Secondary battery electrode, and secondary battery including same
The multi-layer structure of the negative electrode, incorporating carbon-based and silicon-based materials with conductive polymers and carbon nanotubes, addresses stability and output issues in secondary batteries, enhancing lithium ion mobility and rapid charging performance.
Patent Information
- Application Number
- PCT/KR2024/006140
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-28
AI Technical Summary
Secondary batteries, particularly lithium secondary batteries, face challenges with the stability and output characteristics of their negative electrodes due to mechanical and chemical damage during charging and discharging, leading to decreased electrical conductivity and rapid capacity loss.
A negative electrode with a multi-layer structure comprising a first carbon-based active material layer and a second silicon-based active material layer, including conductive polymers and carbon nanotubes, which reduces resistance and improves high-temperature stability and rapid charging performance.
The multi-layer structure enhances the stability and output characteristics of the negative electrode, enabling improved lithium ion mobility and prolonged battery life with enhanced rapid charging capabilities.
Smart Images

Figure KR2024006140_28112024_PF_FP_ABST
Abstract
Description
Anode for secondary battery and lithium secondary battery containing same
[0001] The present disclosure relates to an anode for a secondary battery and a lithium secondary battery including the same. More specifically, the present disclosure relates to an anode for a secondary battery including a double-layered anode active material layer and a lithium secondary battery including the same.
[0002]
[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as electric and hybrid vehicles.
[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are being actively developed and applied due to their high operating voltage and energy density per unit weight, and their advantages in charging speed and weight reduction.
[0005] For example, a secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte that impregnates the electrode assembly. The secondary battery may further include an outer packaging material, for example, in the form of a pouch, that accommodates the electrode assembly and the electrolyte.
[0006] The above-mentioned negative electrode may use a carbon-based active material or a silicon-based active material as the negative electrode active material. However, the negative electrode active material may suffer mechanical and chemical damage, such as particle cracking, when repeated charging and discharging.
[0007] Changing the composition and structure of negative electrode active materials to improve their particle stability can reduce electrical conductivity, degrading the output characteristics of secondary batteries. Therefore, the development of negative electrode active materials that can simultaneously improve cycle life stability and output characteristics is necessary.
[0008]
[0009] An object of the present disclosure is to provide a negative electrode for a secondary battery having improved output characteristics and rapid charging performance.
[0010] An object of the present disclosure is to provide a lithium secondary battery including a negative electrode for a secondary battery having improved output characteristics and rapid charging performance.
[0011]
[0012] According to exemplary embodiments, a negative electrode for a secondary battery may include a negative electrode current collector, a first negative electrode active material layer formed on at least one surface of the negative electrode current collector and including a first negative electrode active material including at least one of a first carbon-based active material and a first silicon-based active material, and a second negative electrode active material layer formed on the first negative electrode active material layer and including a second negative electrode active material including at least one of a second carbon-based active material and a second silicon-based active material and a conductive polymer.
[0013] In some embodiments, the first carbon-based active material may include a graphite-based active material.
[0014] In some embodiments, the first silicon-based active material and the second silicon-based active material are each SiO x (0<x<2) and may include at least one of a silicon-carbon complex.
[0015] In some embodiments, the weight of the second carbon-based active material included in the second negative electrode active material layer may be greater than the weight of the second silicon-based active material included in the second negative electrode active material layer.
[0016] In some embodiments, the content of the second silicon-based active material may be comprised between 2 wt% and 50 wt% of the total weight of the second negative electrode active material layer.
[0017] In some embodiments, the weight of the first carbon-based active material included in the first negative electrode active material layer may be greater than the weight of the second carbon-based active material included in the second negative electrode active material layer.
[0018] In some embodiments, the second negative active material layer may include a second conductive material including carbon nanotubes (CNTs).
[0019] In some embodiments, the carbon nanotube may comprise a single-wall carbon nanotube (SWCNT).
[0020] In some embodiments, the content of the single-walled carbon nanotubes may be comprised in an amount of 0.01 wt% to 1 wt% of the total weight of the second negative electrode active material layer.
[0021] In some embodiments, the Raman R value of the carbon nanotube may be 0.5 or less. The Raman R value is the intensity (I) of the D band of the Raman spectrum obtained by Raman spectroscopy. D ) and the intensity of the G band (I G ) of the rain (I D / I G ) is defined as.
[0022] In some embodiments, the weight ratio of the content of the conductive polymer in the second negative electrode active material layer to the content of the carbon nanotubes in the second negative electrode active material layer may be 0.01 to 2.
[0023] In some embodiments, the first negative active material layer may not include carbon nanotubes.
[0024] In some embodiments, the conductive polymer may be formed from a monomer including at least one of poly(p-phenylene, PPP), polypyrrole (PPy), polythiophene (PT), polyacetylene, polyaniline (PANI), and poly(3,4-ethylenedioxythiophene, PEDOT).
[0025] In some embodiments, the first negative active material layer may not include a conductive polymer.
[0026] In some embodiments, the content of the conductive polymer may be comprised between 0.01 wt% and 1.5 wt% of the total weight of the second negative electrode active material layer.
[0027] A lithium secondary battery according to exemplary embodiments may include the above-described negative electrode for a secondary battery, and a positive electrode disposed opposite the negative electrode.
[0028]
[0029] According to exemplary embodiments, the negative electrode active material layer may be formed in a multi-layer structure. Furthermore, the upper negative electrode active material layer of the multi-layer structure may include a conductive polymer. Accordingly, the resistance of the negative electrode including the multi-layer structured negative electrode active material layer can be reduced without increasing the content of the conductive material. Furthermore, the reduced resistance can improve output characteristics and enhance rapid charging performance.
[0030] According to some embodiments, the negative electrode active material layer of the multi-layer structure may include carbon nanotubes, and the carbon nanotubes of the upper negative electrode active material layer may have a Raman R value within a predetermined range. Accordingly, the deterioration of life characteristics and stability due to an increase in the content of silicon-based active material in the upper negative electrode active material layer can be suppressed. In addition, high-temperature stability can be improved by applying carbon nanotubes having a Raman R value within the predetermined range.
[0031] The anode for a lithium secondary battery of the present disclosure and the lithium secondary battery comprising the same can be widely applied in green technology fields such as electric vehicles, battery charging stations, and other battery-based solar and wind power generation. The anode for a lithium secondary battery of the present disclosure and the lithium secondary battery comprising the same can be used in eco-friendly electric vehicles, hybrid vehicles, etc., which prevent climate change by suppressing air pollution and greenhouse gas emissions.
[0032]
[0033] FIGS. 1 and 2 are schematic cross-sectional views showing a negative electrode for a secondary battery according to exemplary embodiments.
[0034] FIGS. 3 and 4 are schematic plan views and cross-sectional views, respectively, showing lithium secondary batteries according to exemplary embodiments.
[0035]
[0036] According to exemplary embodiments, a negative electrode for a lithium secondary battery may include a negative electrode active material layer having a multi-layer structure, and a lithium secondary battery may include the negative electrode.
[0037] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the drawings. However, the following drawings attached to this disclosure illustrate preferred embodiments of the present disclosure and, together with the contents of the invention described above, serve to further understand the technical concept of the present disclosure. Therefore, this disclosure should not be interpreted as being limited to the matters described in such drawings.
[0038] The terms “bottom”, “top”, etc. used in this application are used in a relative sense to distinguish the positions of the components, and do not specify absolute positions.
[0039] <Cathode for lithium secondary batteries>
[0040] FIG. 1 is a schematic cross-sectional view showing an anode (hereinafter, abbreviated as a cathode) for a lithium secondary battery according to exemplary embodiments.
[0041] Referring to FIG. 1, the negative electrode (130) may include a negative electrode current collector (125) and a negative electrode active material layer (120).
[0042] The negative electrode (130) may include a negative electrode current collector (125) and a negative electrode active material layer (120) formed by coating a negative electrode active material on at least one surface of the negative electrode current collector (125).
[0043] According to exemplary embodiments, the negative electrode active material layer (120) may have a multi-layer structure including a first negative electrode active material layer (122) and a second negative electrode active material layer (124).
[0044] The negative electrode current collector (125) may include, for example, gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof. In one embodiment, the negative electrode current collector (125) may include copper or a copper alloy.
[0045] The negative electrode active material layer (120) may be formed on at least one surface of the negative electrode current collector (125). The negative electrode active material layer (120) may be coated on at least one surface among the upper surface and the lower surface of the negative electrode current collector (125). The negative electrode active material layer (120) may be in direct contact with the surface of the negative electrode current collector (125).
[0046] According to exemplary embodiments, the first negative electrode active material layer (122) may be formed directly on the surface of the negative electrode current collector (125). The second negative electrode active material layer (124) may be formed directly on the surface of the first negative electrode active material layer (122).
[0047] The first negative electrode active material layer (122) may include a first negative electrode active material including at least one of a first carbon-based active material and a first silicon-based active material. The second negative electrode active material layer (124) may include a second negative electrode active material including at least one of a second carbon-based active material and a second silicon-based active material.
[0048] The first carbon-based active material and the second carbon-based active material may each include, for example, at least one of artificial graphite, natural graphite, hard carbon, soft carbon, cokes, carbon black, and fibrous carbon.
[0049] The first silicon-based active material and the second silicon-based active material are silicon (Si), silicon alloy, and SiO, respectively. x (0<x<2), SiO containing lithium or magnesium compounds x (0<x<2), and may include at least one of a silicon-carbon composite. For example, SiO containing the lithium or magnesium compound x SiO pretreated with lithium or magnesium x may include. For example, SiO containing the lithium or magnesium compound x may contain lithium silicate or magnesium silicate.
[0050] In some embodiments, the first silicon-based active material and the second silicon-based active material are SiO x (0<x<2) and at least one of a silicon-carbon composite may be included. Accordingly, volume expansion of the silicon-based active material can be suppressed, and metal charging performance can be further improved.
[0051] In some embodiments, the first carbon-based active material may include a graphite-based active material. For example, graphite may be used alone as the first carbon-based active material. For example, the graphite may be artificial graphite, natural graphite, or a mixture thereof.
[0052] When artificial graphite is used alone as the first carbon-based active material, it can compensate for the decline in electrode life and stability of a lithium secondary battery. When natural graphite is used alone as the first carbon-based active material, the capacity and output characteristics of a lithium secondary battery can be improved. When a mixture of artificial graphite and natural graphite is used as the first carbon-based active material, the mechanical stability of the negative electrode or secondary battery through artificial graphite can be improved, while additional capacity and output characteristics can be improved through natural graphite.
[0053] In some embodiments, the weight (e.g., weight-based content) of the second carbon-based active material included in the second negative electrode active material layer (124) may be greater than the weight (e.g., weight-based content) of the second silicon-based active material included in the second negative electrode active material layer (124). The silicon-based active material has a high lithium ion storage capacity, which may improve the capacity characteristics of the secondary battery, and the carbon-based active material has high high-temperature stability, which may improve the high-temperature stability of the secondary battery. Since the weight of the second carbon-based active material may be greater than the weight of the second silicon-based active material, the high-temperature stability of the second negative electrode active material layer (124), which is provided as a substantially active negative electrode by being closer to the positive electrode and / or the electrolyte, may be improved.
[0054] In some embodiments, the content of the second silicon-based active material may be included in an amount of 2 wt% to 50 wt%, 5 wt% to 50 wt%, 10 wt% to 50 wt%, 20 wt% to 50 wt%, 30 wt% to 50 wt%, 30 wt% to 45 wt%, 35 wt% to 45 wt%, or 38 wt% to 42 wt% of the total weight of the second negative electrode active material layer (124). In this range, lithiation may be promoted from the surface of the negative electrode (130) through the second negative electrode active material layer (124), and the mobility of lithium ions may be increased, thereby improving the rapid charging characteristics of the secondary battery.
[0055] In some embodiments, the weight of the first carbon-based active material included in the first negative electrode active material layer (122) may be greater than the weight of the second carbon-based active material included in the second negative electrode active material layer (124). Accordingly, the stability of the negative electrode (130) through the first negative electrode active material layer (122) adjacent to the negative electrode current collector (125) can be improved, while the capacity of the secondary battery through the second negative electrode active material layer (124) provided as a practical active negative electrode can be improved.
[0056] According to exemplary embodiments, the first negative electrode active material layer (122) and the second negative electrode active material layer (124) may each include a first conductive material and a second conductive material. In some embodiments, the first conductive material and / or the second conductive material may include carbon nanotubes (CNTs). When the carbon nanotubes are used as the first conductive material and / or the second conductive material, the electrical conductivity of the negative electrode active material layer (120) may be improved, and when combined with a silicon-based active material, the charging characteristics may be further improved.
[0057] In some embodiments, the second conductive material may include carbon nanotubes. Accordingly, the charging characteristics through the second negative electrode active material layer (124), which serves as a practical active negative electrode, may be improved.
[0058] In some embodiments, the carbon nanotube may include a single-walled carbon nanotube (SWCNT). Accordingly, the single-walled carbon nanotube may suppress excessive expansion of the silicon-based active material included in the negative electrode active material layer (120), thereby improving the stability of the secondary battery.
[0059] In one embodiment, the content of the single-walled carbon nanotubes may be included in an amount of 0.01 wt% to 1 wt%, 0.01 wt% to 0.5 wt%, 0.05 wt% to 0.5 wt%, or 0.05 wt% to 0.3 wt% of the total weight of the negative electrode active material layer (120). For example, the single-walled carbon nanotubes may be included in each of the first negative electrode active material layer (122) and the second negative electrode active material layer (124) within the above range.
[0060] In the above range, the mobility of lithium ions may not decrease, so that the stability of the negative electrode (130) may be improved while preventing the capacity characteristics and charge characteristics of the negative electrode active material layer (120) from deteriorating.
[0061] In some embodiments, the Raman R value of the carbon nanotubes included in the second negative active material layer (124) may be 0.5 or less. For example, the Raman R value of the carbon nanotubes may be 0.01 to 0.5, 0.01 to 0.4, 0.01 to 0.3, or 0.01 to 0.1.
[0062] The Raman R value is the intensity (I) of the D band of the Raman spectrum obtained by Raman spectroscopy. D ) and intensity of G band (I G ) of the rain (I D / I G ) can be defined as.
[0063] The intensity of the above D band (I D ) in the Raman spectrum is about 1,300 cm -1 About 1,420cm -1 is the peak intensity for the waveband, and the intensity of the G band (I G ) in the Raman spectrum is about 1,540 cm -1 About 1,620cm -1 is the peak intensity for the waveband region.
[0064] The above D band is due to a vibrational mode with symmetry and is not observed in a perfect lattice structure. For example, when carbon atoms forming a hexagonal structure exist, it may appear when the hexagonal structure is not widely developed or there are defects. The above G band is a peak that can be commonly found in carbon-based materials and may appear, for example, when carbon atoms forming the hexagonal structure exist. Accordingly, the Raman R value can be used as an indicator of the crystallinity or defects of the carbon atom structure.
[0065] In one embodiment, a single-walled carbon nanotube having the Raman R value range described above may be used as the carbon nanotube included in the second negative electrode active material layer (124).
[0066] Within the above Raman R value range, the resistance of the second negative electrode active material layer (124) can be reduced and the electrical conductivity can be improved. In addition, the stability of the second negative electrode active material layer (124) can be improved, so that the rapid charging characteristics can be maintained for a long period of time even at high temperatures.
[0067] In some embodiments, the first conductive material and the second conductive material may further include a carbon-based conductive material such as graphite, carbon black, graphene, etc., and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, LaSrMnO3, etc.
[0068] In some embodiments, the first conductive material may not include carbon nanotubes. Accordingly, the capacity of the first carbon-based active material of the first negative electrode active material layer (122) may be increased, and high-temperature stability may be improved.
[0069] In one embodiment, a conductive material other than carbon nanotubes may be used as the first conductive material, while a conductive material including carbon nanotubes may be used as the second conductive material.
[0070] According to exemplary embodiments, the second negative electrode active material layer (124) may include a conductive polymer. By including the conductive polymer in the second negative electrode active material layer (124), the resistance of the negative electrode (130) may be reduced and the output characteristics may be improved without increasing the content of the conductive material described above in the second negative electrode active material layer (124).
[0071] The conductive polymer may be formed from monomers including, for example, poly(p-phenylene, PPP), polypyrrole (PPy), polythiophene (PT), polyacetylene, polyaniline (PANI), poly(3,4-ethylenedioxythiophene, PEDOT), polyfluorene, polypyrene, polyazulene, polynaphthalene, polycarbazole, and polyindole (PIN).
[0072] In one embodiment, the conductive polymer may be formed from a monomer including at least one of polyparaphenylene, polypyrrole, polythiophene, polyacetylene, polyaniline, and poly-3,4-ethylenedioxythiophene. Accordingly, even when a small amount of the conductive polymer is used, the resistance of the second negative electrode active material layer (124) may be reduced and the electrical conductivity may be improved.
[0073] In some embodiments, the content of the conductive polymer may be comprised in an amount of 0.01 wt% to 1.5 wt%, 0.01 wt% to 1.0 wt%, 0.01 wt% to 0.5 wt%, 0.01 wt% to 0.3 wt%, or 0.05 wt% to 0.15 wt% of the total weight of the second negative electrode active material layer (124). In this range, the electrical conductivity may be improved without reducing the capacity characteristics of the second negative electrode active material layer (124).
[0074] In one embodiment, the weight ratio of the content of the conductive polymer in the second negative electrode active material layer (124) to the content of the second conductive material in the second negative electrode active material layer (124) may be 0.01 to 2.0, 0.05 to 2.0, 0.1 to 2.0, 0.3 to 2.0, 0.5 to 1.5, or 0.7 to 1.3. For example, the weight ratio of the conductive polymer in the second negative electrode active material layer (124) to the carbon nanotubes in the second negative electrode active material layer (124) may be within the above range. In the above range, a reduction in the resistance of the negative electrode (130) and an improvement in the output characteristics and rapid charging characteristics through the conductive polymer can be realized without increasing the content of the second conductive material included in the second negative electrode active material layer (124).
[0075] In some embodiments, the conductive polymer may be included only in the second negative electrode active material layer (124). For example, the first negative electrode active material layer (122) may not include the conductive polymer. Accordingly, the conductivity of the second negative electrode active material layer (124), which substantially functions as an active negative electrode, may be improved, while the stability of the negative electrode (130) may be improved through the first negative electrode active material layer (122).
[0076] According to exemplary embodiments, the first negative electrode active material and the first conductive material described above may be mixed and stirred with a binder and / or a dispersing agent in a solvent to produce a first negative electrode slurry. The first negative electrode slurry may be coated on at least one surface of a negative electrode current collector (125), and then dried and compressed to produce a first negative electrode active material layer (122).
[0077] According to exemplary embodiments, the second negative electrode active material, the second conductive material, and the conductive polymer described above may be mixed and stirred with a binder and / or a dispersing agent in a solvent to produce a second negative electrode slurry. The first negative electrode slurry may be coated on at least one surface of a negative electrode current collector (125), and then dried and compressed to produce a first negative electrode active material layer (122).
[0078] An aqueous solvent or a non-aqueous solvent may be used as the solvent. For example, deionized water may be used as the aqueous solvent, and N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, N,N-dimethylaminopropylamine, ethylene oxide, tetrahydrofuran, etc. may be used as the non-aqueous solvent.
[0079] The binder for forming the negative electrode may include, for example, an aqueous binder such as styrene-butadiene rubber (SBR) for compatibility with the carbon-based active material, and may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0080] FIG. 2 is a schematic cross-sectional view showing a negative electrode for a lithium secondary battery according to exemplary embodiments.
[0081] Referring to FIG. 2, the negative electrode active material layer (120) may include a first negative electrode active material layer (122) formed directly on both surfaces of the negative electrode current collector (125) and a second negative electrode active material layer (124) formed on the first negative electrode active material layer (122). For example, the negative electrode active material layer (120) may include a two-layer structure in which the first negative electrode active material layer (122) and the second negative electrode active material layer (124) are sequentially disposed on the negative electrode current collector (125) on both surfaces of the negative electrode current collector (125).
[0082] Lithium secondary battery
[0083] According to exemplary embodiments, a lithium secondary battery may include the negative electrode for a secondary battery described above.
[0084] FIGS. 3 and 4 are schematic plan views and cross-sectional views, respectively, showing lithium secondary batteries according to exemplary embodiments.
[0085] Referring to FIGS. 3 and 4, a lithium secondary battery includes a positive electrode (100) and a negative electrode (130), and may further include a separator (140) interposed between the positive electrode (100) and the negative electrode (130).
[0086] The positive electrode (100) may include a positive electrode active material layer (110) formed by applying a positive electrode active material to a positive electrode current collector (105). The positive electrode active material may include a compound capable of reversibly intercalating and deintercalating lithium ions.
[0087] In exemplary embodiments, the positive electrode active material may include a lithium-nickel metal composite oxide.
[0088] For example, the lithium-nickel metal composite oxide may further include at least one of cobalt (Co) and manganese (Mn). In one embodiment, the positive electrode active material may include a Ni-Co-Mn (NCM)-based lithium oxide.
[0089] In some embodiments, the positive electrode active material or lithium-nickel metal composite oxide may include a layered structure or crystal structure represented by the following chemical formula 1.
[0090] [Chemical Formula 1]
[0091] Li x Ni a M b O 2+z
[0092] In chemical formula 1, 0.9≤x≤1.2, 0.6≤a≤0.99, 0.01≤b≤0.4, -0.5≤z≤0.1 may be satisfied. As described above, M may include Co and / or Mn.
[0093] The chemical structure represented by Chemical Formula 1 represents the bonding relationship included in the layered structure or crystal structure of the positive electrode active material and does not exclude other additional elements. For example, M includes Co and / or Mn, and Co and Mn can serve as the main active element of the positive electrode active material together with Ni. Chemical Formula 1 is provided to express the bonding relationship of the above main active elements and should be understood as a formula encompassing the introduction and substitution of additional elements.
[0094] In one embodiment, auxiliary elements may be further included in addition to the main active element to enhance the chemical stability of the positive electrode active material or the layered structure / crystal structure. The auxiliary elements may be incorporated into the layered structure / crystal structure to form bonds, and in this case, it should be understood that they are also included within the chemical structure range represented by Chemical Formula 1.
[0095] The auxiliary element may include, for example, at least one of Na, Mg, Ca, Y, Ti, Hf, V, Nb, Ta, Cr, Mo, W, Fe, Cu, Ag, Zn, B, Al, Ga, C, Si, Sn, Sr, Ba, Ra, P, or Zr. The auxiliary element may also act as an auxiliary active element that contributes to the capacity / output activity of the positive electrode active material together with Co or Mn, for example, Al.
[0096] For example, the positive electrode active material or the lithium-nickel metal composite oxide may include a layered structure or crystal structure represented by the following chemical formula 1-1.
[0097] [Chemical Formula 1-1]
[0098] Li x Ni a M1 b1 M2 bs O 2+z
[0099] In Chemical Formula 1-1, M1 may include Co and / or Mn. M2 may include the auxiliary elements described above. In Chemical Formula 1-1, 0.9≤x≤1.2, 0.6≤a≤0.99, 0.01≤b1+b2≤0.4, -0.5≤z≤0.1 may be satisfied.
[0100] The above-described positive electrode active material may further include a coating element or doping element. For example, elements substantially identical to or similar to the above-described auxiliary elements may be used as the coating element or doping element. For example, the above-described elements may be used singly or in combination of two or more.
[0101] The above coating element or doping element may be present on the surface of the lithium-nickel metal composite oxide particle, or may penetrate through the surface of the lithium-nickel metal composite oxide particle and be included in the bonding structure represented by Chemical Formula 1 or Chemical Formula 1-1.
[0102] The above-described positive electrode active material can be mixed and stirred with a binder, a conductive agent, and / or a dispersing agent in a solvent to produce a positive electrode slurry. The positive electrode slurry can be coated on at least one surface of a positive electrode current collector (105), followed by drying and rolling to produce a positive electrode (100).
[0103] The positive electrode current collector (105) may be made of materials substantially identical or similar to those of the negative electrode current collector (125) described above. The positive electrode current collector (105) may include, for example, stainless steel, nickel, aluminum titanium, or an alloy thereof. The positive electrode current collector (105) may also include aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver.
[0104] As the solvent, materials substantially identical or similar to the solvents used in the preparation of the first cathode slurry and the second cathode slurry can be used.
[0105] For example, the binder may include an organic binder such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, and the like, an aqueous binder such as styrene-butadiene rubber (SBR), and may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0106] For example, a PVDF series binder may be used as a binder for forming a positive electrode. In this case, the amount of binder for forming a positive electrode active material layer (110) may be reduced and the amount of positive electrode active material may be relatively increased, thereby improving the output and capacity of the secondary battery.
[0107] The conductive material may be included to promote electron transfer between active material particles. For example, the conductive material may include a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, and / or a metal-based conductive material including a perovskite material such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0108] The negative electrode (130) may be the negative electrode for a secondary battery described above.
[0109] In some embodiments, a separator (140) may be interposed between the positive electrode (100) and the negative electrode (130). The separator (140) may include a porous polymer film made of a polyolefin polymer, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, or the like. The separator (140) may also include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, or the like.
[0110] According to exemplary embodiments, an electrode cell is defined by an anode (100), a cathode (130), and a separator (140), and a plurality of the electrode cells may be stacked to form an electrode assembly (150) in the form of, for example, a jelly roll. For example, the electrode assembly (150) may be formed by winding, lamination, folding, or the like of the separator (140).
[0111] The above electrode assembly may be housed together with an electrolyte within a case (160) to define a lithium secondary battery. According to exemplary embodiments, a non-aqueous electrolyte may be used as the electrolyte.
[0112] The non-aqueous electrolyte may include a lithium salt as an electrolyte and an organic solvent. The lithium salt may be, for example, Li + X - is expressed as and the anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2- , CH3CO2 - , SCN - , (CF3CF2SO2)2N - Examples include:
[0113] Examples of the organic solvent that can be used include propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0114] As illustrated in FIG. 3, electrode tabs (positive electrode tab and negative electrode tab) may protrude from the positive electrode collector (105) and negative electrode collector (125) belonging to each electrode cell and extend to one side of the case (160). The electrode tabs may be fused together with the one side of the case (160) to form electrode leads (positive electrode lead (107) and negative electrode lead (127)) that extend or are exposed to the outside of the case (160).
[0115] The above lithium secondary battery can be manufactured in a cylindrical, square, pouch or coin shape using, for example, a can.
[0116] Hereinafter, preferred embodiments are presented to help understand the present disclosure, but these embodiments are only illustrative of the present disclosure and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the embodiments are possible within the scope and technical idea of the present disclosure, and it is natural that such changes and modifications fall within the scope of the appended claims.
[0117]
[0118] Examples and Comparative Examples
[0119] Example 1
[0120] 1) Manufacturing of cathode
[0121] SiO as the first negative electrode active material 1.8 A mixture of 35 wt% of synthetic graphite, 40 wt% of natural graphite, 15 wt% of natural graphite, 0.1 wt% of SWCNT and 1.9 wt% of Super C as a second negative electrode conductive material, 3 wt% of styrene-butadiene rubber (SBR) as a binder, and 5 wt% of carboxymethyl cellulose (CMC) as a thickener was added to and mixed in a deionized water solvent to obtain a first negative electrode slurry.
[0122] After the above first negative electrode slurry was coated on a Cu foil current collector, it was dried and rolled to form a first negative electrode active material layer.
[0123] SiO as the second negative electrode active material x (0<x<2) A mixture of 35 wt% of synthetic graphite, 40 wt% of artificial graphite, and 15 wt% of natural graphite, 0.1 wt% of SWCNT and 1.8 wt% of Super C as a second negative electrode conductive material, 0.1 wt% of polyacetylene as a conductive polymer, 3 wt% of styrene-butadiene rubber (SBR) as a binder, and 5 wt% of carboxymethyl cellulose (CMC) as a thickener were added to and mixed in a deionized water solvent to obtain a second negative electrode slurry.
[0124] The Raman R value of SWCNT used as the second cathode conductive material was 0.08.
[0125] After coating the second negative electrode slurry on the first negative electrode active material layer, drying and rolling were performed to form a second negative electrode active material layer, thereby manufacturing a negative electrode.
[0126] Raman R value (I) of SWCNT of the second negative electrode active material layer D / I G ) is the D band (approximately 1,350 cm -1 ) peak intensity (I D ) and G band (approximately 1,580 cm -1 ) peak intensity (I G ) was measured and the measurement equipment / conditions are as follows.
[0127] i) Raman spectrometer: inVia, Renishaw (UK)
[0128] ii) Argon ion laser light wavelength: 532 nm
[0129] iii) Exposure time: 10 seconds
[0130] iv) Number of accumulated returns: 10 times
[0131] 2) Manufacturing of cathode and secondary batteries
[0132] LiNi as positive electrode active material 0.8 Co 0.1 Mn 0.1 A cathode slurry was prepared by mixing O2, a mixture of carbon black and carbon nanotubes (CNT) as a cathode conductive agent, and polyvinylidene fluoride (PVDF) as a cathode binder in distilled water at a weight ratio of 94:2:4. The cathode slurry was coated on an Al foil current collector, dried, and rolled to prepare a cathode.
[0133] A battery was constructed by incorporating the separator (polyethylene, 13 μm thick) manufactured between the positive and negative electrodes, and the tab portions of the positive electrode and the tab portions of the negative electrode were each welded.
[0134] The welded anode / separator / cathode assembly was placed in a pouch, and the tabbed portion was included in the sealing area, sealing all three sides except the electrolyte injection area. The electrolyte was injected into the remaining portion, the remaining side was sealed, and then the secondary battery was manufactured by impregnating for 12 hours.
[0135] The electrolyte was prepared by dissolving 1M LiPF6 in a mixed solvent of EC / EMC / DEC (25 / 45 / 30; volume ratio), to which 5 wt% of FEC (Florinated Ethylene Carbonate), 0.5 wt% of PS (Propane Sulfone), and 0.5 wt% of ESA (ethylene sulfate) were added.
[0136] Examples 2 to 10 and Comparative Examples 1 to 5
[0137] Examples 2 to 10 and Comparative Examples 1 to 5 were manufactured in the same manner as Example 1, except that the type and content of the active material included in the negative electrode, the content of Super C, SWCNT, and polyacetylene in the second negative electrode active material layer, and the Raman R value of SWCNT used as the second conductive material were adjusted as shown in Tables 1 and 2 below.
[0138] Classification Active material type 1 Negative active material 2 Negative active material Type Content (weight%) Type Content (weight%) Example 1 SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Example 2SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Example 3SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Example 4SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Example 5SiO 1.8 -SiO 1.8-SiC-SiC40 Artificial graphite70 Artificial graphite35 Natural graphite20 Natural graphite15 Example 6SiO 1.8 -SiO 1.8 -SiC-SiC40 Artificial graphite70 Artificial graphite35 Natural graphite20 Natural graphite15 Example 7 SiO 1.8 -SiO 1.8 -SiC-SiC40 Artificial graphite70 Artificial graphite35 Natural graphite20 Natural graphite15 Example 8 SiO 1.8 -SiO 1.8 -SiC-SiC40 Artificial graphite70 Artificial graphite35 Natural graphite20 Natural graphite15 Example 9 SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Example 10SiO 1.8 -SiO 1.8 35SiC35SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Comparative example 1SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Comparative example 2SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial Graphite40Artificial Graphite40Natural Graphite15Natural Graphite15Comparative Example 3SiO 1.8 -SiO 1.8 -SiC20SiC20Artificial graphite50Artificial graphite50Natural graphite20Natural graphite20Comparative example 4SiO 1.8 35SiO 1.8 35SiC-SiC-Artificial graphite40Artificial graphite40Natural graphite15Natural graphite15Comparative example 5SiO 1.8 -SiO 1.8 35SiC35SiC-Artificial Graphite40Artificial Graphite40Natural Graphite15Natural Graphite15
[0139] ClassificationActive material layer typeSuper C content (wt%)SWCNT content (wt%)Polyacetylene content (wt%)Raman R valueExample 1First negative electrode active material layer1.90.1-0.08Second negative electrode active material layer1.80.10.1Example 2First negative electrode active material layer1.90.1-0.08Second negative electrode active material layer1.650.10.25Example 3First negative electrode active material layer1.90.1-0.55Second negative electrode active material layer1.80.10.1Example 4First negative electrode active material layer1.90.1-0.55Second negative electrode active material layer1.650.10.25Example 5First negative electrode active material layer2.0--0.08Second negative electrode active material layer1.80.10.1Example 6First negative electrode Active material layer 2.0--0.08 Second negative electrode active material layer 1.65 0.10.25 Example 7 First negative electrode active material layer 2.0--0.55 Second negative electrode active material layer 1.8 0.10.1 Example 8 First negative electrode active material layer 2.0--0.55 Second negative electrode active material layer 1.65 0.10.25 Example 9 First negative electrode active material layer 1.8 0.10.10.08 Second negative electrode active material layer 1.8 0.10.1 Example 10 First negative electrode active material layer 1.8 0.10.10.08 Second negative electrode active material layer 1.8 0.10.1 Comparative example 1 First negative electrode active material layer 1.8 0.2-0.5 Second negative electrode active material layer 1.8 0.2- Comparative example 2 First negative electrode Active material layer 1.90.1-0.1 Second negative electrode active material layer 1.90.1-Comparative example 3 First negative electrode active material layer 1.90.1-0.3 Second negative electrode active material layer 1.90.1-Comparative example 4 First negative electrode active material layer 1.80.10.10.1 Second negative electrode active material layer 1.80.2-Comparative example 5 First negative electrode active material layer 1.80.10.10.1 Second negative electrode active material layer 1.80.2-
[0140]
[0141] Experimental example
[0142] (1) Resistance measurement of secondary batteries
[0143] The secondary batteries according to the examples and comparative examples were charged at 0.5C CC / CV (4.2V 0.05C CUT-OFF) at room temperature (25℃), and then discharged at 0.5C CC to SOC 60%.
[0144] At the SOC 60% point, the C-rate was changed to 0.2C, 0.5C, 1C, 1.5C, 2C 2.5C, and 3.0C, and the DCIR was measured by discharging and recharging for 10 seconds each.
[0145] (2) Evaluation of room temperature rapid charging characteristics
[0146] For the secondary batteries of the examples and comparative examples, rapid charging was performed in sections at the SOC10 82% point at room temperature (25°C) for 20 minutes, and then discharge (0.33C, SOC10, CC cut-off) was repeated, and the discharge capacity retention rate at 300 cycles compared to the initial discharge capacity was measured as a percentage.
[0147] (3) Evaluation of room temperature cycle characteristics
[0148] For the secondary batteries according to the examples and comparative examples, charging (CC-CV, 2.0C, 4.2V, SOC4 98% CUT-OFF) and discharging (CC 2.0C 2.75V CUT-OFF) were repeated 250 times at room temperature (25°C), and the discharge capacity at 250 times was calculated as a % of the discharge capacity at 1 time, thereby measuring the room temperature cycle characteristics.
[0149] The evaluation results are shown in Table 3 below.
[0150] Resistance of secondary battery (DCIR, mΩ)Rapid charge characteristics (300 cycle, %)Room temperature cycle characteristics (250 cycle, %)Example 11.24582.590.5Example 21.24981.990.2Example 31.24681.190.0Example 41.25080.789.9Example 50.99995.592.5Example 61.03294.892.1Example 71.00894.192.0Example 81.04892.191.7Example 91.24780.189.8Example 101.24980.089.6Comparative example 11.25179.589.5Comparative example Comparative Example 21.26575.084.9 Comparative Example 31.10481.986.1 Comparative Example 41.25479.589.6 Comparative Example 51.25879.389.4
[0151]
[0152] Referring to Table 3, examples including conductive polymers showed reduced resistance of secondary batteries and improved rapid charging characteristics and room temperature cycling characteristics compared to Comparative Examples 1 to 3 that did not include conductive polymers.
[0153] Examples 1 to 8, in which the conductive polymer is included only in the second negative electrode active material layer, showed a somewhat reduced resistance of the secondary battery, and a somewhat improved rapid charging characteristic and room temperature cycling characteristic, compared to Examples 9 and 10, in which the conductive polymer is included in both the first negative electrode active material layer and the second negative electrode active material layer.
[0154] In addition, Examples 1 to 8, in which the conductive polymer is included only in the second negative electrode active material layer, showed a decrease in the resistance of the secondary battery, and improved rapid charging characteristics and room temperature cycling characteristics, compared to Comparative Examples 4 and 5, in which the conductive polymer is included only in the first negative electrode active material layer.
[0155] Examples 2 and 6, in which the ratio of acetylene to SWCNT included in the second negative electrode active material layer exceeds 2.0, showed a slight increase in the resistance characteristics of the secondary battery.
[0156] Examples 3 and 7, in which the Raman R value of the SWCNT included in the second negative electrode active material layer was greater than 0.5, showed somewhat reduced rapid charging characteristics and room temperature cycling characteristics.
[0157] Examples 4 and 8, in which the ratio of acetylene to SWCNT included in the second negative electrode active material layer exceeds 2.0 and the Raman R value of SWCNT included in the second negative electrode active material layer exceeds 0.5, showed a slight increase in the resistance characteristics of the secondary battery, and a slight decrease in the rapid charge characteristics and the room temperature cycle characteristics.
[0158] In Examples 5 to 8, in which graphite (a mixture of artificial graphite and natural graphite) was used alone as the active material of the first negative electrode active material layer, the resistance of the secondary battery was somewhat reduced, and the rapid charging characteristics and room temperature cycling characteristics were somewhat improved.
[0159] Examples 9 and 10, which include a conductive polymer in the first negative electrode active material layer and the second negative electrode active material layer, showed a slight increase in the resistance of the secondary battery, and a slight decrease in the rapid charge characteristics and room temperature cycle characteristics.
[0160] Comparative Examples 1 to 3, which did not include a conductive polymer in the second negative electrode active material layer, showed increased resistance of the secondary battery and decreased rapid charging characteristics and room temperature cycle characteristics.
[0161] Comparative Examples 4 and 5, which included a conductive polymer in the first negative electrode active material layer, showed increased resistance of the secondary battery and decreased rapid charging characteristics and room temperature cycling characteristics.
Claims
1. Negative current collector; A first negative electrode active material layer formed on at least one surface of the negative electrode current collector and including a first negative electrode active material including at least one of a first carbon-based active material and a first silicon-based active material; and A negative electrode for a secondary battery, comprising a second negative electrode active material layer formed on the first negative electrode active material layer and including at least one of a second carbon-based active material and a second silicon-based active material, and a second negative electrode active material layer including a conductive polymer.
2. A negative electrode for a secondary battery according to claim 1, wherein the first carbon-based active material includes a graphite-based active material.
3. In claim 1, the first silicon-based active material and the second silicon-based active material are each SiO x A negative electrode for a secondary battery, comprising at least one of (0<x<2) and a silicon-carbon composite.
4. A negative electrode for a secondary battery according to claim 1, wherein the weight of the second carbon-based active material included in the second negative electrode active material layer is greater than the weight of the second silicon-based active material included in the second negative electrode active material layer.
5. A negative electrode for a secondary battery according to claim 1, wherein the content of the second silicon-based active material is comprised between 2 wt% and 50 wt% of the total weight of the second negative electrode active material layer.
6. A negative electrode for a secondary battery according to claim 1, wherein the weight of the first carbon-based active material included in the first negative electrode active material layer is greater than the weight of the second carbon-based active material included in the second negative electrode active material layer.
7. A negative electrode for a secondary battery according to claim 1, wherein the second negative electrode active material layer includes a second conductive material including carbon nanotubes (CNTs).
8. A negative electrode for a secondary battery according to claim 7, wherein the carbon nanotube comprises a single-wall carbon nanotube (SWCNT).
9. A negative electrode for a secondary battery according to claim 8, wherein the content of the single-walled carbon nanotubes is comprised at 0.01 wt% to 1 wt% of the total weight of the second negative electrode active material layer.
10. In claim 7, the Raman R value of the carbon nanotube is 0.5 or less, The above Raman R value is the intensity (I) of the D band of the Raman spectrum obtained by Raman spectroscopy. D ) and the intensity of the G band (I G ) of the rain (I D / I G ) is defined as a negative electrode for a secondary battery.
11. A negative electrode for a secondary battery according to claim 7, wherein the weight ratio of the content of the conductive polymer in the second negative electrode active material layer to the content of the carbon nanotubes in the second negative electrode active material layer is 0.01 to 2.
12. A negative electrode for a secondary battery according to claim 7, wherein the first negative electrode active material layer does not include carbon nanotubes.
13. In claim 1, the conductive polymer is an anode for a secondary battery formed from a monomer including at least one of poly(p-phenylene, PPP), polypyrrole (PPy), polythiophene (PT), polyacetylene, polyaniline (PANI), and poly(3,4-ethylenedioxythiophene, PEDOT).
14. A negative electrode for a secondary battery according to claim 1, wherein the first negative electrode active material layer does not include a conductive polymer.
15. A negative electrode for a secondary battery according to claim 1, wherein the content of the conductive polymer is comprised between 0.01 wt% and 1.5 wt% of the total weight of the second negative electrode active material layer.
16. A negative electrode for a secondary battery according to claim 1; and A lithium secondary battery comprising a positive electrode positioned opposite the negative electrode.
Citation Information
Patent Citations
Negative electrode for nonaqueous electrolyte secondary battery, method for manufacturing the same, and nonaqueous electrolyte secondary battery
JP2015069711A
Electrode contact member of vacuum circuit breaker
KR1020240035141A
Cleaner
KR1020240053473A
A stackable multi-channel structure and a method of fabricating the same, and a thin film transistor comprising the same
KR1020240154164A
Injection apparatus for filling with syrup
KR102407058B1