Heating unit and method for manufacturing same

The heat generating unit, utilizing a thermoplastic resin composition with a stacked copper and nickel plating layer formed via laser direct structuring and electroless/plating processes, addresses the challenges of rapid heat generation and plating reliability, achieving efficient performance for electronic cigarette vaporization units.

WO2024242523A1PCT designated stage expired Publication Date: 2024-11-28LOTTE CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095593
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-03-20
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing heating units for electronic cigarettes, such as vaporization units with metal coils, face challenges in achieving rapid heat generation and reliable plating, as they typically take around 4 minutes to reach 250°C with a metal coil, and there is a need for improved heat generation performance and plating reliability for applications like electronic cigarettes.

Method used

A heat generating unit is developed using a thermoplastic resin composition with a polyarylether ketone resin and a laser direct structuring additive, featuring a stacked copper and nickel plating layer formed through a laser direct structuring and electroless/plating process, optimizing the cross-sectional thickness ratio and plating process conditions to achieve rapid heat generation and enhanced reliability.

Benefits of technology

The solution enables a heat generating unit that reaches 150°C in 100 seconds or less, with improved plating reliability and heat resistance, suitable for use in electronic cigarettes and other applications, demonstrating excellent heat generation performance and plating reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024095593_28112024_PF_FP_ABST
    Figure KR2024095593_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A heating unit of the present invention comprises: a substrate formed from a thermoplastic resin composition including about 100 parts by weight of a polyaryletherketone resin and about 1-20 parts by weight of an additive for laser direct structuring; and a plating layer formed on at least a partial area of the surface of the substrate by a laser direct structuring process and a plating process, wherein the plating layer is a laminate of a copper plating layer and a nickel plating layer, the plating layer has a cross-sectional thickness of about 100-1,000 μm, and a ratio of the cross-sectional thickness of the copper plating layer to the cross-sectional thickness of the nickel plating layer is about 1:1-1:80. The heating unit has excellent heating performance, plating reliability, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Heating unit and manufacturing method thereof

[0001] The present invention relates to a heating unit and a method for manufacturing the same. More specifically, the present invention relates to a heating unit with excellent heating performance, plating reliability, etc., and a method for manufacturing the same.

[0002]

[0003] A laser direct structuring process (LDS process) can be used to plate a metal layer on at least a portion of the surface of a molded article formed from a thermoplastic resin composition. The LDS process is a process performed prior to the plating step, in which a laser is irradiated on the target area of ​​the molded article surface to modify the target area of ​​the molded article surface to provide properties suitable for plating. To this end, the thermoplastic resin composition for manufacturing the molded article must contain a laser direct structuring additive (LDS additive) capable of forming metal nuclei by the laser. The additive decomposes upon exposure to the laser to generate metal nuclei. In addition, the area irradiated with the laser has a roughened surface. Due to these metal nuclei and surface roughness, the area modified by the laser becomes suitable for plating.

[0004] Electronic cigarettes are atomizing devices that generate vapor by heating and vaporizing a liquid, and include a vaporizer for vaporizing the liquid. The vaporizer is a heating unit that generates heat when power is applied to vaporize the liquid. The vaporizer of an electronic cigarette is typically in the form of a metal coil, such as copper, wound inside or outside a plastic cylinder. A vaporizer (heating coil unit) using a metal coil has a maximum temperature of approximately 250°C and an operating time of approximately 4 minutes, including a heating time of approximately 30 seconds to reach the maximum temperature.

[0005] Recently, research has begun on manufacturing heating units using a metal plating process utilizing a laser direct structuring process, rather than using a metal coil. To be used in devices such as e-cigarettes, heating units manufactured using this plating process must exhibit excellent heating performance, reaching 150°C in less than 100 seconds, and possess excellent plating reliability.

[0006] Therefore, there is a need to develop a heating unit with excellent heating performance, plating reliability, etc. and a manufacturing method thereof.

[0007] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2011-0018319, etc.

[0008]

[0009] The purpose of the present invention is to provide a heating unit having excellent heating performance, plating reliability, etc.

[0010] Another object of the present invention is to provide a method for manufacturing the above-mentioned heating unit.

[0011] The above and other objects of the present invention can all be achieved by the present invention described below.

[0012]

[0013] 1. One aspect of the present invention relates to a heat generating unit. The heat generating unit comprises: a substrate formed from a thermoplastic resin composition comprising about 100 parts by weight of a polyaryletherketone resin and about 1 to about 20 parts by weight of an additive for laser direct structuring; and a plating layer formed on at least a portion of a surface of the substrate by a laser direct structuring process and a plating process; wherein the plating layer is a laminate of a copper plating layer and a nickel plating layer, and the plating layer has a cross-sectional thickness of about 100 to about 1,000 ㎛, and a cross-sectional thickness ratio of the copper plating layer and the nickel plating layer is about 1:1 to about 1:80.

[0014] 2. In the above 1 specific example, the polyaryletherketone resin may include a repeating unit represented by the following chemical formula 1.

[0015] [Chemical Formula 1]

[0016]

[0017] 3. In the above 1 or 2 specific examples, the polyaryl ether ketone resin is prepared at a temperature of 400°C and for 1000 sec according to ASTM D3835. -1 The melt viscosity measured by a capillary viscometer under shear rate conditions may be about 50 to about 500 Pa·s.

[0018] 4. In the above 1 to 3 specific examples, the additive for laser direct structuring may include at least one of a heavy metal complex oxide spinel and a copper salt.

[0019] 5. In the above 1 to 4 specific examples, the plating process may include a copper electroless plating step, a copper electrolytic plating step, and a nickel electrolytic plating step.

[0020] 6. In the above 1 to 5 specific examples, the plating process may include a nickel electroless plating step, a nickel electrolytic plating step, and a copper electrolytic plating step.

[0021] 7. In the above specific examples 1 to 6, the plating layer may have a maximum temperature of about 200 to about 300°C as measured by a thermal imaging camera when 20 A current and 10 V voltage are supplied.

[0022] 8. In the above specific examples 1 to 7, the time taken for the plating layer to reach 150°C as measured by a thermal imaging camera after supplying 20 A current and 10 V voltage may be about 1 to about 100 seconds.

[0023] 9. In the above 1 to 8 specific examples, the thermoplastic resin composition is aged at 25°C for 6 hours on an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm, and then the surface of the specimen is activated in a stripe shape through a laser direct structuring process, and the plating layer is formed on the activated surface through a plating process, and then the plated specimen is left in a chamber under conditions of 85°C and 85% RH for 72 hours, and 100 grids measuring 1 mm × 1 mm are imprinted on the plating layer, and then the number of grids that are not peeled off when the specimen is removed with tape may be about 90 to about 100.

[0024] 10. In the above 1 to 9 specific examples, the thermoplastic resin composition is aged at 25°C for 6 hours on an injection-molded specimen having a size of 50 mm × 90 mm × 3.2 mm, and then the surface of the specimen is activated in a stripe shape through a laser direct structuring process, and the plating layer is formed on the activated surface through a plating process, and then the plated specimen is left in a chamber under 250°C conditions for 200 hours, and 100 grids having a size of 1 mm × 1 mm are imprinted on the plating layer (copper layer), and then the number of grids that are not peeled off when the specimen is detached with tape may be about 90 to about 100.

[0025] 11. Another aspect of the present invention relates to a method for manufacturing a heating unit. The method comprises the steps of: manufacturing a substrate from a thermoplastic resin composition comprising about 100 parts by weight of a polyaryletherketone resin and about 1 to about 20 parts by weight of an additive for laser direct structuring; irradiating a laser onto at least a portion of a surface of the substrate; electrolessly plating copper or nickel onto the laser-irradiated area; electrolytically plating copper or nickel onto the electroless-plated copper or nickel plating layer; and electrolytically plating nickel or copper onto the electrolytically-plated copper or nickel plating layer to form a plating layer; wherein the plating layer is a laminate of a copper plating layer and a nickel plating layer, and the plating layer has a cross-sectional thickness of about 100 to about 1,000 ㎛, and a cross-sectional thickness ratio of the copper plating layer to the nickel plating layer is about 1:1 to about 1:80.

[0026] 12. In the above 11 specific examples, the substrate may be manufactured by injection molding the thermoplastic resin composition using an injection molding machine under conditions of a molding temperature of about 380 to about 480°C and a mold temperature of about 50 to about 200°C.

[0027] 13. In the above 11 or 12 specific examples, the wavelength of the laser may be 248 nm, 308 nm, 355 nm, 532 nm, 1,064 nm or 10,600 nm.

[0028] 14. In embodiments 11 to 13, the electroless plating of copper may be performed in an electroless copper plating solution at about 55°C for about 10 to about 40 minutes, and the electroless plating of nickel may be performed in an electroless nickel plating solution at about 50°C for about 10 to about 40 minutes.

[0029] 15. In specific examples 11 to 14, the electrolytic plating of the copper is performed at a current density of about 10 A / dm 2It can be performed for about 1 to about 3,000 minutes, and the electrolytic plating of nickel is performed at a current density of about 5 A / dm 2 It can be performed for about 1 to about 3,000 minutes.

[0030]

[0031] The present invention has the effect of providing a heating unit having excellent heating performance, plating reliability, etc., and a method for manufacturing the same.

[0032]

[0033] Figure 1 schematically illustrates a heating unit according to one specific example of the present invention.

[0034]

[0035] Hereinafter, the present invention will be described in detail as follows.

[0036] A heating unit according to the present invention comprises (A) a substrate formed from a thermoplastic resin composition; and (B) a plating layer.

[0037] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.

[0038]

[0039] (A) substrate

[0040] According to one specific example of the present invention, a substrate is formed from a thermoplastic resin composition for a laser direct structuring process (LDS process), wherein the thermoplastic resin composition comprises (a) a polyaryletherketone resin and (b) an additive for laser direct structuring.

[0041] (a) polyaryletherketone resin

[0042] A polyaryl ether ketone resin according to one specific example of the present invention can improve the plating reliability, heat resistance, etc. of a heating unit, and a polyaryl ether ketone resin used in a conventional thermoplastic resin composition can be used.

[0043] In a specific example, a polyaryl ether ketone resin (such as a polyether ether ketone resin) containing a repeating unit represented by the following chemical formula 1 can be used.

[0044] [Chemical Formula 1]

[0045]

[0046] In a specific example, the polyaryl ether ketone resin is prepared at a temperature of 400°C and for 1000 sec according to ASTM D3835. -1 The melt viscosity measured by a capillary viscometer under shear rate conditions may be about 50 to about 500 Pa·s, for example, about 100 to about 400 Pa·s. In the above range, the plating reliability and heat resistance of the heating unit may be excellent.

[0047] (b) Additives for laser direct structuring

[0048] According to one specific example of the present invention, the additive for laser direct structuring (LDS) is capable of forming a metal nucleus by a laser, and an additive for laser direct structuring used in a typical resin composition for laser direct structuring can be used. Here, the laser refers to light amplified by stimulated emission (stimulated emission light), and the laser may be ultraviolet light having a wavelength of about 100 to about 400 nm, visible light having a wavelength of about 400 to about 800 nm, or infrared light having a wavelength of about 800 to about 25,000 nm, for example, infrared light having a wavelength of about 1,000 to about 2,000 nm.

[0049] In specific examples, the additive for laser direct structuring may include heavy metal mixture oxide spinel and / or copper salt.

[0050] In specific examples, the heavy metal composite oxide spinel may include magnesium aluminum oxide (MgAl2O4), zinc aluminum oxide (ZnAl2O4), iron aluminum oxide (FeAl2O4), copper iron oxide (CuFe2O4), copper chromium oxide (CuCr2O4), manganese iron oxide (MnFe2O4), nickel iron oxide (NiFe2O4), titanium iron oxide (TiFe2O4), iron chromium oxide (FeCr2O4), magnesium chromium oxide (MgCr2O4), and combinations thereof. For example, copper chromium oxide (CuCr2O4) can be used. Since the copper chromium oxide (CuCr2O4) has a dark color, it can be applied when the color required for the final molded product is a dark color such as black or gray.

[0051] In specific examples, examples of the copper salt include, but are not limited to, copper hydroxide phosphate, copper phosphate, copper sulfate, cuprous thiocyanate, and combinations thereof. For example, copper hydroxide phosphate may be used. The copper hydroxide phosphate is a compound in which copper phosphate and copper hydroxide are combined, and may be specifically Cu3(PO4)2·2Cu(OH)2, Cu3(PO4)2·Cu(OH)2, etc. The copper hydroxide phosphate does not lower the color reproducibility of an additionally added colorant, so that a molded product of a desired color can be easily obtained.

[0052] In a specific example, the additive for laser direct structuring may have an average particle diameter of about 0.01 to about 50 μm, for example, about 0.1 to about 30 μm, specifically about 0.5 to about 10 μm. Within this range, a uniform plating surface can be formed during plating via laser direct structuring. In the present invention, unless otherwise specified, the average particle diameter is a number average diameter, and means the diameter measured by D50 (the particle diameter at the point where the distribution ratio is 50%).

[0053] In a specific example, the additive for laser direct structuring may be included in an amount of about 1 to about 20 parts by weight, for example, about 5 to about 15 parts by weight, based on about 100 parts by weight of the polyaryl ether ketone resin. If the content of the additive for laser direct structuring is less than about 1 part by weight based on about 100 parts by weight of the polyaryl ether ketone resin, there is a concern that when a laser is irradiated on a thermoplastic resin composition (substrate), a sufficient amount of metal nuclei may not be formed for plating, resulting in failure of plating or a decrease in plating reliability, etc., and if it exceeds about 20 parts by weight, there is a concern that the plating reliability, mechanical properties, etc. of the thermoplastic resin composition (substrate) may decrease.

[0054] A thermoplastic resin composition according to one embodiment of the present invention may further include additives included in conventional thermoplastic resin compositions. Examples of the additives include, but are not limited to, inorganic fillers, flame retardants, anti-drip agents, lubricants, nucleating agents, stabilizers, release agents, pigments, dyes, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the polyaryletherketone resin.

[0055] A thermoplastic resin composition according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 360 to about 420°C, for example, about 380 to about 410°C, using a conventional twin-screw extruder.

[0056] In a specific example, the thermoplastic resin composition is aged at 25°C for 6 hours on an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm, then the surface of the specimen is activated in a stripe shape through a laser direct structuring process, and the plating layer is formed on the activated surface through a plating process, and then the plated specimen is left in a chamber under conditions of 85°C and 85% RH for 72 hours, and 100 grids measuring 1 mm × 1 mm are imprinted on the plating layer (copper layer), and then the number of grids that are not peeled off when the specimen is removed with tape may be about 90 to about 100.

[0057] In a specific example, the thermoplastic resin composition is aged at 25°C for 6 hours on an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm, then the surface of the specimen is activated in a stripe shape through a laser direct structuring process, and the plating layer is formed on the activated surface through a plating process, and then the plated specimen is left in a chamber under conditions of 250°C for 200 hours, and 100 grids measuring 1 mm × 1 mm are imprinted on the plating layer (copper layer), and then the number of grids that are not peeled off when the specimen is removed with tape may be about 90 to about 100.

[0058] According to one embodiment of the present invention, a substrate is formed from the thermoplastic resin composition. For example, a molded product can be manufactured using the thermoplastic resin composition using a molding method such as injection molding, compression molding, blow molding, or extrusion molding. The substrate can be easily formed by a person skilled in the art to which the present invention pertains.

[0059]

[0060] (B) Plating layer

[0061] According to one specific example of the present invention, a plating layer is formed on at least a portion of the surface of the substrate by a laser direct structuring process and a plating process, and is a layered structure in which a copper plating layer and a nickel plating layer are laminated. The plating layer may have a cross-sectional thickness of about 100 to about 1,000 ㎛, and a cross-sectional thickness ratio of the copper plating layer and the nickel plating layer may be about 1:1 to about 1:80.

[0062] In a specific example, the plating process may include a copper electroless plating step, a copper electrolytic plating step, and a nickel electrolytic plating step. In this case, a plating layer in the form of a copper plating layer and a nickel plating layer sequentially laminated on a portion of the substrate surface can be obtained.

[0063] In a specific example, the plating process may include a nickel electroless plating step, a nickel electrolytic plating step, and a copper electrolytic plating step. In this case, a plating layer in the form of a nickel plating layer and a copper plating layer sequentially laminated on a portion of the substrate surface may be obtained.

[0064] In a specific example, the plating layer may have a cross-sectional thickness of about 100 to about 1,000 μm, for example, about 100 to about 700 μm, as measured by SEM / EDS (scanning electron microscope / energy dispersive spectroscopy). If the cross-sectional thickness of the plating layer is less than about 100 μm, there is a concern that plating reliability, etc. may be reduced, and if it exceeds about 1,000 μm, there is a concern that heat generation performance, etc. may be reduced.

[0065] In a specific example, the plating layer may have a cross-sectional thickness ratio (copper plating layer:nickel plating layer) of the copper plating layer and the nickel plating layer, as measured by SEM / EDS (scanning electron microscope / energy dispersive spectroscopy), of about 1:1 to about 1:80, for example, about 1:1.1 to about 1:50. When the cross-sectional thickness ratio of the plating layer is less than about 1:1, there is a concern that heat generation performance, plating reliability, etc. may be deteriorated, and when it exceeds about 1:80, there is a concern that heat generation performance, etc. may be deteriorated.

[0066] In a specific example, the plating layer may have a maximum temperature of about 200 to about 300°C, for example, about 230 to about 280°C, as measured by a thermal imaging camera when supplied with 20 A current and 10 V voltage.

[0067] In a specific example, the plating layer may reach a temperature of about 1 to about 100 seconds, for example, about 5 to about 60 seconds, when measured by a thermal imaging camera after supplying 20 A current and 10 V voltage.

[0068]

[0069] A heating unit according to one specific example of the present invention includes the substrate and the plating layer, and thus has excellent heating performance, plating reliability, etc., and can be used as a vaporizing unit (heating unit) of an electronic cigarette, an induction internal circuit, etc. In particular, when the heating unit is used as a vaporizing unit of an electronic cigarette, the shape of the substrate may be cylindrical, and the plating layer may be formed in a coil-like pattern on the inside or outside of the cylindrical substrate.

[0070]

[0071] FIG. 1 schematically illustrates a heat generating unit according to one embodiment of the present invention. The sizes of components constituting the invention in the drawing are exaggerated for clarity of the specification and are not limited thereto. As illustrated in FIG. 1, a heat generating unit (10) according to one embodiment of the present invention may include a substrate (20); and a plating layer (30) formed on at least a portion of the surface of the substrate (20) by a laser direct structuring process and a plating process.

[0072]

[0073] A heat generating unit (10) according to one specific example of the present invention can be manufactured by a manufacturing method including the steps of: manufacturing a substrate (20) from the thermoplastic resin composition; irradiating a laser to at least a portion of a surface area (a plating layer (30) area) of the substrate (20); electrolessly plating copper or nickel on the area irradiated with the laser; electrolytically plating copper or nickel on the electroless-plated plating layer of copper or nickel; and electrolytically plating nickel or copper on the electrolytically-plated plating layer of copper or nickel to form a plating layer (30).

[0074] In a specific example, the substrate (20) may be manufactured by injection molding the thermoplastic resin composition using an injection molding machine at a molding temperature of about 380 to about 480°C and a mold temperature of about 50 to about 200°C.

[0075] In a specific example, the laser direct structuring additive included in the substrate (20) is decomposed by the laser irradiation, thereby generating metal nuclei. In addition, the area irradiated with the laser (the area of ​​the plating layer (30)) has a surface roughness suitable for plating. The wavelength of the laser may be 248 nm, 308 nm, 355 nm, 532 nm, 1,064 nm, or 10,600 nm.

[0076] In a specific example, the electroless plating (metallization) process of copper or nickel may be performed through a conventional electroless plating process. For example, a copper or nickel electroless plating layer may be formed on the laser-irradiated area (plating layer (30) area) of the surface of the substrate (20) by immersing the laser-irradiated substrate (20) in one or more electroless plating baths.

[0077] In a specific example, the electrolytic plating (metallization) process of copper or nickel and the electrolytic plating process of nickel or copper may be performed through a conventional electrolytic plating process. For example, the substrate (20) on which copper or nickel is electrolessly plated may be immersed in one or more electrolytic plating baths, copper or nickel may be electroplated on the electroless plating layer of copper or nickel, and then nickel or copper may be electroplated on the electrolytic plating layer of copper or nickel, thereby finally forming the plating layer (30) on the laser-irradiated area of ​​the surface of the substrate (20).

[0078] In a specific example, the electroless plating of copper can be performed in an electroless copper plating solution (Circuposit 4500, etc.) at about 55°C for about 10 to about 40 minutes, and the electroless plating of nickel can be performed in an electroless nickel plating solution (Ronamax SMT-115, etc.) at about 50°C for about 10 to about 40 minutes.

[0079] In a specific example, the electrolytic plating of the copper is performed at a current density of about 10 A / dm 2 It can be performed for about 1 to about 3,000 minutes, and the electrolytic plating of nickel is performed at a current density of about 5 A / dm 2 It can be performed for about 1 to about 3,000 minutes. In the above range, a plating layer having a desired overall cross-sectional thickness and a cross-sectional thickness ratio of the copper plating layer and the nickel plating layer can be formed.

[0080] In this way, the heating unit (10) in which a plating layer (30) is formed on at least a portion of the surface of the substrate (20) by a laser direct structuring process can be easily formed by a person having ordinary knowledge in the field to which the present invention belongs.

[0081]

[0082] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.

[0083]

[0084] Example

[0085] Below, the specifications of each component used in the examples and comparative examples are as follows.

[0086] (A) Polyaryletherketone resin

[0087] (A1) Polyether ether ketone resin (manufacturer: Victrex, product name: 150G, melt viscosity: approximately 130 Pa·s) was used.

[0088] (A2) Polyether ether ketone resin (manufacturer: Victrex, product name: 450G, melt viscosity: approximately 350 Pa·s) was used.

[0089] (B) Additives for laser direct structuring

[0090] (B1) Copper hydroxide phosphate (Manufacturer: Merck performance materials, Product name: Iriotec) ® 8840) was used.

[0091] (B2) Copper chromium oxide (CuCr2O4, manufacturer: SHEPHERD, product name: Black 1G) was used.

[0092]

[0093] Examples 1 to 3 and Comparative Examples 1 to 5

[0094] After adding each of the above components in the contents as described in Tables 1 and 2 below, thermoplastic resin composition pellets were manufactured by extrusion at about 380°C. The extrusion was performed using a twin-screw extruder with an L / D of 36 and a diameter of 36 mm, and the manufactured pellets were dried at about 100°C for about 4 hours or more, and then injected using a 10 Oz injection molding machine (molding temperature: about 400°C, mold temperature: about 150°C) to manufacture substrate specimens. Next, a copper and / or nickel plating layer was formed as described in Tables 1 and 2 below, thereby manufacturing a heating unit specimen. Here, the electroless plating of copper (Examples 1 to 3, Comparative Examples 1 to 4) was performed in an electroless copper plating solution (Circuposit 4500) at about 55°C for about 10 to about 40 minutes, and the electroless plating of nickel (Comparative Example 5) was performed in an electroless nickel plating solution (Ronamax SMT-115) at about 50°C for about 10 to about 40 minutes. In addition, the electrolytic plating of copper (Examples 1 to 3, Comparative Examples 1 to 4) was performed at a current density of about 10 A / dm 2 It was performed for about 1 to about 3,000 minutes, and the electrolytic plating of nickel (Examples 1 to 3, Comparative Examples 2 to 5) was performed at a current density of about 5 A / dm 2 It was performed for about 1 to about 3,000 minutes. The physical properties of the manufactured heating unit specimens were evaluated using the following method, and the results are shown in Tables 1 and 2 below.

[0095]

[0096] Method of measuring physical properties

[0097] (1) Maximum temperature of plating layer: After supplying 20 A current and 10 V voltage to the plating layer of the heating unit specimens manufactured in the examples and comparative examples, the maximum temperature (unit: ℃) of the plating layer was measured using a thermal imaging camera (manufacturer: FLIR, device name: T335).

[0098] (2) Time for the plating layer to reach 150℃: After supplying 20 A current and 10 V voltage to the plating layer of the heating unit specimens manufactured in the examples and comparative examples, the time (unit: seconds) for the temperature of the plating layer to reach 150℃ was measured using a thermal imaging camera (manufacturer: FLIR, device name: T335).

[0099] (3) High-humidity plating reliability evaluation: After aging an injection-molded specimen (substrate specimen) measuring 50 mm × 90 mm × 3.2 mm at 25°C for 6 hours, the surface of the specimen was activated in a stripe shape through a laser direct structuring process, and a copper and / or nickel plating layer was formed as described in Tables 1 and 2 below. The plated specimen was left in a chamber under conditions of 85°C and 85% RH for 72 hours, and 100 grids measuring 1 mm × 1 mm were imprinted on the plating layer (copper layer). The number of grids that were not peeled off when removed with tape was measured.

[0100] (4) High-temperature plating reliability evaluation: After aging an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm at 25°C for 6 hours, the surface of the specimen was activated in a stripe shape through a laser direct structuring process, and a copper and / or nickel plating layer was formed as described in Tables 1 and 2 below. The plated specimen was left in a chamber at 250°C for 200 hours, and 100 grids measuring 1 mm × 1 mm were engraved on the plating layer (copper layer). The number of grids that were not peeled off when removed with tape was measured.

[0101]

[0102] Example 123 (A1) (parts by weight) 100 100 - (A2) (parts by weight) - 100 (B1) (parts by weight) 10 - 10 (B2) (parts by weight) - 10 - Copper plating layer cross-sectional thickness (㎛) 13 15 257 Nickel plating layer cross-sectional thickness (㎛) 9 5 5 3 13 4 1 Total plating layer cross-sectional thickness (㎛) 10 8 5 4 6 5 9 8 Cross-sectional thickness ratio (copper:nickel) 1:7.3 1:35.4 1:1.3 Maximum temperature (℃) 27 12 4 7 25 7 Time to reach 150℃ (sec) 10 3 5 1 8 High humidity plating reliability (units) 9 7 9 6 8 High temperature plating reliability (units) 9 8 9 5 9 7

[0103]

[0104] Comparative Example 12345 (A1) (parts by weight) 100 100 100 100 - (A2) (parts by weight) ---- 100 (B1) (parts by weight) 10 10 15 - 10 (B2) (parts by weight) --- 10 - Copper plating layer cross-section thickness (㎛) 1,05 21 13 21 13 - Nickel plating layer cross-section thickness (㎛) - 1,09 6 25 8 5 14 3 1 Total plating layer cross-section thickness (㎛) 1,05 21 10 7 5 7 9 6 4 4 3 1 Cross-section thickness ratio (copper:nickel) - 1:99.6 1:0.8 1:3.9 - Maximum temperature (℃) 16 3 17 4 18 4 2 1 1 2 3 1 1 Time to reach 50℃ (sec) 30 4 25 8 19 16 0 8 7 High-humidity plating reliability (units) 9 5 9 46 4 7 5 5 5 High-temperature plating reliability (dog)9597757164

[0105]

[0106] From the above results, it can be seen that the heating unit of the present invention has excellent heating performance (maximum temperature, time to reach 150°C), high humidity and high temperature plating reliability, etc.

[0107] On the other hand, in the case of Comparative Example 1, where a nickel plating layer is not applied and the thickness of the cross-section of the plating layer exceeds the scope of the present invention, it can be seen that the heat generation performance, etc. is deteriorated. In the case of Comparative Example 2, where the thickness of the cross-section of the plating layer exceeds the scope of the present invention and the cross-section thickness ratio of the copper plating layer and the nickel plating layer exceeds the scope of the present invention, it can be seen that the heat generation performance, etc. is deteriorated. In addition, in the case of Comparative Example 3, where the cross-section thickness ratio of the copper plating layer and the nickel plating layer is less than the scope of the present invention, it can be seen that the heat generation performance, high-humidity and high-temperature plating reliability, etc. are deteriorated. In the case of Comparative Example 4, where the thickness of the cross-section of the plating layer is less than the scope of the present invention, it can be seen that the high-humidity and high-temperature plating reliability, etc. are deteriorated. In the case of Comparative Example 5, where a copper plating layer is not applied, it can be seen that the high-humidity and high-temperature plating reliability, etc. are deteriorated.

[0108]

[0109] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.

Claims

1. A substrate formed from a thermoplastic resin composition comprising about 100 parts by weight of a polyaryl ether ketone resin and about 1 to about 20 parts by weight of an additive for laser direct structuring; and A plating layer formed by a laser direct structuring process and a plating process on at least a portion of the surface of the substrate; The above plating layer is a laminate of a copper plating layer and a nickel plating layer, The above plating layer has a cross-sectional thickness of about 100 to about 1,000 ㎛, A heating unit characterized in that the cross-sectional thickness ratio of the copper plating layer and the nickel plating layer is about 1:1 to about 1:

80.

2. A heating unit according to claim 1, characterized in that the polyaryl ether ketone resin includes a repeating unit represented by the following chemical formula 1. [Chemical Formula 1] 3. In the first or second paragraph, the polyaryl ether ketone resin is prepared at a temperature of 400°C and for 1000 sec according to ASTM D3835. -1 A heating unit characterized in that the melt viscosity measured by a capillary viscometer under shear rate conditions is about 50 to about 500 Pa·s.

4. A heating unit according to any one of claims 1 to 3, wherein the additive for laser direct structuring comprises at least one of a heavy metal complex oxide spinel and a copper salt.

5. A heating unit according to any one of claims 1 to 4, characterized in that the plating process includes a copper electroless plating step, a copper electrolytic plating step, and a nickel electrolytic plating step.

6. A heating unit according to any one of claims 1 to 5, wherein the plating process comprises a nickel electroless plating step, a nickel electrolytic plating step, and a copper electrolytic plating step.

7. A heating unit according to any one of claims 1 to 6, wherein the plating layer has a maximum temperature of about 200 to about 300°C as measured by a thermal imaging camera when 20 A current and 10 V voltage are supplied.

8. A heating unit according to any one of claims 1 to 7, wherein the plating layer has a time of reaching 150°C measured by a thermal imaging camera of about 1 to about 100 seconds after supplying 20 A current and 10 V voltage.

9. A heating unit according to any one of claims 1 to 8, wherein the thermoplastic resin composition is formed by aging an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm at 25°C for 6 hours, activating the surface of the specimen in a stripe shape through a laser direct structuring process, forming the plating layer on the activated surface through a plating process, leaving the plated specimen in a chamber under conditions of 85°C and 85% RH for 72 hours, and imprinting 100 grids measuring 1 mm × 1 mm on the plating layer, and then detaching the specimen with tape, the number of grids that are not peeled off is about 90 to about 100.

10. A heating unit according to any one of claims 1 to 9, wherein the thermoplastic resin composition is formed by aging an injection-molded specimen measuring 50 mm × 90 mm × 3.2 mm at 25°C for 6 hours, activating the surface of the specimen in a stripe shape through a laser direct structuring process, forming the plating layer on the activated surface through a plating process, leaving the plated specimen in a chamber under 250°C conditions for 200 hours, and then imprinting 100 grids measuring 1 mm × 1 mm on the plating layer (copper layer), and then detaching the specimen with tape, wherein the number of grids that are not peeled off is about 90 to about 100.

11. A substrate is manufactured from a thermoplastic resin composition comprising about 100 parts by weight of a polyaryl ether ketone resin and about 1 to about 20 parts by weight of an additive for laser direct structuring; Irradiating a laser to at least a portion of the surface of the substrate; Electroless plating of copper or nickel on the laser-irradiated area; Electrolytic plating of copper or nickel on a layer of electroless plating of copper or nickel; and A step of forming a plating layer by electroplating nickel or copper on a plating layer on which copper or nickel is electroplated; The above plating layer is a laminate of a copper plating layer and a nickel plating layer, The above plating layer has a cross-sectional thickness of about 100 to about 1,000 ㎛, A method for manufacturing a heat generating unit, characterized in that the cross-sectional thickness ratio of the copper plating layer and the nickel plating layer is about 1:1 to about 1:

80.

12. A method for manufacturing a heating unit, characterized in that in claim 11, the substrate is manufactured by injection molding the thermoplastic resin composition using an injection molding machine at a molding temperature of about 380 to about 480°C and a mold temperature of about 50 to about 200°C.

13. A method for manufacturing a heating unit, characterized in that the wavelength of the laser in claim 11 or 12 is 248 nm, 308 nm, 355 nm, 532 nm, 1,064 nm or 10,600 nm.

14. A method for manufacturing a heating unit, characterized in that in any one of claims 11 to 13, the electroless plating of copper is performed in an electroless copper plating solution at about 55°C for about 10 to about 40 minutes, and the electroless plating of nickel is performed in an electroless nickel plating solution at about 50°C for about 10 to about 40 minutes.

15. In any one of the 11th to 14th clauses, the copper electrolytic plating is performed at a current density of about 10 A / dm 2 It is performed for about 1 to about 3,000 minutes, and the electrolytic plating of nickel is performed at a current density of about 5 A / dm 2 A method for manufacturing a heating unit, characterized in that it is performed for about 1 to about 3,000 minutes.

Citation Information

Patent Citations

  • Conductive fabric and manufacturing and use thereof

    JP2021077633A

  • High dielectric constant laser direct structuring materials

    KR1020110018319A

  • Portable sterilizer

    KR1020220042590A

  • Apparatus and method for processing metal material

    KR102162526B1

  • Paek / paes compositions

    KR102163638B1