Electrode for lithium-ion secondary battery

The integration of an undercoat layer with carbon nanotubes in lithium-ion battery electrodes addresses the issue of uneven reaction distribution and lifespan extension, enhancing strength and energy density, and reducing the impact of overvoltage factors, thus improving the longevity and performance of lithium-ion batteries for electric vehicles.

WO2024241684A1PCT designated stage expired Publication Date: 2024-11-28KRI INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010968
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-03-21
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium-ion battery electrodes face significant challenges in extending lifespan due to factors like oxidation, lithium ion insertion and desorption, electrolyte decomposition, electrode loosening, and uneven reaction distribution, which lead to reduced energy density and increased costs, especially in applications requiring high mileage and quick charging, such as electric vehicles.

Method used

The development of an electrode structure featuring an undercoat layer containing carbon nanotubes, which reduces the content of binders, thickeners, and dispersants, enhancing strength and uniformity of reactions within the battery while maintaining high energy density, thereby reducing the impact of overvoltage factors and extending battery life.

Benefits of technology

This configuration results in electrodes with improved strength and reduced risk of cracking during manufacturing, enabling uniform reaction distribution and significantly extending battery lifespan, even under high-load conditions, while maintaining energy density and preventing lithium ion inhibition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000066_0000
    Figure 00000066_0000
Patent Text Reader

Abstract

This electrode for a lithium-ion secondary battery electrode comprises an electrode current collector, an undercoat layer, and an electrode active material layer, wherein: the electrode active material layer contains at least an electrode active material and carbon nanotubes; defining the total amount of the electrode active material as 100 mass%, the contained amount of carbon nanotubes is 0.01–1.4 mass%, the contained amount of conductivity aids other than the carbon nanotubes is 0–10.0 mass%, and the contained amount of electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductivity aids other than the carbon nanotubes is 0–2.0 mass%; and the undercoat layer contains at least carbon nanotubes. The electrode for the lithium-ion secondary battery has high strength even if the contained amount of a binder, a thickener, a dispersant, or the like is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Electrodes for lithium-ion secondary batteries

[0001] The present invention relates to an electrode for a lithium ion secondary battery.

[0002] The lithium-ion battery (LIB) business has achieved dramatic growth thanks to relentless technological development aimed at miniaturizing and lightening mobile devices and enhancing their functionality (pursuing convenience) by leveraging the battery's high energy density, high voltage, and safety characteristics. With global environmental and resource issues now in the spotlight, policies such as promoting eco-cars and shifting to renewable energy are expected to continue to drive the growth of the LIB market. If this trend continues, lithium-ion batteries will be needed for personal electric vehicles (EVs) and stationary energy storage (e.g., for renewable energy leveling), and the number of lithium-ion batteries required will be estimated to be approximately 10 times that of 2018 by 2030. This could lead to economically unfavorable situations for users, such as a sharp rise in battery costs due to resource shortages. Therefore, research and development into reuse and recycling, both from the perspective of extending the life of a single battery, has become active. Extending battery life is also effective from the perspective of life cycle assessment (LCA).

[0003] Furthermore, new proposals have been made regarding the future of mobility, including EVs. CASE and MaaS, which aim to further improve user convenience, are becoming a reality, and there are signs that mobility, including EVs, will shift from individual ownership to sharing in the future. Amid this trend, AIEVs (Artificial Intelligence Electric Vehicles), which are expected to be deployed in the market in the future, are EVs equipped with AI, with automated driving, shared vehicles, and vehicles managed by a management company rather than by individuals. The management company provides mobility services (CASE) and various services required by users within the vehicle (MaaS). Furthermore, since the management company can also perform driving control and charging / discharging control, operation can also take into consideration battery life, safety, etc. Furthermore, vehicle sharing can reduce the user's burden to approximately one-fifth of that of individual ownership, making it economically advantageous. In other words, in the future, replacing private cars, which are currently mainly gasoline-powered, with AIEVs (sharing cars) is expected to contribute to the global environment, reduce traffic accidents and congestion, provide a new means of transportation in aging and depopulated areas, reduce personal expenses, and make effective use of travel time. Furthermore, AIEVs will be able to function as huge energy storage systems, automatically charging electricity generated from highly fluctuating renewable energy sources through a management company's management system and discharging it as needed.

[0004] However, to achieve this, it will be necessary to reconsider the development direction of lithium-ion batteries, which are currently the mainstream (Figure 1).

[0005] In particular, dramatically extending the lifespan of batteries installed in electric vehicles is essential. To realize AIEVs, unlike privately owned vehicles, a total vehicle mileage of, for example, 500,000 km or more is required. If the battery life remains at the current level, multiple battery replacements will be necessary, undermining economic viability and leaving resource issues unresolved. The required battery performance emphasizes battery life over the currently mainstream requirements of energy density (mileage) and rapid charging. Specifically, the energy density must be at least 400 Wh / L for a single cell, and the vehicle mileage is 200-300 km with a 20-30 kWh battery installed. However, the target practical operating life must be at least five times longer than the current level.

[0006] Although various studies have been conducted to date on extending the life of batteries, if the target is to extend the practical operating life by at least five times the current life, a new perspective is required. In the present invention, the inventors have focused on the overvoltage factor, in contrast to the many degradation factors that have been studied to date, such as degradation due to oxidation and reduction of active materials and components, degradation associated with the insertion and desorption of lithium ions into and from active materials, consumption of lithium ions due to decomposition of the electrolyte, and degradation due to loosening of electrodes.

[0007] The inventors have explained phenomena such as low-temperature degradation and secondary degradation by defining a new degradation mechanism called "degradation due to overvoltage factor (current × resistance)." Degradation due to overvoltage factor is defined as a degradation factor affected by load current and battery resistance (DC resistance). For example, degradation during low-temperature cycling can be explained as being caused by an increase in resistance at low temperatures, and degradation due to rapid charging can be explained as being caused by an increase in load current. Furthermore, as battery resistance increases with degradation, and as capacity decreases, the load (apparent load) on the active material portion increases when the same current as the initial current is applied. Furthermore, if gas or other substances accumulate within the electrode group, the gas does not allow ions to pass through, so load is placed on the electrode portion and active material other than the gas accumulation. From this perspective, one factor affecting battery life as an overvoltage factor is uneven reaction distribution within the electrode. If the reaction does not occur uniformly within the electrode, some of the active materials used in the electrode will accumulate stress over the long term of the battery. For example, in the case of the negative electrode, this can lead to localized strong reduction, resulting in the consumption of lithium ions, or in the worst case, lithium electrodeposition. In the case of the positive electrode, this can lead to deterioration of the positive electrode active material due to cracking, resulting in a sudden decrease in capacity and a sudden increase in resistance (secondary degradation) after repeated charge / discharge cycles. By uniforming the electrode reaction and preventing uneven reaction distribution within the battery, this secondary degradation (sudden capacity decrease) can be prevented, dramatically extending battery life. Therefore, it is important to uniformize the reaction within the battery, but currently, few efforts have been made to achieve this.

[0008] To achieve uniform reactions within a battery, it is important to create an electrode structure that enables uniform ion migration within the electrode. Previous studies have attempted to achieve this, such as increasing the electrode porosity or reducing the electrode's basis weight. However, these approaches result in a decrease in energy density (mileage), and these approaches alone are limited in terms of achieving the 400 Wh / L level mentioned above. Eliminating factors that can inhibit ion migration within the electrode—specifically, electrode constituent materials such as binders typically used to impart strength to the electrode, thickeners and dispersants typically used to stabilize the electrode slurry—is also considered effective in achieving uniform ion migration within the electrode. However, reducing or eliminating these constituent materials significantly reduces the electrode's strength, making it unable to follow the volumetric changes that occur with charging and discharging. This leads to a lack of current collection paths, resulting in reduced lifespan. Furthermore, electrode manufacturing becomes difficult due to peeling and cracking of the electrode layer during the roll-to-roll conveying, pressing, and slitting processes during electrode manufacturing.

[0009] As a result of extensive investigation, the present inventors have found that by employing an undercoat layer for an electrode active material layer, an electrode with high strength can be obtained even when the contents of binder, thickener, dispersant, etc. in the electrode active material layer are reduced, compared to when an undercoat layer is not formed. However, when pressing during electrode production, even if high-load pressing is not performed, high-load pressure is applied locally, which can cause cracks, and therefore an electrode that can withstand high-load pressing is required.

[0010] The present invention is intended to solve the above-mentioned problems, and has an object to provide an electrode having high strength even when the contents of binder, thickener, dispersant, etc. are reduced.

[0011] In view of the above-mentioned problems, the present inventors have conducted extensive research. As a result, they have found that by employing an undercoat layer containing carbon nanotubes in an electrode active material layer having a reduced content of binder, thickener, dispersant, etc., the electrode active material layer has high strength and is free from cracks even when subjected to high-load pressing during electrode production, compared to when no undercoat layer is formed or when an undercoat layer not containing carbon nanotubes is formed. Based on this finding, the present invention has been completed through further research. That is, the present invention includes the following features.

[0012] Item 1. An electrode for a lithium ion secondary battery comprising an electrode current collector, an undercoat layer, and an electrode active material layer, wherein the electrode active material layer contains at least an electrode active material and carbon nanotubes, and where the total amount of the electrode active material layer is taken as 100% by mass, the content of the carbon nanotubes is 0.01 to 1.4% by mass, the content of the conductive additive other than the carbon nanotubes is 0 to 10.0% by mass, and the content of the electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive additive other than the carbon nanotubes is 0 to 2.0% by mass, and the undercoat layer contains at least carbon nanotubes.

[0013] Item 2. The electrode for a lithium ion secondary battery according to Item 1, wherein the content of the carbon nanotubes is 5 to 100 mass % relative to 100 mass % of the total amount of the undercoat layer.

[0014] Item 3. The electrode for a lithium ion secondary battery according to Item 1 or 2, wherein the undercoat layer further contains an undercoat layer-constituting material other than carbon nanotubes.

[0015] Item 4. The electrode for a lithium ion secondary battery according to Item 3, wherein the content of the undercoat layer constituent materials other than the carbon nanotubes is 0 to 95 mass % relative to 100 mass % of the total amount of the undercoat layer.

[0016] Item 5. The electrode for a lithium ion secondary battery according to any one of Items 1 to 4, wherein the undercoat layer has a thickness of 0.1 to 10.0 μm.

[0017] Item 6. The electrode for a lithium ion secondary battery according to any one of Items 1 to 5, wherein, when the total amount of the electrode active material layer is 100 mass %, the content of the electrode active material is 96.6 to 99.9 mass %, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 2.0 mass %, and the electrode is a negative electrode for a lithium ion secondary battery.

[0018] Item 7. The electrode for a lithium ion secondary battery according to any one of Items 1 to 6, wherein, when the total amount of the electrode active material layer is 100 mass %, the content of the electrode active material is 97.4 to 99.9 mass %, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 1.2 mass %.

[0019] Item 8. The electrode for a lithium ion secondary battery according to Item 7, which is a negative electrode for a lithium ion secondary battery.

[0020] Item 9. The electrode for a lithium ion secondary battery according to any one of Items 1 to 8, wherein, based on 100% by mass of the total amount of the electrode active material layer, the content of the electrode active material is 88.6 to 99.9% by mass, the content of the conductive additive other than the carbon nanotubes is 0 to 10.0% by mass, and the electrode does not contain any electrode constituent materials other than the electrode active material, the carbon nanotubes, and the conductive additive other than the carbon nanotubes, and the electrode is a positive electrode for a lithium ion secondary battery.

[0021] Item 10. The electrode for a lithium ion secondary battery according to any one of Items 1 to 9, wherein the electrode active material is a material capable of absorbing and releasing lithium ions.

[0022] Item 11. The electrode for a lithium ion secondary battery according to any one of Items 1 to 10, wherein the carbon nanotubes are single-walled carbon nanotubes.

[0023] Item 12. The electrode for a lithium ion secondary battery according to any one of Items 1 to 11, which is used to reduce uneven distribution of reactions in a lithium ion secondary battery.

[0024] Item 12-1: Use of the electrode for a lithium ion secondary battery according to any one of Items 1 to 11 for reducing uneven distribution of a reaction in a lithium ion secondary battery.

[0025] Item 13. The electrode for a lithium ion secondary battery according to any one of Items 1 to 12, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

[0026] Item 13-1. Use of the lithium ion secondary battery electrode according to any one of Items 1 to 12 in a lithium ion secondary battery used in an electric vehicle for car sharing.

[0027] Item 14. A lithium ion secondary battery comprising the lithium ion secondary battery electrode according to any one of Items 1 to 13.

[0028] Item 15. The lithium ion secondary battery according to Item 14, which is used in an electric vehicle for car sharing.

[0029] Item 15-1. Use of the lithium ion secondary battery according to Item 14 in an electric vehicle for car sharing.

[0030] Item 16. A method for producing an electrode for a lithium ion secondary battery according to any one of Items 1 to 13, comprising: (1) applying an undercoat layer-forming composition onto an electrode current collector to form an undercoat layer; and (2) forming the electrode active material layer on the undercoat layer formed on the electrode current collector using an electrode active material layer-forming composition, wherein the electrode active material layer-forming composition contains at least an electrode active material and carbon nanotubes, and where the total amount of the electrode active material layer-forming composition is taken as 100 mass%, the content of the carbon nanotubes is 0.01 to 1.4 mass%, the content of the conductive additive other than the carbon nanotubes is 0 to 10.0 mass%, and the content of electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive additive other than the carbon nanotubes is 0 to 2.0 mass%, and the undercoat layer-forming composition contains at least carbon nanotubes.

[0031] Item 17. The manufacturing method according to Item 16, wherein the content of the carbon nanotubes is 5 to 100 mass % relative to 100 mass % of the total amount of the composition for forming an undercoat layer.

[0032] Item 18. The manufacturing method according to Item 16 or 17, wherein the undercoat layer-forming composition further contains an undercoat layer-forming material other than carbon nanotubes.

[0033] Item 19. The manufacturing method according to Item 18, wherein the content of the undercoat layer-forming material other than the carbon nanotubes is 0 to 95 mass % relative to 100 mass % of the total amount of the undercoat layer-forming composition.

[0034] Item 20. The manufacturing method according to any one of Items 16 to 19, wherein the undercoat layer-forming composition is applied so that the undercoat layer has a thickness of 0.1 to 10.0 μm.

[0035] According to the present invention, by employing an undercoat layer containing carbon nanotubes for an electrode active material layer in which the content of binder, thickener, dispersant, etc. is reduced, the strength is high even when the content of binder, thickener, dispersant, etc. in the electrode active material layer is reduced, and cracks do not occur even when high-load pressing is performed during electrode production, compared to when no undercoat layer is formed or when an undercoat layer not containing carbon nanotubes is formed.

[0036] This is a schematic diagram showing the direction of lithium-ion battery development, taking into account a world view in which the use and operation of automobiles will change dramatically.

[0037] In this specification, the term "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of."

[0038] In addition, in this specification, the expression "A to B" means "A or more and B or less."

[0039] 1. Electrodes for Lithium-Ion Secondary Batteries Generally, the active material layer in an electrode often contains significant amounts of other electrode constituent materials, such as binders, thickeners, and dispersants, in addition to the active material. Because these other electrode constituent materials are impermeable to lithium ions, the presence of significant amounts of these other electrode constituent materials inhibits lithium ion migration, preventing uniform charge and discharge. When lithium ion migration is inhibited, reactions concentrate in areas where the inhibition is minimal. This can result in lithium electrodeposition in the case of a negative electrode, or in degradation of the positive electrode active material due to cracking or other factors. This leads to a rapid decrease in capacity and a rapid increase in resistance (secondary degradation) after repeated charge and discharge cycles. On the other hand, simply reducing the amount of other electrode constituent materials does not maintain the electrode's strength enough to maintain its shape. This leads to cracks during electrode fabrication and expansion and contraction during charge and discharge, resulting in damage to the electrode structure and reduced conductivity within the electrode, resulting in current collection degradation and reduced battery life. For this reason, simply reducing the amount of electrode constituent materials other than the electrode active material cannot simultaneously alleviate the uneven reaction distribution and improve the battery life characteristics. As mentioned above, in the case of the negative electrode, the electrode structure breaks down, and the battery life characteristics decrease due to deterioration of current collection, such as a decrease in intra-electrode conductivity. In the case of the positive electrode, as mentioned above, deterioration of current collection, such as a decrease in intra-electrode conductivity, is also induced. Therefore, it has been common technical knowledge that the amount of electrode constituent materials other than the electrode active material cannot be significantly reduced. This tendency is particularly noticeable in the negative electrode, where the electrode structure breaks down.

[0040] In contrast, the electrode for a lithium ion secondary battery of the present invention is an electrode for a lithium ion secondary battery comprising an electrode current collector, an undercoat layer, and an electrode active material layer, wherein the electrode active material layer contains at least an electrode active material and carbon nanotubes, and the content of carbon nanotubes is 0.01 to 1.4 mass%, the content of conductive additives other than the carbon nanotubes is 0 to 10.0 mass%, and the content of electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive additives other than the carbon nanotubes is 0 to 2.0 mass%, assuming the total amount of the electrode active material layer to be 100 mass%, and the undercoat layer contains at least carbon nanotubes.

[0041] By adopting such a configuration, compared to when no undercoat layer is formed or when an undercoat layer not containing carbon nanotubes is formed, even if the contents of binder, thickener, dispersant, etc. in the electrode active material layer are reduced to uniformize the battery reaction, the strength is high and cracks do not occur due to pressing, etc. during electrode production. Furthermore, even if a high load pressure is applied locally by pressing, etc. during electrode production, cracks do not occur. In other words, the lithium ion secondary battery electrode of the present invention can be used to reduce uneven reaction in lithium ion secondary batteries.

[0042] Furthermore, as described above, it has been common technical knowledge in the past that the amount of negative electrode constituent materials other than the negative electrode active material cannot be significantly reduced because significantly reducing or eliminating the amount of electrode constituent materials other than the carbon nanotubes and the conductive additives other than the carbon nanotubes significantly reduces the strength of the electrode, and in the case of a negative electrode, the electrode structure is broken, the conductivity within the electrode is reduced, etc., and the battery life characteristics are reduced due to deterioration of current collection. Therefore, it is particularly useful to apply the lithium ion secondary battery electrode of the present invention, which improves the strength of the electrode while uniforming the battery reaction, to the negative electrode. Therefore, the lithium ion secondary battery electrode of the present invention is preferably an electrode for a lithium ion secondary battery comprising an electrode current collector, an undercoat layer, and an electrode active material layer, wherein the electrode active material layer contains at least an electrode active material and carbon nanotubes, and the total amount of the electrode active material layer is taken as 100 mass%, and the content of the electrode active material is 96.6 to 99.9 mass%, the content of the carbon nanotubes is 0.01 to 1.4 mass%, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 2.0 mass%, and the electrode active material layer is a composition for forming a negative electrode active material layer for a lithium ion secondary battery.

[0043] On the other hand, the present invention does not contain or contains only small amounts of electrode constituent materials such as binders, thickeners, dispersants, etc. that can inhibit the movement of ions within the electrode, and uses only a small amount of carbon nanotubes to collect current between active material particles and maintain the shape of the electrode, while providing an undercoat layer containing carbon nanotubes makes it less likely to inhibit the movement of lithium ions, thereby making it possible to make the reaction within the battery uniform and extend the battery's lifespan.In addition, this improves the strength of the battery and prevents cracks from occurring even when high load pressure is applied locally by pressing, etc. during electrode production, so it is preferable to minimize the amount of electrode constituent materials other than the electrode active material and carbon nanotubes in the electrode active material layer. In this respect, the lithium ion secondary battery electrode of the present invention is an electrode for a lithium ion secondary battery comprising an electrode current collector, an undercoat layer, and an electrode active material layer, wherein the electrode active material layer contains at least an electrode active material and carbon nanotubes, and the content of the electrode active material is preferably 97.4 to 99.9 mass%, the content of the carbon nanotubes is 0.01 to 1.4 mass%, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 1.2 mass%, where the total amount of the electrode active material layer is 100 mass%. As described above, these compositions are particularly useful when applied to negative electrodes, and therefore are more preferably used as negative electrodes for lithium ion secondary batteries.

[0044] (1-1) Undercoat Layer In the present invention, the undercoat layer is present between the electrode current collector and the electrode active material layer, and therefore is unlikely to inhibit the movement of lithium ions even when the electrode active material layer does not contain any electrode constituent materials such as binders, thickeners, dispersants, etc., or contains only small amounts of these materials. This makes it possible to make the reaction within the battery uniform and extend the battery's lifespan. In addition, the strength of the battery is improved, and cracks do not occur even when a high load pressure is applied locally by pressing, etc., during electrode production.

[0045] The undercoat layer is not particularly limited, but it is preferable that the undercoat layer contains at least carbon nanotubes, from the viewpoint of easily improving the strength of the battery and easily making the reaction within the battery uniform, even when the electrode constituent materials such as binders, thickeners, and dispersants in the electrode active material layer are not contained or are contained in very small amounts.

[0046] [1-1-1] Carbon nanotubes In the present invention, by including carbon nanotubes in the undercoat layer, the strength of the electrode can be improved even when the electrode active material layer does not contain any electrode constituent materials such as binders, thickeners, and dispersants or contains only small amounts of such materials, and the occurrence of cracks can be suppressed even when a high load pressure is applied locally by pressing or the like during electrode production.

[0047] Carbon nanotubes are hollow carbon materials in which graphite sheets (i.e., carbon atom planes of a graphite structure or single-layer graphene sheets) are closed in a tube-like shape, and their diameters are on the nanometer scale, with a graphite wall structure. Carbon nanotubes whose wall structure is a single graphite sheet (single-layer graphene sheet) and closed in a tube-like shape are called single-walled carbon nanotubes. On the other hand, carbon nanotubes in which multiple graphite sheets are closed in a tube-like shape and nested are called nested multi-layered carbon nanotubes. In the present invention, both single-walled carbon nanotubes and multi-layered carbon nanotubes can be used. However, single-walled carbon nanotubes are preferred from the viewpoints of improving the strength of the electrode even when the electrode active material layer contains no or only a small amount of electrode constituent materials such as binders, thickeners, and dispersants, and of easily suppressing the occurrence of cracks even when a high load pressure is locally applied by pressing or the like during electrode production.

[0048] Such carbon nanotubes can be used alone or in combination of two or more kinds.

[0049] From the viewpoint of easily increasing the number of carbon nanotubes per volume and easily improving the strength of the electrode, it is preferable that the average outer diameter of the carbon nanotubes is small. Therefore, the average outer diameter of the carbon nanotubes is preferably 0.43 to 25 nm, more preferably 0.43 to 20 nm. The average outer diameter of the carbon nanotubes is measured by observation with a transmission electron microscope (TEM). For carbon nanotubes having such an average outer diameter, the average inner diameter is set according to the average outer diameter.

[0050] The longer the average length of the carbon nanotubes, the easier it is to improve the strength of the electrode, but from the viewpoint of easier improvement of dispersibility, a shorter average length of the carbon nanotubes is preferable. Therefore, the average length of the carbon nanotubes is preferably 0.5 to 200 μm, more preferably 1 to 50 μm. The average length of the carbon nanotubes is measured by observation with an electron microscope (SEM).

[0051] The average aspect ratio of the carbon nanotubes, defined as the ratio of the average length to the average outer diameter of the carbon nanotubes, is preferably 25 to 200,000, more preferably 100 to 50,000, from the viewpoint that the higher the average aspect ratio, the easier it is to improve the strength of the electrode.

[0052] In the present invention, the carbon nanotubes may be either individual or bundled carbon nanotubes, which tend to exhibit strength as a bundle. In either case, the strength of the electrode can be improved even when the electrode active material layer contains no or only a small amount of electrode constituent materials such as binders, thickeners, and dispersants, and the occurrence of cracks can be suppressed even when high pressure is locally applied by pressing or the like during electrode production.

[0053] Furthermore, it is considered preferable that the graphene structure of the carbon nanotubes has few defects, i.e., a high G / D ratio in the Raman spectrum, from the viewpoint of easily suppressing the reactivity between the carbon nanotubes and the electrolyte solution. For this reason, in the present invention, the carbon nanotubes preferably have a G / D ratio in the Raman spectrum of 0.1 to 200, more preferably 50 to 150.

[0054] In the present invention, by incorporating carbon nanotubes into the undercoat layer, the electrode strength can be improved even when the electrode active material layer contains no or only very small amounts of electrode constituent materials such as binders, thickeners, and dispersants, and cracking can be suppressed even when high localized pressure is applied by pressing or the like during electrode production. In this case, even when the carbon nanotube content is small, the electrode strength can be improved and cracking can be suppressed even when high localized pressure is applied by pressing or the like during electrode production. Therefore, in the lithium ion secondary battery electrode of the present invention, the carbon nanotube content is preferably 5 to 100 mass%, more preferably 10 to 100 mass%, and even more preferably 15 to 100 mass%. When multiple carbon nanotubes are used, it is preferable to adjust their total amount so that it falls within the above range. In the undercoat layer, the total amount of the carbon nanotubes and the undercoat layer constituent materials other than the carbon nanotubes (the conductive additive other than the carbon nanotubes and the undercoat layer constituent materials other than the conductive additive) (total amount of the undercoat layer-forming composition) is 100 mass%.

[0055] [1-1-2] Undercoat Layer Constituent Materials Other Than Carbon Nanotubes 1-1-2-1. Conductive Aids Other Than Carbon Nanotubes Examples of conductive aids other than carbon nanotubes include acetylene black, ketjen black, carbon black, graphite, graphene, and amorphous carbon obtained by heat-treating organic materials. The amorphous carbon may also be an amorphous carbon material, as described below. These conductive aids other than carbon nanotubes may be used alone or in combination of two or more.

[0056] Furthermore, the particle size of the conductive additive other than carbon nanotubes in the undercoat layer is not particularly limited, but even if the electrode constituent materials such as binders, thickeners, and dispersants in the electrode active material layer are not included or are present in only small amounts, the movement of lithium ions is less likely to be hindered, making it easier to uniformize the reaction within the battery, making it easier to extend the battery's life, and making it easier to improve the strength of the battery. From the viewpoint of making it less likely to crack even when high load pressure is applied locally, such as by pressing during electrode manufacturing, when the conductive additive other than carbon nanotubes is particulate, the average particle size is preferably 0.001 to 10 μm, more preferably 0.01 to 5 μm, and even more preferably 0.1 to 1 μm. The average particle size of the conductive additive other than carbon nanotubes is measured by laser diffraction / scattering.

[0057] In the lithium ion secondary battery electrode (lithium ion secondary battery negative electrode or lithium ion secondary battery positive electrode) of the present invention, the content of the conductive additive other than carbon nanotubes in the undercoat layer is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, and even if the content of the conductive additive other than carbon nanotubes in the electrode active material layer is very small, it is unlikely to inhibit the movement of lithium ions, making it easy to uniformize the reaction within the battery, making it easy to extend the battery's life, and improving the strength of the battery. Even if a high load is applied locally, cracks are unlikely to occur due to pressing during electrode production, and the undercoat layer and the electrode active material layer are unlikely to peel off. From this viewpoint, the content is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, and even more preferably 0 to 5% by mass. When multiple conductive additives other than carbon nanotubes are used, it is preferable to adjust the total amount so that it is within the above range. In the undercoat layer, the total amount (total amount of the undercoat layer) of the carbon nanotubes and the undercoat layer constituent materials other than the carbon nanotubes (conductive additives other than the carbon nanotubes and undercoat layer constituent materials other than the conductive additives) is 100% by mass.

[0058] 1-1-2-2. Undercoat Layer Constituent Materials Other Than Conductive Aids Examples of undercoat layer constituent materials (negative electrode undercoat layer constituent materials or positive electrode undercoat layer constituent materials) other than conductive aids include carbon nanotubes, conductive aids other than carbon nanotubes, substances (binders) that have adhesive properties with the electrode current collector (negative electrode current collector or positive electrode current collector), thickeners, dispersants, etc.

[0059] Examples of undercoat layer constituent materials (negative electrode undercoat layer constituent materials or positive electrode undercoat layer constituent materials) other than such conductive aids include binders, thickeners, or dispersants, such as fluorine-based polymers (polyvinylidene fluoride resin, polytetrafluoroethylene resin, vinylidene fluoride-hexafluoropropylene copolymer, etc.), polyolefin resins (styrene butadiene copolymer resin, ethylene vinyl alcohol copolymer resin, etc.), synthetic rubbers (styrene butadiene rubber, acrylonitrile butadiene rubber, ethylene propylene diene rubber, etc.), polyacrylonitrile, polyamide, polyimide, polyacrylic acid, polyacrylic acid esters, polyvinyl ether, carboxymethyl cellulose, carboxymethyl cellulose sodium salt, carboxymethyl cellulose ammonium, polyurethane, hydroxypropyl cellulose, hydroxyethyl cellulose, methyl cellulose, etc. These undercoat layer constituent materials (negative electrode undercoat layer constituent materials or positive electrode undercoat layer constituent materials) other than conductive aids can be used alone or in combination of two or more.

[0060] In the lithium ion secondary battery electrode (lithium ion secondary battery negative electrode or lithium ion secondary battery positive electrode) of the present invention, the content of the undercoat layer constituent material (negative electrode undercoat layer constituent material or positive electrode undercoat layer constituent material) other than the conductive aid in the undercoat layer is, even if the electrode constituent material such as binder, thickener, dispersant, etc. in the electrode active material layer is not included or is only a small amount, it is difficult to inhibit the movement of lithium ions, so it is easy to make the reaction within the battery uniform, it is easy to extend the life of the battery, it is easy to improve the strength of the battery, even if a high load pressure is applied locally, cracks are unlikely to occur due to pressing during electrode production, etc. From the viewpoint, 0 to 95% by mass is preferable, 0 to 90% by mass is more preferable, and 0 to 85% by mass is even more preferable. In addition, when using multiple undercoat layer constituent materials (negative electrode undercoat layer constituent material or positive electrode undercoat layer constituent material) other than the conductive aid, it is preferable to adjust the total amount so that it is within the above range. In the undercoat layer, the total amount of the carbon nanotubes, the conductive additive other than the carbon nanotubes, and the undercoat layer constituent materials other than the conductive additive (total amount of the undercoat layer) is 100 mass %.

[0061] [1-1-3] Undercoat layer In the lithium ion secondary battery electrode (lithium ion secondary battery negative electrode or lithium ion secondary battery positive electrode) of the present invention, the thickness of the undercoat layer is preferably at least a certain thickness from the viewpoint of improving the strength of the battery and preventing cracks from occurring due to pressing during electrode production even when high load pressure is applied locally. On the other hand, even if the electrode constituent materials such as binder, thickener, dispersant, etc. in the electrode active material layer are not present or are present in only a small amount, it is difficult to inhibit the movement of lithium ions, making it easy to homogenize the reaction within the battery and extend the life of the battery. Therefore, the thickness of the undercoat layer in the lithium ion secondary battery electrode (lithium ion secondary battery negative electrode or lithium ion secondary battery positive electrode) of the present invention is preferably 0.1 to 10.0 μm, more preferably 0.5 to 7.0 μm, and even more preferably 1.0 to 5.0 μm. The undercoat layer is composed of a substance that inhibits the movement of lithium ions, but if it has the above thickness, it is easy to improve the strength of the battery, cracks are less likely to occur due to pressing or the like during electrode production, the undercoat layer and the electrode active material layer are less likely to peel off, and the effect on the uniformity of the reaction is negligible, making it easy to make the reaction uniform.

[0062] (1-2) Electrode Current Collectors The electrode current collectors (negative electrode current collector and positive electrode current collector) are not particularly limited, and current collectors that are normally used in lithium ion secondary batteries can be used.

[0063] The negative electrode current collector is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as copper, stainless steel, nickel, or a carbon material. This negative electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0064] The positive electrode current collector is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as aluminum, stainless steel, or a carbon material. This positive electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0065] (1-3) Electrode Active Material Layer Four preferred embodiments of the electrode active material layer will be described below in order.

[0066] [1-3-1] Electrode active material layer for lithium ion secondary battery (first embodiment) The electrode active material layer for lithium ion secondary battery according to the first embodiment is an electrode active material layer for lithium ion secondary battery containing an electrode active material and carbon nanotubes, and is preferably a negative electrode active material layer for lithium ion secondary battery, in which the content of the electrode active material is 97.4 to 99.9 mass %, the content of the carbon nanotubes is 0.01 to 1.4 mass %, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 1.2 mass %.

[0067] 1-3-1-1. Electrode active material The electrode active material (negative electrode active material) is not particularly limited, and any material that can be used as a negative electrode active material in a lithium ion secondary battery, that is, a material that can absorb and release lithium ions, can be used. Examples of such materials include carbon materials such as natural graphite, artificial graphite, and amorphous carbon; metal materials that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Si alloys, Sn alloys, and Al alloys; and SiO. x (0<x<2), SnO x (0<x<2), lithium titanium composite oxide (Li 2 TiO 3 Examples of the amorphous carbon include metal oxides capable of absorbing and releasing lithium ions, such as vanadium oxide; and composite materials containing a metal material and a carbon material, such as Si-C composites and Sn-C composites. The amorphous carbon may also be an amorphous carbon material, as described below. These electrode active materials (negative electrode active materials) may be used alone or in combination of two or more. Carbon materials, lithium titanium composite oxides, and the like may also be employed from the viewpoint of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge and particularly improving the charge and discharge cycle characteristics. In particular, when a conductive material such as a carbon material is used as the electrode active material (negative electrode active material), the electrode active material (negative electrode active material) also functions as a conductive additive, making it particularly easy to reduce the content of substances that inhibit the movement of lithium ions.

[0068] As for the electrode active material (negative electrode active material) as described above, from the viewpoint of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge, easily suppressing the capacity decrease due to the volume change, and particularly easily improving the charge and discharge cycle characteristics, it is preferable that the volume change of the electrode active material (negative electrode active material) during charge and discharge is 50% or less, preferably 20% or less. The smaller the volume change, the better, and no lower limit is set, but if a lower limit is set, it would be 0%. Note that this volume change value indicates the degree to which the electrode active material (negative electrode active material) at full charge has expanded compared to the electrode active material (negative electrode active material) at full discharge, and is calculated using the following formula: ((volume at full charge) - (volume at full discharge)) / (volume at full discharge) × 100.

[0069] Examples of electrode active materials (negative electrode active materials) that satisfy such volume changes include carbon materials such as natural graphite, artificial graphite, and amorphous carbon; lithium titanium composite oxide (Li 2 TiO 3 The volume change of these materials varies depending on the type of material and the depth of charge and discharge, but is around 10% in the case of graphite and a few percent in the case of amorphous carbon. In addition, when a plurality of electrode active materials (negative electrode active materials) are used, it is preferable that the average volume change of the electrode active materials (negative electrode active materials) be within the above range.

[0070] The shape of the electrode active material (negative electrode active material) is not particularly limited, and various shapes such as spherical, scale-like, block-like, fibrous, whisker-like, and crushed shapes can be used. Also, electrode active materials (negative electrode active materials) of multiple shapes can be used in combination. The spherical shape may be a perfect sphere or an elliptical shape.

[0071] The particle size of the electrode active material (negative electrode active material) is not particularly limited, but from the viewpoint of facilitating current collection between negative electrode active material particles with a small amount of carbon nanotubes and further extending the life of the battery, the average particle size is preferably 0.1 to 25 μm, more preferably 1 to 20 μm. Furthermore, in consideration of uniformity of the reaction at low temperatures, the average particle size of the electrode active material (negative electrode active material) can also be set to 0.1 to 13.0 μm, preferably 0.5 to 10.0 μm, and more preferably 1.0 to 8.0 μm. The average particle size of the negative electrode active material is measured by a laser diffraction / scattering method.

[0072] The electrode active material layer for a lithium ion secondary battery according to the first aspect uses a very small amount of carbon nanotubes to perform current collection between active material particles and maintain the shape of the electrode. This allows for a reduction in the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material). As a result, the layer is strong enough to maintain the shape of the electrode and is less likely to inhibit the movement of lithium ions, which allows for uniform reactions within the battery and extends the battery's life. Therefore, the electrode active material (negative electrode active material) content is higher than in current electrode active material layer forms (negative electrode active material layers). For this reason, the content of the negative electrode active material is preferably 97.4 to 99.9% by mass, more preferably 97.7 to 99.7% by mass, and even more preferably 98.0 to 99.5% by mass. When multiple electrode active materials (negative electrode active materials) are used, it is preferable to adjust their total amount to be within the above range. In the electrode active material layer for a lithium ion secondary battery according to the first embodiment, the total amount of the electrode active material (negative electrode active material), the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and the carbon nanotubes (total amount of the electrode active material layer) is 100 mass%.

[0073] 1-3-1-2. Carbon Nanotubes In the electrode active material layer for a lithium ion secondary battery according to the first aspect, a very small amount of carbon nanotubes facilitates current collection between active material particles and maintenance of the electrode shape, and the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) can be reduced. Since the movement of lithium ions is not easily hindered, the reaction within the battery can be made uniform and the battery life can be extended. Although carbon nanotubes are also a substance that hinders the movement of lithium ions, a small amount does not hinder the movement of lithium ions, meaning that the reaction within the battery can be kept uniform.

[0074] Carbon nanotubes are hollow carbon materials in which graphite sheets (i.e., carbon atom planes of a graphite structure or single-layer graphene sheets) are closed in a tubular shape, and their diameters are on the nanometer scale, with a graphite wall structure. Carbon nanotubes whose wall structure is a single graphite sheet (single-layer graphene sheet) and closed in a tubular shape are called single-walled carbon nanotubes. On the other hand, carbon nanotubes in which multiple graphite sheets are closed in a tubular shape and nested are called nested multi-layered carbon nanotubes. In the present invention, both single-walled carbon nanotubes and multi-layered carbon nanotubes can be used, but single-walled carbon nanotubes are preferred from the viewpoints of being strong enough to maintain the shape of an electrode, easily collecting current between electrode active materials (negative electrode active materials), and not easily inhibiting the movement of lithium ions, thereby facilitating uniform reactions within the battery and extending the battery's life.

[0075] Such carbon nanotubes can be used alone or in combination of two or more kinds.

[0076] A small average outer diameter of the carbon nanotubes is preferable from the viewpoints of easily increasing the number of carbon nanotubes per volume, reducing the carbon nanotube content required to maintain the shape of the electrode, and minimizing the inhibition of lithium ion migration. Therefore, the average outer diameter of the carbon nanotubes is preferably 0.43 to 20 nm, more preferably 0.43 to 10 nm. The average outer diameter of the carbon nanotubes is measured by observation with a transmission electron microscope (TEM). For carbon nanotubes having such an average outer diameter, the average inner diameter is set according to the average outer diameter.

[0077] The longer the average length of the carbon nanotubes, the more likely they are to have sufficient strength to maintain the shape of the electrode and to facilitate current collection between the negative electrode active materials. On the other hand, from the viewpoints of improving dispersibility and preventing the movement of lithium ions, a shorter average length of the carbon nanotubes is preferable. Therefore, the average length of the carbon nanotubes is preferably 0.5 to 200 μm, more preferably 1 to 50 μm. The average length of the carbon nanotubes is measured by observation with a scanning electron microscope (SEM).

[0078] The average aspect ratio of the carbon nanotubes, defined as the ratio of the average length to the average outer diameter of the carbon nanotubes, is preferably 25 to 200,000, more preferably 100 to 50,000, from the viewpoints that the higher the average aspect ratio, the easier it is to have a strength sufficient to maintain the shape of the electrode with a smaller carbon nanotube content, the easier it is to collect current between negative electrode active materials, and the less it is to inhibit the movement of lithium ions, making it easier to make the reaction within the battery uniform and making it easier to extend the life of the battery.

[0079] In the present invention, the carbon nanotubes may be either individual or bundled carbon nanotubes, which tend to exhibit strength as a bundle. In either case, a very small amount of carbon nanotubes can be used to collect current between active material particles and maintain the shape of the electrode, thereby reducing the amount of electrode constituent material (negative electrode constituent material) other than the electrode active material (negative electrode active material). As a result, the carbon nanotubes have sufficient strength to maintain the shape of the electrode and are less likely to inhibit the movement of lithium ions, which makes the reaction within the battery uniform and extends the battery's lifespan.

[0080] Furthermore, it is considered preferable that the graphene structure of the carbon nanotubes has few defects, i.e., a high G / D ratio in the Raman spectrum, from the viewpoint of easily suppressing the reactivity between the carbon nanotubes and the electrolyte solution. For this reason, in the present invention, the carbon nanotubes preferably have a G / D ratio in the Raman spectrum of 1 to 200, more preferably 50 to 150.

[0081] In the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the first aspect of the present invention, a very small amount of carbon nanotubes facilitates current collection between active material particles, maintains the shape of the electrode, and the amount of negative electrode constituent materials other than the electrode active material (negative electrode active material) can be easily reduced. As a result, the layer is strong enough to maintain the shape of the electrode and is less likely to inhibit the movement of lithium ions, which facilitates uniform reactions within the battery and extends the battery's life. Therefore, in the electrode active material layer for a lithium ion secondary battery according to the first aspect of the present invention, the carbon nanotube content is preferably 0.01 to 1.4% by mass, more preferably 0.1 to 1.2% by mass, and even more preferably 0.2 to 1.0% by mass. When multiple carbon nanotubes are used, it is preferable to adjust the total amount thereof to be within the above range. Although carbon nanotubes are also a substance that inhibits the migration of lithium ions, if the content is about 1.2 mass % or less, they are less likely to inhibit the migration of lithium ions and tend to have a strength sufficient to maintain the shape of the electrode while keeping the reaction in the battery uniform. In the electrode active material layer for a lithium ion secondary battery according to the first aspect of the present invention, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), carbon nanotubes, and electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and carbon nanotubes is 100 mass %.

[0082] 1-3-1-3. Electrode active material and electrode constituent materials other than carbon nanotubes In the electrode active material layer for a lithium ion secondary battery according to the first aspect of the present invention, the small amount of carbon nanotubes described above facilitates current collection between active material particles and maintenance of the electrode shape, and the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) can also be reduced. As a result, the layer is likely to have a strength sufficient to maintain the shape of the electrode and is unlikely to inhibit the movement of lithium ions, which makes it easy to make the reaction within the battery uniform and extend the life of the battery.

[0083] In the present invention, the electrode active material (negative electrode active material) and the electrode constituent material (negative electrode constituent material) other than carbon nanotubes are a general term that refers to substances (binders) that have adhesive properties with the electrode active material (negative electrode active material) and the electrode current collector (negative electrode current collector), as well as conductive additives other than carbon nanotubes, such as carbon black, and substances that inhibit the migration of lithium ions other than carbon nanotubes, such as dispersants (lithium ion migration inhibiting substances).

[0084] Examples of such electrode active materials (negative electrode active materials) and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes in the present invention include, for example, conductive additives such as acetylene black, ketjen black, carbon black, graphene, and amorphous carbon obtained by heat-treating organic materials, and binders, thickeners, or dispersants such as fluorine-based polymers (polyvinylidene fluoride resin, polytetrafluoroethylene resin, vinylidene fluoride-hexafluoropropylene copolymer, etc.), polyolefin resins (styrene butadiene copolymer resin, ethylene vinyl alcohol copolymer resin, etc.), synthetic rubbers (styrene butadiene rubber, acrylonitrile butadiene rubber, ethylene propylene diene rubber, etc.), polyacrylonitrile, polyamide, polyimide, polyacrylic acid, polyacrylic acid esters, polyvinyl ethers, carboxymethyl cellulose, carboxymethyl cellulose sodium salt, carboxymethyl cellulose ammonium, polyurethane, hydroxypropyl cellulose, hydroxyethyl cellulose, methyl cellulose, etc. As the amorphous carbon, amorphous carbon materials described below can also be used. These electrode active materials (negative electrode active materials) and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes can be used alone or in combination of two or more.

[0085] In the electrode active material layer for a lithium ion secondary battery according to the first aspect of the present invention, a very small amount of carbon nanotubes facilitates current collection between active material particles, maintenance of the electrode shape, and the like, and the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) can also be reduced. As a result, the layer is likely to have sufficient strength to maintain the electrode shape and is unlikely to inhibit the movement of lithium ions, which facilitates uniform reactions within the battery and a long battery life. Therefore, it is preferable that the layer does not contain any electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and carbon nanotubes, or if it does contain any, the amount is small. For this reason, in the electrode active material layer for a lithium ion secondary battery according to the first aspect of the present invention, the content of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and carbon nanotubes is preferably 0 to 1.2% by mass, more preferably 0.2 to 1.1% by mass, and even more preferably 0.4 to 1.0% by mass. When multiple electrode active materials (negative electrode active materials) and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes are used, it is preferable to adjust the total amount thereof to be within the above range. Although the electrode active materials (negative electrode active materials) and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes are substances that inhibit the migration of lithium ions, if the amount is about 1.2 mass% or less, they are less likely to inhibit the migration of lithium ions and tend to have sufficient strength to maintain the shape of the electrode while maintaining uniform reactions within the battery. In the negative electrode active material layer for a lithium ion secondary battery according to the first aspect, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), carbon nanotubes, and electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and carbon nanotubes is 100 mass%.

[0086] 1-3-1-4. Electrode active material layer for lithium ion secondary battery The electrode active material layer for lithium ion secondary battery (negative electrode active material layer for lithium ion secondary battery) of the present invention contains the above-mentioned electrode active material (negative electrode active material), carbon nanotubes, and an electrode constituent material (negative electrode constituent material) other than the electrode active material (negative electrode active material) and carbon nanotubes.

[0087] The thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is not particularly limited, but while a thinner layer is preferable in terms of ensuring lithium ion penetration and electrical conductivity and facilitating uniform reaction, the present invention aims to reduce factors that inhibit lithium ion migration to uniformize the battery reaction and improve the battery life, so a thicker layer is also possible in terms of energy density per electrode. For this reason, the thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm.

[0088] [1-3-2] Electrode Active Material Layer for Lithium-Ion Secondary Battery (Second Aspect) The electrode active material layer for a lithium-ion secondary battery according to the second aspect of the present invention is an electrode active material layer for a lithium-ion secondary battery containing an electrode active material and carbon nanotubes, wherein the electrode active material has an average particle size of 0.1 to 13.0 μm and is contained in an amount of 96.6 to 99.9 mass %, the carbon nanotube content is 0.01 to 1.4 mass %, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 2.0 mass %, forming a negative electrode active material layer for a lithium-ion secondary battery. Note that in the electrode active material layer for a lithium-ion secondary battery according to the second aspect of the present invention, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and the carbon nanotubes is 100 mass %.

[0089] When the particle size of the electrode active material (negative electrode active material) is reduced, the number of interfaces between the electrode active material (negative electrode active material) particles increases, resulting in an increase in the number of starting points for structural collapse. Therefore, in the past, it was even more difficult to significantly reduce the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material). In the second aspect, by adopting the configuration described above, even though the particle size of the electrode active material (negative electrode active material) is reduced, the number of interfaces between the electrode active material (negative electrode active material) particles increases, resulting in an increase in the number of starting points for structural collapse, even if the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is significantly reduced, a very small amount of carbon nanotubes facilitates current collection between the electrode active material (negative electrode active material) particles, maintains the shape of the electrode, and the like, and makes it easy to maintain the strength sufficient to maintain the shape of the electrode. Furthermore, since the particle size of the electrode active material (negative electrode active material) is reduced to increase the reaction area, the lithium ion flux per unit area is reduced, and the risk of lithium precipitation is reduced, particularly under high load conditions or long-term use. In addition, the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is significantly reduced, which makes it easy to significantly improve life characteristics. In other words, the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second aspect can be used to reduce uneven reaction in a lithium ion secondary battery.

[0090] 1-3-2-1. Electrode active material The electrode active material (negative electrode active material) is not particularly limited, and any material that can be used as an electrode active material (negative electrode active material) in a lithium ion secondary battery, that is, a material that can absorb and release lithium ions, can be used. Examples of such materials include carbon materials such as natural graphite, artificial graphite, and amorphous carbon; metal materials that can be alloyed with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Si alloys, Sn alloys, and Al alloys; SiO x (0<x<2), SnO x (0<x<2), e Lithium titanium composite oxide (Li 2 TiO 3Examples of the amorphous carbon include metal oxides capable of absorbing and releasing lithium ions, such as vanadium oxide; and composite materials containing a metal material and a carbon material, such as Si-C composites and Sn-C composites. The amorphous carbon may also be an amorphous carbon material, as described below. These electrode active materials (negative electrode active materials) may be used alone or in combination of two or more. In particular, when a conductive material, such as a carbon material, is used as the electrode active material (negative electrode active material), the electrode active material (negative electrode active material) also functions as a conductive additive, making it particularly easy to reduce the content of substances that inhibit the movement of lithium ions.

[0091] The shape of the electrode active material (negative electrode active material) is not particularly limited, and various shapes such as spherical, scale-like, block-like, fibrous, whisker-like, and crushed shapes can be used. Also, electrode active materials (negative electrode active materials) of multiple shapes can be used in combination. The spherical shape may be a perfect sphere or an elliptical shape.

[0092] The average particle size of the electrode active material (negative electrode active material) is 0.1 to 13.0 μm, preferably 0.5 to 10.0 μm, and more preferably 1.0 to 8.0 μm. If the average particle size of the electrode active material (negative electrode active material) is less than 0.1 μm, aggregation is unavoidable, which increases the lithium ion flux per unit area and tends to deteriorate the life characteristics. On the other hand, if the average particle size of the electrode active material (negative electrode active material) exceeds 13.0 μm, there is room for improvement in uniformity of the reaction, especially at low temperatures. The average particle size of the negative electrode active material is measured by a laser diffraction / scattering method.

[0093] As for the electrode active material (negative electrode active material) as described above, from the viewpoint of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge, easily suppressing the capacity decrease due to the volume change, and particularly easily improving the charge and discharge cycle characteristics, it is preferable that the volume change of the electrode active material (negative electrode active material) during charge and discharge is 50% or less, preferably 20% or less. The smaller the volume change, the better, and no lower limit is set, but if a lower limit is set, it would be 0%. Note that this volume change value indicates the degree to which the electrode active material (negative electrode active material) at full charge has expanded compared to the electrode active material (negative electrode active material) at full discharge, and is calculated using the following formula: ((volume at full charge) - (volume at full discharge)) / (volume at full discharge) × 100.

[0094] Examples of electrode active materials (negative electrode active materials) that satisfy such volume changes include carbon materials such as natural graphite, artificial graphite, and amorphous carbon; lithium titanium composite oxide (Li 2 TiO 3 The volume change of these materials varies depending on the type of material and the depth of charge and discharge, but is around 10% in the case of graphite and a few percent in the case of amorphous carbon. In addition, when a plurality of electrode active materials (negative electrode active materials) are used, it is preferable that the average volume change of the electrode active materials (negative electrode active materials) be within the above range.

[0095] In the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second aspect, the electrode active material (negative electrode active material) has a small particle size, which increases the number of interfaces between electrode active material (negative electrode active material) particles and increases the number of starting points for structural collapse. However, even if the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is significantly reduced, a small amount of carbon nanotubes facilitates current collection between electrode active material (negative electrode active material) particles and electrode shape maintenance, etc., and as a result, the electrode (negative electrode) is likely to retain sufficient strength to maintain its shape. Furthermore, because the particle size of the electrode active material (negative electrode active material) is reduced and the reaction area is increased, the lithium ion flux per unit area is reduced, which tends to reduce the risk of lithium precipitation, particularly under high load conditions and long-term use. Furthermore, because the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is significantly reduced, the life characteristics are likely to be significantly improved. For this reason, the electrode active material layer for a lithium ion secondary battery according to the second aspect (negative electrode active material layer for a lithium ion secondary battery) has a higher content of electrode active material (negative electrode active material) compared to current electrode active material layers (negative electrode active material layers). Therefore, in the electrode active material layer for a lithium ion secondary battery (part 1) according to the second aspect, the content of the electrode active material (negative electrode active material) is 96.6 to 99.9 mass%, preferably 97.6 to 99.8 mass%, and more preferably 98.2 to 99.7 mass%. When multiple electrode active materials (negative electrode active materials) are used, it is preferable to adjust the total amount thereof to be within the above range. In the electrode active material layer for a lithium ion secondary battery according to the second aspect, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), carbon nanotubes, and electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and the carbon nanotubes is 100 mass%.

[0096] 1-3-2-2. Carbon nanotubes In the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second aspect, a very small amount of carbon nanotubes facilitates current collection between active material particles and maintenance of the electrode shape. As a result, the electrode (negative electrode) is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) even when the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced, even though the number of interfaces between electrode active material (negative electrode active material) particles is increased due to the small particle size of the electrode active material (negative electrode active material), which increases the number of starting points for structural collapse. In addition, the small particle size of the electrode active material (negative electrode active material) increases the reaction area, thereby reducing the lithium ion flux per unit area and reducing the risk of lithium precipitation, particularly under high load conditions or long-term use. In addition, the significant reduction in the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) tends to significantly improve life characteristics. Although carbon nanotubes are also a substance that inhibits the movement of lithium ions, in small amounts they do not inhibit the movement of lithium ions, meaning that they tend to be strong enough to maintain the shape of the electrode (negative electrode) while keeping the reaction within the battery uniform.

[0097] The carbon nanotubes that can be used are the same as those explained in 1-3-2-1 above.

[0098] In the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second aspect, a very small amount of carbon nanotubes facilitates current collection between electrode active material (negative electrode active material) particles, maintenance of the shape of the electrode, and the like. As a result, even if the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced, the electrode active material layer for a lithium ion secondary battery according to the second aspect is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) even if the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced, despite the fact that the number of interfaces between electrode active material (negative electrode active material) particles is increased due to the small particle size of the electrode active material (negative electrode active material), which increases the number of starting points for structural collapse. In addition, the lithium ion flux per unit area is reduced because the particle size of the electrode active material (negative electrode active material) is reduced and the reaction area is increased, thereby reducing the risk of lithium precipitation, particularly under high load conditions or during long-term use. In addition, the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is significantly reduced, which makes it easy to significantly improve life characteristics. For this reason, the content of carbon nanotubes in the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second embodiment is small. For this reason, in the electrode active material layer for a lithium ion secondary battery according to the second embodiment, the content of carbon nanotubes is 0.01 to 1.4 mass%, preferably 0.1 to 1.2 mass%, and more preferably 0.2 to 1.0 mass%. When a plurality of carbon nanotubes is used, it is preferable to adjust the total amount thereof to be within the above range. Although carbon nanotubes also inhibit the migration of lithium ions, a content of about 1.4 mass% or less is less likely to inhibit the migration of lithium ions, coupled with the small particle size of the electrode active material (negative electrode active material). Furthermore, the electrode active material (negative electrode active material) is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) while maintaining uniform reaction within the battery, despite the small particle size of the electrode active material (negative electrode active material). In the electrode active material layer for a lithium ion secondary battery according to the second embodiment, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and the carbon nanotubes is 100 mass%.

[0099] 1-3-2-3. Electrode active material and electrode constituent materials other than carbon nanotubes In the electrode active material layer for a lithium ion secondary battery according to the second aspect (negative electrode active material layer for a lithium ion secondary battery), a very small amount of carbon nanotubes facilitates current collection between active material particles and maintenance of the electrode shape. As a result, the electrode (negative electrode) is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) even when the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced, even though the number of interfaces between electrode active material (negative electrode active material) particles is increased due to the small particle size of the electrode active material (negative electrode active material), which increases the number of starting points for structural collapse. In addition, the electrode active material layer according to the second aspect (negative electrode active material layer) is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) even when the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced. In addition, the small particle size of the electrode active material (negative electrode active material) increases the reaction area, which reduces the lithium ion flux per unit area, which tends to reduce the risk of lithium precipitation, particularly under high load conditions and long-term use. In addition, the significant reduction in the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) tends to significantly improve life characteristics.

[0100] In the present invention, the electrode constituent material (negative electrode constituent material) and the electrode constituent material (negative electrode constituent material) other than carbon nanotubes may be the same as those explained in 1-3-1-3 above.

[0101] The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the second aspect of the present invention utilizes a very small amount of carbon nanotubes to facilitate current collection between active material particles and maintain the shape of the electrode. As a result, the electrode (negative electrode) is strong enough to maintain its shape even when the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) is reduced, even though the small particle size of the electrode active material (negative electrode active material) increases the number of interfaces between the electrode active material (negative electrode active material) particles, which increases the number of starting points for structural collapse. Furthermore, the small particle size of the electrode active material (negative electrode active material) increases the reactive area, thereby reducing the lithium ion flux per unit area, which tends to reduce the risk of lithium precipitation, particularly under high load conditions or long-term use. Furthermore, the significant reduction in the amount of electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) significantly improves the life characteristics. Therefore, the electrode active material layer does not contain any electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) or, if any, only a small amount of such materials is contained. For this reason, in the electrode active material layer for a lithium ion secondary battery according to the second aspect, the content of the electrode active material (negative electrode active material) and the electrode constituent material (negative electrode constituent material) other than carbon nanotubes is 0 to 2.0% by mass, preferably 0 to 1.2% by mass, and more preferably 0 to 0.8% by mass. When using a plurality of electrode active materials (negative electrode active materials) and electrode constituent materials (negative electrode constituent materials) other than carbon nanotubes, it is preferable to adjust the total content thereof to be within the above range. Although the electrode active material (negative electrode active material) and the electrode constituent material (negative electrode constituent material) other than carbon nanotubes are substances that inhibit the migration of lithium ions, if the content is about 2.0% by mass or less, the migration of lithium ions is less likely to be inhibited, coupled with the small particle size of the electrode active material (negative electrode active material). Furthermore, despite the small particle size of the electrode active material (negative electrode active material), the electrode (negative electrode) is likely to have sufficient strength to maintain the shape of the electrode (negative electrode) while maintaining a uniform reaction within the battery. In the electrode active material layer for a lithium ion secondary battery according to the second embodiment, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) other than the electrode active material (negative electrode active material) and the carbon nanotubes is 100 mass%.

[0102] 1-3-2-4. Electrode active material layer for lithium ion secondary battery The electrode active material layer for lithium ion secondary battery (negative electrode active material layer for lithium ion secondary battery) of the present invention contains the above-mentioned electrode active material (negative electrode active material), carbon nanotubes, and an electrode constituent material (negative electrode constituent material) other than the electrode active material (negative electrode active material) and carbon nanotubes.

[0103] The thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is not particularly limited, but while a thinner layer is preferable in terms of ensuring lithium ion penetration and electrical conductivity and facilitating uniform reaction, the present invention aims to reduce factors that inhibit lithium ion migration to uniformize the battery reaction and improve the battery life, so a thicker layer is also possible in terms of energy density per electrode. For this reason, the thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm.

[0104] [1-3-3] Electrode Active Material Layer for Lithium-Ion Secondary Battery (Third Aspect) The electrode active material layer for lithium-ion secondary batteries according to the third aspect of the present invention is an electrode active material layer for lithium-ion secondary batteries containing an electrode active material and carbon nanotubes, wherein the electrode active material content is 88.6 to 99.9 mass%, the carbon nanotube content is 0.01 to 1.4 mass%, and the content of a conductive additive other than carbon nanotubes is 0 to 10.0 mass%, and the composition does not contain any electrode constituent materials other than the electrode active material, the carbon nanotubes, and the conductive additive other than carbon nanotubes, and is a positive electrode active material layer-forming composition for lithium-ion secondary batteries. Note that in the electrode active material layer for lithium-ion secondary batteries according to the third aspect, the total amount of the electrode active material (positive electrode active material), the carbon nanotubes, and the electrode active material (positive electrode active material) and the conductive additive other than carbon nanotubes (total amount of the electrode active material layer for lithium-ion secondary batteries) is 100 mass%.

[0105] By adopting such a configuration, it is easy to maintain the strength sufficient to maintain the shape of the electrode (positive electrode), and since the amount of the lithium ion inhibitor is reduced, it is easy to suppress the inhibition of the movement of lithium ions, and as a result, it is easy to make the reaction in the battery uniform and to extend the life of the battery. In other words, the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect can be used to reduce uneven distribution of the reaction in a lithium ion secondary battery.

[0106] 1-3-3-1. Electrode active material The electrode active material (positive electrode active material) is not particularly limited, and any material that can be used as an electrode active material (positive electrode active material) in a lithium ion secondary battery, that is, a material that can absorb and release lithium ions, can be used. For example, α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel-type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x1 Ni γ1 Mn β1 Co(1-x1-γ1-β1)]O 2 (0≦x1<0.5, 0≦γ1≦1, 0≦β1≦1, 0≦γ1+β1≦1), Li[Li x2 Ni γ2 Co β2 Al(1-x2-γ2-β2)]O 2 (0≦x2<0.5, 0≦γ2≦1, 0≦β2≦1, 0≦γ2+β2≦1). Examples of lithium transition metal oxides having a spinel crystal structure include Li x3 Mn 2 O 4 (0.9≦x3<1.5), Li x4 Ni γ4 Mn (2-γ4) O 4 (0.9≦x4<1.5, 0≦γ4≦2) and the like. Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 Examples of the chalcogen compound include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. The atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. These electrode active materials (positive electrode active materials) can be used alone or in combination of two or more. Among these, the lithium transition metal composite oxides are preferred as the electrode active material (positive electrode active material) from the viewpoint of achieving high energy density, and polyanion compounds are preferred from the viewpoint of achieving high safety.

[0107] The particle form of the electrode active material (positive electrode active material) is not particularly limited, and various forms such as secondary particles and single particles can be used. The shape is also not particularly limited, and various forms such as spherical, scale-like, block-like, fibrous, whisker-like, and crushed can be used. Positive electrode active materials of multiple shapes can also be used in combination. Note that the spherical form may be a perfect sphere or an elliptical form.

[0108] The particle size of the electrode active material (cathode active material) is not particularly limited, but from the viewpoint of facilitating current collection between electrode active material (cathode active material) particles with a small amount of carbon nanotubes and further extending the life of the battery, the average particle size is preferably 0.1 to 25 μm, more preferably 1 to 20 μm. Furthermore, in consideration of uniformity of the reaction at low temperatures, the average particle size of the electrode active material (cathode active material) can be set to 0.1 to 13.0 μm, preferably 0.5 to 10.0 μm, and more preferably 1.0 to 8.0 μm. The average particle size of the electrode active material (cathode active material) is measured by a laser diffraction / scattering method.

[0109] The electrode active material layer for a lithium ion secondary battery according to the third aspect (positive electrode active material layer for a lithium ion secondary battery) uses a very small amount of carbon nanotubes to facilitate current collection between active material particles and maintaining the shape of the electrode (positive electrode). Therefore, by not including any electrode constituent material (positive electrode constituent material) other than the conductive additive, the amount of electrode constituent material (positive electrode constituent material) other than the electrode active material (positive electrode active material) can also be reduced. As a result, the electrode (positive electrode) is likely to have sufficient strength to maintain its shape, and is unlikely to inhibit the movement of lithium ions, which makes it easy to uniformize the reaction within the battery and extend the battery's life. Therefore, compared to current electrode active material layers (positive electrode active material layers), the electrode active material (positive electrode active material) content is higher. Therefore, in the electrode active material layer for a lithium ion secondary battery according to the third aspect, the electrode active material (positive electrode active material) content is 88.6 to 99.9% by mass, preferably 90.8 to 98.4% by mass, and more preferably 93.0 to 97.8% by mass. In the case where a plurality of electrode active materials (positive electrode active materials) are used, it is preferable to adjust the total amount thereof to be within the above range. In the positive electrode active material layer for a lithium ion secondary battery according to the third aspect, the total amount of the electrode active materials (positive electrode active materials), the carbon nanotubes, and the conductive additive other than the carbon nanotubes (total amount of the composition) is 100 mass%.

[0110] 1-3-3-2. Carbon Nanotubes The electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) of the present invention facilitates current collection between active material particles and maintaining the shape of the electrode (positive electrode) with a very small amount of carbon nanotubes. Therefore, since it does not contain any electrode constituent materials (positive electrode constituent materials) other than the conductive additive, the amount of electrode constituent materials (positive electrode constituent materials) other than the electrode active material (positive electrode active material) can also be reduced. As a result, it is easy to maintain the shape of the electrode (positive electrode) and is less likely to inhibit the movement of lithium ions, which makes it easy to homogenize the reaction within the battery and extend the life of the battery. Although carbon nanotubes are also a substance that inhibits the movement of lithium ions, in small amounts they do not inhibit the movement of lithium ions, meaning that they are easy to maintain the shape of the electrode (positive electrode) while maintaining the reaction within the battery homogenously.

[0111] The carbon nanotubes that can be used are the same as those explained in 1-3-1-2 above.

[0112] The electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect of the present invention uses only a small amount of carbon nanotubes to facilitate current collection between electrode active material (positive electrode active material) particles and to maintain the shape of the electrode (positive electrode). Therefore, the layer does not contain any electrode constituent materials (positive electrode constituent materials) other than the conductive additive, and the amount of electrode constituent materials (positive electrode constituent materials) other than the electrode active material (positive electrode active material) can also be reduced. As a result, the layer is strong enough to maintain the shape of the electrode (positive electrode) and is less likely to inhibit the movement of lithium ions, which facilitates uniform reactions within the battery and extends the battery's life. Therefore, in the electrode active material layer for a lithium ion secondary battery according to the third aspect of the present invention, the carbon nanotube content is 0.01 to 1.4% by mass, preferably 0.1 to 1.2% by mass, and more preferably 0.2 to 1.0% by mass. When multiple carbon nanotubes are used, it is preferable to adjust the total amount to be within the above range. Although carbon nanotubes are also a substance that inhibits the migration of lithium ions, if the content is about 1.4 mass % or less, they are less likely to inhibit the migration of lithium ions and tend to have a strength sufficient to maintain the shape of the electrode (positive electrode) while keeping the reaction in the battery uniform. Note that in the electrode active material layer for a lithium ion secondary battery according to the third aspect, the total amount (total amount of the composition) of the electrode active material (positive electrode active material), the carbon nanotubes, and the conductive additive other than the carbon nanotubes is 100 mass %.

[0113] 1-3-3-3. Conductive Aids Other Than Carbon Nanotubes In the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect, a very small amount of carbon nanotubes is used to facilitate current collection between electrode active materials (positive electrode active materials) and maintenance of the shape of the electrode (positive electrode), and as a result, the layer does not contain any electrode constituent materials (positive electrode constituent materials) other than the conductive aid, and the amount of electrode constituent materials (positive electrode constituent materials) other than the electrode active material (positive electrode active material) can also be reduced. As a result, the layer is likely to have sufficient strength to maintain the shape of the electrode (positive electrode) and is unlikely to inhibit the movement of lithium ions, which makes it easier to uniformize the reaction within the battery and extend the life of the battery.

[0114] However, depending on the particle form, particle diameter, particle shape, and electronic conductivity of the electrode active material (cathode active material), it is also possible to include a certain amount of a conductive additive in addition to a very small amount of carbon nanotubes in the electrode active material layer for a lithium ion secondary battery according to the third aspect (cathode active material layer), from the viewpoint of easily maintaining current collection between particles of the electrode active material (cathode active material). For example, when a lithium transition metal composite oxide in the form of secondary particles is used as the electrode active material (cathode active material), it is preferable to include a certain amount of a conductive additive in addition to carbon nanotubes.

[0115] Examples of conductive additives other than carbon nanotubes in the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect include carbon blacks such as acetylene black, furnace black, and ketjen black; flake graphite; graphene; and amorphous carbon obtained by heat-treating an organic material. These conductive additives other than carbon nanotubes can be used alone or in combination of two or more. Among these, carbon black is preferred from the viewpoints that it is less likely to inhibit the movement of lithium ions, makes it easier to make the reaction in the battery uniform, and makes it easier to extend the life of the battery.

[0116] In the electrode active material layer for a lithium ion secondary battery according to the third aspect, the content of the conductive additive other than carbon nanotubes is 0 to 10.0% by mass, preferably 1.0 to 8.0% by mass, and more preferably 2.0 to 6.0% by mass, from the viewpoints of not inhibiting lithium ion migration, facilitating uniform reactions within the battery, and prolonging the battery's life. When multiple conductive additives other than carbon nanotubes are used, it is preferable to adjust their total amount to be within the above range. In the electrode active material layer for a lithium ion secondary battery according to the third aspect, the total amount of the electrode active material (positive electrode active material), carbon nanotubes, and conductive additives other than carbon nanotubes (total amount of the electrode active material layer) is 100% by mass.

[0117] 1-3-3-4. Electrode Constituent Materials Excluding Electrode Active Material, Carbon Nanotubes, and Conductive Aids Other Than Carbon Nanotubes The electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect uses a very small amount of carbon nanotubes to facilitate current collection between electrode active material (positive electrode active material) particles and to maintain the shape of the electrode (positive electrode). As a result, the layer does not contain any electrode constituent materials (positive electrode constituent materials) other than the electrode active material (cathode active material) and the conductive aid, and the amount of electrode constituent materials (positive electrode constituent materials) other than the electrode active material (cathode active material) can also be reduced. As a result, the layer is likely to have sufficient strength to maintain the shape of the electrode (positive electrode) and is unlikely to inhibit the movement of lithium ions, which makes it easy to uniformize the reaction within the battery and extend the battery's lifespan.

[0118] Conventional electrode active material layers for lithium ion secondary batteries (positive electrode active material layers for lithium ion secondary batteries) typically contain, in addition to an electrode active material (positive electrode active material) and a conductive additive, some substances that inhibit the migration of lithium ions (lithium ion migration inhibiting substances), such as substances (binders) that have adhesive properties with the electrode active material (positive electrode active material) and the electrode current collector (positive electrode current collector), thickeners, dispersants, etc.

[0119] In contrast, the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) according to the third aspect can easily perform current collection between electrode active material (positive electrode active material) particles and maintain the shape of the electrode (positive electrode) by using a very small amount of carbon nanotubes, and as a result, as described above, it is possible to have a configuration that does not include any electrode constituent material (positive electrode constituent material) other than the conductive additive.

[0120]

[0063] Examples of other target electrode constituent materials (positive electrode constituent materials) that are not contained in the electrode active material layer for a lithium ion secondary battery according to the third aspect (positive electrode active material layer for a lithium ion secondary battery) include, for example, binders, thickeners, or dispersants, such as fluorine-based polymers (polyvinylidene fluoride resin, polytetrafluoroethylene resin, vinylidene fluoride-hexafluoropropylene copolymer, etc.), polyolefin-based resins (styrene-butadiene copolymer resin, ethylene-vinyl alcohol copolymer resin, etc.), synthetic rubbers (styrene-butadiene rubber, acrylonitrile-butadiene rubber, ethylene-propylene-diene rubber, etc.), polyacrylonitrile, polyamide, polyimide, polyacrylic acid, polyacrylic acid esters, polyvinyl ethers, carboxymethyl cellulose, carboxymethyl cellulose sodium salt, carboxymethyl cellulose ammonium, polyurethane, hydroxypropyl cellulose, hydroxyethyl cellulose, and methyl cellulose.

[0121] 1-3-3-5. Electrode active material layer for lithium ion secondary battery The electrode active material layer for lithium ion secondary battery of the present invention (positive electrode active material layer for lithium ion secondary battery) contains the above-mentioned electrode active material (positive electrode active material), carbon nanotubes, and a conductive additive other than carbon nanotubes, but does not contain any electrode constituent materials other than the electrode active material (positive electrode active material), carbon nanotubes, and a conductive additive other than carbon nanotubes.

[0122] The thickness of the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) of the present invention is not particularly limited, but while a thinner layer is preferable in terms of ensuring lithium ion penetration and electrical conductivity and facilitating a uniform reaction, the present invention aims to reduce factors that inhibit lithium ion migration, uniformize the battery reaction, and improve the battery life, so a thicker layer is also possible in terms of the energy density per electrode. For this reason, the thickness of the electrode active material layer for a lithium ion secondary battery (positive electrode active material layer for a lithium ion secondary battery) of the present invention is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm.

[0123] [1-3-4] Electrode active material layer for lithium ion secondary battery (fourth aspect) The electrode active material layer for lithium ion secondary battery according to the fourth aspect is an electrode active material layer for lithium ion secondary battery containing an electrode active material and carbon nanotubes, wherein the electrode active material contains an amorphous carbon material, and the content of the carbon nanotubes is 0.01 to 0.8 mass % relative to 100 mass % of the total amount of the composition, and the electrode active material layer is a negative electrode active material layer for lithium ion secondary battery.

[0124] Amorphous carbon materials have low electronic conductivity compared to graphite materials, so forming a uniform electron conduction path is necessary to maintain uniform reactions within the battery. On the other hand, when using a conductive additive with a small aspect ratio, such as carbon black, a large amount of conductive additive is required to form the electron conduction path, which may inhibit lithium ion migration. On the other hand, carbon nanotubes with a high aspect ratio can form a uniform electron conduction path with a small amount. Thus, by combining an amorphous carbon material and carbon nanotubes, a uniform electron conduction path is formed while suppressing inhibition of lithium ion migration, which facilitates uniform reactions within the battery. Furthermore, although carbon nanotubes can inhibit lithium ion migration, the carbon nanotube content in the present invention is extremely small, which facilitates uniform reactions within the battery and, due to the synergistic effect with the amorphous carbon material, facilitates battery life extension. In other words, the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect can be used to reduce uneven reaction distribution in a lithium ion secondary battery.

[0125] 1-3-4-1. Electrode Active Material As the amorphous carbon material used as the electrode active material (negative electrode active material), an amorphous layered carbon material is preferred from the viewpoint of easily making the reaction in the battery uniform and easily extending the battery life.

[0126] The interlayer distance of the (002) plane of the amorphous layered carbon material is preferably 0.35 nm or more, more preferably 0.36 nm or more, from the viewpoint of easily making the reaction in the battery uniform and easily extending the battery life. The upper limit of the interlayer distance of the (002) plane of the amorphous layered carbon material is not particularly limited, but is usually 0.40 nm. The interlayer distance of the amorphous layered carbon material is measured by X-ray diffraction.

[0127] The average particle size of the amorphous layered carbon material is preferably 1 to 10 μm, more preferably 3 to 8 μm, from the viewpoint of facilitating uniform reaction within the battery and extending the battery life. The average particle size of the amorphous layered carbon material is measured by a laser diffraction / scattering method.

[0128] Examples of amorphous carbon materials that satisfy the above conditions include hard carbon (non-graphitizable carbon material), soft carbon (easily graphitizable carbon material), and mesophase pitch carbide. These amorphous carbon materials can be used alone or in combination of two or more. Among them, hard carbon is preferred from the viewpoint of easily making the reaction in the battery uniform and easily extending the battery life. In the present invention, hard carbon refers to an amorphous carbon material in which the interlayer distance of the (002) plane does not become less than 0.34 nm when fired at 3000°C. Soft carbon refers to an amorphous carbon material in which the interlayer distance of the (002) plane becomes less than 0.34 nm when fired at 3000°C.

[0129] The shape of the electrode active material (negative electrode active material) is not particularly limited, and various shapes such as spherical, scale-like, block-like, fibrous, whisker-like, and crushed shapes can be used. Also, electrode active materials (negative electrode active materials) of multiple shapes can be used in combination. The spherical shape may be a perfect sphere or an elliptical shape.

[0130] The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material) and a trace amount of carbon nanotubes. This suppresses the inhibition of lithium ion migration while forming a uniform electron conduction path, thereby facilitating uniform reactions within the battery and increasing the battery's lifespan. In the present invention, the content of the electrode active material (negative electrode active material) is preferably 79.2 to 99.8% by mass, more preferably 83.5 to 96.4% by mass, and even more preferably 77.8 to 94.9% by mass. When multiple electrode active materials (negative electrode active materials) are used, it is preferable to adjust the total amount thereof to be within the above range. In the electrode active material layer for a lithium ion secondary battery according to the fourth aspect (negative electrode active material layer for a lithium ion secondary battery), the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, the conductive additive other than the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) excluding the electrode active material (negative electrode active material), the carbon nanotubes, and the conductive additive other than the carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is 100 mass%.

[0131] 1-3-4-2. Carbon Nanotubes The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material) and uses a trace amount of carbon nanotubes, which suppresses the inhibition of lithium ion migration and forms a uniform electron conduction path, making it easier to make the reaction within the battery uniform and to extend the battery's life. Although carbon nanotubes are also a substance that inhibits the migration of lithium ions, a small amount does not inhibit the migration of lithium ions, which means that it is easier to make the reaction within the battery uniform and to extend the battery's life.

[0132] The carbon nanotubes that can be used are the same as those explained in 1-3-1-2 above.

[0133] The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material). By using a trace amount of carbon nanotubes, inhibition of lithium ion migration is suppressed while forming a uniform electron conduction path, which facilitates uniform reactions within the battery and extends the battery's life. Therefore, the carbon nanotube content is small. Therefore, in the present invention, the carbon nanotube content is 0.01 to 0.8% by mass, preferably 0.02 to 0.5% by mass, and more preferably 0.05 to 0.2% by mass. When multiple carbon nanotubes are used, it is preferable to adjust the total amount so that it falls within the above range. Although carbon nanotubes also inhibit lithium ion migration, a content of approximately 0.8% by mass or less is less likely to inhibit lithium ion migration, making it easier to maintain uniform reactions within the battery. In the electrode active material layer for a lithium ion secondary battery according to the fourth aspect (negative electrode active material layer for a lithium ion secondary battery), the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, the conductive additive other than the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) excluding the electrode active material (negative electrode active material), the carbon nanotubes, and the conductive additive other than the carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is 100 mass%.

[0134] 1-3-4-3. Conductive Aids Other Than Carbon Nanotubes The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material) and uses a very small amount of carbon nanotubes, which suppresses the inhibition of lithium ion migration and forms a uniform electron conduction path, making it easier to make the reaction within the battery uniform and to extend the battery's lifespan.

[0135] However, in the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect, it is possible to contain a certain amount of a conductive additive in addition to a very small amount of carbon nanotubes, from the viewpoint of easily maintaining current collection between particles of the electrode active material (negative electrode active material), depending on the particle form, particle diameter, particle shape, and electronic conductivity of the amorphous carbon material. For example, when an amorphous carbon material having spherical particle shape is used as the electrode active material (negative electrode active material), it is preferable to contain a certain amount of a conductive additive in addition to carbon nanotubes.

[0136] Usable conductive additives other than carbon nanotubes may be the same as those explained in 1-3-3-3 above.

[0137] In the present invention, when a conductive additive other than carbon nanotubes is contained, the content of the conductive additive other than carbon nanotubes is preferably 0.1 to 10.0 mass%, more preferably 1.0 to 8.0 mass%, and even more preferably 2.0 to 6.0 mass%, from the viewpoint of easily uniforming the reaction in the battery and easily extending the battery life. When multiple conductive additives other than carbon nanotubes are used, it is preferable to adjust the total amount thereof to be within the above range. In the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect, the total amount (total amount of the composition) of the electrode active material (negative electrode active material), carbon nanotubes, conductive additives other than carbon nanotubes, and electrode constituent materials (negative electrode constituent materials) excluding the electrode active material (negative electrode active material), carbon nanotubes, and conductive additives other than carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is 100 mass%.

[0138] For the same reason, the content of carbon nanotubes is preferably 0.1 to 100.0% by mass, more preferably 0.5 to 50% by mass, and even more preferably 1.0 to 20.0% by mass, where the total amount of carbon nanotubes and conductive additives other than carbon nanotubes is 100% by mass. When multiple conductive additives other than carbon nanotubes are used, it is preferable to adjust the total amount so that it is within the above range.

[0139] 1-3-4-4. Electrode Constituent Materials (Other Electrode Constituent Materials) Excluding Electrode Active Material, Carbon Nanotubes, and Conductive Aids Other Than Carbon Nanotubes The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material) and uses a very small amount of carbon nanotubes, thereby forming a uniform electron conduction path while suppressing inhibition of lithium ion migration, which makes it easier to make the reaction within the battery uniform and to extend the battery's lifespan.

[0140] In the present invention, the electrode active material (negative electrode active material), electrode constituent materials (negative electrode constituent materials) excluding carbon nanotubes and conductive additives other than carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is a general term for substances that inhibit the migration of lithium ions (lithium ion migration inhibiting substances), excluding carbon nanotubes and conductive additives other than carbon nanotubes, such as substances (binders) and dispersants that have adhesive properties with the electrode active material (negative electrode active material) and the electrode current collector (negative electrode current collector).

[0141] The usable electrode active material (negative electrode active material), electrode constituent materials (negative electrode constituent materials) excluding carbon nanotubes and conductive additives other than carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) can be the same as those described in 1-3-3-4 above. The electrode active material (negative electrode active material), electrode constituent materials (negative electrode constituent materials) excluding carbon nanotubes and conductive additives other than carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) can be used alone or in combination of two or more.

[0142] The electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect uses an amorphous carbon material as the electrode active material (negative electrode active material) and a trace amount of carbon nanotubes, which suppresses the inhibition of lithium ion migration while forming a uniform electron conduction path, thereby facilitating uniform reactions within the battery and increasing the battery's lifespan. From this perspective, it is preferable that the content of electrode constituent materials (negative electrode constituent materials) excluding the electrode active material (negative electrode active material), carbon nanotubes, and conductive additives other than carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is small, while from the perspective of easily having enough strength to maintain the shape of the electrode, it is preferable that the content be equal to or greater than a certain level. For this reason, in the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) according to the fourth aspect, the content of the electrode active material (negative electrode active material), the electrode constituent material (negative electrode constituent material) excluding carbon nanotubes and conductive additives other than carbon nanotubes (other electrode constituent material (negative electrode constituent material)) is preferably 0.1 to 10.0 mass%, more preferably 1.0 to 8.0 mass%, and even more preferably 2.0 to 6.0 mass%. Note that when a plurality of electrode active materials (negative electrode active materials), electrode constituent materials (negative electrode constituent material) excluding carbon nanotubes and conductive additives other than carbon nanotubes (other electrode constituent material (negative electrode constituent material)) are used, it is preferable to adjust the total amount thereof to be within the above range. In the electrode active material layer for a lithium ion secondary battery according to the fourth aspect (negative electrode active material layer for a lithium ion secondary battery), the total amount (total amount of the composition) of the electrode active material (negative electrode active material), the carbon nanotubes, the conductive additive other than the carbon nanotubes, and the electrode constituent materials (negative electrode constituent materials) excluding the electrode active material (negative electrode active material), the carbon nanotubes, and the conductive additive other than the carbon nanotubes (other electrode constituent materials (negative electrode constituent materials)) is 100 mass%.

[0143] 1-3-4-5. Electrode active material layer for lithium ion secondary battery The electrode active material layer for lithium ion secondary battery (negative electrode active material layer for lithium ion secondary battery) of the present invention contains the above-described electrode active material and carbon nanotubes, and, if necessary, contains a conductive additive other than carbon nanotubes and an electrode constituent material (negative electrode constituent material) (other electrode constituent material (negative electrode constituent material)) excluding the electrode active material (negative electrode active material), carbon nanotubes, and the conductive additive other than carbon nanotubes.

[0144] The thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is not particularly limited, but while a thinner layer is preferable in terms of ensuring lithium ion penetration and electrical conductivity and facilitating uniform reaction, the present invention aims to reduce factors that inhibit lithium ion migration to uniformize the battery reaction and improve the battery life, so a thicker layer is also possible in terms of energy density per electrode. For this reason, the thickness of the electrode active material layer for a lithium ion secondary battery (negative electrode active material layer for a lithium ion secondary battery) of the present invention is preferably 1 to 300 μm, more preferably 10 to 150 μm, and even more preferably 50 to 100 μm.

[0145] 2. Manufacturing Method of Electrode for Lithium-Ion Secondary Battery The manufacturing method of an electrode for a lithium-ion secondary battery of the present invention is not particularly limited, but may include: (1) a step of applying an undercoat layer-forming composition onto an electrode current collector to form an undercoat layer; and (2) a step of forming the electrode active material layer on the undercoat layer formed on the electrode current collector using an electrode active material layer-forming composition, wherein the electrode active material layer-forming composition contains at least an electrode active material and carbon nanotubes, and where the total amount of the electrode active material layer-forming composition is taken as 100 mass%, the content of the carbon nanotubes is 0.01 to 1.4 mass%, the content of the conductive additive other than the carbon nanotubes is 0 to 10.0 mass%, the content of the electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive additive other than the carbon nanotubes is 0 to 2.0 mass%, and the undercoat layer-forming composition contains at least carbon nanotubes.

[0146] (2-1) Step (1) In step (1), the electrode current collector and undercoat layer can be those described above. The undercoat layer-forming composition is a composition capable of forming the undercoat layer described above and can contain the same components as those in the undercoat layer described above. The contents of the components in the undercoat layer-forming composition can also be the same as those in the undercoat layer described above.

[0147] In the undercoat layer-forming composition, when at least carbon nanotubes, and, if necessary, a conductive additive other than carbon nanotubes, and, if necessary, an undercoat layer-forming material other than the conductive additive are mixed to form a paste composition for the undercoat layer, it is possible to make the paste-like composition by adding one or more organic solvents such as water, alcohol (methanol, ethanol, n-propyl alcohol, isopropyl alcohol, etc.), acetone, N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, etc. In this case, the content of each component is the total amount of carbon nanotubes, and, if necessary, a conductive additive other than carbon nanotubes, and, if necessary, an undercoat layer-forming material other than the conductive additive, that is, a value when the total amount of solids is 100 mass%.

[0148] The method for producing the composition for forming an undercoat layer is not particularly limited. For example, the composition for forming an undercoat layer can be produced by mixing the above-mentioned components by a conventional method.

[0149] The undercoat layer can be produced by forming the above-mentioned undercoat layer-forming composition into a layer. For example, when the undercoat layer-forming composition is a paste composition for forming an undercoat layer, the paste composition can be applied onto an electrode current collector by a conventional method, and dried by a conventional method as needed to form a layer.

[0150] (2-2) Step (2) In step (1), the electrode current collector, undercoat layer, and electrode active material layer described above can be used. The electrode active material layer-forming composition is a composition capable of forming the electrode active material layer described above and can contain the same components as those in the electrode active material layer described above. The content of each component in the electrode active material layer-forming composition can also be the same as that in the electrode active material layer described above.

[0151] In the electrode active material layer-forming composition, when at least an electrode active material, carbon nanotubes, and, if necessary, a conductive additive other than carbon nanotubes are mixed, and, if necessary, electrode constituent materials excluding the electrode active material, carbon nanotubes, and conductive additive other than carbon nanotubes are mixed to form a paste composition for the electrode active material layer, the paste can be formed by adding one or more organic solvents such as water, alcohol (methanol, ethanol, n-propyl alcohol, isopropyl alcohol, etc.), acetone, N-methylpyrrolidone, dimethyl sulfoxide, dimethylformamide, etc. In this case, the content of each component is the total amount of the electrode active material, carbon nanotubes, and, if necessary, the conductive additive other than carbon nanotubes, and the electrode constituent materials excluding the electrode active material, carbon nanotubes, and conductive additive other than carbon nanotubes, if necessary, i.e., the total amount of solids is expressed as 100% by mass.

[0152] The method for producing the composition for forming an electrode active material layer is not particularly limited. For example, the composition for forming an electrode active material layer can be produced by mixing the above-mentioned components by a conventional method.

[0153] The electrode active material layer can be produced by forming the above-mentioned electrode active material layer-forming composition into a layer. For example, when the electrode active material layer-forming composition is a paste composition for forming an electrode active material layer, the paste composition can be used to form the electrode active material layer on the undercoat layer obtained in step (1) by a conventional method. Specifically, the electrode active material layer-forming paste composition can be applied or transferred onto the undercoat layer obtained in step (1), and dried by a conventional method as necessary to form the electrode active material layer into a layer.

[0154] 3. Lithium-ion secondary battery The lithium-ion secondary battery of the present invention includes the lithium-ion secondary battery electrode (lithium-ion secondary battery negative electrode or lithium-ion secondary battery positive electrode) of the present invention described above. When the lithium-ion secondary battery electrode of the present invention is used as the negative electrode, the lithium-ion secondary battery electrode of the present invention can be used as the positive electrode, or a positive electrode used in a known lithium-ion secondary battery can be used. When the lithium-ion secondary battery electrode of the present invention is used as the positive electrode, the lithium-ion secondary battery electrode of the present invention can be used as the negative electrode, or a negative electrode used in a known lithium-ion secondary battery can be used. The lithium-ion secondary battery of the present invention can also include a container for storing an electrolyte used in a known lithium-ion secondary battery and these electrode components.

[0155] When a known negative electrode for use in a lithium ion secondary battery is used as the negative electrode, the negative electrode is not particularly limited, and any known negative electrode can be used. An example of a known negative electrode is shown below.

[0156] The negative electrode current collector constituting the negative electrode is preferably made of a material that is electrochemically stable at the potential used and has high electronic conductivity, such as copper, stainless steel, nickel, a carbon material, etc. This negative electrode current collector can be, for example, a foil-shaped or mesh-shaped member.

[0157] The negative electrode active material used to form the negative electrode is usually a material capable of absorbing and releasing lithium ions, such as carbon materials such as natural graphite, artificial graphite, and amorphous carbon; metal materials capable of forming an alloy with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Si alloys, Sn alloys, and Al alloys; SiO x (0<x<2), SnO x (0<x<2), lithium titanium composite oxide (Li 2 TiO 3Examples of such negative electrode active materials include metal oxides capable of absorbing and releasing lithium ions, such as vanadium oxide; and composite materials containing a metal material and a carbon material, such as Si-C composites and Sn-C composites. These negative electrode active materials can be used alone or in combination of two or more. From the viewpoint of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge and particularly improving the charge and discharge cycle characteristics, carbon materials, lithium titanium composite oxides, and the like can also be used. In particular, when a conductive material such as a carbon material is used as the negative electrode active material, the negative electrode active material also functions as a conductive additive, making it particularly easy to reduce the content of substances that inhibit the movement of lithium ions.

[0158] As for the electrode active material (negative electrode active material) as described above, from the viewpoint of particularly suppressing the volume change of the electrode active material (negative electrode active material) during charge and discharge, easily suppressing the capacity decrease due to the volume change, and particularly easily improving the charge and discharge cycle characteristics, it is preferable that the volume change of the electrode active material (negative electrode active material) during charge and discharge is 150% or less, preferably 120% or less. The smaller the volume change, the better, and no lower limit is set, but if a lower limit is set, it is 0%. Note that this volume change value indicates the degree to which the electrode active material (negative electrode active material) at full charge has expanded compared to the electrode active material (negative electrode active material) at full discharge, and is calculated using the following formula: (volume at full charge) - (volume at full discharge) / (volume at full discharge) x 100.

[0159] As the negative electrode constituent material other than the negative electrode active material constituting the negative electrode, the same conductive additive other than carbon nanotubes or other positive electrode constituent material as used in the electrode for a lithium ion secondary battery of the present invention described above can be used, and the content thereof can be at a level that is normally used.

[0160] When a known positive electrode for use in a lithium ion secondary battery is used as the positive electrode, any known positive electrode can be used as long as it can supply lithium ions to the negative electrode. An example of a known positive electrode is shown below.

[0161] Examples of the positive electrode current collector that constitutes the positive electrode include materials that are electrochemically stable at the potential used and have high electronic conductivity, such as aluminum, stainless steel, and carbon materials.

[0162] The positive electrode active material used to form the positive electrode is usually a material capable of absorbing and releasing lithium ions. For example, α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel-type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x1 Ni γ1 Mn β1 Co(1-x1-γ1-β1)]O 2 (0≦x1<0.5, 0≦γ1≦1, 0≦β1≦1, 0≦γ1+β1≦1), Li[Li x2 Ni γ2 Co β2 Al(1-x2-γ2-β2)]O 2 (0≦x2<0.5, 0≦γ2≦1, 0≦β2≦1, 0≦γ2+β2≦1). Examples of lithium transition metal oxides having a spinel crystal structure include Li x3 Mn 2 O 4 (0.9≦x3<1.5), Li x4 Ni γ4 Mn (2-γ4) O 4 (0.9≦x4<1.5, 0≦γ4≦2) and the like. Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4Examples of the positive electrode active material include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. The atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. These positive electrode active materials may be used alone or in combination of two or more. Among these, the lithium transition metal composite oxides are preferred as the positive electrode active material from the viewpoint of achieving high energy density.

[0163] As the positive electrode constituent material other than the positive electrode active material that constitutes the positive electrode, the same materials as the electrode active material and the electrode constituent material other than carbon nanotubes in the electrode for a lithium ion secondary battery of the present invention described above can be used, and the content thereof can also be the same as the electrode active material and the electrode constituent material other than carbon nanotubes in the electrode for a lithium ion secondary battery of the present invention.

[0164] The electrolyte solution is an electrolyte solution in which a salt is dissolved in an aprotic organic solvent, and is placed between the positive electrode and the negative electrode. For example, it is preferable that the electrolyte solution is impregnated and held in a separator made of nonwoven fabric or the like to prevent short-circuiting between the positive electrode and the negative electrode.

[0165] Examples of the aprotic organic solvent that constitutes the above-mentioned electrolytic solution include esters such as ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, methyl formate, and methyl acetate; furans such as tetrahydrofuran and 2-methyltetrahydrofuran; ethers such as dioxolane, diethyl ether, dimethoxyethane, diethoxyethane, and methoxyethoxyethane; dimethyl sulfoxide; sulfolanes such as sulfolane and methylsulfolane; acetonitrile, etc. These aprotic organic solvents may be used alone or in combination of two or more.

[0166] On the other hand, examples of salts that can be dissolved in such aprotic organic solvents include lithium salts such as lithium perchlorate, lithium fluoroborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium halides, lithium chloroaluminate, and lithium bis(fluorosulfonyl)imide. These salts may be used alone or in combination of two or more.

[0167] Since the lithium ion secondary battery of the present invention uses the lithium ion secondary battery electrode of the present invention (lithium ion secondary battery negative electrode or lithium ion secondary battery positive electrode) for the negative electrode and / or positive electrode, it has a strength sufficient to maintain the shape of the electrode, does not crack due to pressing or the like during electrode production, does not peel off from the undercoat layer and the electrode active material layer, and is unlikely to inhibit the movement of lithium ions, thereby making the reaction within the battery uniform and extending the battery's life. Therefore, this lithium ion secondary battery is expected to be deployed on the market in the future, and can be effectively used for car sharing electric vehicles, particularly AIEVs (Artificial Intelligence Electric Vehicles), which are required to have even longer life.

[0168] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0169] In the following examples, the graphite particles used as the negative electrode active material all have a volume change of 10%, calculated by the following formula: (volume at full charge) - (volume at full discharge) / (volume at full discharge) x 100.

[0170] [Examples 1 to 5 and Comparative Examples 1 to 5: Negative Electrodes for Lithium-Ion Secondary Batteries] Comparative Example 1 As the negative electrode active material, 99.5 mass% of graphite particles (spherical coated natural graphite; average particle diameter 17 μm), 0.5 mass% of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length >5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) negative electrode current collector, and dried with a doctor blade to form a negative electrode active material layer with a weight per unit area of ​​10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0171] Comparative Example 2: 100% by mass of graphite particles (spherical coated natural graphite; average particle size 17 μm) as the negative electrode active material were mixed with an appropriate amount of N-methylpyrrolidone to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) as the negative electrode current collector, and after drying with a doctor blade, the weight per unit area of ​​the negative electrode active material layer was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0172] Comparative Example 3: 90% by mass of graphite (flake graphite; average particle size 1 μm) as a conductive additive other than carbon nanotubes, 10% by mass of carbomethyl cellulose (CMC) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of water were mixed and kneaded to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) negative electrode current collector with a doctor blade so that the undercoat layer would have a thickness of 4 μm after drying, and then dried at 60° C. to form an undercoat layer on the negative electrode current collector.

[0173] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm.2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0174] Comparative Example 4: 40% by mass of graphite (flake graphite; average particle size 1 μm) as a conductive additive other than carbon nanotubes, 60% by mass of carbomethyl cellulose (CMC) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of water were mixed and kneaded to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) negative electrode current collector with a doctor blade so that the undercoat layer would have a thickness of 4 μm after drying, and then dried at 60° C. to form an undercoat layer on the negative electrode current collector.

[0175] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0176] Comparative Example 5: 40% by mass of acetylene black (AB; average particle size 30 nm) as a conductive additive other than carbon nanotubes, 60% by mass of carbomethyl cellulose (CMC) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of water were mixed and kneaded to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) negative electrode current collector with a doctor blade so that the undercoat layer would have a thickness of 4 μm after drying, and then dried at 60° C. to form an undercoat layer on the negative electrode current collector.

[0177] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0178] Example 1 40% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm per single-walled CNT, G / D: 80 to 150), 60% by mass of carbomethyl cellulose (CMC) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of water were mixed and kneaded to form a slurry. This slurry was applied to a copper foil (thickness 10 μm) negative electrode current collector with a doctor blade so that the thickness of the undercoat layer after drying would be 4 μm, and the coating was dried at 60°C to form an undercoat layer on the negative electrode current collector.

[0179] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0180] Example 2 16.7% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), 83.3% by mass of polyvinylidene fluoride (PVdF) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied with a doctor blade to a copper foil (thickness 10 μm) negative electrode current collector so that the thickness of the undercoat layer after drying would be 4 μm, and the mixture was dried at 60 ° C. to form an undercoat layer on the negative electrode current collector.

[0181] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0182] Example 3 100% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter of 2 nm, average length of >5 μm per single-walled CNT, G / D: 80 to 150) and an appropriate amount of N-methylpyrrolidone were mixed and kneaded to form a slurry. This slurry was applied to a copper foil (thickness: 10 μm) negative electrode current collector using a doctor blade so that the thickness of the undercoat layer after drying would be 4 μm, and the coating was dried at 60°C to form an undercoat layer on the negative electrode current collector.

[0183] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0184] Example 4: 83.3% by mass of multi-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 20 nm, average length >10 μm per single-walled CNT, G / D: 0.5 to 10), 16.7% by mass of carbomethyl cellulose (CMC) as an undercoat layer constituent material other than the conductive additive, and an appropriate amount of water were kneaded together to form a slurry. This slurry was applied with a doctor blade to a copper foil (thickness 10 μm) negative electrode current collector so that the thickness of the undercoat layer after drying would be 4 μm, and the coating was dried at 60°C to form an undercoat layer on the negative electrode current collector.

[0185] Next, 99.5% by mass of graphite particles (spherical coated natural graphite; average particle diameter 17 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0186] Example 5 100% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter of 2 nm, average length of >5 μm per single-walled CNT, G / D: 80 to 150) were mixed with an appropriate amount of N-methylpyrrolidone to form a slurry. This slurry was applied to a copper foil (thickness: 10 μm) negative electrode current collector using a doctor blade so that the thickness of the undercoat layer after drying would be 4 μm, and the coating was dried at 60°C to form an undercoat layer on the negative electrode current collector.

[0187] Next, 99.0% by mass of graphite particles (flaky natural graphite; average particle diameter 5 μm) as a negative electrode active material, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), 0.5% by mass of carbomethyl cellulose (CMC), and an appropriate amount of water were kneaded together to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade so that the weight per unit area of ​​the negative electrode active material layer after drying was 10.3 to 10.9 mg / cm. 2 The mixture was dried at 80° C. to obtain a pre-press negative electrode.

[0188] [Example 6 and Comparative Example 6: Positive electrode for lithium ion secondary battery] Comparative Example 6: LiNi was used as the positive electrode active material. 0.8 Co 0.15 Al 0.05 O 2 98.0 mass% of carbon nanotubes (NCA; average particle diameter 12 μm), 1.5 mass% of acetylene black (AB; average particle diameter 30 nm) as a conductive additive other than carbon nanotubes, 0.5 mass% of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone were mixed and kneaded to form a slurry, which was then applied to an aluminum foil (thickness 15 μm) serving as a positive electrode current collector. After drying with a doctor blade, the mass per unit area of ​​the positive electrode active material layer was 20.05 to 21.29 mg / cm. 2 The mixture was dried at 100° C. to obtain a pre-press positive electrode.

[0189] Example 6 100% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter of 2 nm, average length of >5 μm per single-walled CNT, G / D: 80 to 150) were mixed with an appropriate amount of N-methylpyrrolidone to form a slurry. This slurry was applied with a doctor blade to an aluminum foil (thickness 15 μm) positive electrode current collector so that the thickness of the undercoat layer after drying would be 4 μm, and the coating was dried at 60°C to form an undercoat layer on the positive electrode current collector.

[0190] Next, LiNi was used as the positive electrode active material. 0.8 Co 0.15 Al 0.05 O 2 A mixture of 98.0% by mass of carbon nanotubes (NCA; average particle diameter 12 μm), 1.5% by mass of acetylene black (AB; average particle diameter 30 nm) as a conductive additive other than carbon nanotubes, 0.5% by mass of single-walled carbon nanotubes (bundled single-walled CNT aggregates; average outer diameter 2 nm, average length > 5 μm, G / D: 80 to 150 per single-walled CNT), and an appropriate amount of N-methylpyrrolidone was kneaded to form a slurry. This slurry was applied to the undercoat layer formed above with a doctor blade, and the weight per unit area of ​​the positive electrode active material layer after drying was 20.05 to 21.29 mg / cm. 2 The mixture was dried at 100° C. to obtain a pre-press positive electrode.

[0191] Test Example 1: Press Resistance Test The pre-press negative electrodes or pre-press positive electrodes obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were punched out to 2 cm × 5 cm, roll-pressed under a linear pressure of 1 kN / cm or 2 kN / cm, and the surface state of the electrode was observed to evaluate the press resistance.

[0192] Then, the evaluation was made as follows: ○: No lifting at all in the negative electrode or positive electrode; △: Lifting occurs in part in the negative electrode or positive electrode; ×: Cracks occur in the negative electrode active material layer or positive electrode active material layer, or the negative electrode active material layer or positive electrode active material layer peels off from the negative electrode current collector or positive electrode current collector.

[0193] The results are shown in Table 1.

[0194]

Claims

1. An electrode for a lithium ion secondary battery comprising an electrode current collector, an undercoat layer and an electrode active material layer, wherein the electrode active material layer contains at least an electrode active material and carbon nanotubes, and, assuming a total amount of the electrode active material layer to be 100% by mass, the carbon nanotube content is 0.01 to 1.4% by mass, the content of conductive additives other than the carbon nanotubes is 0 to 10.0% by mass, the content of electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive additives other than the carbon nanotubes is 0 to 2.0% by mass, and the undercoat layer contains at least carbon nanotubes.

2. The electrode for a lithium ion secondary battery according to claim 1, wherein the content of the carbon nanotubes is 5 to 100 mass % with the total amount of the undercoat layer being 100 mass %.

3. The electrode for a lithium ion secondary battery according to claim 1 or 2, wherein the undercoat layer further contains an undercoat layer-constituting material other than carbon nanotubes.

4. The electrode for a lithium ion secondary battery according to claim 3, wherein the content of the undercoat layer constituent materials other than the carbon nanotubes is 0 to 95 mass % with the total amount of the undercoat layer being 100 mass %.

5. The electrode for a lithium ion secondary battery according to any one of claims 1 to 4, wherein the undercoat layer has a thickness of 0.1 to 10.0 µm.

6. The electrode for a lithium ion secondary battery according to any one of claims 1 to 5, wherein, assuming the total amount of the electrode active material layer to be 100 mass%, the content of the electrode active material is 96.6 to 99.9 mass%, the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 2.0 mass%, and the electrode is a negative electrode for a lithium ion secondary battery.

7. An electrode for a lithium ion secondary battery according to any one of claims 1 to 5, wherein the total amount of the electrode active material layer is taken as 100 mass%, the content of the electrode active material is 97.4 to 99.9 mass%, and the content of electrode constituent materials other than the electrode active material and the carbon nanotubes is 0 to 1.2 mass%.

8. The electrode for a lithium ion secondary battery according to claim 7, which is a negative electrode for a lithium ion secondary battery.

9. The electrode for a lithium ion secondary battery according to any one of claims 1 to 5, wherein, assuming the total amount of the electrode active material layer to be 100 mass%, the content of the electrode active material is 88.6 to 99.9 mass%, the content of the conductive additive other than the carbon nanotubes is 0 to 10.0 mass%, and the electrode does not contain any electrode constituent materials other than the electrode active material, the carbon nanotubes, and the conductive additive other than the carbon nanotubes, and the electrode is a positive electrode for a lithium ion secondary battery.

10. The electrode for a lithium ion secondary battery according to any one of claims 1 to 9, wherein the electrode active material is a material capable of absorbing and releasing lithium ions.

11. The electrode for a lithium ion secondary battery according to any one of claims 1 to 10, wherein the carbon nanotubes are single-walled carbon nanotubes.

12. The electrode for a lithium ion secondary battery according to any one of claims 1 to 11, which is used to reduce uneven distribution of reactions in a lithium ion secondary battery.

13. The electrode for a lithium ion secondary battery according to any one of claims 1 to 12, which is for a lithium ion secondary battery used in an electric vehicle for car sharing.

14. A lithium ion secondary battery comprising the electrode for a lithium ion secondary battery according to any one of claims 1 to 13.

15. The lithium ion secondary battery according to claim 14, which is used in an electric vehicle for car sharing.

16. A method for producing an electrode for a lithium ion secondary battery according to any one of claims 1 to 13, comprising: (1) a step of applying an undercoat layer-forming composition onto an electrode collector to form an undercoat layer; and (2) a step of forming the electrode active material layer on the undercoat layer formed on the electrode collector using an electrode active material layer-forming composition, wherein the electrode active material layer-forming composition contains at least an electrode active material and carbon nanotubes, and, assuming a total amount of the electrode active material layer-forming composition to be 100% by mass, the carbon nanotube content is 0.01 to 1.4% by mass, the conductive assistant other than the carbon nanotubes content is 0 to 10.0% by mass, the electrode constituent materials excluding the electrode active material, the carbon nanotubes, and the conductive assistant other than the carbon nanotubes content is 0 to 2.0% by mass, and the undercoat layer-forming composition contains at least carbon nanotubes.

17. The method according to claim 16, wherein the content of the carbon nanotubes is 5 to 100 mass % with respect to the total amount of the composition for forming the undercoat layer being 100 mass %.

18. The method according to claim 16 or 17, wherein the composition for forming an undercoat layer further contains an undercoat layer-constituting material other than carbon nanotubes.

19. The method according to claim 18, wherein the content of the undercoat layer constituent materials other than the carbon nanotubes is 0 to 95 mass % with the total amount of the composition for forming the undercoat layer being 100 mass %.

20. The method according to any one of claims 16 to 19, wherein the composition for forming an undercoat layer is applied so that the thickness of the undercoat layer is 0.1 to 10.0 μm.

Citation Information

Patent Citations

  • Charger and charging method

    JP2013070500A

  • Electric vehicle

    JP2018121411A

  • Electrode for energy storage device and energy storage device

    JP2019175744A

  • Electrode for energy storage device and energy storage device

    JP2019175749A

  • Cathode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

    JP2021150051A