Smart IC substrate, smart IC module, and IC card comprising same

The smart IC substrate addresses corrosion issues by using a dual-layer plating structure with a protective layer, ensuring reliable and efficient wire bonding and electrical connectivity, and reducing manufacturing costs.

WO2024242487A1PCT designated stage expired Publication Date: 2024-11-28LG INNOTEK CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007004
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-20
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing smart IC substrates face issues with corrosion and reduced electrical conductivity during the wire bonding process due to the reactivity of the plating layers, leading to potential damage and inefficiencies in the manufacturing process.

Method used

A smart IC substrate with a dual-layer plating structure, where the second plating layer is protected by a less reactive metal layer with a lower ionization tendency, preventing oxidation and maintaining electrical conductivity, and allowing for the use of various materials and reduced process costs.

Benefits of technology

The solution enhances the reliability and efficiency of the wire bonding process by reducing corrosion and maintaining electrical conductivity, improving the electrical connection characteristics and process efficiency while allowing for the use of different materials and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007004_28112024_PF_FP_ABST
    Figure KR2024007004_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A smart IC substrate according to an embodiment comprises: a substrate including a first surface and a second surface opposite the first surface; a bonding layer disposed on the first surface; a metal layer disposed on the bonding layer; a first plating layer disposed on one surface of the metal layer; and a second plating layer disposed on the other surface of the metal layer, wherein the first plating layer includes a first first layer and a second first layer on the first first layer, the second plating layer includes a first second layer and a second second layer on the first second layer, the second second layer includes a different metal than the second first layer, a protective layer is disposed on the second second layer, and the protective layer includes a less reactive metal than the second second layer.
Need to check novelty before this filing date? Find Prior Art

Description

Smart IC substrate, smart IC module and IC card including the same

[0001] The present invention relates to a smart IC substrate, a smart IC module, and an IC card including the same.

[0002] An IC card is a plastic card with an integrated circuit chip capable of storing and processing information. An IC card contains the necessary information, which is then transmitted to a reader in the form of an electrical signal.

[0003] The above IC card is manufactured by inserting a smart IC module into the main body of the card.

[0004] The above smart IC module is classified into a single type or a dual type depending on the arrangement of the metal layers. The single type has the metal layer and plating layer arranged on only one side of the substrate. In addition, the dual type has the metal layer and plating layer arranged on both sides of the substrate.

[0005] Additionally, the smart IC module is categorized into contact, contactless, hybrid, and combi cards depending on how the card is used. The contact card transmits and receives information through physical contact. Furthermore, the contactless card transmits and receives information without physical contact. Furthermore, the hybrid card and combi card include both the contact and contactless functions.

[0006] Accordingly, the smart IC module includes a contact surface and a bonding surface. The contact surface is in contact with an external device, and a chip is placed on the bonding surface. The bonding surface is inserted into the interior of the card body.

[0007] The chip positioned on the bonding surface and the conductive pattern positioned on the contact surface are electrically connected by wire bonding. Accordingly, the smart IC module includes a plurality of holes. The chip and the conductive pattern are wire bonded through the holes.

[0008] To facilitate the above wire bonding, the conductive pattern includes a pad portion. The pad portion is formed by a plating layer. The wire and the plating layer include a metal. The material of the wire may be restricted by the metal of the plating layer.

[0009] For example, the metal of the wire may be limited by the strength, resistance, and electrical conductivity of the metal of the plating layer. Additionally, the plating layer may corrode during the process. This may reduce the electrical conductivity of the plating layer.

[0010] Therefore, a new structure of a smart IC substrate, a smart IC module, and an IC card including the same that can solve the above problems is required.

[0011] As a prior art related to the above smart IC substrate, it is disclosed in Korean Patent Publication No. KR10-2022-0110247.

[0012] The embodiment provides a smart IC substrate having improved reliability.

[0013] Additionally, the embodiment provides a smart IC substrate to which wires of various materials can be applied.

[0014] Additionally, the embodiment provides a smart IC module and IC card having improved process efficiency.

[0015] A smart IC substrate according to an embodiment comprises a substrate including a first surface and a second surface opposite to the first surface; a bonding layer disposed on the first surface; a metal layer disposed on the bonding layer; a first plating layer disposed on one surface of the metal layer; and a second plating layer disposed on the other surface of the metal layer, wherein the first plating layer includes a 1-1 layer and a 1-2 layer on the 1-1 layer, the second plating layer includes a 2-1 layer and a 2-2 layer on the 2-1 layer, the 2-2 layer including a different metal from the 1-2 layer, and a protective layer is disposed on the 2-2 layer, and the protective layer includes a metal having less reactivity than the 2-2 layer.

[0016] A smart IC substrate according to an embodiment includes a protective layer. The protective layer includes a metal having a lower reactivity than the plating layer. Specifically, the protective layer includes a metal having a lower ionization tendency than the plating layer.

[0017] Specifically, the protective layer comprises a metal less reactive than the second layer. Accordingly, the second layer can be prevented from being oxidized or discolored. Alternatively, when the second layer is partially oxidized during the process, the corrosion rate of the second layer can be reduced.

[0018] Accordingly, the electrical conductivity and rigidity of the second plating layer are maintained. Therefore, damage to the second plating layer during wire bonding can be prevented. In addition, the electrical connection characteristics between the chip and the conductive pattern are improved after the wire bonding.

[0019] Additionally, the corrosion rate of the second plating layer is reduced. Accordingly, the electrical conductivity of the second plating layer is maintained. Accordingly, the electrical connection characteristics of the chip and the conductive pattern can be maintained during use of the IC card.

[0020] Additionally, the protective layer may be formed by the same process as the first plating layer. Specifically, the protective layer may be formed by the same process as the first and second layers. Therefore, a separate process for forming the protective layer is omitted. Accordingly, process efficiency may be improved.

[0021] In addition, a smart IC substrate according to an additional embodiment includes a first plating layer and a second plating layer. The second plating layer is wire-bonded to a chip. The first plating layer includes a 1-1 layer and a 1-2 layer on the 1-1 layer. The second plating layer includes a 2-1 layer and a 2-2 layer on the 2-1 layer.

[0022] The materials of the first plating layer and the second plating layer are different. The second-second layer has a lower melting point and resistance than the first-second layer. Furthermore, the second-second layer has higher electrical and thermal conductivity than the first-second layer. Accordingly, the process efficiency and electrical characteristics of the smart IC module are improved.

[0023] Additionally, the second layer is formed to a greater thickness than the first layer. At this time, the second layer is formed of a material other than gold. Therefore, the process cost is reduced.

[0024] In addition, a smart IC substrate according to an additional embodiment may further include a second-third layer. Accordingly, the second-second layer and the second-third layer may form a gold-silver alloy. Accordingly, the hardness of the second plating layer is improved. Accordingly, when wire-bonding the second plating layer and the chip, cracking of the second plating layer can be prevented. In addition, a material with high hardness can be used as the material of the wire. Accordingly, wires of various materials can be used.

[0025] Additionally, the second and third layers can be formed by the same process as the first and second layers. Furthermore, the second and third layers are formed with a thin film thickness. Accordingly, the process efficiency of the smart IC substrate is improved.

[0026] In addition, a smart IC substrate according to an additional embodiment may further include a second layer. Accordingly, the second layer and the second layer may form a gold-silver alloy. In addition, the second layer and the second layer may form a gold-silver alloy. Accordingly, the hardness of the second plating layer is improved. Accordingly, when the second plating layer and the chip are wire-bonded, cracking of the second plating layer can be prevented. In addition, a material with high hardness can be used as the material of the wire. Accordingly, wires of various materials can be used.

[0027] In addition, the 2nd to 4th layers can be formed by the same process as the 1st to 2nd layers. In addition, the 2nd to 4th layers are formed with a thin film thickness. Accordingly, the process efficiency of the smart IC substrate is improved.

[0028] FIG. 1 is a top view of a first surface of a smart IC substrate according to a first embodiment.

[0029] FIG. 2 is a top view of a second surface of a smart IC substrate according to the first embodiment.

[0030] Figure 3 is a cross-sectional view taken along area AA' of Figure 2.

[0031] FIG. 4 is a top view of a second surface of a smart IC module according to the first embodiment.

[0032] Figure 5 is a cross-sectional view taken along the BB' area of ​​Figure 4.

[0033] Figure 6 is a top view of the first surface of a smart IC substrate according to the second embodiment.

[0034] Figure 7 is a top view of the second surface of a smart IC substrate according to the second embodiment.

[0035] Fig. 8 is a cross-sectional view taken along the CC' area of ​​Fig. 7.

[0036] Fig. 9 is a top view of a second surface of a smart IC module according to a second embodiment.

[0037] Fig. 10 is a cross-sectional view taken along the DD' area of ​​Fig. 9.

[0038] Fig. 11 is a top view of the first surface of a smart IC substrate according to the third embodiment.

[0039] Fig. 12 is a top view of the second surface of a smart IC substrate according to the third embodiment.

[0040] Figure 13 is a cross-sectional view taken along the EE' area of ​​Figure 12.

[0041] Fig. 14 is a cross-sectional view taken along the EE' area of ​​Fig. 12.

[0042] Fig. 15 is a top view of the second side of a smart IC module according to the third embodiment.

[0043] Figure 16 is a cross-sectional view taken along the GG' area of ​​Figure 15.

[0044] Figures 17 and 18 are cross-sectional views taken along the HH' area of ​​Figure 15.

[0045] FIGS. 19 to 22 are drawings showing various embodiments of the second plating layer illustrated in FIGS. 1 to 18.

[0046] Fig. 23 is an exploded perspective view of a smart IC card according to an embodiment.

[0047] Fig. 24 is a drawing for explaining the combination of a smart IC module according to an embodiment.

[0048] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings. However, the technical concept of the present invention is not limited to the described embodiments, but may be implemented in various different forms. Within the scope of the technical concept of the present invention, one or more of the components of the embodiments may be selectively combined or substituted for use.

[0049] In addition, terms (including technical and scientific terms) used in the embodiments of the present invention may be interpreted as having a meaning that can be generally understood by a person of ordinary skill in the technical field to which the present invention belongs, unless explicitly and specifically defined and described, and terms that are commonly used, such as terms defined in a dictionary, may be interpreted in consideration of the contextual meaning of the relevant technology.

[0050] In addition, the terms used in the embodiments of the present invention are for the purpose of describing the embodiments and are not intended to limit the present invention. In this specification, the singular may also include the plural unless specifically stated in the phrase, and when it is described as “and (and) at least one (or more) of B, C,” it may include one or more of all combinations that can be combined with A, B, and C.

[0051] Additionally, in describing components of embodiments of the present invention, terms such as first, second, A, B, (a), (b), etc. may be used. These terms are only intended to distinguish the components from other components, and are not intended to limit the nature, order, or sequence of the components.

[0052] And, when a component is described as being 'connected', 'coupled' or 'connected' to another component, it may include not only cases where the component is directly connected, coupled or connected to the other component, but also cases where the component is 'connected', 'coupled' or 'connected' by another component between the component and the other component.

[0053] Additionally, when it is described as being formed or disposed "above or below" each component, above or below includes not only cases where the two components are in direct contact with each other, but also cases where one or more other components are formed or disposed between the two components.

[0054] Additionally, when expressed as “upper or lower,” it can include the meaning of not only the upward direction but also the downward direction based on one component.

[0055]

[0056] Hereinafter, a smart IC substrate, a smart IC module, and a smart IC card including the same according to an embodiment will be described with reference to the drawings.

[0057]

[0058] A smart IC substrate (1000) and a smart IC module (2000) according to the first embodiment will be described with reference to FIGS. 1 to 5.

[0059] Referring to FIGS. 1 to 3, the smart IC substrate includes a substrate (100), a bonding layer (200), a metal layer (300), and a plating layer.

[0060] The above-described substrate (100) includes a first side (1S) and a second side (2S). The first side (1S) and the second side (2S) are opposite sides.

[0061] The first surface (1S) is a contact surface. Specifically, the first surface (1S) is a surface that can recognize information of the smart IC module through direct or indirect contact. In addition, the second surface (2S) is a bonding surface. Specifically, the second surface (2S) is a surface on which a chip is mounted and bonded to the main body of the IC card.

[0062] The above substrate (100) comprises a resin material. The substrate (100) may comprise a prepreg comprising glass fibers. Specifically, the substrate (100) may comprise a material in which glass fibers and a silicon-based filler (Si filler) are dispersed within an epoxy resin.

[0063] Alternatively, the substrate (100) may be rigid or flexible. For example, the substrate (100) may include glass or plastic. Specifically, the substrate (100) may include chemically strengthened / semi-strengthened glass such as soda lime glass or aluminosilicate glass. Alternatively, the substrate (100) may include polyimide (PI), polyethylene terephthalate (PET), propylene glycol (PPG), polycarbonate (PC), or sapphire.

[0064] Alternatively, the substrate (100) may include an optically isotropic film. For example, the substrate (100) may include a cyclic olefin copolymer (COC), a cyclic olefin polymer (COP), an optically isotropic polycarbonate (PC), or an optically isotropic polymethyl methacrylate (PMMA).

[0065] Alternatively, the substrate (100) may be bent while having a partially curved surface. That is, the substrate (100) may be bent while having a partially flat surface and a partially curved surface. In detail, the ends of the substrate (100) may be bent while having a curved surface. Alternatively, the substrate (100) may be bent while having a random curvature.

[0066] The substrate (100) may have a thickness within a set range. For example, the thickness of the substrate (100) may be 80 μm to 150 μm, 90 μm to 140 μm, or 100 μm to 120 μm. When the thickness of the substrate (100) is less than 80 μm, the support capacity of the substrate (100) decreases. In addition, when the thickness of the substrate (100) exceeds 150 μm, the thickness of the smart IC substrate may increase. As a result, the size of the IC card increases.

[0067] The above substrate (100) has insulating properties. As a result, the substrate (100) prevents short circuits between circuits. In addition, the substrate (100) serves to support the circuit during the process of forming the circuit.

[0068]

[0069] The above-mentioned substrate (100) includes a hole. In detail, the above-mentioned substrate (100) includes a plurality of holes (H) spaced apart from each other along a horizontal direction.

[0070] At least one of the plurality of holes is a wire-bonded region. For example, all of the plurality of holes are wire-bonded regions. Alternatively, some of the plurality of holes may be wire-bonded regions, while others may not be wire-bonded regions. The chip (C) and the plating layer are wire-bonded through the hole (H).

[0071] The above hole (H) has a width within a set range. The width of the hole (H) can be defined as the diameter of the hole or the minimum distance between the inner sides of the hole. For example, the width of the hole (H) can be 500 ㎛ to 1000 ㎛, 600 ㎛ to 900 ㎛, or 700 ㎛ to 800 ㎛. When the width of the hole (H) is less than 500 ㎛, wire bonding through the hole (H) becomes difficult. In addition, when the width of the hole (H) exceeds 1000 ㎛, the support capacity of the substrate (100) decreases.

[0072] The above bonding layer (200) is disposed on the above substrate (100). In detail, the above bonding layer (200) is disposed on the first surface (1S).

[0073] The bonding layer (200) comprises a resin material. For example, the bonding layer (200) may comprise at least one of an epoxy resin, an acrylic resin, and a polyimide resin. In addition, the bonding layer (200) may comprise at least one additive selected from the group consisting of natural rubber, a plasticizer, a curing agent, and a phosphorus-based flame retardant. This enhances the flexibility of the bonding layer (200).

[0074] The bonding layer (200) may have a thickness within a set range. For example, the thickness of the bonding layer (200) may be 15 μm to 35 μm, 20 μm to 30 μm, or 22 μm to 28 μm. When the thickness of the bonding layer (200) is less than 15 μm, the adhesive strength of the bonding layer (200) decreases. As a result, the metal layer on the bonding layer (200) may be delaminated. In addition, when the thickness of the bonding layer (200) exceeds 35 μm, the thickness of the smart IC substrate may increase. As a result, the size of the IC card increases.

[0075] The metal layer (300) is disposed on the substrate (100). The metal layer (300) is disposed on the bonding layer (200). The metal layer (300) includes a metal material. For example, the metal layer (300) may include at least one material selected from the group consisting of gold (Au), silver (Ag), platinum (Pt), titanium (Ti), tin (Sn), copper (Cu), and zinc (Zn). Preferably, the metal layer (300) includes copper.

[0076] The metal layer (300) may have a thickness within a set range. For example, the thickness of the metal layer (300) may be 30 μm to 75 μm, 40 μm to 65 μm, or 50 μm to 60 μm. When the thickness of the metal layer (300) is less than 30 μm, the resistance of the metal layer (300) increases. In addition, when the thickness of the metal layer (300) exceeds 75 μm, the thickness of the smart IC substrate may increase. As a result, the size of the IC card increases. In addition, process efficiency may decrease.

[0077] The above metal layer (300) includes a plurality of conductive patterns (P). The conductive patterns (P) can be formed by patterning the metal layer (300).

[0078] The conductive patterns (P) are arranged on the first surface (1S). The conductive patterns (P) are arranged on the bonding layer (200). The conductive patterns (P) are arranged on the contact surface. The conductive patterns (P) are arranged spaced apart from each other on the first surface (1S). The holes (H) are arranged in areas corresponding to each conductive pattern (P).

[0079] The plating layer is disposed on the metal layer (300). In detail, the plating layer is disposed on one side (301) of the metal layer and the other side (302) opposite to the one side (301).

[0080] Referring to FIG. 3, the plating layer is divided into multiple plating layers depending on the location. Specifically, the plating layer may include a first plating layer (410) and a second plating layer (420) positioned at different locations. The first plating layer (410) may be referred to as an upper plating layer, and the second plating layer (420) may be referred to as a lower plating layer.

[0081] The first plating layer (410) is disposed on one surface (301) of the metal layer (300). The conductive pattern (P) is formed by the metal layer (300) and the first plating layer (410). The second plating layer (420) is disposed on the other surface (302) of the metal layer (300). The second plating layer (420) is disposed in an area overlapping the hole (H). The second plating layer (420) may be a pad portion to which the wire is bonded. That is, the second plating layer (420) may be disposed within the hole (H). The second plating layer (420) is disposed on the other surface (302) of the metal layer (300) exposed through the hole (H).

[0082] The first plating layer (410) includes a 1-1 layer (411) and a 1-2 layer (412). The 1-1 layer (411) is in contact with the metal layer (300). The 1-2 layer (412) is in contact with the 1-1 layer (411). Accordingly, the 1-1 layer (411) is disposed between the metal layer (300) and the 1-2 layer (412).

[0083] Meanwhile, although not shown in the drawing, an organic coating layer may be further disposed on the first-second layer (412). The organic coating layer protects the first-second layer (412). Accordingly, corrosion of the first-second layer (412) can be prevented.

[0084] The second plating layer (420) includes a 2-1 layer (421) and a 2-2 layer (422). The 2-1 layer (421) is in contact with the metal layer (300). The 2-2 layer (422) is in contact with the 2-1 layer (421). Accordingly, the 2-1 layer (421) is disposed between the metal layer (300) and the 2-2 layer (422).

[0085] The first-first layer (411) and the second-first layer (421) may include the same material. Specifically, the first-first layer (411) and the second-first layer (421) may include the same metal. For example, the first-first layer (411) and the second-first layer (421) may include nickel.

[0086] The first-second layer (412) and the second-second layer (422) may include different materials. Specifically, the first-second layer (412) and the second-second layer (422) may include different metals. For example, the first-second layer (412) may include gold (Au) or palladium (Pd). Additionally, the second-second layer (422) may include silver (Ag).

[0087] The above wire is bonded to the second plating layer (420). Accordingly, the second plating layer (420) must be formed to a sufficient thickness. Accordingly, if the 2-2 layer (422) includes gold, the process cost may increase. Since the 2-2 layer (422) includes silver, even if the 2-2 layer (422) is formed to a sufficient thickness, an increase in the process cost can be prevented.

[0088] The first plating layer (410) and the second plating layer (420) may have different sizes. For example, the thickness (T1) of the first plating layer (410) and the thickness (T2) of the second plating layer (420) may be different.

[0089] The thickness (T2) of the second plating layer (420) is greater than the thickness (T1) of the first plating layer (410). The thickness (T1-1) of the 1-1 layer (411) and the thickness (T2-1) of the 2-1 layer (421) may be different. In detail, the thickness (T1-1) of the 1-1 layer (411) may be smaller than the thickness (T2-1) of the 2-1 layer (421). In addition, the thickness (T1-2) of the 1-2 layer (412) and the thickness (T2-2) of the 2-2 layer (422) may be different. In detail, the thickness (T1-2) of the 1-2 layer (412) may be smaller than the thickness (T2-2) of the 2-2 layer (422). Accordingly, the thickness (T2) of the second plating layer (420) is greater than the thickness (T1) of the first plating layer (410).

[0090] The thickness (T1-1) of the first layer (411) may be 1 µm to 3 µm. In addition, the thickness (T2-1) of the second layer (421) may be 2 µm to 9 µm.

[0091] The thickness (T1-2) of the first-second layer (412) may be 0.01 μm to 0.1 μm. The first plating layer (410) is disposed on the first surface (1S) of the substrate (100). Therefore, the first plating layer (410) may be exposed to the outside of the IC card. The first-first layer (411) includes nickel. As a result, harmful toxicity may be transmitted to the user.

[0092] Accordingly, the 1-2 layer (421) is disposed on the 1-1 layer (411). This prevents the 1-1 layer (411) from being exposed to the outside. In addition, the 1-2 layer (422) includes gold. Therefore, corrosion of the first plating layer (410) is prevented. In addition, the aesthetic appeal of the user is improved. In addition, the 1-2 layer (412) is disposed with a very thin thickness. Therefore, the process cost is reduced and the process efficiency is improved.

[0093] The thickness (T2-2) of the second-second layer (422) may be 1 μm to 9 μm, 2 μm to 8 μm, or 3 μm to 7 μm. The second plating layer (420) is wire-bonded with the chip (C). Therefore, the thickness (T2-2) of the second-second layer (422) is greater than the thickness of the first-second layer (412). When the thickness (T2-2) of the second-second layer (422) is less than 1 μm, the wire is not stably bonded. In addition, when the thickness (T2-2) of the second-second layer (422) exceeds 9 μm, the process cost increases and the process efficiency decreases.

[0094] The wire is bonded to the 2-2 layer (422). When the organic coating layer is disposed on the 2-2 layer (422), the wire and the 2-2 layer (422) are not bonded. In addition, the wire and the 2-2 layer (422) are not electrically connected. Accordingly, the organic coating layer is not disposed on the 2-2 layer (422). In addition, silver is more reactive than gold. Therefore, the 2-2 layer (422) containing silver can be easily corroded.

[0095] Accordingly, the second-second layer (422) may be oxidized. Specifically, the second-second layer (422) may be oxidized during the process or during use. In addition, the oxidation rate of the second-second layer (422) may be high. Alternatively, the second-second layer (422) may be discolored.

[0096] Accordingly, the smart IC substrate includes a protective layer (450). The protective layer (450) is disposed on the other surface (302) of the metal layer. The protective layer (450) is disposed on the 2-2 layer (422). The protective layer (450) can be in contact with the 2-2 layer (422).

[0097] Alternatively, the second-second layer (422) may be oxidized during the process. Accordingly, a thin oxide layer (422a) may be formed on the second-second layer (422). If the thickness of the oxide layer (422a) increases, the second plating layer (420) may be damaged during wire bonding.

[0098] The above oxide layer (422a) is disposed with a very thin thickness. The oxide layer (422a) is disposed with a thin film thickness. The oxide layer (422a) is formed with a thickness that does not interfere with the movement of a signal when the signal moves from the protective layer (450) to the second-second layer (422).

[0099] The thickness of the above-mentioned oxide layer (422a) may be smaller than the thickness of the above-mentioned 2-1 layer (421). The thickness of the above-mentioned oxide layer (422a) may be smaller than the thickness of the above-mentioned 1-2 layer (412). The thickness of the above-mentioned oxide layer (422a) may be smaller than the thickness of the above-mentioned protective layer (450).

[0100] For example, the oxide layer (422a) may include silver oxide (Ag2O). Accordingly, the protective layer (450) may be disposed on the oxide layer (422a). Accordingly, the protective layer (450) may be in contact with the oxide layer (422a).

[0101] The protective layer (450) includes a conductive material. For example, the protective layer (450) may include a metal. Specifically, the protective layer (450) may include a metal having a lower reactivity than the second-second layer (422). Specifically, the protective layer (450) may include a metal having a lower ionization tendency than the second-second layer (422). For example, the protective layer (450) may include palladium (Pd), iridium (Ir), platinum (Pt), or gold (Au). For example, the protective layer (450) may include gold or palladium.

[0102] When the protective layer (450) contains gold or palladium, process efficiency can be improved. Specifically, when forming the first and second layers (412), the protective layer (450) can be formed simultaneously. Accordingly, the process of forming the protective layer (450) separately is omitted.

[0103] The above protective layer (450) may be formed with a thickness within a set range. The thickness (T3) of the protective layer (450) may be smaller than the thickness (T1-1) of the 1-1 layer. The thickness (T3) of the protective layer (450) may be smaller than the thickness (T1-2) of the 1-2 layer. The thickness (T3) of the protective layer (450) may be smaller than the thickness (T2-1) of the 2-1 layer. The thickness (T3) of the protective layer (450) may be smaller than the thickness (T2-2) of the 2-2 layer.

[0104] The protective layer (450) may have a thin film thickness. Specifically, the thickness (T3) of the protective layer may be less than 0.03 μm. More specifically, the thickness (T3) of the protective layer may be 0.001 μm to less than 0.03 μm, 0.002 μm to 0.02 μm, or 0.003 μm to 0.01 μm.

[0105] If the thickness of the protective layer (450) is less than 0.001 ㎛, the protective layer (450) cannot effectively protect the 2-2 layer. Accordingly, the 2-2 layer (422) may be oxidized significantly, and the thickness of the oxidation layer (422a) may increase. In addition, if the thickness of the protective layer (450) is 0.03 ㎛ or more, the process efficiency decreases and the process cost increases.

[0106] Hereinafter, a smart IC module according to the first embodiment will be described with reference to FIGS. 4 and 5.

[0107] Referring to FIGS. 4 and 5, the smart IC module (2000) includes the smart IC substrate (1000) and chip (C) described above.

[0108] The above chip (C) is placed on the second surface (2S). In detail, the chip (C) is placed on the bonding surface.

[0109] The chip (C) is connected to the second plating layer (420). In detail, the chip (C) and the second plating layer (430) are wire-bonded by a wire (W). Accordingly, the chip (C) and the conductive patterns (P) are electrically connected.

[0110] The above wire (W) comprises a metal. In detail, the wire (W) may comprise the same or different material as the second plating layer (420). For example, the wire (W) may comprise gold, copper, or aluminum.

[0111] A molding member (M) may be placed on the chip (C). The molding member (M) is placed so as to cover the chip (C) and the wire (W). Accordingly, damage to the wire bonding due to external impact can be prevented.

[0112] A smart IC substrate according to the first embodiment includes the protective layer. The protective layer includes a metal having a lower reactivity than the second-second layer. Accordingly, the second-second layer can be prevented from being oxidized or discolored. Alternatively, when the second-second layer is partially oxidized during the process, the corrosion rate of the second-second layer can be reduced.

[0113] Accordingly, the electrical conductivity and rigidity of the second plating layer are maintained. Therefore, damage to the second plating layer can be prevented during the wire bonding. In addition, the electrical connection characteristics between the chip and the conductive pattern are improved after the wire bonding.

[0114] Additionally, the corrosion rate of the second plating layer is reduced. Accordingly, the electrical conductivity of the second plating layer is maintained. Accordingly, the electrical connection characteristics of the chip and the conductive pattern can be maintained during use of the IC card.

[0115] Additionally, the protective layer can be formed by the same process as the first and second layers. Therefore, a separate process for forming the protective layer is omitted. Accordingly, process efficiency can be improved.

[0116] Hereinafter, a smart IC substrate and a smart IC module according to a second embodiment will be described with reference to FIGS. 6 to 10. Descriptions of similar or identical elements to those of the first embodiment will be omitted. Furthermore, identical reference numerals are used for elements identical to those of the first embodiment.

[0117] Referring to FIGS. 6 to 8, the smart IC substrate according to the second embodiment includes a substrate (100), a bonding layer (200), a metal layer (300), and a plating layer.

[0118] The above-described substrate (100) includes a first surface (1S) and a second surface (2S). The first surface (1S) and the second surface (2S) are opposite surfaces. The first surface (1S) is defined as a contact surface. In addition, the second surface (2S) is defined as a bonding surface.

[0119] The material, shape and thickness of the above-mentioned description (100) are the same as those of the first embodiment.

[0120] The above-mentioned substrate (100) includes a hole. In detail, the above-mentioned substrate (100) includes a first hole (H1) and a second hole (H2).

[0121] The size of the first hole (H1) and the size of the second hole (H2) are different. Specifically, the size of the first hole (H1) is smaller than the size of the second hole (H2). The shape of the first hole (H1) is different from the shape of the second hole (H2). For example, the first hole (H1) may be formed in a circular shape. In addition, the second hole (H2) may be formed in a polygonal shape. In addition, the number of the first hole (H1) and the number of the second hole (H2) are different. In detail, the number of the first holes (H1) is greater than the number of the second holes (H2).

[0122] The above second hole (H2) is an area where the chip (C) is placed. The above first hole (H1) is an area where wire bonding is performed. That is, the chip (C) placed inside the second hole (H2) is wire bonded to the plating layer through the first hole (H1).

[0123] The first hole (H1) above includes a plurality of holes. At least one of the plurality of holes is a wire-bonding region. For example, all of the plurality of holes are wire-bonding regions. Alternatively, some of the plurality of holes are wire-bonding regions.

[0124] The first hole (H1) has a width within a set range. The width of the first hole (H1) may be defined as the diameter of the first hole or the minimum distance between the inner surfaces of the first hole. For example, the width of the first hole (H1) may be 500 μm to 1000 μm, 600 μm to 900 μm, or 700 μm to 800 μm. When the width of the first hole (H1) is less than 500 μm, wire bonding through the first hole (H1) becomes difficult. In addition, when the width of the first hole (H1) exceeds 1000 μm, the support capacity of the substrate (100) decreases.

[0125] The above bonding layer (200) is placed on the above substrate (100). The material and thickness of the bonding layer (200) are the same as in the first embodiment.

[0126] The metal layer (300) is disposed on the substrate (100). The metal layer (300) is disposed on the bonding layer (200). The material and thickness of the metal layer (300) are the same as those of the first embodiment.

[0127] The above metal layer (300) includes a plurality of conductive patterns (P). The conductive patterns (P) are formed by patterning the metal layer (300).

[0128] The conductive patterns (P) are arranged on the first surface (1S). The conductive patterns (P) are arranged on the bonding layer (200). The conductive patterns (P) are arranged on the contact surface.

[0129] The above conductive patterns (P) are arranged spaced apart from each other. The holes (H) are arranged in areas corresponding to each conductive pattern (P).

[0130] The plating layer is disposed on the metal layer (300). In detail, the plating layer is disposed on one side (301) of the metal layer and the other side (302) opposite to the one side (301).

[0131] Referring to Fig. 8, the plating layer is divided into multiple plating layers according to location. Specifically, the plating layer may include a first plating layer (410), a second plating layer (420), and a third plating layer (430) arranged at different locations. The second plating layer (420) may be a pad portion to which the wire is bonded.

[0132] The first plating layer (410) is disposed on one surface (301) of the metal layer (300). The second plating layer (420) and the third metal layer (430) are disposed on the other surface (302) of the metal layer (300). The second plating layer (420) is disposed in an area overlapping the first hole (H1). The third plating layer (430) is disposed in an area overlapping the second hole (H2).

[0133] The first plating layer (410) includes a 1-1 layer (411) and a 1-2 layer (412). The 1-1 layer (411) is in contact with the metal layer (300). The 1-2 layer (412) is in contact with the 1-1 layer (411). Accordingly, the 1-1 layer (411) is disposed between the metal layer (300) and the 1-2 layer (412).

[0134] The second plating layer (420) includes a 2-1 layer (421) and a 2-2 layer (422). The 2-1 layer (421) is in contact with the metal layer (300). The 2-2 layer (422) is in contact with the 2-1 layer (421). Accordingly, the 2-1 layer (421) is disposed between the metal layer (300) and the 2-2 layer (422).

[0135] The third plating layer (430) includes a third-first layer (431) and a third-second layer (432). The third-first layer (431) is in contact with the metal layer (300). The third-second layer (432) is disposed in contact with the third-first layer (431). Accordingly, the third-first layer (431) is disposed between the metal layer (300) and the third-second layer (432).

[0136] The second plating layer (420) and the third plating layer (430) may include the same material. The second plating layer (420) and the third plating layer (430) may be formed with the same layer structure. In detail, the second plating layer (420) may have the layer structure of FIG. 3. In addition, the third plating layer (430) may have the same layer structure as the second plating layer.

[0137] Therefore, the second plating layer (420) and the third plating layer (430) can be formed by the same process. In detail, the second plating layer (420) and the third plating layer (430) can be formed simultaneously.

[0138] The above smart IC substrate includes a protective layer (450). The protective layer (450) is disposed on the other surface (302) of the metal layer. The protective layer (450) is disposed on the second plating layer (420). In addition, the protective layer (450) is not disposed on the third plating layer (430). That is, the protective layer (450) is selectively disposed.

[0139] In detail, the protective layer (450) is disposed on the 2-2 layer (422). The protective layer (450) may be in contact with the 2-2 layer (422). Alternatively, the 2-2 layer (422) may be oxidized during the process. Accordingly, an oxide layer (422a) may be formed on the 2-2 layer (422). For example, the oxide layer (422a) may include silver oxide (Ag2O). Accordingly, the protective layer (450) may be disposed on the oxide layer (422a). Accordingly, the protective layer (450) may be in contact with the oxide layer (422a).

[0140] Since the material and thickness of the above protective layer (450) are the same as those of the first embodiment, the following description is omitted.

[0141] Below, a smart IC module according to a second embodiment is described with reference to FIGS. 9 and 10.

[0142] Referring to FIGS. 9 and 10, the smart IC module (2000) includes the smart IC substrate (1000) and chip (C) described above.

[0143] The above chip (C) is placed inside the second hole (H2). In detail, the chip (C) is placed on the third plating layer (430).

[0144] The chip (C) is connected to the second plating layer (420). In detail, the chip (C) and the second plating layer (430) are wire-bonded by a wire (W). Accordingly, the chip (C) and the conductive patterns (P) are electrically connected.

[0145] A molding member (M) may be placed on the chip (C). The molding member (M) is placed so as to cover the chip (C) and the wire (W). Accordingly, damage to the wire bonding due to external impact can be prevented.

[0146] The smart IC substrate according to the second embodiment includes a first hole and a second hole. Accordingly, the smart IC substrate includes a receiving portion in which a chip is placed. Consequently, the thickness of the smart IC substrate manufactured using the smart IC substrate is reduced. In other words, the smart IC module is formed with a thin thickness. Consequently, the thickness of the IC card can be reduced.

[0147] Additionally, the smart IC substrate according to the second embodiment includes an optionally disposed protective layer. The protective layer is disposed on a plating layer to be wire-bonded. Specifically, the protective layer is disposed on a second plating layer.

[0148] The protective layer comprises a metal less reactive than the second layer. Accordingly, the second layer can be prevented from being oxidized or discolored. Alternatively, when the second layer is partially oxidized during the process, the corrosion rate of the second layer can be reduced.

[0149] Accordingly, the electrical conductivity and rigidity of the second plating layer are maintained. Therefore, damage to the second plating layer can be prevented during the wire bonding. In addition, the electrical connection characteristics between the chip and the conductive pattern are improved after the wire bonding.

[0150] Additionally, the corrosion rate of the second plating layer is reduced. Accordingly, the electrical conductivity of the second plating layer is maintained. Accordingly, the electrical connection characteristics of the chip and the conductive pattern can be maintained during use of the IC card.

[0151] Additionally, the protective layer can be formed by the same process as the first and second layers. Therefore, a separate process for forming the protective layer is omitted. Accordingly, process efficiency can be improved.

[0152] Additionally, the protective layer is not disposed on the third plating layer. Therefore, process efficiency is improved and process costs are reduced.

[0153] Hereinafter, a smart IC substrate and a smart IC module according to a third embodiment will be described with reference to FIGS. 11 to 18. Descriptions of similar or identical elements to those of the first embodiment will be omitted. Furthermore, identical reference numerals are assigned to elements identical to those of the first embodiment.

[0154] Referring to FIGS. 11 to 14, the smart IC substrate includes a substrate (100), a bonding layer (200), a metal layer (300), and a plating layer.

[0155] The above-described substrate (100) includes a first surface (1S) and a second surface (2S). The first surface (1S) and the second surface (2S) are opposite surfaces. The first surface (1S) is defined as a contact surface. In addition, the second surface (2S) is defined as a bonding surface.

[0156] The material, shape and thickness of the above-mentioned description (100) are the same as those of the first embodiment.

[0157] The above-described substrate (100) includes a hole (H). The hole (H) includes a plurality of holes. At least one of the plurality of holes is a region for wire bonding. For example, all of the plurality of holes are regions for wire bonding. Alternatively, some of the plurality of holes are regions for wire bonding. The chip (C) and the plating layer are wire bonded through the hole (H).

[0158] The above hole (H) has a width within a set range. The width of the hole (H) can be defined as the diameter of the hole or the minimum distance between the inner sides of the hole. For example, the width of the hole (H) can be 500 ㎛ to 1000 ㎛, 600 ㎛ to 900 ㎛, or 700 ㎛ to 800 ㎛. When the width of the hole (H) is less than 500 ㎛, wire bonding through the hole (H) becomes difficult. In addition, when the width of the hole (H) exceeds 1000 ㎛, the support capacity of the substrate (100) decreases.

[0159] The bonding layer (200) is disposed on the substrate (100). In detail, the bonding layer (200) includes a first bonding layer (210) and a second bonding layer (220). The first bonding layer (210) is disposed on the first surface (1S). The second bonding layer (220) is disposed on the second surface (2S).

[0160] The material and thickness of the above bonding layer (200) are the same as in the first embodiment.

[0161] The metal layer (300) is disposed on the substrate (100). The metal layer (300) includes a first metal layer (310) and a second metal layer (320). The first metal layer (310) is disposed on the first bonding layer (210). The second metal layer (320) is disposed on the second bonding layer (220).

[0162] The material and thickness of the above metal layer (300) are the same as in the first embodiment.

[0163] The above metal layer (300) includes a plurality of conductive patterns (P). The conductive patterns (P) are formed by patterning the metal layer (300).

[0164] The conductive patterns (P) are arranged on the first surface (1S). The conductive patterns (P) are arranged on the bonding layer (200). The conductive patterns (P) are arranged on the contact surface.

[0165] The above conductive patterns (P) are arranged spaced apart from each other. The holes (H) are arranged in areas corresponding to each conductive pattern (P).

[0166] The above smart IC substrate (1000) includes a wiring pattern (500). The wiring pattern (500) is disposed on the second surface (2S). The wiring pattern (500) is disposed on the second bonding layer (220). The wiring pattern (500) is disposed on the bonding surface.

[0167] The above wiring pattern (500) is connected to an external antenna pattern. Accordingly, the smart IC module can be operated in a contactless manner.

[0168] The above wiring pattern (500) may include a wiring portion (510) and a connection portion (520).

[0169] The above wiring section (510) may include a first wiring section (511), a second wiring section (512), and a third wiring section (513). The first wiring section (511) and the connection section (520) are disposed inside the molding area (MA). The second wiring section (512) and the third wiring section (513) are disposed outside the molding area (MA).

[0170] The first wiring section (511) and the third wiring section (513) can be connected by the second wiring section (512).

[0171] The first wiring portion (511), the second wiring portion (512), and the third wiring portion (513) may have different line widths. For example, the line width of the second wiring portion (512) may be larger than the line width of the first wiring portion (511). Accordingly, after the molding portion (M) is placed inside the molding area (MA), the wiring portion placed outside the molding portion (M) can be prevented from being damaged.

[0172] The line width of the third wiring portion (513) may be larger than the line widths of the first wiring portion (511) and the second wiring portion (512). The third wiring portion (513) is an area connected to the card body. Since the line width of the third wiring portion (513) is formed large, the smart IC substrate and the card body can be easily connected.

[0173] The above connecting portion (520) may include a first connecting portion (521) and a second connecting portion (522). In detail, at least one of the plurality of wiring patterns may include the first connecting portion (521) and the second connecting portion (522).

[0174] The sizes of the first connecting portion (521) and the second connecting portion (522) may be smaller than the size of the hole (H). In addition, the size of the second connecting portion (522) may be smaller than the size of the third wiring portion (513). For example, the area of ​​the second connecting portion (522) may be smaller than the area of ​​the third wiring portion (513). As a result, the space of the chip mounting area can be secured widely, and the packaging size can be reduced.

[0175] In addition, the first connection portion (521) or the second connection portion (522) is wire-bonded to the chip. The connection portion includes two or more connection portions. Therefore, if a problem occurs in the wire bonding of one connection portion, the problem can be resolved by wire bonding to another connection portion. For example, if a problem occurs in the wire bonding of the first connection portion (521), additional wire bonding can be performed to the second connection portion (522).

[0176] The plating layer is disposed on the metal layer (300). Referring to FIGS. 13 and 14, the plating layer is divided into a plurality of plating layers depending on the location. Specifically, the plating layer may include a first plating layer (410), a second plating layer (420), and a fourth plating layer (440) disposed at different locations.

[0177] The first plating layer (410) is disposed on one surface (311) of the first metal layer (310). The second plating layer (420) is disposed on the other surface (312) of the first metal layer (310). The second plating layer (420) is disposed in an area overlapping the hole (H). The second plating layer (420) may be a pad portion to which the wire is bonded. The fourth plating layer (440) is disposed on one surface (321) of the second metal layer (320). The wiring pattern (500) is formed by the second metal layer (320) and the fourth plating layer (440). The fourth plating layer (440) may include a pad portion to which the wire is bonded.

[0178] The first plating layer (410) includes a 1-1 layer (411) and a 1-2 layer (412). The 1-1 layer (411) is in contact with the first metal layer (310). The 1-2 layer (412) is in contact with the 1-1 layer (411). Accordingly, the 1-1 layer (411) is disposed between the first metal layer (310) and the 1-2 layer (412).

[0179] The second plating layer (420) includes a 2-1 layer (421) and a 2-2 layer (422). The 2-1 layer (421) is in contact with the first metal layer (310). The 2-2 layer (422) is in contact with the 2-1 layer (421). Accordingly, the 2-1 layer (421) is disposed between the first metal layer (310) and the 2-2 layer (422).

[0180] The fourth plating layer (440) includes a 4-1 layer (441) and a 4-2 layer (442). The 4-1 layer (441) is in contact with the second metal layer (320). The 4-2 layer (432) is in contact with the 4-1 layer (441). Accordingly, the 4-1 layer (441) is disposed between the second metal layer (320) and the 4-2 layer (442).

[0181] The fourth plating layer (440) may include the same material as the second plating layer (420). It may be formed with the same layer structure as the second plating layer (420) and the fourth plating layer (440). In detail, the second plating layer (420) may have the layer structure of FIG. 3. In addition, the fourth plating layer (440) may have the same layer structure as the second plating layer.

[0182] The smart IC substrate includes a protective layer. The protective layer includes a first protective layer (451) and a second protective layer (452). The first protective layer (451) and the second protective layer (452) are disposed at different positions. The first protective layer (451) is disposed on the other surface (312) of the first metal layer. The second protective layer (452) is disposed on one surface (321) of the second metal layer.

[0183] The first protective layer (451) is disposed on the second plating layer (420). Specifically, the first protective layer (451) is disposed on the 2-2 layer (422). The first protective layer (451) may be in contact with the 2-2 layer (422). Alternatively, the 2-2 layer (422) may be oxidized during the process. Accordingly, an oxide layer (422a) may be formed on the 2-2 layer (422). For example, the oxide layer (422a) may include silver oxide (Ag2O). Accordingly, the first protective layer (451) may be disposed on the oxide layer (422a). Accordingly, the first protective layer (451) may be in contact with the oxide layer (422a).

[0184] The second protective layer (452) is disposed on the fourth plating layer (440). Specifically, the second protective layer (452) is disposed on the 4-2 layer (442). The second protective layer (452) may be in contact with the 4-2 layer (442). Alternatively, the 4-2 layer (442) may be oxidized during the process. Accordingly, an oxide layer may be formed on the 4-2 layer (442). For example, the oxide layer may include silver oxide (Ag2O). Accordingly, the second protective layer (452) may be disposed on the oxide layer. Accordingly, the second protective layer (452) may be in contact with the oxide layer.

[0185] The first protective layer (451) and the second protective layer (452) include a conductive material. For example, the first protective layer (451) and the second protective layer (452) may include a metal.

[0186] In detail, the first protective layer (451) may include a metal having a lower reactivity than the second-second layer (422). In detail, the first protective layer (451) may include a metal having a lower ionization tendency than the second-second layer (422). For example, the first protective layer (451) may include palladium (Pd), iridium (Ir), platinum (Pt), or gold (Au).

[0187] Additionally, the second protective layer (452) may include a metal having a lower reactivity than the 4-2 layer (442). Specifically, the second protective layer (452) may include a metal having a lower ionization tendency than the 4-2 layer (442). For example, the second protective layer (452) may include palladium (Pd), iridium (Ir), platinum (Pt), or gold (Au).

[0188] The first protective layer (451) and the second protective layer (452) may contain the same material. Alternatively, the first protective layer (451) and the second protective layer (452) may contain different materials.

[0189] For example, the first protective layer (451) and the second protective layer (452) may include gold or palladium.

[0190] When the first protective layer (451) and the second protective layer (452) include gold or palladium, process efficiency can be improved. Specifically, when forming the first-second layer (412), at least one of the first protective layer (451) and the second protective layer (452) can be formed together. Accordingly, the process of forming the protective layer separately is omitted.

[0191] Since the thickness of the first protective layer and the second protective layer is the same as in the first embodiment, the following description is omitted.

[0192] Hereinafter, a smart IC module according to a third embodiment will be described with reference to FIGS. 15 to 18.

[0193] Referring to FIGS. 15 to 18, the smart IC module (2000) includes the smart IC substrate (1000) and chip (C) described above.

[0194] The above chip (C) is placed on the second bonding layer (220).

[0195] The chip (C) is connected to the second plating layer (420) and the fourth plating layer (440). In detail, the chip (C) and the second plating layer (430) are wire-bonded by a wire (W). Accordingly, the chip (C) and the conductive patterns (P) are electrically connected. In addition, the chip (C) and the fourth plating layer (440) are wire-bonded by the wire (W). Accordingly, the chip (C) and the antenna pattern are electrically connected.

[0196] A molding member (M) is placed on the chip (C). The molding member (M) is placed so as to cover the chip (C) and the wire (W). Accordingly, damage to the wire due to external impact can be prevented.

[0197] Referring to FIGS. 17 and 18, the second protective layer (452) can be optionally placed.

[0198] Referring to FIG. 17, the second protective layer (452) can be disposed entirely on the 4-2 layer (442).

[0199] Referring to FIG. 18, the second protective layer (452) may be optionally placed on the 4-2 layer (442).

[0200] The fourth plating layer (440) may include a first region (1A) and a second region (2A). The first region (1A) is a region where the wire (W) is bonded. The first region (1A) corresponds to the molding region. The first region (1A) is a region where the molding member (M) is disposed. The first region (1A) is a region where the first wiring portion (511) and the connection portion (520) are disposed. The second region (2A) is a region where the wire (W) is not bonded. The second region (2A) corresponds to a region other than the molding region. The second region (2A) is a region where the molding member (M) is not disposed. The second region (2A) is a region where the second wiring portion (512) and the third wiring portion (513) are disposed.

[0201] The second protective layer (452) may be disposed in the first region (1A). In addition, the second protective layer (452) may not be disposed in the second region (2A). That is, the second protective layer (452) is disposed in the inner region of the molding member and is not disposed in the outer region of the molding member.

[0202]

[0203] A smart IC substrate according to a third embodiment includes a protective layer. The protective layer includes a metal having a lower reactivity than the 2-2 layer and the 4-2 layer. Accordingly, the 2-2 layer and the 4-2 layer can be prevented from being oxidized or discolored. Alternatively, when the 2-2 layer and the 4-2 layer are partially oxidized during a process, the corrosion rate of the 2-2 layer and the 4-2 layer can be reduced.

[0204] Accordingly, the electrical conductivity and rigidity of the second plating layer and the fourth plating layer are maintained. Therefore, damage to the second plating layer and the fourth plating layer can be prevented during the wire bonding. In addition, the electrical connection characteristics of the chip and the conductive pattern are improved after the wire bonding.

[0205] In addition, the corrosion rate of the second plating layer and the fourth plating layer is reduced. Accordingly, the electrical conductivity of the second plating layer and the fourth plating layer is maintained. Accordingly, the electrical connection characteristics of the chip and the conductive pattern can be maintained during use of the IC card.

[0206] Additionally, the protective layer can be formed by the same process as the first and second layers. Therefore, a separate process for forming the protective layer is omitted. Accordingly, process efficiency can be improved.

[0207] Additionally, the protective layer is optionally disposed. Specifically, the second protective layer on the fourth plating layer is optionally disposed. Specifically, the second protective layer is disposed only on the inside of the molding member and not on the outside of the molding member. Accordingly, process efficiency is improved and process costs are reduced.

[0208]

[0209] Hereinafter, various modified embodiments of the second plating layer (420) of the embodiment will be described. Specifically, the following description focuses on the structure of the second plating layer (420) that is different from the structure of the smart IC substrate of any of the structures of FIGS. 1 to 18.

[0210] Referring to Fig. 19, the second plating layer (420) includes a 2-1 layer (421) and a 2-2 layer (422). The 2-1 layer (421) is disposed in contact with the metal layer (300). The 2-2 layer (422) is disposed in contact with the 2-1 layer (421). Accordingly, the 2-1 layer (421) is disposed between the metal layer (300) and the 2-2 layer (422). At this time, the 2-1 layer (421) may include nickel.

[0211] The first-second layer (412) and the second-second layer (422) may include different materials. In detail, the first-second layer (412) and the second-second layer (422) may include different metals. For example, the first-second layer (412) may include gold (Au) or palladium (Pd). The second-second layer (422) includes a metal having different physical or chemical properties from the first-second layer (412). For example, the melting point of the second-second layer (422) may be lower than the melting point of the first-first layer (412). The second plating layer (420) is wire-bonded to the chip. The wire bonding is performed using heat and pressure. Since the melting point of the second layer (422) is low, the second plating layer (420) is easily melted. Therefore, the wire bonding process becomes easy.

[0212] The electrical conductivity of the second-second layer (422) may be greater than the electrical conductivity of the first-first layer (412). The second plating layer (420) is wire-bonded to the chip. Since the electrical conductivity of the second-second layer (422) is greater, a signal transmitted from the chip is easily transmitted through the second plating layer (420).

[0213] The resistance of the 2-2 layer (422) may be smaller than the resistance of the 1-1 layer (412). The 2nd plating layer (420) is wire-bonded to the chip. Since the resistance of the 2-2 layer (422) is small, a signal transmitted from the chip is easily transmitted through the 2nd plating layer (420). The thermal conductivity of the 2-2 layer (422) may be higher than the thermal conductivity of the 1-1 layer (412). The 2nd plating layer (420) is wire-bonded to the chip. Heat is generated during the wire bonding. Since the thermal conductivity of the 2-2 layer (422) is large, heat is prevented from being concentrated in a specific area. That is, the 2nd plating layer (420) may have heat dissipation characteristics. Therefore, the reliability of the smart IC substrate is improved. For example, the second-second layer (422) may include silver (Ag). The thickness (T2) of the second plating layer (420) is greater than the thickness (T1) of the first plating layer (410).

[0214] For example, the thickness (T2-1) of the 2-1 layer (421) may be 2 µm to 9 µm. And, the thickness (T2-2) of the 2-2 layer (422) may be 1 µm to 9 µm, 2 µm to 8 µm, or 3 µm to 7 µm. The second plating layer (420) is wire-bonded with the chip (C). Therefore, the thickness (T2-2) of the 2-2 layer (422) is formed to be greater than the thickness of the 1-2 layer (412). When the thickness (T3-2) of the 2-2 layer (422) is less than 1 µm, the wire is not stably bonded. In addition, when the thickness (T2-2) of the 2-2 layer (422) exceeds 9 µm, the process cost increases and the process efficiency decreases.

[0215] According to a fourth embodiment, a smart IC substrate has different materials for the first plating layer and the second plating layer. The second-second layer has a lower melting point and resistance than the first-second layer. In addition, the second-second layer has higher electrical conductivity and thermal conductivity than the first-second layer. Accordingly, the process efficiency and electrical characteristics of the smart IC module are improved. In addition, the second-second layer is formed to a greater thickness than the first-second layer. In this case, the second-second layer is formed of a material other than gold. Therefore, the process cost is reduced.

[0216] Referring to Fig. 20, the second plating layer (420) includes a 2-1 layer (421), a 2-2 layer (422), and a 2-3 layer (423). The description of the 2-1 layer (421) and the 2-2 layer (422) is the same as that of Fig. 19.

[0217] The 2-3 layer (423) is disposed between the 2-1 layer (421) and the 2-2 layer (422). The 2-3 layer (423) includes a different material from the 2-1 layer (421). In addition, the 2-3 layer (423) includes a different material from the 2-2 layer (422). The 2-3 layer (423) may include the same material as the first plating layer (410). In detail, the 2-3 layer (423) includes the same material as the 1-2 layer (412). For example, the 2-3 layer (423) may include gold (Au).

[0218] The above 2-3 layer (423) may be formed with a thin film thickness. For example, the thickness (T2-3) of the 2-3 layer (423) may be the same as or similar to the thickness of the 1-2 layer (412). The 2-3 layer (423) and the 1-2 layer (412) may be formed by the same process. The 2-3 layer (423) and the 1-2 layer (412) may be formed simultaneously. For example, after the 1-1 layer (411) and the 2-1 layer (421) are formed, immersion plating may be performed. As a result, the 1-2 layer (412) and the 2-3 layer (423) may be formed on the 1-1 layer (411) and the 2-1 layer (421), respectively. For example, the thickness (T2-3) of the 2nd-3rd layer (423) may be 0.01 µm to 0.1 µm.

[0219] The smart IC substrate according to the fifth embodiment may further include the second-third layer. Accordingly, the second-second layer and the second-third layer may form a gold-silver alloy. Accordingly, the hardness of the second plating layer is improved. Accordingly, when the second plating layer and the chip are wire-bonded, cracking of the second plating layer can be prevented. In addition, a material having high hardness can be used as the wire material. Accordingly, wires of various materials can be used. In addition, the second-third layer may be formed by the same process as the first-second layer. In addition, the second-third layer is formed with a thin film thickness. Accordingly, the process efficiency of the smart IC substrate is improved.

[0220] Referring to Fig. 21, the second plating layer (420) includes a 2-1 layer (421), a 2-2 layer (422), a 2-3 layer (423), and a 2-4 layer (424). The description of the 2-1 layer (421) and the 2-2 layer (422) is the same as that of Fig. 19.

[0221] The above 2-3 layer (423) is positioned between the 2-1 layer (421) and the 2-2 layer (422). The description of the 2-3 layer (423) is the same as that of Fig. 20.

[0222] The 2-4 layer (424) is disposed on the 2-2 layer (422). The 2-4 layer (424) includes a different material from the 2-1 layer (421). In addition, the 2-4 layer (424) includes a different material from the 2-2 layer (422). The 2-4 layer (424) may include the same material as the 2-3 layer (423). In addition, the 2-4 layer (424) may include the same material as the first plating layer (410). In detail, the 2-4 layer (424) includes the same material as the 1-2 layer (412). For example, the 2-4 layer (424) may include gold (Au). The thickness (T2-4) of the 2-4th layer (424) is different from the thickness (T2-1) of the 2-1st layer (421). In detail, the thickness (T2-4) of the 2-4th layer (424) is smaller than the thickness (T2-1) of the 2-1st layer (421). The thickness (T2-4) of the 2-4th layer (424) is different from the thickness (T2-2) of the 2-2nd layer (422). In detail, the thickness (T2-4) of the 2-4th layer (424) is smaller than the thickness (T2-2) of the 2-2nd layer (422).

[0223] The above 2-4 layer (424) may be formed with a thin film thickness. For example, the thickness (T2-4) of the 2-4 layer (424) may be the same as or similar to the thickness (T2-3) of the 2-3 layer (423). Alternatively, the thickness (T2-4) of the 2-4 layer (424) may be the same as or similar to the thickness of the 1-2 layer (412). The 2-4 layer (424) and the 1-2 layer (412) may be formed by the same process. When the 2-4 layer (424) and the 1-2 layer (412) are formed by the same process, the 2-3 layer (423) and the 1-2 layer (412) are formed by different processes.

[0224] The 2-4 layer (424) and the 1-2 layer (412) may be formed simultaneously. For example, after forming the 1-1 layer (411) and the 2-1 layer (421), the 2-3 layer (423) and the 2-2 layer (422) may be sequentially formed on the 2-1 layer (421). Subsequently, immersion plating may be performed. As a result, the 1-2 layer (412) and the 2-4 layer (424) may be formed on the 1-1 layer (411) and the 2-2 layer (422), respectively. For example, the thickness (T2-4) of the 2-4 layer (424) may be 0.01 μm to 0.1 μm.

[0225] The smart IC substrate according to the sixth embodiment may further include the second-third layer and the second-fourth layer. Accordingly, the second-second layer and the second-third layer may form a gold-silver alloy. In addition, the second-third layer and the second-fourth layer may form a gold-silver alloy. Accordingly, the hardness of the second plating layer is improved. Accordingly, when the second plating layer and the chip are wire-bonded, cracking of the second plating layer can be prevented. In addition, a material having high hardness can be used as the material of the wire. Accordingly, wires of various materials can be used.

[0226] In addition, the 2nd-4th layer can be formed by the same process as the 1st-2nd layer. In addition, the 2nd-4th layer is formed with a thin film thickness. Accordingly, the process efficiency of the smart IC substrate is improved. In addition, the surface of the 2nd plating layer (420) can include gold. Therefore, corrosion of the 2nd plating layer (420) can be prevented.

[0227] Referring to Fig. 22, the second plating layer (420) includes a 2-1 layer (421), a 2-2 layer (422), a 2-3 layer (423), and a 2-4 layer (424). The description of the 2-1 layer (421) and the 2-2 layer (422) is the same as that of Fig. 19.

[0228] The above 2-3 layer (423) is disposed on the above 2-2 layer (422). The above 2-3 layer (423) includes a different material from the above 2-1 layer (421). In addition, the above 2-3 layer (423) includes a different material from the above 2-2 layer (422).

[0229] The second-third layer (423) may include the same material as the first plating layer (410). Specifically, the second-third layer (423) includes the same material as the first-second layer (412). For example, the second-third layer (423) may include gold (Au).

[0230] The thickness (T2-3) of the 2-3 layer (423) is different from the thickness (T2-1) of the 2-1 layer (421). In detail, the thickness (T2-3) of the 2-3 layer (423) is smaller than the thickness (T2-1) of the 2-1 layer (421). The thickness (T2-3) of the 2-3 layer (423) is different from the thickness (T2-2) of the 2-2 layer (422). In detail, the thickness (T2-3) of the 2-3 layer (423) is smaller than the thickness (T2-2) of the 2-2 layer (422).

[0231] The above 2-3 layer (423) may be formed with a thin film thickness. For example, the thickness (T2-3) of the 2-3 layer (423) may be the same as or similar to the thickness of the 1-2 layer (412). The 2-3 layer (423) and the 1-2 layer (412) may be formed by the same process. The 2-3 layer (423) and the 1-2 layer (412) may be formed simultaneously. For example, after forming the 1-1 layer (411) and the 2-1 layer (421), the 2-2 layer (422) may be formed on the 2-1 layer (421). Subsequently, immersion plating may be performed. By this, the 1-2 layer (412) and the 2-3 layer (423) can be formed on the 1-1 layer (411) and the 2-2 layer (422), respectively. For example, the thickness (T2-3) of the 2-3 layer (423) can be 0.01 µm to 0.1 µm.

[0232] The above 2-4 layer (424) is disposed on the above 2-3 layer (423). The above 2-4 layer (424) includes a different material from the above 2-1 layer (421). In addition, the above 2-4 layer (424) includes a different material from the above 2-3 layer (423).

[0233] The second-fourth layer (424) may include the same material as the second-second layer (422). For example, the second-fourth layer (424) may include silver (Ag).

[0234] The thickness (T2-4) of the 2-4th layer (424) is different from the thickness (T2-1) of the 2-1st layer (421). In detail, the thickness (T2-4) of the 2-4th layer (424) is smaller than the thickness (T2-1) of the 2-1st layer (421). The thickness (T2-4) of the 2-4th layer (424) is different from the thickness (T2-2) of the 2-2nd layer (422). In detail, the thickness (T2-4) of the 2-4th layer (424) is smaller than the thickness (T2-2) of the 2-2nd layer (422).

[0235] The above 2-4 layer (424) may be formed with a thin film thickness. For example, the thickness (T2-4) of the 2-4 layer (424) may be the same as or similar to the thickness (T2-3) of the 2-3 layer (423). Alternatively, the thickness (T2-4) of the 2-4 layer (424) may be the same as or similar to the thickness of the 1-2 layer (412). For example, the thickness (T2-4) of the 2-4 layer (424) may be 0.01 μm to 0.1 μm.

[0236] The smart IC substrate according to the seventh embodiment may further include the second-third layer and the second-fourth layer. Accordingly, the second-second layer and the second-third layer may form a gold-silver alloy. In addition, the second-third layer and the second-fourth layer may form a gold-silver alloy. Accordingly, the hardness of the second plating layer is improved. Accordingly, when the second plating layer and the chip are wire-bonded, cracking of the second plating layer can be prevented. In addition, a material having high hardness can be used as the wire material. Accordingly, wires of various materials can be used. In addition, the second-fourth layer is formed with a thin film thickness. Accordingly, the process efficiency of the smart IC substrate is improved. In addition, the surface of the second plating layer (420) may include silver. Accordingly, the second plating layer (420) melts at a low temperature. Therefore, the second plating layer and the wire can be easily bonded.

[0237] Meanwhile, although not shown in the drawing, the first plating layer (410) may not be disposed on one surface (301) of the metal layer (300). For example, the metal layer (300) may include an alloy. For example, the metal layer (300) may include a nickel (Ni)-chromium (Cr)-iron (Fe) alloy. Accordingly, the corrosion resistance of the metal layer (300) may be improved. Accordingly, even if a separate first plating layer (410) is not disposed on one surface (301) of the metal layer (300), corrosion of the metal layer (300) can be prevented. Accordingly, a separate plating layer may not be disposed on the contact surface. In addition, the thickness of the smart IC substrate can be reduced.

[0238]

[0239] Hereinafter, an IC card according to an embodiment will be described with reference to FIGS. 23 and 24.

[0240] Referring to FIGS. 23 and 24, the IC card (3000) may include a main body (3100), an upper layer (3210), and a lower layer (3220).

[0241] The above main body (3100) includes a receiving portion (3110). The smart IC module (2000) is placed inside the receiving portion (3110).

[0242] The above IC card can be operated in various modes. For example, the above IC card can be operated as a contact card.

[0243] Alternatively, an antenna pattern (not shown) may be arranged on the main body (3100). Specifically, the antenna pattern may be arranged in a coil shape at the edge of the main body (3100). Accordingly, the IC card may be operated as a contactless card, a combination card, or a hybrid card.

[0244] The smart IC module (2000) is inserted into the interior of the receiving portion (3110). The smart IC module (2000) and the main body (3100) are bonded by an adhesive layer (3120). As a result, the smart IC module (2000) is inserted into and fixed in the receiving portion (3110).

[0245] The upper layer (3210) is disposed on the upper portion of the main body (3100). The upper layer (3210) may include a transparent material. The upper layer (3210) may include a transparent resin material. The upper layer (3210) may be disposed as at least one layer. That is, the upper layer (3210) may include a plurality of layers.

[0246] The lower layer (3220) is disposed below the main body (3100). A magnetic stripe may be disposed on the lower layer (3220). The lower layer (3220) may include a transparent material. The lower layer (3220) may include a transparent resin material. The lower layer (3220) may be disposed as at least one layer. That is, the lower layer (3220) may include a plurality of layers.

[0247] The features, structures, effects, etc. described in the above-described embodiments are included in at least one embodiment of the present invention, and are not necessarily limited to just one embodiment. Furthermore, the features, structures, effects, etc. exemplified in each embodiment can be combined or modified in other embodiments by those skilled in the art to which the embodiments pertain. Therefore, the contents related to such combinations and modifications should be construed as falling within the scope of the present invention.

[0248] In addition, although the above description focuses on embodiments, these are merely examples and do not limit the present invention. Those skilled in the art to which the present invention pertains will appreciate that various modifications and applications not exemplified above are possible without departing from the essential characteristics of the present embodiments. For example, each component specifically shown in the embodiments can be modified and implemented. In addition, differences related to such modifications and applications should be interpreted as being included within the scope of the present invention defined in the appended claims.

Claims

1. A substrate comprising a first side and a second side opposite to the first side; A bonding layer disposed on the first surface; A metal layer disposed on the above bonding layer; A first plating layer disposed on one surface of the metal layer; and A second plating layer is disposed on the other surface of the metal layer, The first plating layer includes a 1-1 layer and a 1-2 layer on the 1-1 layer, The second plating layer includes a 2-1 layer and a 2-2 layer on the 2-1 layer, The above 2-2 layer comprises a different metal from the above 1-2 layer, A protective layer is placed on the above 2-2 layer, A smart IC substrate wherein the protective layer comprises a metal having a lower ionization tendency than the second-second layer.

2. In paragraph 1, A smart IC substrate wherein the protective layer comprises the same metal as the first and second layers.

3. In paragraph 1, The thickness of the above 2-2 layer is greater than the thickness of the above 1-2 layer, A smart IC substrate wherein the thickness of the above protective layer is smaller than the thickness of the first and second layers.

4. In paragraph 1, A smart IC substrate having an organic coating layer disposed on the first and second layers.

5. In paragraph 1, A smart IC substrate wherein the thickness of the first plating layer is smaller than the thickness of the second plating layer.

6. In paragraph 1, At least one of the first and second layers and the protective layer comprises gold, The above 2-2 layer is a smart IC substrate containing silver.

7. In paragraph 1, A smart IC substrate in which an oxide layer is disposed between the second layer and the protective layer.

8. In paragraph 1, The above description includes a first hole and a second hole, The size of the above first hole is smaller than the size of the above second hole, The second plating layer is disposed in an area overlapping the first hole, Further comprising a third plating layer disposed in an area overlapping the second hole, The third plating layer includes a 3-1 layer and a 3-2 layer on the 3-1 layer, A smart IC substrate in which the above protective layer is not disposed on the 3-2 layer.

9. A substrate comprising a plurality of holes, and comprising a first side and a second side opposite to the first side; A first bonding layer disposed on the first surface; A second bonding layer disposed on the second surface; A first metal layer disposed on the first bonding layer; A second metal layer disposed on the second bonding layer; A first plating layer disposed on one surface of the first metal layer; A second plating layer disposed on the other surface of the first metal layer; A fourth plating layer is disposed on one surface of the second metal layer, The first plating layer includes a 1-1 layer and a 1-2 layer on the 1-1 layer, The second plating layer includes a 2-1 layer and a 2-2 layer on the 2-1 layer, The fourth plating layer includes a 4-1 plating layer and a 4-2 plating layer on the 4-1 plating layer, The above 2-2 layer and the above 4-2 plating layer contain a different metal from the above 1-2 layer, A first protective layer is placed on the above 2-2 layer, A second protective layer is placed on the above 4-2 layer, The above first protective layer contains a metal having a lower ionization tendency than the above second-second layer, A smart IC substrate wherein the second protective layer comprises a metal having a lower ionization tendency than the fourth-second layer.

10. In paragraph 9, A smart IC substrate, wherein at least one of the first protective layer and the second protective layer comprises the same metal as the first and second layers.

Citation Information

Patent Citations

  • Smart IC contact structure of smart card module

    KR100810896B1

  • Printed circuit board for smart IC and manufacturing method therefor

    KR1020130134768A

  • Printed circuit board and manufacturing method therefor

    KR1020140078105A

  • Output stabilizing apparatus for multi-user intercommunication and output stabilizing mehotd using the same

    KR1020240079559A

  • Improved IC chip card

    WO2018035258A1