance. Example 4 also adds ethyl orthosilicate to a chitosan solution to prepare a mixed sol. This mixed sol is then mixed with low-melting-point glass frit. The mixed sol contains a large number of amino and hydroxyl groups, which increase the surface tension of the low-melting-point glass frit, improve its dispersibility in pure water, and enhance the stability of the slurry. This mixed sol is then used to prepare a carbon-coated aluminum foil current collector, achieving a room-temperature penetration resistance of 2.006 mΩ, further enhancing performance. However, the resistance of Comparative Example 1 is greatly increased, reaching 3mΩ, and the safety performance of lithium batteries at high temperatures is reduced.
[0083] Finally, it should be noted that the above description is merely a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included within the scope of protection of the present application.
Claims
1. A slurry for a current collector, composed of the following raw materials, by weight: 70-90 parts of pure water, 20-30 parts of a binder, 4-8 parts of carbon powder, 0.05-1 part of a cross-linking agent, and 0.5-3 parts of a low-melting-point glass powder.
2. The current collector slurry according to claim 1, in: The adhesive is any one or more of an acrylic adhesive, a polyacrylate adhesive, a styrene-butadiene emulsion adhesive, a polyurethane adhesive, a polyvinyl alcohol adhesive, and a polyvinyl acetate adhesive.
3. The current collector slurry according to claim 1 or 2, in: The carbon powder is any one or more of acetylene black, natural graphite, artificial graphite and carbon nanotubes.
4. The current collector slurry according to any one of claims 1 to 3, in: The cross-linking agent is any one or more of sodium hydroxide, calcium hydroxide and lithium hydroxide.
5. A method for preparing a carbon-coated aluminum foil current collector, The following steps are involved: Step 1: Take pure water and a binder, stir evenly to obtain a homogeneous solution; add carbon powder to the homogeneous solution, disperse it, and obtain a premixed slurry; add a crosslinking agent to the premixed slurry, continue stirring, and obtain a mixed slurry; Step 2: Take pure water and low melting point glass powder, sand grind them to obtain a glass powder solution; Step 3: Add the glass powder solution to the mixed slurry, disperse and sand grind to obtain the current collector slurry; apply the current collector slurry on the surface of the aluminum foil, bake, and obtain the carbon-coated aluminum foil current collector.
6. The method for preparing the carbon-coated aluminum foil current collector according to claim 5, in: In step 2, the number of sand grinding is 1-7 times; after sand grinding, the particle size distribution of the low melting point glass powder is D50≤2μm.
7. The method for preparing the carbon-coated aluminum foil current collector according to claim 5 or 6, in: In step 1, the dispersion time is 0.5-1h, and the dispersion speed is 500-3000rpm.
8. The method for preparing the carbon-coated aluminum foil current collector according to any one of claims 5 to 7, in: The preparation method of the low melting point glass powder is as follows: bismuth trioxide, boron oxide, phosphorus pentoxide, silicon dioxide, and titanium dioxide are taken, dried for 2-3 hours, and mixed evenly; sintered at 900-920° C. for 20-30 minutes, water quenched, washed, ground at a speed of 500-600 rpm for 1-2 hours, sieved, and dried to obtain the low melting point glass powder.
9. The method for preparing the carbon-coated aluminum foil current collector according to claim 8, in: The method also includes modifying the surface of the low-melting-point glass powder, and the modification method is: taking deionized water, adding acetic acid, stirring evenly, adding chitosan, and continuing stirring for 20-30 minutes to obtain a chitosan solution; taking tetraethyl orthosilicate, ethanol, and chitosan solution, ultrasonically oscillating for 50-70 minutes, and standing for 4-6 hours to obtain a mixed sol; taking the mixed sol and low-melting-point glass powder, mixing evenly, and drying to obtain a modified low-melting-point glass powder.
10. The method for preparing the carbon-coated aluminum foil current collector according to any one of claims 5 to 9, in: The coating method is any one of gravure coating and slit coating.
Citation Information
Patent Citations
Water-based conducting sizing agent for coating on surface of current collector of high-safety lithium battery and preparation method application thereof
CN107248577A
Glass positive electrode material and preparation method and application thereof
CN111484247A
Carbon-coated aluminum foil and preparation process thereof
CN115579453A
Slurry for current collector and preparation method of carbon-coated aluminum foil current collector
CN116387527A
Preparation method for mixed capacitor negative electrode slurry
WO2016090958A1
Cited By
Carbon-coated current collector and preparation method thereof, pole piece and battery
CN120784378A