Method for restoring bending die and restored bending die
The method addresses the issue of irregularities in bending die regeneration by using a grindstone with circumferential convex parts to form recesses, ensuring a smooth surface and preventing line formation on the workpiece, thereby maintaining high appearance quality in the regenerated bending dies and the workpieces.
Patent Information
- Application Number
- PCT/JP2024/018386
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional methods for regenerating bending dies often result in steps or irregularities at the cutting edge or V-groove, leading to deteriorated appearance quality of the workpiece during coining processes due to tolerance variations and uneven wear, which can cause lines on the surface of the workpiece.
A method involving a build-up process using a grindstone with circumferential convex parts to form recesses between the base material and built-up portions, ensuring a smooth, step-free surface by gouging to include the external ends of the built-up parts, thereby maintaining the appearance quality and preventing line formation on the workpiece.
The method effectively regenerates bending dies with a high appearance quality, preventing step formation and ensuring no lines are created on the workpiece surface during coining, thus maintaining the quality of the bent workpiece.
Smart Images

Figure JP2024018386_28112024_PF_FP_ABST
Abstract
Description
Bending die recycling method and recycled bending die
[0001] The present invention relates to a method for recycling a bending die and a recycled bending die.
[0002] Patent Document 1 describes a method for restoring a worn die. The die restoring method described in Patent Document 1 involves overlay welding on the edge portion of a press punch die that has worn or chipped due to use, and then mechanically grinding the overlay-welded portion to restore a new edge portion.
[0003] The mold recycling method described in Patent Document 1 is not limited to recycling press punching dies, but is also commonly used as a method for recycling other dies, and punch dies and die dies for bending dies are also targets for recycling using this method.
[0004] A conventional method for recycling bending dies will be described with reference to Figures 7A and 7B, using a punch die as a specific example. Figure 7A is a right side view showing a conventional punch die 101. Figure 7B is a diagram for explaining the conventional die recycling method, and (a) to (c) in Figure 7B are side views corresponding to the first to third steps, respectively.
[0005] As shown in FIG. 7A, a conventional punch die 101 has a main body 111 that is attached to a punch holder, and a cutting edge 112 that is formed at the tip of the main body 111 and that comes into contact with a workpiece.
[0006] Fig. 7B is an enlarged view of a tip region 112A of the cutting edge 112 of Fig. 7A. The cutting edge 112, which has been subjected to multiple bending processes, has a worn surface 112c whose outer shape has worn away from the outer shape of the reference cutting edge line LNa when not in use, which is shown by the two-dot chain line in Fig. 7B (a).
[0007] When the wear has progressed to a certain extent, as shown in (b) of Fig. 7B, metal is welded to form a padded portion 113 having a size and cross-sectional shape that includes the reference cutting edge line LNa. Thereafter, the padded portion 113 is ground using a punch forming grindstone 105 having a shape that corresponds to the reference cutting edge line LNa so that the outer shape of the padded portion 113 matches the reference cutting edge line LNa, resulting in a recycled punch top 114 shown in (c) of Fig. 7B.
[0008] Japanese Patent Application Publication No. 7-265972
[0009] The finished dimensions of a bending die are set with a tolerance that takes into account variations in manufacturing processing within a range that allows for specified performance. Specifically, the punch die 101 has a tolerance of, for example, +0 mm to -0.05 mm for its thickness dimension. Meanwhile, the grinding surface shape of the punch forming grindstone 105 shown in FIG. 7B (b) is designed to form a grinding surface of ±0 mm corresponding to the reference cutting edge line LNa. Therefore, if the pre-use dimensions of the cutting edge 112 of the punch die to be recycled are formed near the upper limit of the tolerance, the cutting edge 112 and the recycled punch top 114 formed by grinding the buildup 113 with the punch forming grindstone 105 will have a continuous surface without any steps, as shown in FIG. 7B (c).
[0010] In contrast, if the thickness dimension of the cutting edge portion 112 before use is formed near the lower limit of the tolerance, a gap Δd corresponding to the tolerance will be formed between the punch forming grindstone 105 and the cutting edge portion 112, as shown in FIG. 8A . The recycled punch top 114 formed by grinding the built-up portion 113 has a ground surface corresponding to the reference cutting edge line LNa. However, as shown in FIG. 8B , a steep step 115 that is convex on the built-up portion 113 side is formed at the end of the built-up portion 113. This step 115 is formed along the longitudinal direction of the punch die 101 (the left-right direction shown in FIG. 1 ). While FIG. 8A shows a case where the gap Δd is formed on the left side of the figure, it may also be formed on the right side of the figure or on both sides, and there is a risk that the step 115 will be formed on the right side or both sides, respectively.
[0011] The same situation applies to die molds, and if the width of the V-groove portion is biased toward the side with a larger tolerance, there is a risk that a steep step will be formed on at least one of the pair of inclined surfaces of the V-groove portion, causing the buildup portion to become convex.
[0012] If such a step 115 is formed in the cutting edge 112 of the punch die 101, which is a bending die, and in the V-groove portion of the die die, the appearance quality of the punch die 101 and the die die will deteriorate, and if the bending process is so-called coining, a line corresponding to the step 115 will be formed on the surface of the workpiece, which may deteriorate the appearance quality of the workpiece, and therefore improvement is desired.
[0013] A bending die regeneration method according to one aspect of the present invention has the following configuration: That is, the bending die regeneration method includes: a buildup step of forming a buildup portion covering the entire surface to be regenerated on a base material of the bending die, the base material having a surface to be regenerated that has a shape different from a reference shape; and a shaping step of rotating a grinding wheel having a grinding part that grinds the buildup portion to shape the buildup portion into the reference shape and regenerate the buildup portion, wherein the grinding part of the grinding wheel has a peripheral convex part that is carved out to include the external end of the buildup portion that connects to the base material, and the shaping step forms a recess in the bending die by the peripheral convex part that includes the external boundary between the base material and the buildup portion.
[0014] A recycled bending die according to one aspect of the present invention has the following configuration: a first portion that is substantially plate-shaped and made of a first material, and that has, at one edge thereof, a cutting edge or V-groove having a V-shaped cross section formed by a first surface and a second surface, and a second portion that is provided at the tip of the cutting edge or V-groove and is made of a second material different from the first material, and the first surface and the second surface each have a recess formed in a range that includes an apparent boundary between the first portion and the second portion.
[0015] According to the bending die recycling method and recycled bending die of the present invention, no steps are created in the cutting edge of the punch die and in the V-groove of the die die, so the appearance quality is not reduced, and even if the bending process is coining, no lines are left on the surface of the workpiece, so the appearance quality is not reduced.
[0016] FIG. 1 is a perspective view showing the appearance of a punch die 1, which is a recycled bending die according to a first embodiment of the present invention. FIG. 2 is a cross-sectional view illustrating a method for shaping a cutting edge portion 12 of the punch die 1. FIG. 3A is a cross-sectional view illustrating a first step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment of the present invention. FIG. 3B is a cross-sectional view illustrating a second step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3C is a cross-sectional view illustrating a third step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3D is a cross-sectional view illustrating a fourth step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3E is a cross-sectional view illustrating a first step of shaping the cutting edge portion 12 in the method for recycling a bending die according to a second embodiment of the present invention. FIG. 3F is a cross-sectional view illustrating a second step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the second embodiment. FIG. 4 is a perspective view showing the appearance of a die 2, which is a recycled bending die according to a second embodiment of the present invention. FIG. 5A is a cross-sectional view illustrating a first step of forming a V-groove portion 22 in the method for recycling a bending die according to the first embodiment of the present invention. FIG. 5B is a cross-sectional view illustrating a second step of forming a V-groove portion 22 in the method for recycling a bending die according to the first embodiment. FIG. 5C is a cross-sectional view illustrating a third step of forming a V-groove portion 22 in the method for recycling a bending die according to the first embodiment. FIG. 5D is a cross-sectional view illustrating a fourth step of forming a V-groove portion 22 in the method for recycling a bending die according to the first embodiment. FIG. 6A is a plan view showing a punch forming grindstone 5 used in the methods for recycling bending dies according to the first and second embodiments. FIG. 6B is a plan view showing a die forming grindstone 6 used in the methods for recycling bending dies according to the first and second embodiments. FIG. 7A is a side view showing a punch 101 of a conventional recycled bending die. Fig. 7B is a diagram for explaining a conventional method for regenerating a bending die, in which (a) to (c) are cross-sectional views corresponding to steps 1 to 3, respectively. Fig. 8A is a cross-sectional view showing an example of a molding step of a cutting edge portion 112 in a conventional method for regenerating a bending die.FIG. 8B is a perspective cross-sectional view showing the cutting edge portion 112 of a conventional recycled bending die.
[0017] An embodiment of the present invention will be described with reference to Figures 1 to 6B, taking as examples a punch 1 according to a first embodiment and a die 2 according to a second embodiment. The punch 1 and the die 2 are each included in a recycled bending die K.
[0018] (Punch Die 1) FIG. 1 is a perspective view showing the appearance of a punch die 1, which is an example of a recycled bending die according to a first embodiment of the present invention. FIG. 2 is a cross-sectional view illustrating a method for shaping the cutting edge portion 12 of the punch die 1. FIG. 3A is a cross-sectional view illustrating a first step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment of the present invention. FIG. 3B is a cross-sectional view illustrating a second step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3C is a cross-sectional view illustrating a third step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3D is a cross-sectional view illustrating a fourth step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the first embodiment. FIG. 3E is a cross-sectional view illustrating a first step of shaping the cutting edge portion 12 in the method for recycling a bending die according to a second embodiment of the present invention. FIG. 3F is a cross-sectional view illustrating a second step of shaping the cutting edge portion 12 in the method for recycling a bending die according to the second embodiment. Fig. 6A is a plan view showing a punch forming grindstone 5 used in the bending die regeneration method according to the first and second embodiments. Fig. 6B is a plan view showing a die forming grindstone 6 used in the bending die regeneration method according to the first and second embodiments. For ease of explanation, the up, down, left, right, front, and back directions are defined as the directions indicated by arrows in Fig. 1.
[0019] As shown in Figure 1, the punch die 1 of the recycled bending die K has a punch body 11 as a substantially plate-shaped base material A extending up, down, left, and right, and a cutting edge 12 formed on one edge, i.e., the lower edge, of the punch body 11. The punch body 11 is attached to a punch holder of a bending machine. The punch die 1 moves up and down in accordance with the operation of the attached bending machine, and when it descends, the cutting edge 12 comes into contact with the upper surface of a workpiece W (see Figure 3D) placed between the punch die 1 and a die 2 (see Figure 4), which will be described later, and presses the workpiece W downward, thereby bending the workpiece W.
[0020] 1 and 2, the cutting edge 12 is V-shaped in side view, with a pair of tapered inclined surfaces. The inclined plane on the front side of the cutting edge 12 is the first inclined surface 12a, which serves as the first outer surface, and the inclined plane on the rear side is the second inclined surface 12b, which serves as the second outer surface. In the cutting edge 12, the first inclined surface 12a has a first recess 121 extending in the left-right direction near the tip, and the second inclined surface 12b has a second recess 122 extending in the left-right direction near the tip. The first recess 121 and the second recess 122 are collectively referred to as recess E.
[0021] As shown in Fig. 2, the first inclined surface 12a and the second inclined surface 12b are formed by grinding using a punch forming grindstone 5. The punch forming grindstone 5 is a grindstone having a cylindrical or disk-shaped base body 50, and a grinding portion 5G having a predetermined grinding surface is formed on the circumferential surface of the base body 50. The predetermined grinding surface has a shape corresponding to the final finished shape of the cutting edge portion 12. The punch forming grindstone 5 is included in the general term grindstone C, and the grinding portion 5G is included in the general term grinding portion Ca.
[0022] Specifically, the grinding portion 5G has a first concave inclined grinding wheel surface 5a that forms the first inclined surface 12a of the cutting edge portion 12 and a second concave inclined grinding wheel surface 5b that forms the second inclined surface 12b of the cutting edge portion 12. The first concave inclined grinding wheel surface 5a has a first circumferential convex portion 51 that forms the first concave portion 121 of the cutting edge portion 12, and the second concave inclined grinding wheel surface 5b has a second circumferential convex portion 52 that forms the second concave portion 122 of the cutting edge portion 12. The first circumferential convex portion 51 and the second circumferential convex portion 52 are convex portions formed around the entire circumference in shapes corresponding to the shapes of the first concave portion 121 and the second concave portion 122, respectively. The first circumferential convex portion 51 and the second circumferential convex portion 52 are included in the general term circumferential convex portion Ca1.
[0023] The punch forming grindstone 5 is attached to a grinding machine (not shown) and rotates about an axis CL5, while being pressed against the cutting edge 12. As a result, the cutting edge 12 is ground into a shape corresponding to the grinding portion 5G.
[0024] The worn cutting edge 12 is the surface Aa to be refurbished, and is refurbished by the bending die refurbishment method according to this embodiment, which will be described next. In the description, reference will be made to Figures 3A to 3D.
[0025] 3A shows the cutting edge portion 12 having a leading wear surface 12c, which is the surface Aa to be regenerated in a worn state. The outermost two-dot chain line is a virtual reference cutting edge line LN1a in a new, unworn state. The outer shape in a worn state is shown by a solid worn cutting edge line LN1b. The two-dot chain removal cutting edge line LN1c indicates the removal position of the portion to be removed in the next process. The removal cutting edge line LN1c is set as a straight line extending in the front-to-rear direction above the worn cutting edge line LN1b.
[0026] First, as shown in Fig. 3B, the portion of the worn cutting edge 12 below (toward the tip end of) the removal edge line LN1c is removed by grinding or the like. The removal is performed over the entire range in the longitudinal direction (left-right direction) of the punch 1. As a result, a removal surface 12d, which is a flat surface extending in the front-rear and left-right directions, is formed at the position of the removal edge line LN1c.
[0027] Next, as shown in Figure 3C, a buildup portion 13 is formed at the tip of the cutting edge 12. The buildup portion 13 completely covers the removal surface 12d, and buildup end positions P2a and P2b, which are the upper ends of the buildup, are located closer to the base (upper side) of the cutting edge 12 than the removal surface end positions P1a and P1b, which are the positions where the removal surface 12d connects to the first inclined surface 12a and the second inclined surface 12b. The buildup portion 13 is collectively referred to as buildup portion B. Furthermore, if the external end of the buildup portion B that connects to the base material A is referred to as end Ba, the buildup end positions P2a and P2b are collectively referred to as end Ba.
[0028] The method for forming the build-up portion 13 is not limited. For example, methods such as laser cladding, PTA (Plasma Transferred Arc Welding), and thermal spraying can be used. The metal to be built-up is also not limited, and may be a material different from the material of the punch body 11 of the base material A, and may be selected appropriately depending on the application and specifications.
[0029] The removal amount and build-up amount for obtaining the removal surface 12d may be adjusted as appropriate according to the amount of wear of the cutting edge 12. When the removal amount is large, the removal surface end positions P1a and P1b are positioned higher, and therefore the build-up end positions P2a and P2b need to be positioned even higher to cover the removal surface 12d, requiring a larger build-up amount.
[0030] Next, the padding 13 is cut and formed by the punch forming grindstone 5 described with reference to Fig. 2 to form the recycled punch top 14 corresponding to the reference cutting edge line LN1a. As described above, the punch forming grindstone 5 has a first peripheral convex portion 51 and a second peripheral convex portion 52. Therefore, a first recess 121 corresponding to the first peripheral convex portion 51 is formed on the first inclined surface 12a of the recycled punch top 14, and a second recess 122 corresponding to the second peripheral convex portion 52 is formed on the second inclined surface 12b.
[0031] As shown in FIG. 3D , the first recess 121 is formed by removing a range including the buildup end position P2a from the first inclined surface 12a. The second recess 122 is formed by removing a range including the buildup end position P2b from the second inclined surface 12b. The depth Dp1 of the first recess 121 and the second recess 122 is determined according to the tolerance set for the dimension in the thickness direction (front-rear direction) of the punch die 1. For example, if the tolerance for the dimension D1 in the thickness direction (see FIG. 2 ) is set to "+0 mm to -0.05 mm," the depth Dp1 may be set to a value exceeding 0.05 mm in theory, but may be set to, for example, 0.1 mm to allow for some margin of error.
[0032] The shapes of the first recess 121 and the second recess 122 are not limited as long as they do not protrude from the first inclined surface 12a and the second inclined surface 12b, respectively. The shapes of the first recess 121 and the second recess 122 may be concave curved surfaces with curved cross sections, or may include three-dimensional flat surfaces in which some of the curved cross sections are straight. For example, the first recess 121 may be connected to the first inclined surface 12a so that its upper and lower ends are clearly curved. Furthermore, the first recess 121 may be shaped so that its upper and lower ends are smoothly connected to the first inclined surface 12a by being rounded, which is desirable from the perspective of minimizing the impact on the workpiece W during coining. The same applies to the second recess 122.
[0033] As described above, according to the bending die recycling method of the first embodiment, the worn cutting edge shape is recycled to obtain a punch die 1 having a recycled punch top 14 with an unused cutting edge shape.
[0034] In the regeneration method according to the first embodiment described above, whether or not to remove the tip portion of the cutting edge 12 may be determined depending on the degree of wear. That is, when regeneration is performed when the degree of wear is small, the regeneration method according to the second embodiment described below may be performed without removing the tip portion.
[0035] Specifically, in the method for restoring a bending die according to the second embodiment, when the amount of wear on the cutting edge 12 to be restored, which has the tip wear surface 12c shown in Fig. 3A, is less than a predetermined amount, a padding portion 13 is formed without removing the tip, as shown in Fig. 3E. The padding portion 13 completely covers the tip wear surface 12c, which is the surface Aa to be restored, and padding end positions P2a and P2b, which are the upper ends of the padding portion 13, are located closer to the base (upper side) of the cutting edge 12 than removal surface end positions P3a and P3b, which are the positions where the tip wear surface 12c connects with the first inclined surface 12a and the second inclined surface 12b.
[0036] In the second embodiment, the cladding method for forming the cladding portion 13 is not limited. For example, methods such as laser cladding, PTA (Plasma Transferred Arc Welding), and thermal spraying can be used. The cladding metal is also not limited, and may be selected appropriately depending on the application and specifications.
[0037] Next, as shown in Fig. 3F, the punch forming grindstone 5 described with reference to Fig. 2 is used to cut the buildup 13 to form a recycled punch top 14 corresponding to the reference cutting edge line LN1a. As described above, the punch forming grindstone 5 has a first peripheral convex portion 51 and a second peripheral convex portion 52. Therefore, a first recess 121 corresponding to the first peripheral convex portion 51 is formed on the first inclined surface 12a of the recycled punch top 14, and a second recess 122 corresponding to the second peripheral convex portion 52 is formed on the second inclined surface 12b.
[0038] In the bending die recycling method according to the second embodiment, the depth Dp1 of the first recess 121 and the second recess can be determined in the same manner as in the first embodiment, depending on the tolerance set for the dimension in the thickness direction (front-to-back direction in Figure 3F) of the punch die 1.
[0039] (Die mold 2) Next, the procedure for regenerating the die mold 2, which is an example of the regenerated bending mold K according to the second embodiment of the present invention, using the bending mold regeneration method according to the first embodiment of the present invention will be described with reference to Figures 4 to 5D.
[0040] As shown in Fig. 4, the die 2 has a die body 21 as a substantially plate-shaped base material A extending vertically and horizontally, and a V-groove 22 formed on an upper edge of the die body 21. The die body 21 is attached to a die holder of a bending machine. In a bending machine of the type in which the die side is fixed and the punch side is raised and lowered, the die 2 contacts the underside of a workpiece W (see Fig. 5A) placed between the punch 1 which rises and lowers above, and the V-groove 22 receives the workpiece pressed downward by the descending punch 1, thereby bending the workpiece. In Fig. 5A, for simplicity of illustration, the workpiece W is shown spaced apart above the die 2.
[0041] As shown in Figure 4, the V-groove portion 22 is formed in a V-groove shape with a pair of inclined surfaces tapering downward. The inclined flat surface on the front side of the V-groove portion 22 is a first groove surface 22a as a first inner surface, and the inclined flat surface on the rear side is a second groove surface 22b as a second inner surface. In the V-groove portion 22, the first groove surface 22a has a first recess 221 extending in the left-right direction, and the second groove surface 22b has a second recess 222 extending in the left-right direction. The first recess 221 and the second recess 222 are collectively referred to as recess E.
[0042] The first groove surface 22a and the second groove surface 22b are ground by a die forming grindstone 6 (see FIG. 5D) to form a predetermined surface. The die forming grindstone 6 will be described later.
[0043] A V-groove portion 22 worn through use can be regenerated by applying the bending die regeneration method according to the first embodiment as follows. Figure 5A shows the V-groove portion 22, which is the surface Aa to be regenerated in a worn state. The outermost two-dot chain line is the reference groove line LN2a, which indicates the outer shape of the unused, unworn state. The outer shape of the worn state is indicated by the solid wear groove line LN2b. The two-dot chain removal groove line LN2c indicates the position to be removed in the next process. The pair of front and rear removal groove lines LN2c are set below the wear groove line LN2b as straight lines with inclination angles close to those of the first groove surface 22a and the second groove surface 22b, respectively.
[0044] 5B, the portion of the V-groove portion 22 in this worn state that is located on the tip side (upper side) of the removal groove line LN2c is removed by polishing or the like. The removal is performed over the entire range in the longitudinal direction (left-right direction) of the die 2. As a result, a first removal surface 22ad and a second removal surface 22bd, which are flat surfaces extending in the front-rear and left-right directions at the position of the removal groove line LN2c, are formed on the first groove surface 22a and the second groove surface 22b, respectively.
[0045] Next, as shown in FIG. 5C , padding portions 23 are formed at both front and rear end portions of the V-groove portion 22. The front padding portion 23 is referred to as the first padding portion 23a, and the rear padding portion 23 is referred to as the second padding portion 23b. The front first padding portion 23a is formed to completely cover the first removal surface 22ad. That is, padding end position P4a, which is the lower end of the padding, is located closer to the back of the V-groove portion 22 than removal surface end position P3a, which is the connection position between the removal surface 2ad and the first groove surface 22a. Similarly, the rear second padding portion 23b is formed to completely cover the second removal surface 22bd. That is, padding end position P4b, which is the lower end of the padding, is located closer to the back of the V-groove portion 22 than removal surface end position P3b, which is the connection position between the second removal surface 2bd and the second groove surface 22b. The padding portions 23 are collectively referred to as padding portions B. Moreover, the build-up end positions P4a and P4b are collectively included in the end Ba.
[0046] There is no limitation on the method of cladding in the V-groove portion 22. For example, methods such as laser cladding, PTA (Plasma Transferred Arc Welding) welding, and thermal spraying can be used. In addition, the metal to be cladded is also not limited, and may be a material different from the material of the die main body portion 21 of the base material A, and may be selected appropriately depending on the application and specifications.
[0047] The removal amount and build-up amount for obtaining the first removal surface 22ad and the second removal surface 22bd may be adjusted and set as appropriate according to the amount of wear of the first groove surface 22a and the second groove surface 22b of the V-groove portion 22. When the removal amount is large, the removal surface end positions P3a, P3b are positioned further downward, and therefore, in order to cover the first removal surface 22ad and the second removal surface 22bd, the build-up end positions P4a, P4b must be positioned further downward, requiring a larger build-up amount.
[0048] Next, as shown in Fig. 5D, the die forming grindstone 6 is used to cut and form the buildup portion 23, forming a recycled die groove portion 24 corresponding to the reference groove line LN2a. As shown in Figs. 5D and 6B, the die forming grindstone 6 is a grindstone having a cylindrical or disk-shaped base body 60, and a predetermined grinding portion 6G is formed on the circumferential surface. The predetermined grinding portion 6G has a shape corresponding to the final finished shape of the V-groove portion 22. The die forming grindstone 6 is included in the general term grinding wheel C, and the grinding portion 6G is included in the general term grinding portion Ca.
[0049] The grinding portion 6G has a first convex inclined grinding wheel surface 6a that forms the first groove surface 22a of the V-groove portion 22 and a second convex inclined grinding wheel surface 6b that forms the second groove surface 22b of the V-groove portion 22. The first convex inclined grinding wheel surface 6a has a first circumferential convex portion 61 that forms the first recessed portion 221 of the V-groove portion 22, and the second convex inclined grinding wheel surface 6b has a second circumferential convex portion 62 that forms the second recessed portion 222 of the V-groove portion 22. The first circumferential convex portion 61 and the second circumferential convex portion 62 are convex portions formed around the entire circumference in shapes corresponding to the shapes of the first recessed portion 221 and the second recessed portion 222, respectively. The first circumferential convex portion 61 and the second circumferential convex portion 62 are included in the general term circumferential convex portion Ca1.
[0050] The die forming grinding wheel 6 is attached to a grinding machine (not shown) and rotates about an axis CL6, and is pressed against the V-groove portion 22. As a result, the V-groove portion 22 is ground into a shape corresponding to the grinding portion 6G.
[0051] By using this die forming grinding wheel 6 to cut and form a V-groove portion 22 having a padding portion 23, a first recess 221 corresponding to the first circumferential convex portion 61 is formed on the first groove surface 22a of the recycled die groove portion 24, and a second recess 222 corresponding to the second circumferential convex portion 62 is formed on the second groove surface 22b.
[0052] As shown in FIG. 5D , the first recess 221 is formed by removing a range including the buildup end position P4a from the first groove surface 22a. The second recess 222 is formed by removing a range including the buildup end position P4b from the second groove surface 22b. The depth Dp2 of the first recess 221 and the second recess 222 is determined according to the tolerance set for the dimension in the thickness direction (front-to-back direction in FIG. 5D ) of the die 2. For example, if the tolerance for the dimension D2 in the thickness direction (see FIG. 4 ) is set to "+0 mm to -0.05 mm," the depth Dp2 may be set to a value exceeding 0.05 mm in calculation, but may be set to, for example, 0.1 mm to allow for some margin of error.
[0053] The shapes of the first recess 221 and the second recess 222 are not limited as long as they do not protrude from the first groove surface 22a and the second groove surface 22b, respectively. The shapes of the first recess 221 and the second recess 222 may be concave curved surfaces with curved cross sections, or may include three-dimensional flat surfaces in which some of the curved cross sections are straight. For example, the first recess 221 may be connected to the first groove surface 22a so that its upper and lower ends are clearly curved. Furthermore, the first recess 221 may be shaped so that its upper and lower ends are smoothly connected to the first groove surface 22a by being rounded, which is desirable from the perspective of minimizing the impact on the workpiece W during coining. The same applies to the second recess 222.
[0054] As described above, the worn V-groove shape is restored by the bending die restoration method according to the first embodiment, and a die 2 having an unused restored die groove portion 24 is obtained.
[0055] Whether or not to remove the portion on the tip side of the V-groove portion 22 may be determined depending on the degree of wear. That is, when regenerating when the degree of wear is small, the method for regenerating a bending die according to the second embodiment described above may be carried out by forming the padding portion 23 without removing the portion on the tip side, and grinding the V-groove portion 22 with the die forming grindstone 6 to form it into the reference groove shape.
[0056] As described above, according to the first and second embodiments of the present invention, the ranges including the ends of the buildup portions 13, 23 are hollowed out to form the first recesses 121, 221 and the second recesses 122, 222, so that no steps are formed at the ends. Therefore, the recycled bending die K has a high appearance quality, and further, when the bending is performed by so-called coining, there is no risk of lines corresponding to the steps being formed on the workpiece W, and the bent workpiece W has a high appearance quality.
[0057] The embodiment of the present invention is not limited to the above-described configurations and procedures, and may be modified within the scope of the gist of the present invention.
[0058] The first recesses 121, 221 and the second recesses 122, 222 are formed by carving out the portions that will become the ends of the padding portions 13, 23, respectively, and the depth, formation range, cross-sectional shape, etc. of the carved out portions can be freely set depending on the range of the worn portion and the degree of wear.
[0059] The punch body 11 and the die body 21, which are the base material A, are formed from a first metal material, and the padding portions 13 and 23, which are the padding portions B, are formed from a second metal material. The first and second materials do not have to be the same, and the second material that comes into contact with the workpiece W may be a metal material different from the first material that has better wear resistance or chipping resistance.
[0060] Although the regeneration of bending dies having worn portions has been described, the regeneration in this invention is not limited to regeneration from wear, but also includes repair of portions that have been damaged due to corrosion, overload, etc.
[0061] As described in detail above, a method for recycling bending dies according to one embodiment of the present invention includes a build-up process for forming a build-up portion B covering the entire surface Aa to be recycled on a base material A of a recycled bending die K having a surface Aa to be recycled that has a shape different from the reference shape, and a shaping process for rotating a grinding wheel C having a grinding portion Ca that grinds the build-up portion B to shape the build-up portion B into the reference shape and regenerate it, wherein the grinding portion Ca of the grinding wheel C has a peripheral convex portion Ca1 that is carved out to include the external end portion Ba of the build-up portion B that connects to the base material A, and the shaping process forms a recess E in the recycled bending die K by the peripheral convex portion Ca1 that includes the external boundary between the base material A and the build-up portion B.
[0062] As a result, a recess E is formed that includes the boundary between the base material A and the built-up portion B, and no steep step is formed where the built-up portion B protrudes from the surface of the recycled bending die K. Therefore, the recycled bending die K has high appearance quality, and even if the recycled bending process is coining, no line corresponding to the step is formed on the surface of the workpiece W, so the appearance quality is not reduced.
[0063] In addition, in this one embodiment, the recycled bending mold K is a punch mold 1, and the cutting edge portion of the punch mold 1 has a first outer surface 12a and a second outer surface 12b that approach each other toward the tip, and the recess E may be simultaneously formed as a first recess 121 on the first outer surface 12a and a second recess 122 on the second outer surface 12b.
[0064] This reduces the time required to regenerate the punch die 1, which is the regenerated bending die K.
[0065] In addition, in this one aspect, the recycled bending mold K is a die mold 2 having a V-groove portion 22, and the V-groove portion 22 has a first inner surface 22a and a second inner surface 22b that approach each other as they move toward the back, and the recess E may be simultaneously formed as a first recess 221 on the first inner surface 22a and a second recess 222 on the second inner surface 22b.
[0066] This reduces the time required to regenerate the die 2, which is the regenerated bending tool K.
[0067] In this embodiment, the build-up portion B may be formed by stacking metal powder.
[0068] This allows for thin buildup and precise control of buildup thickness. It also makes the welded surface, which is the layered surface, smooth.
[0069] A recycled bending die according to one embodiment of the present invention comprises a first portion MA, which is approximately plate-shaped and formed from a first material, and which has at one edge a cutting edge portion 12 or a V-groove portion 22 whose cross-sectional shape is V-shaped and made up of a first surface and a second surface, and a second portion MB, which is provided on the tip side of the cutting edge portion 12 or V-groove portion 22 and is formed from a second material different from the first material, and the first surface and the second surface each have a recess E formed in a range that includes the external boundary between the first portion MA and the second portion MB.
[0070] As a result, when the first region MA is the base material A and the second region MB is the built-up portion B, there is a recess E including the boundary between them, so no steep step is formed where the built-up portion B is convex from the surface of the recycled bending die K. Therefore, the appearance quality of the recycled bending die K is not degraded, and even if the bending process is coining, no line corresponding to the step is left on the surface of the workpiece W, so the appearance quality is not degraded.
[0071] This aspect may also be a punch die 1 having a cutting edge portion 12 in the first region MA.
[0072] As a result, a steep step where the padding portion B becomes a convex portion is not formed on the surface of the recycled punch die 1, and the recycled punch die 1 does not leave lines on the surface of the workpiece W due to the padding portion B, so the appearance quality of the workpiece W is not reduced.
[0073] Also, this aspect may be a die 2 having a V-groove portion 22 in the first portion MA.
[0074] As a result, a steep step is not formed on the surface of the recycled die mold 2 where the built-up portion B becomes a convex portion, and the recycled die mold 2 does not leave lines on the surface of the workpiece W due to the built-up portion B, so the appearance quality of the workpiece W is not reduced.
[0075] REFERENCE SIGNS LIST 1 punch die 11 punch body 12 cutting edge 12a first inclined surface (first outer surface) 12b second inclined surface (second outer surface) 12c tip wear surface (surface to be recycled) 12d removal surface 121 first recess 122 second recess 13 buildup portion 14 recycled punch top 2 die die 21 die body 22 V-groove 22a first groove surface 22ad first removal surface 22b second groove surface 22bd second removal surface 221 first recess 222 second recess 23 buildup portion 23a first buildup portion 23b second buildup portion 24 recycled die groove 5 punch forming grindstone 5a first concave inclined grindstone surface 5b second concave inclined grindstone surface 5G grinding portion 50 base 51 first peripheral convex portion 52 Second peripheral convex portion 6 Die forming grinding wheel 6a First convex inclined grinding wheel surface 6b Second convex inclined grinding wheel surface 6G Grinding portion 60 Base body 61 First peripheral convex portion 62 Second peripheral convex portion A Base material Aa Surface to be recycled B Built-up portion C Grinding wheel Ca Grinding portion E Recess CL5, CL6 Axis Dp1, Dp2 Depth D1, D2 Dimension K Recycled bending die MA First portion MB Second portion LN1a Reference cutting edge line LN1b Wear cutting edge line LN1c Removal cutting edge line LN2a Reference groove line LN2b Wear groove line LN2c Removal groove line P1a, P1b, P3a, P3b Removal surface end positions P2a, P2b, P4a, P4b Built-up end positions Double work
Claims
1. A method for regenerating a bending die, comprising: a build-up process for forming a build-up portion covering the entire surface to be regenerated on a base material of a bending die having a surface to be regenerated that is a shape different from a reference shape; and a shaping process for shaping the build-up portion into the reference shape by rotating a grinding wheel having a grinding portion that grinds the build-up portion, wherein the grinding portion of the grinding wheel has a peripheral convex portion that is carved out to include the visible end portion of the build-up portion that connects to the base material, and the shaping process forms a recess in the bending die by the peripheral convex portion that includes the visible boundary between the base material and the build-up portion.
2. A method for recycling a bending die as described in claim 1, wherein the bending die is a punch die, the cutting edge of the punch die has a first outer surface and a second outer surface which approach each other as the cutting edge approaches the tip, and the recesses are simultaneously formed as a first recess on the first outer surface and a second recess on the second outer surface.
3. A method for regenerating a bending die as described in claim 1, wherein the bending die is a die having a V-groove portion, the V-groove portion having a first inner surface and a second inner surface which approach each other as they approach the back, and the recesses are simultaneously formed as a first recess on the first inner surface and a second recess on the second inner surface.
4. A method for regenerating bending dies according to any one of claims 1 to 3, in which the build-up portion is formed by stacking metal powder.
5. A recycled bending die comprising: a first portion which is approximately plate-shaped and made of a first material, and which has at one edge a cutting edge or V-groove portion whose cross-sectional shape is V-shaped formed by a first surface and a second surface; and a second portion which is provided on the tip side of the cutting edge or V-groove portion and which is made of a second material different from the first material, wherein the first surface and the second surface each have a recess formed in an area including the apparent boundary between the first portion and the second portion.
6. A recycled bending die according to claim 5, which is a punch die having the cutting edge portion in the first portion.
7. A recycled bending die according to claim 5, which is a die having the V-groove portion in the first portion.
Citation Information
Patent Citations
Method for weld-repairing and welding metallic member, and welding device
JP1993261556A
Production of press die
JP1994297055A
Welding material for cladding and overlay welding method
JP2004066261A
Punch and die for press brake
JP2014076464A