Lithium secondary battery comprising amorphous silicon thin film anode and manufacturing method therefor
The use of a phosphorus-doped amorphous silicon thin film anode and a low-reactivity electrolyte assembled under pressure addresses the conductivity and stability issues in lithium secondary batteries, enabling high-speed charging and extended lifespan by preventing electrode peeling and cracking.
Patent Information
- Application Number
- PCT/KR2024/005561
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-28
AI Technical Summary
Lithium secondary batteries face issues with low electrical conductivity and volume expansion of silicon anodes, leading to electrode cracking and peeling, which affects their cycle characteristics and safety due to reactions with organic electrolytes.
An amorphous silicon thin film anode is used, doped with elements like phosphorus and deposited on a current collector using PECVD, combined with a low-reactivity electrolyte and assembled under pressure to enhance electrical conductivity and prevent peeling.
The solution enables high-speed charging, improved electrical conductivity, and suppressed peeling due to volume changes, resulting in better cycle characteristics and lifespan of the lithium secondary battery.
Smart Images

Figure KR2024005561_28112024_PF_FP_ABST
Abstract
Description
Lithium secondary battery including amorphous silicon thin film cathode and method for manufacturing the same
[0001] This specification claims the benefit of Korean Patent Application No. 10-2023-0065563, filed with the Korean Intellectual Property Office on May 22, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a lithium secondary battery comprising an amorphous silicon thin film negative electrode. More specifically, the present invention relates to a lithium secondary battery comprising a positive electrode, an amorphous silicon thin film negative electrode, and an electrolyte having low reactivity with the negative electrode, which enables high-speed charging and suppresses delamination of the electrode during operation.
[0003]
[0004] With the steady increase in technological development and demand for electronic devices, lithium secondary batteries are being studied in a wide range of fields, from small devices like mobile phones, laptops, and camcorders to large-scale devices like electric vehicles and power storage systems. In particular, research on lithium secondary batteries primarily focuses on high energy density, stability, and safety, with the goal of providing safe lithium secondary batteries with long lifespans and high capacities.
[0005] Lithium secondary batteries, as a type of secondary battery, offer greater capacity per unit area and higher energy density than nickel-cadmium and manganese batteries. However, lithium secondary batteries are prone to overheating and have poor output, making them difficult to use as next-generation batteries.
[0006] Furthermore, lithium secondary batteries utilize liquid electrolytes containing organic solvents, which pose a high risk of leakage and fire, making it essential to ensure safety. Consequently, interest in and research into lithium secondary batteries, which offer both high energy density and high output while maintaining safety, has grown significantly.
[0007] Recently, active research has been conducted on lithium secondary batteries using Li-Si as a next-generation anode active material. The theoretical specific capacity of silicon (Si) is 3,579 mAh / g, which is superior to the specific capacity of graphite carbon, a commercial anode (372 mAh / g). However, silicon suffers from low electrical conductivity and, during charge / discharge, repeated lithium insertion and desorption causes volume expansion and contraction, leading to electrode cracking. Furthermore, persistent side reactions with the organic electrolyte can lead to active material exfoliation. This leads to electrical short-circuits between electrode / current collector, electrode / electrode, and electrode / electrolyte, resulting in deterioration of continuous cycling characteristics.
[0008] To improve the low electrical conductivity of silicon anodes and surface deterioration due to volume change, various research methods such as silicon structure improvement and surface modification are being conducted, and there is a need to realize the manufacture of lithium secondary batteries with high reversible capacity and excellent charge / discharge cycle characteristics through more diverse research.
[0009]
[0010] The problem to be solved by the present invention is to provide a silicon anode having fast charging and long life characteristics and a lithium secondary battery including the same by improving the existing low electrical conductivity and deterioration problems due to volume change.
[0011] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0012]
[0013] One embodiment of the present invention provides a lithium secondary battery comprising: a negative electrode in which an amorphous silicon active material is laminated on a negative electrode current collector; a positive electrode in which a positive electrode active material is laminated on a positive electrode current collector; and an electrolyte having low reactivity with the negative electrode; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0014] The above amorphous silicon active material is characterized by a thickness of 0.05 μm or more and 10 μm or less.
[0015] The above amorphous silicon active material is characterized by being doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic. Preferably, the above amorphous silicon active material is characterized by being doped with the phosphorus (P) element.
[0016] The above amorphous silicon active material has an element doping concentration of 1.0x10 11 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 It is characterized by the following.
[0017] The above amorphous silicon active material is characterized in that it is laminated on the negative electrode current collector using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
[0018] The above negative electrode collector is characterized by including one or more of Ni, Cu, Fe, Ti, C, Ag, and stainless steel.
[0019] The above positive electrode active material is characterized by including an oxide or a mixture thereof including at least one of Ni, Co, Mn, Fe, Al, Mg, and V and Li.
[0020] The above positive electrode collector is characterized by including one or more of Al, Fe, Ni, Ti, Ag, and stainless steel.
[0021] The electrolyte having low reactivity with the above cathode is characterized by being at least one of an oxide system, a halide system, a complex hydride system, and a sulfide system.
[0022] It is characterized in that the above lithium secondary battery is manufactured by applying pressure of 4 MPa or more and 125 MPa or less.
[0023] Another embodiment of the present invention provides a method for manufacturing a lithium secondary battery, comprising the steps of: manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector; manufacturing a negative electrode by depositing amorphous silicon on a negative electrode current collector; and manufacturing an electrolyte having low reactivity with the negative electrode, and bonding the positive electrode to one surface of the electrolyte and the negative electrode to the other surface; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0024]
[0025] A lithium secondary battery according to one embodiment of the present invention uses a PECVD process in manufacturing an anode by depositing an amorphous silicon active material on an anode current collector, thereby enabling doping of other elements simultaneously with silicon deposition, having a fast deposition speed, and being easily applicable to a large-area process.
[0026] In addition, a lithium secondary battery according to one embodiment of the present invention has the advantage of being capable of high-speed charging by improving electrical conductivity by doping other elements into amorphous silicon.
[0027] In addition, since the lithium secondary battery according to one embodiment of the present invention is manufactured under pressurized conditions, the amorphous silicon negative electrode has an advantage in suppressing peeling due to volume change during battery operation.
[0028] The effects of the present invention are not limited to the effects described above, and effects not mentioned will be clearly understood by those skilled in the art from the present specification and the attached drawings.
[0029]
[0030] Figure 1 is a cross-sectional view of a lithium secondary battery according to one embodiment of the present invention.
[0031] Figures 2a to 2c are SEM photographs of an amorphous Si thin film after operation of a lithium secondary battery according to Comparative Examples 1 to 3, and Figure 2d is an SEM photograph of an amorphous Si thin film after operation of a lithium secondary battery according to Example 1.
[0032] Figure 3 is a graph showing the capacity change according to cycle operation of a lithium secondary battery manufactured in Example 1 and Comparative Example 1 of the present invention.
[0033]
[0034] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0035] Throughout this specification, when it is said that an element is "on" another element, this includes not only cases where the element is in contact with the other element, but also cases where another element exists between the two elements.
[0036]
[0037] Hereinafter, the present invention will be described in more detail.
[0038]
[0039] Fig. 1 is a cross-sectional view of a lithium secondary battery according to one embodiment of the present invention. Referring to Fig. 1, one embodiment of the present invention provides a lithium secondary battery (10) including: a negative electrode in which an amorphous silicon active material (2) is laminated on a negative electrode current collector (1); a positive electrode in which a positive electrode active material (4) is laminated on a positive electrode current collector (5); and an electrolyte (3) having low reactivity with the negative electrode; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0040]
[0041] The negative electrode current collector (1) is not limited as long as it has conductivity and does not cause chemical changes during battery charging and discharging, and is made of at least one selected from Ni, Cu, Fe, Ti, C, Ag, and stainless steel, and preferably Cu, Ni, or stainless steel.
[0042]
[0043] The above amorphous silicon active material (2) has an amorphous structure and is manufactured by depositing it on a negative electrode current collector. The silicon active material deposition method may include PECVD (Plasma Enhanced Chemical Vapor Deposition), RF sputtering, CVD (Chemical Vapor Deposition), MOCVD (Metal-Organic Chemical Vapor Deposition), ALD (Atomic Layer Depostion), MLD (Molecular Layer Deopsition), and LAD (Laser-Assisted Deposition), and PECVD is preferably used.
[0044] The above amorphous silicon active material (2) is characterized by a thickness of 0.05 μm or more and 10 μm or less.
[0045] If the thickness of the above amorphous silicon active material (2) is less than 0.05 μm, it may be difficult to use a lithium secondary battery due to low energy density.
[0046] Meanwhile, if the amorphous silicon active material (2) has a thickness exceeding 10 μm, it may be difficult to use in a lithium secondary battery due to a peeling problem caused by a large volume change during battery operation.
[0047] The above amorphous silicon active material is characterized in that it is disposed on the negative electrode current collector by a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
[0048] In the process of placing the amorphous silicon active material (2) on the negative electrode current collector (1) using PECVD, one or more of silane, disilane, dichlorosilane, and tetraethylorthosilicate may be used as a precursor gas.
[0049] In the process of placing the above amorphous silicon active material (2) on the above negative electrode current collector (1), argon, helium, hydrogen, etc. can be used as a carrier gas, and hydrogen can be preferably used.
[0050] The above amorphous silicon active material (2) is characterized by being doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic. Preferably, the above amorphous silicon active material is characterized by being doped with the phosphorus (P) element.
[0051] The type of doping desired for the amorphous silicon active material (2) doping material may vary depending on the type of dopant gas. The dopant gas may include ammonia, phosphine, nitrogen, nitrogen trifluoride, trimethylphosphine, triethylphosphine, oxygen, ozone, carbon dioxide, arsine, tertiarybutylarsine, and trimethylarsine.
[0052] The above amorphous silicon active material (2) has a doping concentration of 1.0x1011 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 It is characterized by the following.
[0053] The doping concentration of the above amorphous silicon active material (2) is 1.0x10 11 atoms / cm 3 If it is less than that, it may be difficult to use lithium secondary batteries due to low electrical conductivity.
[0054] Meanwhile, the doping concentration of the amorphous silicon active material (2) is 5.0x10 22 atoms / cm 3 If it exceeds , the energy density may be low, making it difficult to use lithium secondary batteries.
[0055]
[0056] The electrolyte (3) having low reactivity with the above cathode is an ionic inorganic substance, and is characterized by being at least one selected from among sulfide-based, oxide-based, complex hydride-based, and halide-based inorganic substances.
[0057] The above sulfide-based ion-conducting inorganic particles are Li6PS5Cl(LPSCl), Li 10 GeP2S 12 (LGPS), Li2S-P2S5(LPS) solid electrolyte materials, etc. According to one embodiment of the present invention, LPSCl having an argyrodite structure can be used as a sulfide-based solid electrolyte.
[0058] The above oxide-based ion-conducting inorganic particles are Li 3x La 2 / 3-x TiO3(LLTO), L7La3Zr2O 12 (LLZO) may be included.
[0059] The above halide-based ion-conducting inorganic particles may include Li3YCl6, Li3YBr6, etc.
[0060] The above complex hydride-based ion-conducting inorganic particles may include LiBH4, LiNH2, LiAlH4, etc.
[0061] The thickness of the electrolyte (3) having low reactivity with the above cathode is not particularly limited, but may be, for example, 20 μm or more and 1000 μm or less.
[0062]
[0063] The above positive electrode active material (4) is characterized by including an oxide containing at least one of Ni, Co, Mn, Fe, Al, Mg, and V and Li, or a mixture thereof, and the oxide containing Li may include, but is not limited to, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium phosphate, and lithium vanadium oxide.
[0064] The above-mentioned positive electrode current collector (5) is not limited as long as it has conductivity and does not cause chemical changes during battery charging and discharging, and is made of at least one selected from among Al, Fe, Ni, Ti, Ag, and stainless steel, but is not limited to these.
[0065]
[0066] The above positive electrode, negative electrode and electrolyte are characterized in that they are assembled under pressure.
[0067] The pressure range during the manufacture of a lithium secondary battery (10) according to one embodiment of the present invention is characterized by manufacturing it by applying pressure of 4 MPa or more and 125 MPa or less.
[0068] When the pressure range is less than 4 MPa during the manufacture of the above lithium secondary battery (10), non-contact between the electrolyte and the negative or positive electrode may occur, making it difficult to implement the lithium secondary battery.
[0069] In addition, when the pressure range exceeds 125 MPa during the manufacture of the lithium secondary battery (10), cracks may occur in the negative electrode or positive electrode due to excessive pressure, making it difficult to implement the lithium secondary battery, and there may be a problem of reduced charge and discharge capacity.
[0070]
[0071] Another embodiment of the present invention provides a method for manufacturing a lithium secondary battery, comprising the steps of: manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector; manufacturing a negative electrode by depositing amorphous silicon on a negative electrode current collector; and manufacturing an electrolyte having low reactivity with the negative electrode, and bonding the positive electrode to one surface of the electrolyte and the negative electrode to the other surface; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0072] A method for manufacturing a lithium secondary battery according to one embodiment of the present invention first includes a step of manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector.
[0073] The above positive electrode active material slurry is prepared by mixing a positive electrode active material including an oxide or a mixture thereof containing at least one of Ni, Co, Mn, Fe, Al, Mg, and V and Li, with a conductive agent, a binder, and an ionic inorganic substance in a solvent.
[0074] The conductive material may be, for example, carbon (e.g., Super-P). In addition, the conductive material may be any one selected from the group consisting of carbon black, acetylene black, Ketjen black, and carbon fiber, or a mixture of two or more thereof.
[0075] The above binder may be, for example, NBR (Nitrile Butadiene Rubber). In addition, a polymer compound may be a polymer compound that mixes one or more of diene-based, fluorine-based, acrylic-based, and silicone-based polymer compounds. Throughout the specification of this patent, when a part is said to "include" a certain component, this does not mean that other components are excluded, but rather that other components may be included, unless otherwise specifically stated.
[0076] Throughout this specification, when it is said that an element is "on" another element, this includes not only cases where the element is in contact with the other element, but also cases where another element exists between the two elements.
[0077]
[0078] Hereinafter, the present invention will be described in more detail.
[0079]
[0080] Figure 1 is a cross-sectional view of a lithium secondary battery according to one embodiment of the present invention. Referring to Figure 1, one embodiment of the present invention provides a lithium secondary battery (10) including: a negative electrode in which an amorphous silicon active material (2) is laminated on a negative electrode current collector (1); a positive electrode in which a positive electrode active material (4) is laminated on a positive electrode current collector (5); and an electrolyte (3) having low reactivity with the negative electrode; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0081] The above negative electrode current collector (1) is not limited as long as it has conductivity and does not cause chemical changes during battery charging and discharging, and includes at least one selected from Ni, Cu, Fe, Ti, C, Ag, and stainless steel, and preferably may include Cu, Ni, or stainless steel.
[0082] The above amorphous silicon active material (2) has an amorphous structure and is manufactured by depositing it on a negative electrode current collector. The silicon active material deposition method may include PECVD (Plasma Enhanced Chemical Vapor Deposition), RF sputtering, CVD (Chemical Vapor Deposition), MOCVD (Metal-Organic Chemical Vapor Deposition), ALD (Atomic Layer Depostion), MLD (Molecular Layer Deopsition), or LAD (Laser-Assisted Deposition), and PECVD is preferably used.
[0083] The above amorphous silicon active material (2) is characterized by a thickness of 0.05 μm or more and 10 μm or less.
[0084] If the thickness of the above amorphous silicon active material (2) is less than 0.05 μm, it may be difficult to use a lithium secondary battery due to low energy density.
[0085] Meanwhile, if the amorphous silicon active material (2) has a thickness exceeding 10 μm, it may be difficult to use in a lithium secondary battery due to a peeling problem caused by a large volume change during battery operation.
[0086] The above amorphous silicon active material can be deposited on the negative electrode current collector using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
[0087] In the process of depositing the amorphous silicon active material (2) on the negative electrode current collector (1) using PECVD, one or more of silane, disilane, dichlorosilane, and tetraethylorthosilicate may be used as a precursor gas.
[0088] In the process of laminating the above amorphous silicon active material (2) on the above negative electrode current collector (1), argon, helium, hydrogen, etc. can be used as a carrier gas, and hydrogen can be preferably used.
[0089] The above amorphous silicon active material (2) is characterized by being doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic. Preferably, the above amorphous silicon active material is characterized by being doped with the phosphorus (P) element.
[0090] The type of doping desired for the amorphous silicon active material (2) doping material may vary depending on the type of dopant gas. The dopant gas may include ammonia, phosphine, nitrogen, nitrogen trifluoride, trimethylphosphine, triethylphosphine, oxygen, ozone, carbon dioxide, arsine, tertiarybutylarsine, or trimethylarsine.
[0091] The above amorphous silicon active material (2) has an element doping concentration of 1.0x10 11 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 It is characterized by the following.
[0092] The doping concentration of the above amorphous silicon active material (2) is 1.0x10 11 atoms / cm 3 If it is less than that, it may be difficult to use lithium secondary batteries due to low electrical conductivity.
[0093] Meanwhile, the doping concentration of the amorphous silicon active material (2) is 5.0x10 22 atoms / cm 3If it exceeds , the energy density may be low, making it difficult to use lithium secondary batteries.
[0094]
[0095] The electrolyte (3) having low reactivity with the above cathode is an ionic inorganic substance, and is characterized by being at least one selected from among sulfide-based, oxide-based, complex hydride-based, and halide-based inorganic substances.
[0096] The above sulfide-based ion-conducting inorganic particles are Li6PS5Cl(LPSCl), Li 10 GeP2S 12 (LGPS), Li2S-P2S5(LPS) solid electrolyte materials, etc. According to one embodiment of the present invention, LPSCl having an argyrodite structure can be used as a sulfide-based solid electrolyte.
[0097] The above oxide ionic inorganic particles are Li 3x La 2 / 3-x TiO3(LLTO), L7La3Zr2O 12 (LLZO) may be included.
[0098] The above halide-based ionic inorganic particles may include Li3YCl6, Li3YBr6, etc.
[0099] The above complex hydride ionic inorganic particles may include LiBH4, LiNH2, LiAlH4, etc.
[0100] The thickness of the electrolyte (3) having low reactivity with the above cathode is not particularly limited, but may be, for example, 20 μm or more and 1000 μm or less.
[0101]
[0102] The above positive electrode active material (4) is characterized by including an oxide or a mixture thereof containing at least one of Ni, Co, Mn, Fe, Al, Mg, and V and Li, and the oxide containing Li may include, but is not limited to, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium phosphate, lithium vanadium oxide, etc.
[0103] The above-mentioned positive electrode current collector (5) is not limited as long as it has conductivity and does not cause chemical changes during battery charging and discharging, and is made of at least one selected from among Al, Fe, Ni, Ti, Ag, and stainless steel, but is not limited to these.
[0104]
[0105] The above positive electrode, negative electrode and electrolyte are characterized in that they are assembled under pressure.
[0106] The pressure range during the manufacture of a lithium secondary battery (10) according to one embodiment of the present invention is characterized by manufacturing it by applying pressure of 4 MPa or more and 125 MPa or less.
[0107] When the pressure range is less than 4 MPa during the manufacture of the above lithium secondary battery (10), non-contact between the electrolyte and the negative or positive electrode may occur, making it difficult to implement the lithium secondary battery.
[0108] In addition, when the pressure range exceeds 125 MPa during the manufacture of the lithium secondary battery (10), cracks may occur in the negative electrode or positive electrode due to excessive pressure, making it difficult to implement the lithium secondary battery, and there may be a problem of reduced charge and discharge capacity.
[0109]
[0110] Another embodiment of the present invention provides a method for manufacturing a lithium secondary battery, comprising the steps of: manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector; manufacturing a negative electrode by depositing amorphous silicon on a negative electrode current collector; and manufacturing an electrolyte having low reactivity with the negative electrode, and bonding the positive electrode to one surface of the electrolyte and the negative electrode to the other surface; wherein the positive electrode, the negative electrode, and the electrolyte are assembled under pressure.
[0111] A method for manufacturing a lithium secondary battery according to one embodiment of the present invention first includes a step of manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector.
[0112] The above positive electrode active material slurry is prepared by mixing a conductive material, a binder, and an ionic inorganic material in a solvent with a positive electrode active material including at least one of Ni, Co, Mn, Fe, Al, Mg, and V and an oxide or mixture thereof containing Li.
[0113] The conductive material may be, for example, carbon (e.g., Super-P). In addition, the conductive material may be any one selected from the group consisting of carbon black, acetylene black, Ketjen black, and carbon fiber, or a mixture of two or more thereof.
[0114] The above binder may be, for example, NBR (Nitrile Butadiene Rubber). In addition, it may be a polymer compound comprising one or more selected from diene-based, fluorine-based, acrylic-based, and silicone-based polymer compounds.
[0115] The solvent may be, for example, toluene. In addition, it may be any one selected from non-polar organic solvents such as anisole, xylene, etc., or a mixed organic solvent comprising a mixture of these.
[0116] The above ionic inorganic material is characterized by being at least one of an oxide system, a halide system, a complex hydride system, and a sulfide system.
[0117] The positive electrode is manufactured by applying the above positive electrode active material slurry onto a positive electrode current collector made of at least one selected from Al, Fe, Ni, Ti, Ag, and stainless steel.
[0118] Next, a step of manufacturing a cathode by depositing amorphous silicon on a cathode current collector is performed.
[0119] The above amorphous silicon cathode is characterized in that the cathode is manufactured by depositing the anode current collector using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
[0120] In the process of applying the amorphous silicon active material (2) onto the negative electrode current collector (1) using the above PECVD, one or more of silane, disilane, dichlorosilane, and tetraethylorthosilicate may be used as a precursor gas.
[0121] In the process of applying the above amorphous silicon active material (2) onto the negative electrode current collector (1), argon, helium, hydrogen, etc. can be used as a carrier gas, and hydrogen is preferably used.
[0122] The above amorphous silicon active material (2) is characterized by being doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic. Preferably, the above amorphous silicon active material is characterized by being doped with the nitrogen element.
[0123] The type of doping desired for the amorphous silicon active material (2) doping material may vary depending on the type of dopant gas. The dopant gas may include ammonia, phosphine, nitrogen, nitrogen trifluoride, trimethylphosphine, triethylphosphine, oxygen, ozone, carbon dioxide, arsine, tertiarybutylarsine, and trimethylarsine.
[0124] The above amorphous silicon active material (2) has a doping concentration of 1.0x10 11 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 It is characterized by the following.
[0125] The doping concentration of the above amorphous silicon active material (2) is 1.0x10 11 atoms / cm 3 If it is less than that, it may be difficult to use lithium secondary batteries due to low electrical conductivity.
[0126] Meanwhile, the doping concentration of the amorphous silicon active material (2) is 5.0x10 22 atoms / cm 3 If it exceeds , the energy density may be low, making it difficult to use lithium secondary batteries.
[0127] Next, a step is performed to manufacture an electrolyte having low reactivity with the cathode, attach the cathode to one side of the electrolyte, and attach the cathode to the other side.
[0128] Finally, the positive electrode, negative electrode, and electrolyte are assembled under pressure to manufacture a lithium secondary battery.
[0129] According to one embodiment of the present invention, the pressure range during the manufacture of a lithium secondary battery is characterized by manufacturing it by pressurizing it at a pressure of 4 MPa or more and 125 MPa or less.
[0130] When the pressure range is less than 4 MPa during the manufacture of the above lithium secondary battery, non-contact between the electrolyte and the negative or positive electrode may occur, making it difficult to implement the lithium secondary battery.
[0131] In addition, when the pressure range exceeds 125 MPa during the manufacture of the lithium secondary battery, cracks may occur in the negative electrode or positive electrode due to excessive pressure, making it difficult to implement the lithium secondary battery, and there may be a problem of reduced charge and discharge capacity.
[0132]
[0133] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0134]
[0135] [Example]
[0136] (Example 1)
[0137] The cathode was fabricated by depositing an amorphous Si thin film doped with P as an n-type on a Cu substrate by the plasma-enhanced chemical vapor deposition (PECVD) method. The amorphous Si thin film doped with P had an initial vacuum of 6.7 Х 10 -4After adjusting the working pressure to 79 Pa, the deposition was performed under the conditions of a flow ratio of hydrogen, silane, and phosphine gases of 4:1:1, a high-frequency power of 30 W, and a working temperature of 220°C. LPSCl was used as the electrolyte, and lithium metal was used as the anode. The negative electrode, electrolyte, and anode were assembled under a pressure of 20 MPa to manufacture a lithium secondary battery.
[0138] (Comparative Example 1)
[0139] Amorphous Si thin films were deposited on Cu substrates by plasma-enhanced chemical vapor deposition (PECVD) method. The amorphous Si thin films were deposited at an initial vacuum of 6.7 Х 10 -4 After adjusting the working pressure to 53.3 Pa, the deposition was performed under the conditions of a high-frequency power of 30 W and a working temperature of 220°C under the conditions of a flow rate ratio of hydrogen and silane gases of 1:1 each. The electrolyte was a mixture of ethylene carbonate (EC) and diethylene carbonate (DEC) mixed solvent (volume ratio = 1:1) with 1 M LiPF6 added to a mixture of 10 wt% fluoroethylene carbonate (FEC), and lithium metal was used as the positive electrode to manufacture a lithium secondary battery.
[0140] (Comparative Example 2)
[0141] A lithium secondary battery was manufactured using a thin film according to Example 1 of the present invention as a negative electrode. Here, the amorphous Si thin film doped with P of Example 1 was used as the negative electrode, and the electrolyte was a mixed solution in which 1 M LiPF6 was added to a mixed solvent of ethylene carbonate (EC) and diethylene carbonate (DEC) (volume ratio = 1: 1) and 10 wt% fluoroethylene carbonate (FEC) was added, and lithium metal was used as the positive electrode to manufacture a lithium secondary battery.
[0142] (Comparative Example 3)
[0143] An amorphous Si thin film according to Comparative Example 1 of the present invention was used as a cathode, LPSCl was used as an electrolyte, and lithium metal was assembled as a cathode under a pressure of 20 MPa to manufacture a lithium secondary battery.
[0144] (Comparative Example 4)
[0145] A P-doped amorphous Si thin film according to Example 1 of the present invention was used as a cathode, LPSCl was used as an electrolyte, and lithium metal was assembled as a cathode without pressurization to manufacture a lithium secondary battery.
[0146] (Comparative Example 5)
[0147] A P-doped amorphous Si thin film according to Example 1 of the present invention was used as a cathode, LPSCl was used as an electrolyte, and lithium metal was assembled as a cathode under a pressure of 130 MPa to manufacture a lithium secondary battery.
[0148]
[0149] (Experimental Example 1: Electrical Conductivity Measurement Evaluation)
[0150] The electrical characteristics of Example 1 and Comparative Example 1 were measured using the Transfer Line Method (TLM) to obtain the electrical conductivity σ. c was evaluated and the results are shown in Table 1. The contact resistance evaluation was performed by forming a TLM element structure with different intermetal distances and measuring the resistance according to the intermetal distance, and the contact resistance R was calculated from the y-intercept of this graph. c And the surface resistance R with a slope s Find the average transmission distance L between metals here. T and the width W of the metal, the contact resistance R c , surface resistance R s and contact resistance ρ c The contact resistance was calculated from the following mathematical expression 1, which is the relationship between the contact resistance and the contact resistance ρ calculated from the following mathematical expression 2. c Electrical conductivity σ through c was calculated.
[0151] [Mathematical Formula 1]
[0152] R c = ρ c / (L T W)=(R S L T ) / W
[0153] [Equation 2]
[0154] σ c = 1 / ρ c
[0155] Comparative Example 1 Example 1 Electrical Conductivity 6.72X10 -8 S / cm6.87X10 -3 S / cm
[0156] Referring to Table 1 above, it was confirmed that the electrical conductivity of the silicon thin film cathode according to Example 1 of the present invention showed a higher electrical conductivity than that of Comparative Example 1. Since Example 1 has a high electrical conductivity, rapid charging and discharging at a high current (1C) is possible during the driving process, and Comparative Example 1, which has a low electrical conductivity, has a high overvoltage and puts a strain on the electrode during rapid charging and discharging under high current conditions.
[0157]
[0158] (Experimental Example 2: Evaluation of the driving characteristics of amorphous silicon thin film)
[0159] The operability of the lithium secondary batteries according to Example 1 and Comparative Examples 1 to 5 and the presence of cracking on the thin film surface after charge and discharge operation were checked, and the evaluation results are shown in Table 2. The charge and discharge operation was measured by performing charge and discharge 100 times each under the current condition of 1C at the operating voltage of 1.5 V to 0.1 V. At this time, the operability was evaluated as ○ when a capacity of 500 mAh / g or more was developed during charge and discharge operation, and × when no capacity was developed. The surface stability was evaluated as × when cracking and peeling of the Si thin film occurred with reference to Fig. 2, △ when cracking occurred, and ○ when neither cracking nor peeling occurred.
[0160] Referring to Table 2, it was confirmed that the battery manufactured without pressurization in Comparative Example 4 and the battery manufactured by pressurizing at 130 MPa or more in Comparative Example 5 did not operate due to lack of interface contact and excessive pressure, respectively.
[0161] Referring to FIG. 2d, it can be confirmed that the P-doped amorphous Si thin film manufactured in Example 1 did not experience any cracking or peeling after driving.
[0162] Referring to FIGS. 2a and 2b, it can be confirmed that the amorphous Si thin films manufactured in Comparative Examples 1 and 2 not only had cracks on the surface of the thin films after operation, but also had peeling. In Comparative Examples 1 and 2, the cracking phenomenon on the electrodes became more severe because a high overvoltage was applied and a strain was applied to the electrodes during rapid charge / discharge under high current conditions. Specifically, since Comparative Examples 1 and 2 used highly reactive organic liquid electrolytes, a side-reactive layer was formed on the electrode surface during the operation process. The silicon electrode undergoes a volume change during the charge / discharge process, and the side-reactive layer cannot withstand this and collapses, exposing the electrode surface again, which forms a side-reactive layer again, causing a continuous increase in battery resistance. This is also a major cause of the strain on the electrodes, which induces the cracking phenomenon on the electrodes.
[0163] Referring to Fig. 2c, it can be confirmed that the surface of the amorphous Si thin film manufactured in Comparative Example 3, which used the low-reactivity electrolyte and changed the electrical conductivity variable, was cracked after driving.
[0164]
[0165] Driveability Surface Stability Surface Photo Example 1○○ Degree 2d Comparative Example 1○× Degree 2a Comparative Example 2○× Degree 2b Comparative Example 3○△ Degree 2c Comparative Example 4×-- Comparative Example 5×--
[0166] (Experimental Example 3: Evaluation of the life characteristics of lithium secondary batteries)
[0167] The charge / discharge life characteristics of the lithium secondary batteries according to Example 1 and Comparative Example 1 were evaluated, and the evaluation results are shown in Fig. 3. The charge / discharge characteristics were measured by repeatedly performing charging and discharging under a current condition of 1C at a driving voltage of 1.5 V to 0.1 V.
[0168] Referring to FIG. 3, it was found that the lithium secondary battery according to Example 1 exhibited better life characteristics than the lithium secondary battery according to Comparative Example 1. This shows that the lithium secondary battery according to Example 1 has superior life characteristics because the negative electrode according to Example 1 has high electrical conductivity, has little side reaction with the electrolyte, and is operated in a pressurized environment to suppress volume expansion.
[0169]
[0170] Although the present invention has been described above through limited embodiments, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.
Claims
1. A cathode in which an amorphous silicon active material is laminated on a cathode current collector; A cathode in which a cathode active material is laminated on a cathode current collector; and An electrolyte having low reactivity with the above cathode; A lithium secondary battery characterized in that the positive electrode, negative electrode, and electrolyte are assembled under pressure.
2. In paragraph 1, A lithium secondary battery, characterized in that the above amorphous silicon active material has a thickness of 0.05 μm or more and 10 μm or less.
3. In paragraph 1, A lithium secondary battery, characterized in that the above amorphous silicon active material is doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic.
4. In paragraph 1, The above amorphous silicon active material has a doping concentration of 1.0x10 11 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 A lithium secondary battery characterized by the following:
5. In paragraph 1, A lithium secondary battery, characterized in that the amorphous silicon active material is disposed on the negative electrode current collector by a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
6. In paragraph 1, A lithium secondary battery, characterized in that the negative electrode current collector comprises one or more of Ni, Cu, Fe, Ti, C, Ag, and stainless steel.
7. In paragraph 1, A lithium secondary battery, characterized in that the positive electrode active material comprises an oxide containing at least one of Ni, Co, Mn, Fe, Al, Mg, and V and Li, or a mixture thereof.
8. In paragraph 1, A lithium secondary battery, characterized in that the positive electrode collector comprises one or more of Al, Fe, Ni, Ti, Ag, and stainless steel.
9. In paragraph 1, A lithium secondary battery, characterized in that the electrolyte having low reactivity with the negative electrode is at least one of an oxide system, a halide system, a complex hydride system, and a sulfide system.
10. In paragraph 1, A lithium secondary battery, characterized in that the lithium secondary battery is pressurized at a pressure of 4 MPa or more and 125 MPa or less during the manufacture of the lithium secondary battery.
11. A step of manufacturing a positive electrode by applying a positive electrode active material slurry containing a positive electrode active material onto a positive electrode current collector; A step of manufacturing a negative electrode by depositing an amorphous silicon active material on a negative electrode current collector; and A step of manufacturing an electrolyte having low reactivity with the cathode, attaching the cathode to one surface of the electrolyte, and attaching the cathode to the other surface; A method for manufacturing a lithium secondary battery, characterized in that the positive electrode, negative electrode, and electrolyte are assembled under pressure.
12. In paragraph 11, A method for manufacturing a lithium secondary battery, characterized in that the amorphous silicon active material has a thickness of 0.05 μm or more and 10 μm or less.
13. In paragraph 11, A method for manufacturing a lithium secondary battery, wherein the amorphous silicon active material is doped with one or more elements of nitrogen, oxygen, phosphorus, and arsenic.
14. In paragraph 11, The above amorphous silicon active material has a doping concentration of 1.0x10 11 atoms / cm 3 Ideal 5.0x10 22 atoms / cm 3 A method for manufacturing a lithium secondary battery, characterized by the following.
15. In paragraph 11, A method for manufacturing a lithium secondary battery, characterized in that the amorphous silicon active material is deposited on the negative electrode current collector using a PECVD (Plasma Enhanced Chemical Vapor Deposition) method.
16. In paragraph 11, A method for manufacturing a lithium secondary battery, characterized in that the lithium secondary battery is manufactured by applying pressure of 4 MPa or more and 125 MPa or less.
Citation Information
Patent Citations
Electrode for lithium battery, lithium battery using it, and lithium secondary battery
JP2005235397A
Normal pressure synthesis of sulfide solid electrolyte composition for the solid lithium secondary batteries
KR1020170056338A
Anodes for lithium-based energy storage devices
WO2019165412A1
KR20200069215A