Opacified coating composition

The use of polymer fibers with a hydrophobic core and hydrophilic shell in an aqueous coating composition improves opacifier particle distribution, enhancing opacity and reducing costs by minimizing the need for expensive titanium dioxide and complex vesiculated polymer particles.

WO2024243629A1PCT designated stage expired Publication Date: 2024-12-05THE UNIV OF SYDNEY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/AU2024/050557
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing opacified coating compositions face challenges in achieving optimal opacity while minimizing cost, as they often require expensive titanium dioxide particles and complex manufacturing processes, such as those involving vesiculated polymer particles, which are costly and difficult to scale up.

Method used

An aqueous coating composition comprising a polymer binder, opacifier particles, and polymer fibers with a hydrophobic core and hydrophilic shell structure, where the polymer fibers improve the distribution and retention of opacifier particles, enhancing opacity without the need for vesiculated polymer particles.

Benefits of technology

The composition achieves enhanced opacity and reduced film porosity, allowing for a lower concentration of opacifier particles while maintaining or exceeding the opacity of traditional formulations, thus reducing costs and simplifying manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure AU2024050557_05122024_PF_FP_ABST
    Figure AU2024050557_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an aqueous coating composition comprising a polymer binder, opacifier particles and polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] OPACIFIED COATING COMPOSITION

[0002] FIELD OF THE INVENTION

[0003] The present invention relates in general to coating compositions and in particular to opacified coating compositions.

[0004] BACKGROUND OF THE INVENTION

[0005] Opacifiers play a pivotal role in many coating compositions such as paints, adhesives and the like, having the primary function of scattering and or absorbing light incident on a polymer film derived from the coating composition. How well a coating composition is able to visually obliterate a surface over which it is applied is referred to as its opacity. Titanium dioxide particles are commonly used as an opacifier in coating composition formulations and it, together with a polymer binder of the formulation, are the two main contributors to paint formulation cost.

[0006] Formulators are constantly seeking to balance reducing the cost of coating compositions while minimising or avoiding adversely affecting their properties.

[0007] Maintaining optimum distribution of opacifying particles throughout a coating composition and in the resulting polymer film derived therefrom is important to derive the best opacifying effect from the particles. Formulators go to great lengths to prevent aggregation of the opacifying particles in the compositions and resulting polymer film. For example, sophisticated surfactant systems are often used to enhance distribution of the opacifying particles. While the use of surfactants to minimise opacifying particle aggregation is effective, the surfactant in polymer film derived from such compositions can be leached from the film giving rise to undesirable surface effects and compromised film durability.

[0008] In the formulation of low sheen and flat coating compositions, cheaper mineral extender particles such as calcite, clay or talc can be incorporated in the formulations to reduce specula reflection down to a desired level.

[0009] With the aim of reducing cost, mineral extenders may be added to a coating compositions at such a level that there is insufficient polymer binder to bind (space fill) all the pigment present. The term "critical pigment volume concentration" (CPVC) is often used to describe the point where complete space filling can no longer occur. The addition of mineral extender beyond the CPVC can therefore lead to the formation of air voids in the coating composition film as drying occurs. Those voids scatter light in their own right and can contribute to coating composition film opacity thereby allowing an opportunity to reduce the level of titanium dioxide and still achieve acceptable opacity. The accompanying formula cost saving, however, is at the expense of other coating composition film properties such as scrub resistance and stain resistance. In the case of stain resistance, the problem is that of stains penetrating into the voids in the film (film porosity).

[0010] Vesiculated polymer particles have been used in paint formulations to great effect by providing voids of air in paint films that enhance opacity without the disadvantage of film porosity.

[0011] Vesiculated polymer particles can be prepared in the form of an aqueous dispersion using suspension and emulsion polymerisation techniques. When in the form of an aqueous dispersion, the voids of the particles are typically filled with water. When such a dispersion is dried, for example as part of a paint formulation applied as a film, the voids of the particles should become filled with air and thus enhance the opacifying properties of the particle s / applied coating.

[0012] The vesiculated polymer particles may also contain within their void region common opacifying particles such as titanium dioxide. The combination of the opacifying properties of the vesiculated polymer particles per se and the opacifying particles contained therein have been found to impart improved opacity to coating compositions.

[0013] Despite the advantages vesiculated polymer particles may provide, their methods of manufacture are often complex and introduce problems such as increased cost and difficulties in scale up.

[0014] Accordingly, there remains an opportunity for improving upon prior art techniques for delivering opacified coating compositions, or at the very least to provide a useful alternative. SUMMARY OF THE INVENTION

[0015] The present invention provides an aqueous coating composition comprising a polymer binder, opacifier particles and polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles.

[0016] It has now been found polymer films derived from the aqueous coating composition in accordance with the invention exhibit enhanced opacity relative to polymer films derived from the same composition absent the polymer fibres.

[0017] Without wishing to be limited by theory, it is believed the polymer fibres interact with the opacifier particles to improve their distribution throughout both the composition and polymer films derived from the composition. That improved distribution is believed to be reflected in the improved opacity of the resulting polymer film, relative to a polymer film derived from the same composition absent the polymer fibres. The polymer fibres are not readily leached from the resulting polymer film and advantageously do not impart adverse properties to either the composition or resulting polymer film.

[0018] The present invention also provides a method of producing an aqueous coating composition, the method comprising blending together a polymer binder, opacifier particles and polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles.

[0019] In one embodiment, the opacifier particles are selected from particles of metal oxide (e.g. titanium oxide, zinc oxide, iron oxide), carbon black, cobalt silicates, dibromanthrone, arylamide, copper phthalocyanine and combinations thereof.

[0020] In some embodiments, the polymer fibres have an average diameter of less than 150 nm, or less than 130 nm, or less than 110 nm, or less than 100 nm. Further aspects and / or embodiments of the invention are discussed in more detail below.

[0021] BRIEF DESCRIPTION OF DRAWINGS

[0022] The present invention will herein be described with reference to the following non-limiting drawings in which:

[0023] Figure 1 presents a plot of dry hiding power versus fPVC TiO2, which demonstrates that the inclusion of polymer fibres improves the opacity of a dry coating;

[0024] Figure 2 presents a plot of wet hiding power versus fPVC TiO2, which demonstrates that the inclusion of polymer fibres improves the opacity of a wet coating; and

[0025] Figure 3 presents an SEM image of polymer fibres used in accordance with the invention prepared in Example 9(b).

[0026] DETAILED DESCRIPTION OF THE INVENTION

[0027] The present invention provides an aqueous coating composition comprising a polymer binder.

[0028] Aqueous coating compositions find use in many different forms such as paints, adhesives, textile coatings, carpet backings and construction materials etc. An aqueous coating composition in accordance with the present invention is well suited for use as a paint and accordingly it may be convenient to hereinafter describe the invention with an emphasis toward that form of composition. However, it is to be understood the aqueous coating compositions according to the invention can be used in other forms / applications.

[0029] By being an "aqueous" coating composition is meant the composition is water-based and not organic solvent-based.

[0030] By being "water-based" is meant the liquid content of the coating composition will comprise at least 50 vol%, or at least 60 vol%, or at least 70 vol%, or at least 80 vol%, or at least 90 vol% water. The aqueous coating composition comprises a polymer binder. Those skilled in the art will be familiar with polymer binders suitable for use in aqueous coating compositions. Such polymer binders are also known in the art as aqueous polymer binders, an aqueous dispersion of polymer particles or simply as a latex.

[0031] A role aqueous coating compositions may be to form a polymer fdm on the surface of a substrate on which the coating composition has been applied. That polymer fdm generally serves to at least protect the substrate from the elements and in most cases also alter the visual appearance of the substrate, for example to hide, colour or obscure sight of the substrate.

[0032] The mechanism of polymer fdm formation of aqueous coating compositions / polymer binders has been well studied and is quite different to the process of polymer fdm formation of their organic solvent-based counterparts.

[0033] The initial consideration in the fdm formation process of aqueous coating compositions is the loss of water. As in the case of solvent loss in solvent-based compositions, that is effected by evaporation loss and / or loss through absorption into the substrate. However, unlike solventbased compositions, aqueous coating compositions comprise discrete, typically spherical-like, fdm forming particles of polymer dispersed throughout the aqueous phase. In order to produce a continuous fdm it is therefore necessary that those polymer particles overcome their coulombic and / or steric repulsions and begin to flatten and coalesce. By "coalesce" or "coalescence" it is meant that the polymer particles flow together to form a continuous fdm in which individual particles have lost their identity.

[0034] Polymer particle coalescence plays an important role in the polymer fdm formation process of aqueous coating compositions. Those skilled in the art are well versed with producing aqueous polymer binders (polymer dispersions or latexes) and their subsequent formulation into aqueous coating compositions to produce polymer fdm forming coating compositions.

[0035] For avoidance of any doubt, the aqueous coating compositions in accordance with the invention are intended to be fdm forming (i.e. a fdm forming aqueous coating composition).

[0036] The aqueous coating compositions according to the present invention can advantageously comprise a diverse range of polymer binders. Examples of suitable polymer binders include, but are not limited to, acrylic (e.g. styrene-acrylic copolymer, vinyl acetate -acrylic copolymer, urethane-acrylic copolymer and alkyd-acrylic copolymer) and vinyl acetate-ethylene copolymer binders.

[0037] In the art, reference to an acrylic polymer binder embraces all aqueous polymer dispersions that comprise polymer formed using (meth)acrylic acid monomer and / or (meth)acrylic ester (e.g. (meth)acrylates) monomer. Accordingly, the reference to an acrylic polymer binder herein embraces acrylic copolymer aqueous polymer dispersions such as styrene-acrylic copolymer, vinyl acetate -acrylic copolymer, urethane-acrylic copolymer and alkyd-acrylic copolymer aqueous polymer dispersions.

[0038] Examples of suitable polymer binders might therefore also be described to include, but are not limited to, acrylic and vinyl acetate-ethylene copolymer binders.

[0039] The polymer binder will generally be present in the aqueous coating composition in an amount ranging from about 5 wt. % to about 90 wt. %, or from about 10 wt. % to about 80 wt. %.

[0040] Generally, polymer that forms the polymer binder will have a weighted average molecular weight (Mw) in the range of about 10,000 to about 1,000,000, or from about 50, 000 to about 500,000.

[0041] As used herein, unless stated otherwise, reference to molecular weight is intended to be a weight average molecular weight (Mw) as measured by gel permeation chromatography.

[0042] The polymer binder used in accordance with the invention can advantageously be prepared using conventional techniques, apparatus and reagents well known to those skilled in the art.

[0043] The polymer binder will generally be formed through the polymerisation of ethylenically unsaturated monomers. Such monomers will generally be selected from those capable of undergoing free radical polymerisation in an aqueous environment. The polymer binder may comprise at least two different polymerised ethylenically unsaturated monomers and present in the form of a copolymer. In the context of the present invention, the polymer binder of course also comprises water.

[0044] Advantageously, a wide range of ethylenically unsaturated monomers may be used to form the polymer binder. The monomers will generally be capable of being polymerised with other monomers. The factors which determine copolymerisability of various monomers are well documented in the art. For example, see: Greenlee, R.Z., in Polymer Handbook 3rdEdition (Brandup, J., and Immergut. E.H. Eds) Wiley: New York, 1989 p 11 / 53.

[0045] Suitable ethylenically unsaturated monomers that may be used include those of general formula where U and W are independently selected from the group consisting of -CO2H, -CO2R2, -COR2, -CSR2, -CSOR2, -COSR2, -CONH2, -CONHR2, -CONR22, hydrogen, halogen and optionally substituted C1-C4 alkyl wherein the substituents are independently selected from the group consisting of hydroxy, -CO2H, -CO2R1, -COR2, -CSR2, -CSOR2, -COSR2, -CN, -CONH2, -CONHR2, -CONR22, -OR2, -SR2, -O2CR2, -SCOR2, and - OCSR2; and

[0046] V is selected from the group consisting of hydrogen, R2, -CO2H, -CO2R2, -COR2, -CSR2, -CSOR2, -COSR2, -CONH2, -CONHR2, -CONR22, -OR2, -SR2, -O2CR2, -SCOR2, and - OCSR2; where R2is selected from the group consisting of optionally substituted C1-C18 alkyl, optionally substituted C2-C18 alkenyl, optionally substituted aryl, optionally substituted heteroaryl, optionally substituted carbocyclyl, optionally substituted heterocyclyl, optionally substituted aralkyl, optionally substituted heteroarylalkyl, optionally substituted alkaryl, optionally substituted alkylheteroaryl and polymer chains wherein the substituents are independently selected from the group consisting of alkyleneoxidyl (epoxy), hydroxy, alkoxy, acyl, acyloxy, formyl, alkylcarbonyl, carboxy, sulfonic acid, alkoxy- or aryloxy-carbonyl, isocyanato, cyano, silyl, halo, amino, including salts and derivatives thereof. Preferred polymer chains include, but are not limited to, polyalkylene oxide, polyarylene ether and polyalkylene ether.

[0047] Examples of such monomers include, but are not limited to, maleic anhydride, N-alkylmaleimide, N-aryhnaleimide, dialkyl fumarate and cyclopolymerisable monomers, acrylate and methacrylate esters, acrylic and methacrylic acid, styrene, acrylamide, methacrylamide, and methacrylonitrile, mixtures of these monomers, and mixtures of these monomers with other monomers. As one skilled in the art would recognise, the choice of comonomers is determined by their steric and electronic properties. The factors which determine copolymerisability of various monomers are well documented in the art. For example, see: Greenlee, RZ. in Polymer Handbook 3rdEdition (Brandup, J., and Immergut, E.H Eds.) Wiley: New York. 1989 pII / 53.

[0048] Specific examples of useful ethylenically unsaturated monomers include the following: methyl methacrylate, ethyl methacrylate, propyl methacrylate (all isomers), butyl methacrylate (all isomers), 2-ethylhexyl methacrylate, isobomyl methacrylate, methacrylic acid, benzyl methacrylate, phenyl methacrylate, methacrylonitrile, alpha-methylstyrene, methyl acrylate, ethyl acrylate, propyl acrylate (all isomers), butyl acrylate (all isomers), 2-ethylhexyl acrylate, isobomyl acrylate, acrylic acid, benzyl acrylate, phenyl acrylate, acrylonitrile, styrene, functional methacrylates, acrylates and styrenes selected from glycidyl methacrylate, 2- hydroxyethyl methacrylate, hydroxypropyl methacrylate (all isomers), hydroxybutyl methacrylate (all isomers), N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl methacrylate, triethyleneglycol methacrylate, itaconic anhydride, itaconic acid, glycidyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate (all isomers), hydroxybutyl acrylate (all isomers), N,N-dimethylaminoethyl acrylate, N,N-diethylaminoethyl acrylate, triethyleneglycol acrylate, methacrylamide, N-methylacrylamide, N,N-dimethylacrylamide, N- tert-butylmethacrylamide, N-n-butylmethacrylamide, N-methylolmethacrylamide, N- ethylolmethacrylamide, N-tert-butylacrylamide, N-n-butylacrylamide, N-methylolacrylamide, N-ethylolacrylamide, vinyl benzoic acid (all isomers), diethylamino styrene (all isomers), alpha- methylvinyl benzoic acid (all isomers), diethylamino alpha-methylstyrene (all isomers), p- vinylbenzene sulfonic acid, p-vinylbenzene sulfonic sodium salt, trimethoxysilylpropyl methacrylate, triethoxysilylpropyl methacrylate, tributoxysilylpropyl methacrylate, dimethoxymethylsilylpropyl methacrylate, diethoxymethylsilylpropyl methacrylate, dibutoxymethylsilylpropyl methacrylate, diisopropoxymethylsilylpropyl methacrylate, dimethoxysilylpropyl methacrylate, diethoxysilylpropyl methacrylate, dibutoxysilylpropyl methacrylate, diisopropoxysilylpropyl methacrylate, trimethoxysilylpropyl acrylate, triethoxysilylpropyl acrylate, tributoxysilylpropylacrylate, dimethoxymethylsilylpropyl acrylate, diethoxymethylsilylpropyl acrylate, dibutoxymethylsilylpropyl acrylate, diisopropoxymethylsilylpropyl acrylate, dimethoxysilylpropyl acrylate, diethoxysilylpropyl acrylate, dibutoxysilylpropyl acrylate, diisopropoxysilylpropyl acrylate, vinyl acetate, vinyl butyrate, vinyl benzoate, vinyl chloride, vinyl fluoride, vinyl bromide, maleic anhydride, N- phenylmaleimide, N-butylmaleimide, N-vinylpyrrolidone, N-vinylcarbazole, butadiene, ethylene and chloroprene. This list is not exhaustive.

[0049] The polymer binder may also be provided with crosslinkable functionality. Such crosslinkable functionality of the polymer binder may promote formation of a crosslinked structure of a polymer film derived from the aqueous coating composition.

[0050] The polymer binder may therefore be prepared using crosslinking monomers.

[0051] In one embodiment, the polymer binder comprises polymerised residues of one or more crosslinking monomers.

[0052] Polymer binder comprising polymerised residues of one or more crosslinking monomers may herein be conveniently referred to as a crosslinkable polymer binder.

[0053] Those skilled in the art will appreciate that such a crosslinkable polymer binder may be prepared using various types of crosslinking monomers.

[0054] For example, multi -ethylenically unsaturated monomers can be used to afford a crosslinked polymer structure through polymerisation of at least two unsaturated groups to provide a crosslink. In that case, the crosslinked structure is typically provided through a free radical reaction mechanism.

[0055] Alternatively, a crosslinkable polymer binder may be prepared using ethylenically unsaturated monomers which also contain a reactive (or crosslinkable) functional group that is not susceptible to taking part in free radical reactions (i.e. "functionalised" unsaturated monomers). In that case, the monomers are incorporated into the polymer backbone through polymerisation of the unsaturated group, and the resulting pendant functional group provides means through which crosslinking may occur. By utilising monomers that provide complementary pairs of reactive functional groups (i.e. groups that will react with each other), the pairs of reactive functional groups can react through non radical reaction mechanisms to provide crosslinks. Formation of such crosslinks will generally occur during polymerisation of the monomers.

[0056] A variation on using complementary pairs of reactive functional groups is where the monomers are provided with non-complementary reactive functional groups. In that case, the functional groups will not react with each other but instead provide sites which can subsequently be reacted with a crosslinking agent to form the crosslinks. It will be appreciated that the crosslinking agents will be used in an amount to react with substantially all of the non- complementary reactive functional groups. Formation of the crosslinks under those circumstances will generally occur after the monomers polymerised to form the polymer binder.

[0057] A combination of those techniques for introducing crosslinkable character to the polymer binder may be used.

[0058] The terms "multi-ethylenically unsaturated monomers" and "functionalised unsaturated monomers" mentioned above can conveniently and collectively also be referred to herein as "crosslinking ethylenically unsaturated monomers" or "crosslinking monomers". By the general term "crosslinking ethylenically unsaturated monomers" or "crosslinking monomers" it is meant an ethylenically unsaturated monomer through which a crosslink is or will be derived. Accordingly, a multi-ethylenically unsaturated monomer will typically afford a crosslink during polymerisation, whereas a functionalised unsaturated monomer can provide means through which a crosslink can be derived either during or after polymerisation. It will be appreciated that not all unsaturated monomers that contain a functional group will be used in accordance with the invention for the purpose of functioning as a crosslinking monomer. For example, acrylic acid should not be considered as a crosslinking monomer unless it is used to provide a site through which a crosslink is to be derived.

[0059] Examples of suitable multi-ethylenically unsaturated monomers include, but are not limited to, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, 1,4-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, glycerol di(meth)acrylate, glycerol allyloxy di(meth)acrylate, l,l,l-tris(hydroxymethyl)ethane di(meth)acrylate, 1,1,1- tris(hydroxymethyl)ethane tri(meth)acrylate, 1, 1, l-tris(hydroxymethyl)propane di(meth)acrylate, l,l,l-tris(hydroxymethyl)propane tri(meth)acrylate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diallyl phthalate, diallyl terephthalte, divinyl benzene, methylol (meth)acrylamide, triallylamine, oleyl maleate, glyceryl propoxy triacrylate, allyl methacrylate, methacrylic anhydride and methylenebis (meth) acrylamide.

[0060] Examples of ethylenically unsaturated monomers that contain a crosslinkable functional group that is not susceptible to taking part in free radical reactions include, but are not limited to, acetoacetoxyethyl methacrylate, glycidyl methacrylate, A-mcthylolacrylamidc. (isobutoxymethyl)acrylamide, hydroxyethyl acrylate, / -butyl-carbodiimidocthyl methacrylate, acrylic acid, □-methacryloxypropyltriisopropoxysilane, 2-isocyanoethyl methacrylate and diacetone acrylamide.

[0061] Examples of suitable pairs of monomers mentioned directly above that provide complementary reactive functional groups include JV-methylolacrylamide and itself, (isobutoxymethyl)acrylamide and itself, □-methacryloxypropyltriisopropoxysilane and itself, 2- isocyanoethyl methacrylate and hydroxyethyl acrylate, and / -butyl-carbodiimidocthyl methacrylate and acrylic acid.

[0062] Examples of suitable crosslinking agents that can react with the reactive functional groups of one or more of the functionalised unsaturated monomers mentioned above include, but are not limited to, hexamethylene diamine, melamine, trimethylolpropane tris(2 -methyl- 1 -aziridine propionate) and adipic bishydrazide.

[0063] Examples of pairs of crosslinking agents and functionalised unsaturated monomers that provide complementary reactive groups include hexamethylene diamine and acetoacetoxyethyl methacrylate, hexamethylene diamine and glycidyl methacrylate, melamine and hydroxyethyl acrylate, trimethylolpropane tris(2-methyl-l -aziridine propionate) and acrylic acid, adipic bishydrazide and diacetone acrylamide.

[0064] Further detail concerning the free radical polymerisation of ethylenically unsaturated monomers is outlined below.

[0065] The aqueous coating compositions according to the present invention also comprises opacifier particles. The opacifier particles are used in the composition to assist with imparting opacity and colour to a polymer film derived from the composition. Opacity of the so formed polymer film occurs as a result of the opacifier particles scattering and / or absorbing light incident on the film, which in turn assists with hiding, obscuring and / or colouring a substrate surface on which the film has been applied.

[0066] The opacity of a polymer film derived from a coating composition in accordance with the invention is that determined by measuring the hiding power of a coating of the composition applied to a substrate. The opacity of the wet composition or the dry polymer film derived from the composition can be measured. The opacity of the dry polymer film derived from the composition general has the most practical relevance. The method of measuring the opacity of a dry polymer film involves preparing a film of the coating composition with known characteristics (i.e. dry film thickness and density) and using a spectrophotometer to determine the reflectance of incident light on the film that is applied on top of black and white tiles. The scatter coefficient can then be calculated which in turn relates to the hiding power of the film. Similarly, the method of measuring the opacity of a wet polymer film involves preparing a film of the coating composition with known characteristics (i.e. wet film thickness and density) and using a cryptometer to determine the reflectance of incident light on the film that is applied on top of black and white tiles. The scatter coefficient can then be calculated which in turn relates to the hiding power of the film.

[0067] Opacifier particles are also know in the art as pigment particles.

[0068] The aqueous coating compositions according to the present invention can advantageously be prepared using conventional opacifier particles.

[0069] The opacifier particles used in accordance with the invention are also not vesiculated polymer particles or contained within vesiculated polymer particles. Those skilled in the art will be familiar with the vesiculated polymer particles, which are essentially polymer particles that typically have a central void or hollow section. Vesiculated polymer particles have been used in aqueous coating compositions as opacifier particles. Such vesiculated polymer particles have also been prepared with conventional opacifier particles (e.g. titanium dioxide) located or contained within their void or hollow section. While such vesiculated polymer particles have been found to impart good opacifying properties to polymer films, their manufacture is quite complex and difficult to scale commercially.

[0070] For avoidance of any doubt, while the opacifier particles used in accordance with the invention are not vesiculated polymer particles or contained within vesiculated polymer particles, the aqueous coating composition in accordance with the invention may nevertheless still comprise vesiculated polymer particles, including those which contain within their structure conventional opacifier particles. The present invention is based on the surprising finding that enhanced opacifying properties can be derived using a relatively simple system in which polymer fibres interact with conventional opacifier particles to improve their distribution throughout both the composition and polymer films derived from the composition. Accordingly, the enhanced opacifying properties derived through application of the present invention can advantageously be achieved without using costly and preparatively challenging vesiculated polymer particles. In other words, provided the present invention uses opacifier particles that are not vesiculated polymer particles or contained within vesiculated polymer particles, the aqueous coating composition in accordance with the invention may nevertheless still comprise vesiculated polymer particles, including those which contain within their structure conventional opacifier particles.

[0071] In one embodiment, the aqueous coating composition in accordance with the invention comprises no more than 10 wt%, or no more than 5 wt%, or no more than 2 wt% of vesiculated polymer particles, relative to the total amount of opacifying particles present.

[0072] In another embodiment, the aqueous coating composition in accordance with the invention comprises no vesiculated polymer particles.

[0073] The present invention advantageously provides for aqueous coating compositions that can form polymer films having excellent opacity imparted with a reduced amount of conventional opacifier particles and without reliance upon vesiculated polymer particle technology.

[0074] Examples of opacifier particles that may be used in accordance with the invention include, but are not limited to, particles of metal oxide (e.g. titanium oxide, zinc oxide, iron oxide), carbon black, cobalt silicates, dibromanthrone, arylamide, copper phthalocyanine and combinations thereof.

[0075] In one embodiment, the opacifier particles are not polymer opacifier particles.

[0076] In one embodiment, the opacifier particles are inorganic opacifier particles.

[0077] The opacifier particles used in accordance with the present invention may have average diameter ranging from about 100 nm to about 1000 nm.

[0078] In some embodiments, the opacifier particles have an average diameter ranging from about 100 nm to about 600 nm, or from about 200 nm to about 600 nm, or from about 250 nm to about 450 nm, or about 300 nm.

[0079] The opacifier particles will generally be present in the aqueous coating composition in an amount ranging from about 5 wt. % to about 40 wt. %, or from about 10 wt. % to about 30 wt. 0 / / o.

[0080] A polymer film (wet or dry) derived from an aqueous coating composition in accordance with the present invention can exhibit higher opacity relative to a polymer film derived from the same aqueous coating composition absent the polymer fibres.

[0081] Accordingly, aqueous coating composition in accordance can advantageously be formulated with less opacifier particles and yet still provide for polymer films having excellent opacity.

[0082] For example, a polymer film derived from an aqueous coating composition in accordance with the invention can exhibit the same opacity of a polymer film derived from the same composition absent the polymer fibres and having up to about 5 wt.%, or up to about 10 wt. %, or up to about 15 wt. %, or up to about 20 wt. % more opacifier particles. In other words, the aqueous coating compositions in accordance with the invention can be formulated with up to about 20 wt. % less opacifier particles and yet still produce a polymer film having equivalent opacity to a polymer film derived from the same composition absent the polymer fibres and up to about 20 wt. % more opacifier particles. For example, if an aqueous coating composition formulation contains 25 wt% TiO2, then a 20% improvement in opacity of that formulation would mean a level of 20 wt% TiO2 (i.e. 25 - (25 x 20%)) could be used in accordance with the present invention to provide the same opacity.

[0083] In one embodiment, a polymer film derived from the aqueous coating composition has an opacity that is at least 5 %, or at least 10 %, or at least 15 %, or at least 20 % higher than a polymer film derived from the same composition absent the polymer fibres.

[0084] The aqueous coating composition also comprises polymer fibres.

[0085] In the context of the present invention a polymer fibre(s) is intended to mean a mass of polymer comprising morphology characterised by a thread, worm or filament like structure. The fibre morphology of the mass of polymer will have an aspect ratio >1. For example, the fibre morphology of the mass of polymer may have an aspect ratio >5, >20, >40, >60, >80, >100, or >200. The polymer fibre may include non-fibre like features. For example, the polymer fibre may terminate at one or both of its thread, worm or filament like ends with a mass of polymer not having a fibre morphology, such as a globular morphology. The polymer fibre may also include along its thread, worm or filament like structure (i.e. between its ends) a mass of polymer not having a fibre morphology, such as a globular morphology. When present, the nonfibre like features may have a similar height to the average diameter of the fibre morphology. For example, if present a globular morphology may be relatively flat having a height similar to the average diameter of the fibre morphology.

[0086] In one embodiment, the polymer fibres are provided in the form of a polymer mass comprising at least about 30 wt. %, about 40 wt. %, about 50 wt. %, about 60 wt. %, about 70 wt. %, about 80 wt. %, about 90 wt. %, or about 95 wt. % of polymer having fibre morphology.

[0087] Unless indicated otherwise, reference herein to features of the polymer fibre used in accordance with the invention are intended to be a reference to features of the morphology characterised by the thread, worm or filament like structure. For example, polymer fibres used in accordance with the invention have an average diameter of less than 200 nm. That diameter is intended to be a reference to the fibre morphology of the polymer fibre and not any other feature of the polymer fibre that does not have fibre morphology.

[0088] In some embodiments, the polymer fibres have an average diameter of less than 150 nm, or less than 130 nm, or less than 110 nm, or less than 100 nm.

[0089] In other embodiments, the polymer fibres have an average diameter ranging from about 20 nm to 200 nm, or about 20 nm to about 150 nm, or about 20 nm to about 130 nm, or about 20 nm to about 110 nm, or about 20 nm to about 100 nm, or about 20 nm to about 90 nm, or about 20 nm to about 80 nm.

[0090] Without wishing to be limited by theory, it is believed the fibre morphology feature of the polymer fibres used in accordance with the invention plays an important role in delivering improved opacity to polymer films derived from the aqueous coating compositions. The thread, worm or filament like features of the polymer fibre is believed to interact with the opacifier particles and assist with promoting their even distribution throughout the aqueous coating composition and also throughout a polymer film derived from the composition. Such even distribution reduces or avoids undesirable aggregation of the opacifier particles and thereby maximises the opacifying effect of the particles in the composition / film. In some embodiments, the polymer fibres have an average diameter less than 100 nm. Without wishing to be limited by theory, providing the polymer fibres with an average diameter of less than 100 nm may provide for an optimal spatial interaction with the opacifier particles that in turn maximises the opacifying effect imparted by the opacifier particles. As the diameter of the polymer fibre increases, so too does the spatial separation between opacifier particles interacting with the fibre. That increase in spatial separation between the opacifier particles is believed to reduce their opacifying effect.

[0091] In some embodiments, the polymer fibres have a length ranging from about 0. 1 micron to about 100 microns, or about 0.5 microns to about 20 microns.

[0092] The amount of polymer fibres used in the aqueous coating composition can vary depending upon the other constituent components of the composition, for example the type and amount of opacifier particles being used.

[0093] For a given aqueous coating composition the optimum amount of polymer fibre to be used can be determined by simply preparing a number of test samples with a progressively increasing amount of polymer fibre and measuring the opacity of the polymer films derived from the samples. The opacity measurements will readily identify an optimum amount of polymer fibre to be used. That same data can advantageously be used to calculate how much opacifier particles can be removed from the composition while still maintaining acceptable opacity.

[0094] In one embodiment, the polymer fibres are provided in the form of a polymer mass and that polymer mass is present in an amount ranging from about 0. 1 wt. % to about 30 wt. %, or about 1 wt. % to about 10 wt. %, relative to a dry mass of a polymer film derived from the aqueous coating composition.

[0095] The polymer mass that provides the polymer fibres may comprising at least about 10 wt. %, about 20 wt. %, about 30 wt. %, about 40 wt. %, about 50 wt. %, about 60 wt. %, about 70 wt. %, about 80 wt. %, about 90 wt. %, or about 95 wt. % of polymer having fibre morphology.

[0096] Size (diameter, length etc) and morphology attributes of both the opacifier particles and polymer fibres can be determined using electron microscopy techniques such as TEM and SEM in conjunction with image analysis software (e.g. ImageJ).

[0097] In addition to the polymer fibres having an average diameter of less than 200 nm, they also have a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure.

[0098] Block copolymers are known in the art to self-assemble or become arranged so as to present in the form of a polymer fibre having a core-shell structure. When presented in an aqueous environment, block copolymers having a hydrophobic block and a hydrophilic block preferentially arrange into polymer fibres having a hydrophobic core and a hydrophilic shell.

[0099] Conventional block copolymers that self-assemble or become arranged into the form of a fibre having a hydrophobic core and a hydrophilic shell can advantageously be used in accordance with the invention.

[0100] By virtue of the polymer fibres used in accordance with the invention having a hydrophobic core and a hydrophilic shell, those skilled in the art will be appreciate the block copolymer from which they are formed correspondingly comprises a hydrophobic block and a hydrophilic block.

[0101] In other words, the polymer fibres have a composition formed from a block copolymer comprising a hydrophilic polymer block and hydrophobic polymer block that arrange so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure.

[0102] The hydrophilic and hydrophobic polymer blocks may be a homo-polymer hydrophilic block and a homo-polymer hydrophobic polymer block, respectively. Alternatively, the hydrophilic and hydrophobic polymer blocks may in their own right each be a co-polymer hydrophilic block and co-polymer hydrophobic polymer block, respectively. The hydrophilic and hydrophobic polymer blocks may independently be each made up from a combination of homo-polymer and co-polymer blocks.

[0103] A polymer block within the block copolymer will typically comprise no fewer than about 5 polymerised monomer units.

[0104] In some embodiments, the block copolymer comprises a hydrophobic polymer block and a hydrophilic polymer block having a hydrophobic polymer block to hydrophilic polymer block molecular weight ratio ranging from about 0.5 to about 10, or about 1 to about 8, or about 3 to about 7.

[0105] The block copolymer used in accordance with the invention may be described as comprising an AB block copolymer structure, where A represents the hydrophilic block (that ultimately forms the shell of the polymer fibre) and B represents a hydrophobic block (that ultimately forms the core of the polymer fibre).

[0106] The hydrophilic and hydrophobic polymer blocks may be directly or indirectly covalently coupled.

[0107] Whether or not the hydrophilic and hydrophobic polymer blocks are directly or indirectly covalently coupled will typically depend upon the technique used for producing the block copolymer.

[0108] For example, a run of hydrophilic monomers may be polymerised to first form the hydrophilic block, followed by introduction of hydrophobic monomer to be polymerised to form the hydrophobic block that is directly covalently coupled to the hydrophilic block.

[0109] Alternatively, hydrophilic monomer may be polymerised to form the hydrophilic block and separately hydrophobic monomer may be polymerised to form the hydrophobic block. Those two separately prepared polymer blocks may then be indirectly covalently coupled through a coupling agent (CA).

[0110] In that case, the block copolymer used in accordance with the invention may be described as comprising an A-CA-B block copolymer structure, where A represents the hydrophilic block (that ultimately forms the shell of the polymer fibre) and B represents a hydrophobic block (that ultimately forms the core of the polymer fibre) and CA represents a coupling agent that covalently couples A with B.

[0111] Hydrophobic monomer and hydrophilic monomer may also be selectively polymerised using a polymerisation agent (PA) that also functions to indirectly couple at least one of the hydrophilic or hydrophobic polymer blocks. For example, the block copolymer used in accordance with the invention may be described as comprising an AB-PA-BA block copolymer structure, where A represents a hydrophilic block (that ultimately forms the shell of the polymer fibre) and B represents a hydrophobic block (that ultimately forms the core of the polymer fibre) and PA represents a polymerisation agent that, in this case covalently couples B with B (and consequently AB with BA). Here, each B may be the same or different, each A may be the same or different and each A and B may independently be a homo-polymer or co-polymer.

[0112] Alternatively, a polymerisation agent may be used to form a block copolymer comprising a PA- BA block copolymer structure, where A represents a hydrophilic block (that ultimately forms the shell of the polymer fibre) and B represents a hydrophobic block (that ultimately forms the core of the polymer fibre) and PA represents a polymerisation agent. Each A and B may independently be a homo-polymer or co-polymer.

[0113] The block copolymers used in accordance with the present invention may be conveniently prepared using conventional free radical polymerisation techniques and reagents.

[0114] Controlled radical polymerisation (CRP) can be used to effectively produce the block copolymers.

[0115] Those skilled in the art will appreciate CRP is typically performed using a polymerisation agent commonly known in the art as a controlled radical polymerisation agent or moiety.

[0116] As used herein, a "controlled radical polymerisation agent (moiety)" is intended to mean a polymerisation agent that can participate in and control or mediate the radical polymerisation of one or more ethylenically unsaturated monomers so as to form a polymer chain.

[0117] Examples of CRP include iniferter polymerisation, stable free radical mediated polymerisation (SFRP), atom transfer radical polymerisation (ATRP), and reversible addition fragmentation chain transfer (RAFT) polymerisation.

[0118] In one embodiment, the block copolymer used in accordance with the present invention is a RAFT block copolymer.

[0119] By being a "RAFT block copolymer" is meant a block copolymer that has been prepared by RAFT polymerisation. A polymer prepared by RAFT polymerisation is therefore often conveniently referred to as a RAFT polymer. By virtue of the mechanism of polymerisation, such polymers will comprise residue of the RAFT agent that facilitated polymerisation of the monomer.

[0120] RAFT agents suitable for use in preparing the block copolymers comprise a thiocarbonylthio group (which is a divalent moiety represented by: -C(S)S-). RAFT polymerisation and RAFT agents are described in numerous publications such as WO 98 / 01478, Moad G.; Rizzardo, E; Thang S, H. Polymer 2008, 49, 1079-113 land Aust. J. Chem., 2005, 58, 379-410; Aust. J. Chem., 2006, 59, 669-692; and Aust. J. Chem., 2009, 62, 1402-1472. Suitable RAFT agents for use in preparing the block copolymers include xanthate, dithioester, dithiocarbamate and trithiocarbonate compounds.

[0121] A RAFT agent suitable for preparing the block copolymers used in accordance with the invention may be represented by general formula (II) or (III): where Z and R are groups, and R* and Z* are x-valent and y-valent groups, respectively, that are independently selected such that the agent can function as a RAFT agent in the polymerisation of one or more ethyl enically unsaturated monomers; x is an integer > 1; and y is an integer > 2.

[0122] To function as a RAFT agent in the polymerisation of one or more ethylenically unsaturated monomers, those skilled in the art will appreciate that R and R* will typically be an optionally substituted organic group that function as a free radical leaving group under the polymerisation conditions employed and yet, as a free radical leaving group, retain the ability to reinitiate polymerisation. Those skilled in the art will also appreciate that Z and Z* will typically be an optionally substituted organic group that function to give a suitably high reactivity of the C=S moiety in the RAFT agent towards free radical addition without slowing the rate of fragmentation of the RAFT-adduct radical to the extent that polymerisation is unduly retarded.

[0123] In formula (II), R* is a x-valent group, with x being an integer > 1. Accordingly, R* may be mono-valent, di-valent, tri-valent or of higher valency. Generally, x will be an integer ranging from 1 to about 20, for example from about 2 to about 10, or from 1 to about 5.

[0124] Similarly, in formula (III), Z* is a y-valent group, with y being an integer > 2. Accordingly, Z* may be di -valent, tri-valent or of higher valency. Generally, y will be an integer ranging from 2 to about 20, for example from about 2 to about 10, or from 2 to about 5.

[0125] Examples of R in suitable RAFT agents include optionally substituted, and in the case of R* in suitable RAFT agents include a x-valent form of optionally substituted, alkyl, alkenyl, alkynyl, aryl, acyl, carbocyclyl, heterocyclyl, heteroaryl, alkylthio, alkenylthio, alkynylthio, arylthio, acylthio, carbocyclylthio, heterocyclylthio, heteroarylthio, alkylalkenyl, alkylalkynyl, alkylaryl, alkylacyl, alkylcarbocyclyl, alkylheterocyclyl, alkylheteroaryl, alkyloxyalkyl, alkenyloxyalkyl, alkynyloxyalkyl, aryloxyalkyl, alkylacyloxy, alkylcarbocyclyloxy, alkylheterocyclyloxy, alkylheteroaryloxy, alkylthioalkyl, alkenylthioalkyl, alkynylthioalkyl, arylthioalkyl, alkylacylthio, alkylcarbocyclylthio, alkylheterocyclylthio, alkylheteroarylthio, alkylalkenylalkyl, alkylalkynylalkyl, alkylarylalkyl, alkylacylalkyl, arylalkylaryl, arylalkenylaryl, arylalkynylaryl, arylacylaryl, arylacyl, arylcarbocyclyl, arylheterocyclyl, arylheteroaryl, alkenyloxyaryl, alkynyloxyaryl, aryloxyaryl, alkylthioaryl, alkenylthioaryl, alkynylthioaryl, arylthioaryl, arylacylthio, arylcarbocyclylthio, arylheterocyclylthio, arylheteroarylthio, and a polymer chain.

[0126] For avoidance of any doubt reference herein to "optionally substituted", alkyl, alkenyl... etc, is intended to mean each group such as alkyl and alkenyl is optionally substituted.

[0127] Examples of R in suitable RAFT agents also include optionally substituted, and in the case of R* an x-valent form of optionally substituted, alkyl; saturated, unsaturated or aromatic carbocyclic or heterocyclic ring; alkylthio; dialkylamino; an organometallic species; and a polymer chain.

[0128] More specific examples of R in suitable RAFT agents include optionally substituted, and in the case of R* in suitable RAFT agents include an x-valent form of optionally substituted, Ci-Cis alkyl, C2-C18 alkenyl, C2-C18 alkynyl, Ce-Cis aryl, Ci-Cis acyl, C3-C18 carbocyclyl, C2-C18 heterocyclyl, C3-C18 heteroaryl, Ci-Cis alkylthio, C2-C18 alkenylthio, C2-C18 alkynylthio, GrC’is arylthio, Ci-Cis acylthio, C3-C18 carbocyclylthio, C2-C18 heterocyclylthio, C3-C18 heteroarylthio, C3-C18 alkylalkenyl, C3-C18 alkylalkynyl, C7-C24 alkylaryl, C2-C18 alkylacyl, C4-C18 alkylcarbocyclyl, C3-C18 alkylheterocyclyl, C4-C18 alkylheteroaryl, C2-C18 alkyloxyalkyl, C3-C18 alkenyloxyalkyl, C3-C18 alkynyloxyalkyl, C7-C24 aryloxyalkyl, C2-C18 alkylacyloxy, C2-C18 alkylthioalkyl, C3-C18 alkenylthioalkyl, C3-C18 alkynylthioalkyl, C7-C24 arylthioalkyl, C2-C18 alkylacylthio, C4-C18 alkylcarbocyclylthio, C3-C18 alkylheterocyclylthio, C4-C18 alkylheteroarylthio, C4-C18 alkylalkenylalkyl, C4-C18 alkylalkynylalkyl, C8-C24 alkylarylalkyl, C3-C18 alkylacylalkyl, C13-C24 arylalkylaryl, C14-C24 arylalkenylaryl, C14-C24 arylalkynylaryl, C13-C24 arylacylaryl, C7-C18 arylacyl, C9-C18 arylcarbocyclyl, Cs-Cis arylheterocyclyl, C9-C18 arylheteroaryl, Cs-Cis alkenyloxyaryl, Cs-Cis alkynyloxyaryl, C12-C24 aryloxyaryl, alkylthioaryl, Cs-Cis alkenylthioaryl, Cs-Cis alkynylthioaryl, C12-C24 arylthioaryl, C7-C18 arylacylthio, C9-C18 arylcarbocyclylthio, Cs-Cis arylheterocyclylthio, C9-C18 arylheteroarylthio, and a polymer chain having a number average molecular weight in the range of about 500 to about 80,000, for example in the range of about 500 to about 30,000

[0129] Where R in suitable RAFT agents include, and in the case of R* in suitable RAFT agents include an x-valent form of, an optionally substituted polymer chain, the polymers chain may be formed by any suitable polymerisation process such as radical, ionic, coordination, step-growth or condensation polymerisation. The polymer chains may comprise homopolymer, block polymer, multiblock polymer, gradient copolymer, or random or statistical copolymer chains.

[0130] Examples of Z in suitable RAFT agents include optionally substituted, and in the case of Z* in suitable RAFT agents include a y-valent form of optionally substituted: F, Cl, Br, I, alkyl, aryl, acyl, amino, carbocyclyl, heterocyclyl, heteroaryl, alkyloxy, aryloxy, acyloxy, acylamino, carbocyclyloxy, heterocyclyloxy, heteroaryloxy, alkylthio, arylthio, acylthio, carbocyclylthio, heterocyclylthio, heteroarylthio, alkylaryl, alkylacyl, alkylcarbocyclyl, alkylheterocyclyl, alkylheteroaryl, alkyloxyalkyl, aryloxyalkyl, alkylacyloxy, alkylcarbocyclyloxy, alkylheterocyclyloxy, alkylheteroaryloxy, alkylthioalkyl, arylthioalkyl, alkylacylthio, alkylcarbocyclylthio, alkylheterocyclylthio, alkylheteroarylthio, alkylarylalkyl, alkylacylalkyl, arylalkylaryl, arylacylaryl, arylacyl, arylcarbocyclyl, arylheterocyclyl, arylheteroaryl, aryloxyaryl, arylacyloxy, arylcarbocyclyloxy, arylheterocyclyloxy, arylheteroaryloxy, alkylthioaryl, arylthioaryl, arylacylthio, arylcarbocyclylthio, arylheterocyclylthio, arylheteroarylthio, dialkyloxy- , diheterocyclyloxy- or diaryloxy- phosphinyl, dialkyl-, diheterocyclyl- or diaryl- phosphinyl, cyano (i.e. -CN), and -S-R, where R is as defined in respect of formula (III). More specific examples of Z in suitable RAFT agents include optionally substituted, and in the case of Z* in suitable RAFT agents include a y-valent form of optionally substituted: F, Cl, Ci- Ci8 alkyl, Ce-Cig aryl, Ci-Cis acyl, amino, C3-C18 carbocyclyl, C2-C18 heterocyclyl, C3-C18 heteroaryl, Ci-Cis alkyloxy, Ce-Cis aryloxy, Ci-Cis acyloxy, C3-C18 carbocyclyloxy, C2-C18 heterocyclyloxy, C3-C18 heteroaryloxy, Ci-Cis alkylthio, GrC’is arylthio, Ci-Cis acylthio, C3- Cis carbocyclylthio, C2-C18 heterocyclylthio, C3-C18 heteroarylthio, C7-C24 alkylaryl, C2-C18 alkylacyl, C4-C18 alkylcarbocyclyl, C3-C18 alkylheterocyclyl, C4-C18 alkylheteroaryl, C2-C18 alkyloxyalkyl, C7-C24 aryloxyalkyl, C2-C18 alkylacyloxy, C4-C18 alkylcarbocyclyloxy, C3-C18 alkylheterocyclyloxy, C4-C18 alkylheteroaryloxy, C2-C18 alkylthioalkyl, C7-C24 arylthioalkyl, C2-C18 alkylacylthio, C4-C18 alkylcarbocyclylthio, C3-C18 alkylheterocyclylthio, C4-C18 alkylheteroarylthio, C8-C24 alkylarylalkyl, C3-C18 alkylacylalkyl, C13-C24 arylalkylaryl, C13-C24 arylacylaryl, C7-C18 arylacyl, C9-C18 arylcarbocyclyl, Cs-Cis arylheterocyclyl, C9-C18 arylheteroaryl, C12-C24 aryloxyaryl, C7-C18 arylacyloxy, C9-C18 arylcarbocyclyloxy, Cs-Cis arylheterocyclyloxy, C9-C18 arylheteroaryloxy, C7-C18 alkylthioaryl, C12-C24 arylthioaryl, C7-C18 arylacylthio, C9-C18 arylcarbocyclylthio, Cs-Cis arylheterocyclylthio, C9-C18 arylheteroarylthio, dialkyloxy- , diheterocyclyloxy- or diaryloxy- phosphinyl (i.e. -P(=O)ORk2), dialkyl-, diheterocyclyl- or diaryl- phosphinyl (i.e. -P(=O)Rk2), where Rkis selected from optionally substituted Ci-Cis alkyl, optionally substituted Cs-Cis aryl, optionally substituted C2-C18 heterocyclyl, and optionally substituted C7-C24 alkylaryl, cyano (i.e. -CN), and -S-R, where R is as defined in respect of formula (III).

[0131] If desired, residues from a polymerisation agent used to make the block copolymer may be removed. For example, if RAFT polymerisation is used, where appropriate the RAFT agent residues may be removed from the block copolymer. Techniques for removing such agent residues are known in the art.

[0132] In the lists herein defining groups from which Z, Z*, R and R* may be selected, each alkyl, alkenyl, alkynyl, aryl, carbocyclyl, heteroaryl, heterocyclyl, and polymer chain moiety may be optionally substituted. For avoidance of any doubt, where a given Z, Z*, R or R* contains two or more of such moieties (e.g. alkylaryl), each of such moieties may be optionally substituted with one, two, three or more optional substituents as herein defined.

[0133] In the lists herein defining groups from which Z, Z*, R and R* may be selected, where a given

[0134] Z, Z*, R or R* contains two or more subgroups (e.g. [group A][group B]), the order of the subgroups is not intended to be limited to the order in which they are presented. Thus, a Z. Z*, R or R* with two subgroups defined as [group A] [group B] (e.g. alkylaryl) is intended to also be a reference to a Z, Z*, R or R* with two subgroups defined as [group B] [group A] (e.g. arylalkyl).

[0135] The Z, Z*, R or R* may be branched and / or optionally substituted. Where the Z, Z*, R or R* comprises an optionally substituted alkyl moiety, an optional substituent includes where a -CH2- group in the alkyl chain is replaced by a group selected from -O-, -S-, -NRa-, -C(O)- (i.e. carbonyl), -C(O)O- (i.e. ester), and -C(O)NRa- (i.e. amide), where Ramay be selected from hydrogen, alkyl, alkenyl, alkynyl, aryl, carbocyclyl, heteroaryl, heterocyclyl, arylalkyl, and acyl.

[0136] Reference herein to a x-valent, y-valent, multi-valent or di -valent "form of. ..." is intended to mean that the specified group is a x-valent, y-valent, multi-valent or di-valent radical, respectively. For example, where x or y is 2, the specified group is intended to be a divalent radical. In that case, a divalent alkyl group is in effect an alkylene group (e.g. -CH2-).

[0137] Similarly, the divalent form of the group alkylaryl may, for example, be represented by -(CeFU)- CH2-, a divalent alkylarylalkyl group may, for example, be represented by -CH2-(C6H4)-CH2-, a divalent alkyloxy group may, for example, be represented by -CH2-O-, and a divalent alkyloxyalkyl group may, for example, be represented by -CH2-O-CH2-. Where the term "optionally substituted" is used in combination with such a x-valent, y-valent, multi-valent or divalent groups, that group may or may not be substituted or fused as herein described. Where the x-valent, y-valent, multi-valent, di-valent groups comprise two or more subgroups, for example [group A] [group B] [group C] (e.g. alkylarylalkyl), if viable one or more of such subgroups may be optionally substituted. Those skilled in the art will appreciate how to apply this rationale in providing for higher valent forms.

[0138] Examples of specific RAFT agents that may be used in preparing the block copolymers include, but are not limited to, those agents represented by the following general formula (IV) to (VIII): where R3is selected from Ci to C20 alkyl.

[0139] Preparation of the block copolymer will generally involve the polymerisation of ethylenically unsaturated monomers. Factors that determine copolymerisability of ethylenically unsaturated monomers are well documented in the art. For example, see: Greenlee, R. Z., in Polymer Handbook 3rdedition (Brandup, J, and Immergut. E. H. Eds) Wiley: New York, 1989, p 11 / 53 (the entire contents of which are incorporated herein by reference). Examples of suitable ethylenically unsaturated monomers that may be used to prepare the block copolymers include those of general formula (I) described herein.

[0140] Those skilled in the art will be able to select suitable monomers to provide for the hydrophilic polymer block and the hydrophobic polymer block.

[0141] Those skilled in the art will also appreciate that the terms "hydrophilic" and "hydrophobic" used herein are not intended to define absolute qualities of a particular substance but rather to be an indicator of a favourable or unfavourable interactions (e.g. attractive or repulsive interactions) with water. In other words, the terms "hydrophilic" and "hydrophobic" are used herein as primary indicators to define characteristics such as like attracting like and unlike repelling unlike.

[0142] As a convenient point of reference, those skilled in the art commonly refer to Hansch parameters for evaluating the hydrophobicity of monomers and polymers derived therefrom. Details concerning the calculation of Hansch parameters may be found in Hansch, Fujita, J. American Chemical Society, 1964, 86, pages 1616-1626; H. Kubinyi, methods and principles of medicinal chemistry, volume 1, R. Mannhold et al., PublisherVCH, Weinheim (1993); C. Hansch and A. Leo, substituent constants for correlation analysis, in chemistry and biology, Wiley, New York (1979); and C. Hansch, P. Maloney, T. Fujita and R. Muir Nature, 1962, 194, pages 178-180.

[0143] In the context of Hansch parameters and the present invention, a hydrophilic monomer or polymer derived therefrom will have a Hansch parameter of less than or equal to 1.4 and a hydrophobic monomer or polymer derived therefrom will have a Hansch parameter of greater than 1.4.

[0144] Examples of hydrophobic ethylenically unsaturated monomers that may be polymerised to form the hydrophobic polymer block include, but are not limited to, styrene, alpha-methyl styrene, butyl acrylate, butyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, amyl methacrylate, hexyl methacrylate, lauryl methacrylate, stearyl methacrylate, ethyl hexyl methacrylate, crotyl methacrylate, cinnamyl methacrylate, oleyl methacrylate, ricinoleyl methacrylate, vinyl butyrate, vinyl tert-butyrate, vinyl stearate and vinyl laurate.

[0145] Examples of hydrophilic ethylenically unsaturated monomers that may be polymerised to form the hydrophilic polymer block include, but are not limited to, acrylic acid, methacrylic acid, hydroxyethyl methacrylate, hydroxypropyl methacrylate, acrylamide and methacrylamide, hydroxyethyl acrylate, N-methylacrylamide, dimethylaminoethyl methacrylate, 4- styrene sulfonic acid and phosphoethyl methacrylate.

[0146] Provided the hydrophobic polymer block is overall hydrophobic in character, it may contain one or more polymerised residues of hydrophilic monomer. Equally, provided the hydrophilic polymer block is overall hydrophilic in character, it may contain one or more polymerised residues of hydrophobic monomer.

[0147] The block copolymer that provides for the polymer fibre may also be provided with crosslinkable functionality. Such crosslinkable functionality of the block copolymer may promote formation of a crosslinked structure within the polymer fibre itself and / or between the polymer fibre and the polymer binder.

[0148] The block copolymer may be prepared using crosslinking monomers.

[0149] In one embodiment, the block copolymer comprises polymerised residues of one or more crosslinking monomers.

[0150] Where the block copolymer comprises polymerised residues of one or more crosslinking monomers, those polymerised residues may be present in one or both of the hydrophilic and hydrophobic polymer blocks.

[0151] Polymer fibre formed from block copolymer comprising polymerised residues of one or more crosslinking monomers may herein be conveniently referred to as a crosslinkable polymer fibre.

[0152] Those skilled in the art will appreciate that such crosslinkable polymer fibres may be prepared using various types of crosslinking monomers. For example, the block copolymer may be prepared using one or more of the crosslinking monomers herein described in the context of preparing the polymer binder.

[0153] To facilitate crosslinking between the polymer binder and the polymer fibre, both the block copolymer and the polymer fibre may be prepared using one or more crosslinking monomers.

[0154] A block copolymer used for preparing the polymer fibres used in accordance with the invention will generally have a weight average molecular weight (Mw) ranging from about 500 to about 1,000,000, or from about 5,000 to about 200,000.

[0155] The molecular weight of (and correspondingly the number of polymerised monomer residue repeat units that make up) the respective hydrophilic and hydrophobic polymer blocks that form the block copolymer will vary depending upon the type of monomers used. Those skilled in the art can readily select not only the type of monomers to use but also the molecular weight / number of repeat units of the respective hydrophilic and hydrophobic polymer blocks so as to produce a block copolymer that self assembles to afford the required polymer fibre morphology.

[0156] As a guide only, a hydrophilic polymer block of the block copolymer used in accordance with the invention will generally comprise 5 to about 1,000, or about 20 to about 200 polymerised monomer repeat units.

[0157] As a guide only, a hydrophobic polymer block of the block copolymer used in accordance with the invention will generally comprise about 50 to about 10,000, or about 100 to about 500 polymerised monomer repeat units.

[0158] The block copolymer and may be prepared in a single polymerisation reaction or multiple polymerisation reactions.

[0159] One or more surfactants may be used to assist with preparation of the block copolymer and / or formation of the polymer fibre. A surfactant can assist with improving colloidal stability as the polymer fibre forms and also control over the resulting fibre morphology.

[0160] Where a free radical polymerisation technique is to be used in polymerising one or more ethylenically unsaturated monomers so as to form a block copolymer or polymer binder used in accordance with the invention, the polymerisation will usually require initiation from a source of free radicals.

[0161] A source of initiating radicals can be provided by any suitable means of generating free radicals, such as the thermally induced homolytic scission of suitable compound(s) (thermal initiators such as peroxides, peroxyesters, or azo compounds), the spontaneous generation from monomers (e.g. styrene), redox initiating systems, photochemical initiating systems or high energy radiation such as electron beam, X-ray or gamma-radiation.

[0162] Thermal initiators are generally chosen to have an appropriate half-life at the temperature of polymerisation. These initiators can include one or more of the following compounds:

[0163] 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-cyanobutane), dimethyl 2,2'- azobis(isobutyrate), 4,4'-azobis(4-cyanovaleric acid), 1,1'- azobis(cyclohexanecarbonitrile), 2-(t-butylazo)-2-cyanopropane, 2,2'-azobis{2-methyl- N-[ 1 , 1 -bis(hydroxymethyl)-2-hydroxyethyl]propionamide} , 2,2'-azobis[2-methyl-N-(2- hydroxyethyl)propionamide], 2,2'-azobis(N,N'-dimethyleneisobutyramidine) dihydrochloride, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis(N,N'- dimethyleneisobutyramidine), 2,2'-azobis {2-methyl-N-[ 1 , 1 -bis(hydroxymethyl)-2- hydroxyethyl]propionamide }, 2,2'-azobis {2-methyl-N-[ 1 , 1 -bis(hydroxymethyl)-2- ethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'- azobis(isobutyramide) dihydrate, 2,2'-azobis(2,2,4-trimethylpentane), 2,2'-azobis(2- methylpropane), t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butyl peroxyneodecanoate, t-butylperoxy isobutyrate, t-amyl peroxypivalate, t-butyl peroxypivalate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, dicumyl peroxide, dibenzoyl peroxide, dilauroyl peroxide, potassium peroxydisulfate, ammonium peroxydisulfate, di-t-butyl hyponitrite, dicumyl hyponitrite. This list is not exhaustive.

[0164] Photochemical initiator systems are generally chosen to have an appropriate quantum yield for radical production under the conditions of the polymerisation. Examples include benzoin derivatives, benzophenone, acyl phosphine oxides, and photo-redox systems.

[0165] Redox initiator systems are generally chosen to have an appropriate rate of radical production under the conditions of the polymerisation; these initiating systems can include, but are not limited to, combinations of the following oxidants and reductants: oxidants: potassium, peroxydisulfate, hydrogen peroxide, t-butyl hydroperoxide. reductants: iron (II), titanium (III), potassium thiosulfite, potassium bisulfite.

[0166] Other suitable initiating systems are described in commonly available texts. See, for example, Moad and Solomon "The Chemistry of Free Radical Polymerisation", Pergamon, London, 1995, pp 53-95.

[0167] Initiators that are more readily solvated in hydrophilic media include, but are not limited to, 4,4- azobis(cyanovaleric acid), 2,2'-azobis{2-methyl-N-[l, l-bis(hydroxymethyl)-2- hydroxyethyl] propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'- azobis(N,N'-dimethyleneisobutyramidine), 2,2'-azobis(N,N'-dimethyleneisobutyramidine) dihydrochloride, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis{2-methyl-N-[l,l- bis(hydroxymethyl)-2-ethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2- hydroxyethyl)propionamide], 2,2'-azobis(isobutyramide) dihydrate, and derivatives thereof.

[0168] Initiators that are more readily solvated in hydrophobic media include azo compounds exemplified by the well-known material 2,2'-azobisisobutyronitrile. Other suitable initiator compounds include the acyl peroxide class such as acetyl and benzoyl peroxide as well as alkyl peroxides such as cumyl and t-butyl peroxides. Hydroperoxides such as t-butyl and cumyl hydroperoxides are also widely used.

[0169] The aqueous coating compositions in accordance with the invention may also comprise other conventional additives used in such compositions including, but not limited to, thickeners, antifungal agents, UV absorbers extenders, co-solvents, coalescents, etc. Such additives will be used in amounts well-known to those skilled in the art.

[0170] The present invention also provides a method of producing an aqueous coating composition. The method comprises blending together the polymer binder, opacifier particles and polymer fibres described herein.

[0171] Conventional techniques and equipment can advantageously be used in blending together the constituent components of the aqueous coating composition.

[0172] For example, the polymer fibres may be combined with the opacifying particles (which are in dry or dispersed form), the combination of which is then mixed with the polymer binder. Alternatively, the polymer binder and opacifying particles may be combined and then subsequently mixed with the polymer fibres. A preference is that the polymer fibres are added as the final formulation component. Incorporation of the polymer fibres may be effected through the use of a disperser blade (also known as a Cowles blade) or a general mixing blade.

[0173] The aqueous coating compositions in accordance with the invention may also comprise one or more other constituent components (additives) commonly used in the art. When present, such other additives may be introduced at an appropriate time during formulation using conventional techniques known to those skilled in the art. Those skilled in the art will be well familiar with the nature of such additives. Examples include, but are not limited to, thickeners, extenders, matting agents, rheology modifiers, wet edge extenders, bases, dispersants, opaque polymers, coalescing agents, antimicrobial agents, UV absorbers, and tinting agents.

[0174] In one embodiment, the coating composition further comprises one or more additives selected from thickeners, pigments, extenders, matting agents, rheology modifiers, wet edge extenders, bases, dispersants, opaque polymers, coalescing agents, antimicrobial agents, UV absorbers, and tinting agents.

[0175] The amount of additives used in the aqueous coating compositions are well known to those skilled in the art.

[0176] For example, the amount of pigment and extender used, commonly expressed in terms of the pigment volume concentration (PVC), will generally range in an amount from about 0% to about 80%.

[0177] As known to those skilled in the art, the PVC may be determined according to the following equation:

[0178] Volume of pigment and extender (if present) Dry volume of the coating composition

[0179] Furthermore, the volume of opacifying pigment present, such as titanium dioxide (TiCF). may be expressed as fPVC TiCh and will generally range from 0% to about 30%, or from about 10% to about 30%.

[0180] The value of fPVC TiCh can be calculated according to the following equation:

[0181] Volume of Ti02 (if present) fPVC TiO2 = - - - — - — - -

[0182] Dry volume of the coating composition

[0183] The present invention also provides a method for increasing opacity of an aqueous coating composition comprising polymer binder and opacifier particles, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles, the method comprising including in the composition polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, the increased opacity being relative to the composition absent the polymer fibres.

[0184] As used herein, the term "alkyl", used either alone or in compound words denotes straight chain, branched or cyclic alkyl, for example C1-20 alkyl, e.g. C1-10 or C1-6. Examples of straight chain and branched alkyl include methyl, ethyl, w-propyl. isopropyl, w-butyl. scc-butyl. / -butyl, n- pentyl, 1,2-dimethylpropyl, 1,1-dimethyl-propyl, hexyl, 4-methylpentyl, 1 -methylpentyl, 2- methylpentyl, 3 -methylpentyl, 1,1-dimethylbutyl, 2,2-dimethylbutyl, 3, 3 -dimethylbutyl, 1,2- dimethylbutyl, 1,3 -dimethylbutyl, 1,2,2-trimethylpropyl, 1,1,2-trimethylpropyl, heptyl, 5- methylhexyl, 1 -methylhexyl, 2,2-dimethylpentyl, 3,3-dimethylpentyl, 4,4-dimethylpentyl, 1,2- dimethylpentyl, 1,3-dimethylpentyl, 1,4-dimethyl -pentyl, 1,2, 3 -trimethylbutyl, 1,1,2- trimethylbutyl, 1,1,3-trimethylbutyl, octyl, 6-methylheptyl, 1 -methylheptyl, 1, 1,3,3- tetramethylbutyl, nonyl, 1-, 2-, 3-, 4-, 5-, 6- or 7-methyloctyl, 1-, 2-, 3-, 4- or 5 -ethylheptyl, 1-, 2- or 3 -propylhexyl, decyl, 1-, 2-, 3-, 4-, 5-, 6-, 7- and 8 -methylnonyl, 1-, 2-, 3-, 4-, 5- or 6- ethyloctyl, 1-, 2-, 3- or 4-propylheptyl, undecyl, 1-, 2-, 3-, 4-, 5-, 6-, 7-, 8- or 9-methyldecyl, 1-, 2-, 3-, 4-, 5-, 6- or 7-ethylnonyl, 1-, 2-, 3-, 4- or 5 -propyloctyl, 1-, 2- or 3 -butylheptyl, 1- pentylhexyl, dodecyl, 1-, 2-, 3-, 4-, 5-, 6-, 7-, 8-, 9- or 10-methylundecyl, 1-, 2-, 3-, 4-, 5-, 6-, 7- or 8-ethyldecyl, 1-, 2-, 3-, 4-, 5- or 6-propylnonyl, 1-, 2-, 3- or 4-butyloctyl, 1-2 -pentylheptyl and the like. Examples of cyclic alkyl include mono- or polycyclic alkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl and the like. Where an alkyl group is referred to generally as "propyl", butyl" etc, it will be understood that this can refer to any of straight, branched and cyclic isomers where appropriate. An alkyl group may be optionally substituted by one or more optional substituents as herein defined.

[0185] The term "alkenyl" as used herein denotes groups formed from straight chain, branched or cyclic hydrocarbon residues containing at least one carbon to carbon double bond including ethylenically mono-, di- or polyunsaturated alkyl or cycloalkyl groups as previously defined, for example C2-20 alkenyl (e.g. C2-10 or C2-6). Examples of alkenyl include vinyl, allyl, 1- methylvinyl, butenyl, iso-butenyl, 3-methyl-2-butenyl, 1-pentenyl, cyclopentenyl, 1-methyl- cyclopentenyl, 1-hexenyl, 3-hexenyl, cyclohexenyl, 1-heptenyl, 3-heptenyl, 1-octenyl, cyclooctenyl, 1-nonenyl, 2-nonenyl, 3-nonenyl, 1-decenyl, 3-decenyl, 1,3-butadienyl, 1,4- pentadienyl, 1,3-cyclopentadienyl, 1,3-hexadienyl, 1,4-hexadienyl, 1,3-cyclohexadienyl, 1,4- cyclohexadienyl, 1,3 -cycloheptadienyl, 1,3, 5 -cycloheptatrienyl and 1,3,5,7-cyclooctatetraenyl. An alkenyl group may be optionally substituted by one or more optional substituents as herein defined.

[0186] As used herein the term "alkynyl" denotes groups formed from straight chain, branched or cyclic hydrocarbon residues containing at least one carbon-carbon triple bond including ethylenically mono-, di- or polyunsaturated alkyl or cycloalkyl groups as previously defined. Unless the number of carbon atoms is specified the term preferably refers to C2-20 alkynyl (e.g. C2-10 or C2-6). Examples include ethynyl, 1-propynyl, 2-propynyl, and butynyl isomers, and pentynyl isomers. An alkynyl group may be optionally substituted by one or more optional substituents as herein defined.

[0187] The term "halogen" ("halo") denotes fluorine, chlorine, bromine or iodine (fluoro, chloro, bromo or iodo). Preferred halogens are chlorine, bromine or iodine.

[0188] The term "aryl" (or "carboaryl)" denotes any of single, polynuclear, conjugated and fused residues of aromatic hydrocarbon ring systems (e.g. Ce-is aryl). Examples of aryl include phenyl, biphenyl, terphenyl, quaterphenyl, naphthyl, tetrahydronaphthyl, anthracenyl, dihydroanthracenyl, benzanthracenyl, dibenzanthracenyl, phenanthrenyl, fluorenyl, pyrenyl, idenyl, azulenyl, chrysenyl. Preferred aryl include phenyl and naphthyl. An aryl group may or may not be optionally substituted by one or more optional substituents as herein defined. The term "arylene" is intended to denote the divalent form of aryl.

[0189] The term "carbocyclyl" includes any of non-aromatic monocyclic, polycyclic, fused or conjugated hydrocarbon residues, for example C3-20 (e.g. C3-10 or C3-8). The rings may be saturated, e.g. cycloalkyl, or may possess one or more double bonds (cycloalkenyl) and / or one or more triple bonds (cycloalkynyl). Particularly preferred carbocyclyl moieties are 5-6- membered or 9-10 membered ring systems. Suitable examples include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, cyclopentenyl, cyclohexenyl, cyclooctenyl, cyclopentadienyl, cyclohexadienyl, cyclooctatetraenyl, indanyl, decalinyl and indenyl. A carbocyclyl group may be optionally substituted by one or more optional substituents as herein defined. The term "carbocyclylene" is intended to denote the divalent form of carbocyclyl.

[0190] The term "heterocyclyl" when used alone or in compound words includes any of monocyclic, polycyclic, fused or conjugated hydrocarbon residues, for example C3-20 (e.g. C3-10 or C3-8) wherein one or more carbon atoms are replaced by a heteroatom so as to provide a non-aromatic residue. Suitable heteroatoms include O, N, S, P and Se, particularly O, N and S. Where two or more carbon atoms are replaced, this may be by two or more of the same heteroatom or by different heteroatoms. The heterocyclyl group may be saturated or partially unsaturated, i.e. possess one or more double bonds. Particularly preferred heterocyclyl are 5-6 and 9-10 membered heterocyclyl. Suitable examples of heterocyclyl groups may include azridinyl, oxiranyl, thiiranyl, azetidinyl, oxetanyl, thietanyl, 2H-pyrrolyl, pyrrolidinyl, pyrrolinyl, piperidyl, piperazinyl, morpholinyl, indolinyl, imidazolidinyl, imidazolinyl, pyrazolidinyl, thiomorpholinyl, dioxanyl, tetrahydrofuranyl, tetrahydropyranyl, tetrahydropyrrolyl, tetrahydrothiophenyl, pyrazolinyl, dioxalanyl, thiazolidinyl, isoxazolidinyl, dihydropyranyl, oxazinyl, thiazinyl, thiomorpholinyl, oxathianyl, dithianyl, trioxanyl, thiadiazinyl, dithiazinyl, trithianyl, azepinyl, oxepinyl, thiepinyl, indenyl, indanyl, 3H-indolyl, isoindolinyl, 4H- quinolazinyl, chromenyl, chromanyl, isochromanyl, pyranyl and dihydropyranyl. A heterocyclyl group may be optionally substituted by one or more optional substituents as herein defined. The term "heterocyclylene" is intended to denote the divalent form of heterocyclyl.

[0191] The term "heteroaryl" includes any of monocyclic, polycyclic, fused or conjugated hydrocarbon residues, wherein one or more carbon atoms are replaced by a heteroatom so as to provide an aromatic residue. Preferred heteroaryl have 3-20 ring atoms, e.g. 3-10. Particularly preferred heteroaryl are 5-6 and 9-10 membered bicyclic ring systems. Suitable heteroatoms include, O, N, S, P and Se, particularly O, N and S. Where two or more carbon atoms are replaced, this may be by two or more of the same heteroatom or by different heteroatoms. Suitable examples of heteroaryl groups may include pyridyl, pyrrolyl, thienyl, imidazolyl, furanyl, benzothienyl, isobenzothienyl, benzofuranyl, isobenzofuranyl, indolyl, isoindolyl, pyrazolyl, pyrazinyl, pyrimidinyl, pyridazinyl, indolizinyl, quinolyl, isoquinolyl, phthalazinyl, 1,5-naphthyridinyl, quinozalinyl, quinazolinyl, quinolinyl, oxazolyl, thiazolyl, isothiazolyl, isoxazolyl, triazolyl, oxadialzolyl, oxatriazolyl, triazinyl, and furazanyl. A heteroaryl group may be optionally substituted by one or more optional substituents as herein defined. The term "heteroarylene" is intended to denote the divalent form of heteroaryl.

[0192] The term "acyl" either alone or in compound words denotes a group containing the moiety C=O (and not being a carboxylic acid, ester or amide) Preferred acyl includes C(O)-Re, wherein Reis hydrogen or an alkyl, alkenyl, alkynyl, aryl, heteroaryl, carbocyclyl, or heterocyclyl residue. Examples of acyl include formyl, straight chain or branched alkanoyl (e.g. C1-20) such as acetyl, propanoyl, butanoyl, 2-methylpropanoyl, pentanoyl, 2,2-dimethylpropanoyl, hexanoyl, heptanoyl, octanoyl, nonanoyl, decanoyl, undecanoyl, dodecanoyl, tridecanoyl, tetradecanoyl, pentadecanoyl, hexadecanoyl, heptadecanoyl, octadecanoyl, nonadecanoyl and icosanoyl; cycloalkylcarbonyl such as cyclopropylcarbonyl cyclobutylcarbonyl, cyclopentylcarbonyl and cyclohexylcarbonyl; aroyl such as benzoyl, toluoyl and naphthoyl; aralkanoyl such as phenylalkanoyl (e.g. phenylacetyl, phenylpropanoyl, phenylbutanoyl, phenylisobutylyl, phenylpentanoyl and phenylhexanoyl) and naphthylalkanoyl (e.g. naphthylacetyl, naphthylpropanoyl and naphthylbutanoyl]; aralkenoyl such as phenylalkenoyl (e.g. phenylpropenoyl, phenylbutenoyl, phenylmethacryloyl, phenylpentenoyl and phenylhexenoyl and naphthylalkenoyl (e.g. naphthylpropenoyl, naphthylbutenoyl and naphthylpentenoyl); aryloxyalkanoyl such as phenoxyacetyl and phenoxypropionyl; arylthiocarbamoyl such as phenylthiocarbamoyl; arylglyoxyloyl such as phenylglyoxyloyl and naphthylglyoxyloyl; arylsulfonyl such as phenylsulfonyl and napthylsulfonyl; heterocycliccarbonyl; heterocyclicalkanoyl such as thienylacetyl, thienylpropanoyl, thienylbutanoyl, thienylpentanoyl, thienylhexanoyl, thiazolylacetyl, thiadiazolylacetyl and tetrazolylacetyl; heterocyclicalkenoyl such as heterocyclicpropenoyl, heterocyclicbutenoyl, heterocyclicpentenoyl and heterocyclichexenoyl; and heterocyclicglyoxyloyl such as thiazolyglyoxyloyl and thienylglyoxyloyl. The Rxresidue may be optionally substituted as described herein.

[0193] The term "sulfoxide", either alone or in a compound word, refers to a group -S(O)Rfwherein Rfis selected from hydrogen, alkyl, alkenyl, alkynyl, aryl, heteroaryl, heterocyclyl, carbocyclyl, and aralkyl. Examples of preferred Rfinclude Ci-2oalkyl, phenyl and benzyl.

[0194] The term "sulfonyl", either alone or in a compound word, refers to a group S(O)2-Rf, wherein Rfis selected from hydrogen, alkyl, alkenyl, alkynyl, aryl, heteroaryl, heterocyclyl, carbocyclyl and aralkyl. Examples of preferred Rfinclude Ci-2oalkyl, phenyl and benzyl.

[0195] The term "sulfonamide", either alone or in a compound word, refers to a group S(O)NRfRfwherein each Rfis independently selected from hydrogen, alkyl, alkenyl, alkynyl, aryl, heteroaryl, heterocyclyl, carbocyclyl, and aralkyl. Examples of preferred Rfinclude Ci-2oalkyl, phenyl and benzyl. In a preferred embodiment at least one Rfis hydrogen. In another form, both Rfare hydrogen.

[0196] The term, "amino" is used here in its broadest sense as understood in the art and includes groups of the formula NRaRbwherein Raand Rbmay be independently selected from hydrogen, alkyl, alkenyl, alkynyl, aryl, carbocyclyl, heteroaryl, heterocyclyl, arylalkyl, and acyl. Raand Rb, together with the nitrogen to which they are attached, may also form a monocyclic, or polycyclic ring system e.g. a 3-10 membered ring, particularly, 5-6 and 9-10 membered systems. Examples of "amino" include NEE, NHalkyl (e.g. Ci-2oalkyl), NHaryl (e.g. NHphenyl), NHaralkyl (e.g. NHbenzyl), NHacyl (e.g. NHC(0)Ci-2oalkyl, NHC(O)phenyl), Nalkylalkyl (wherein each alkyl, for example C1-20, may be the same or different) and 5 or 6 membered rings, optionally containing one or more same or different heteroatoms (e.g. O, N and S).

[0197] The term "amido" is used here in its broadest sense as understood in the art and includes groups having the formula C(O)NRaRb, wherein Raand Rbare as defined as above. Examples of amido include C(O)NH2, C(O)NHalkyl (e.g. Ci-2oalkyl), C(O)NHaryl (e.g. C(O)NHphenyl), C(O)NHaralkyl (e.g. C(O)NHbenzyl), C(O)NHacyl (e.g. C(0)NHC(0)Ci-2oalkyl, C(O)NHC(O)phenyl), C(O)Nalkylalkyl (wherein each alkyl, for example C 1-20, may be the same or different) and 5 or 6 membered rings, optionally containing one or more same or different heteroatoms (e.g. O, N and S).

[0198] The term "carboxy ester" is used here in its broadest sense as understood in the art and includes groups having the formula CCER8, wherein Rgmay be selected from groups including alkyl, alkenyl, alkynyl, aryl, carbocyclyl, heteroaryl, heterocyclyl, aralkyl, and acyl. Examples of carboxy ester include CCECi^oalkyl, CCfaryl (e.g.. CCEphenyl), CCfaralkyl (e.g. CO2 benzyl).

[0199] In this specification "optionally substituted" is taken to mean that a group may or may not be substituted or fused (so as to form a condensed polycyclic group) with one, two, three or more of organic and inorganic groups, including those selected from: alkyl, alkenyl, alkynyl, carbocyclyl, aryl, heterocyclyl, heteroaryl, acyl, aralkyl, alkaryl, alkheterocyclyl, alkheteroaryl, alkcarbocyclyl, halo, haloalkyl, haloalkenyl, haloalkynyl, haloaryl, halocarbocyclyl, haloheterocyclyl, haloheteroaryl, haloacyl, haloaryalkyl, hydroxy, hydroxyalkyl, hydroxyalkenyl, hydroxyalkynyl, hydroxycarbocyclyl, hydroxyaryl, hydroxyheterocyclyl, hydroxyheteroaryl, hydroxyacyl, hydroxyaralkyl, alkoxyalkyl, alkoxyalkenyl, alkoxyalkynyl, alkoxycarbocyclyl, alkoxyaryl, alkoxyheterocyclyl, alkoxyheteroaryl, alkoxyacyl, alkoxyaralkyl, alkoxy, alkenyloxy, alkynyloxy, aryloxy, carbocyclyloxy, aralkyloxy, heteroaryloxy, heterocyclyloxy, acyloxy, haloalkoxy, haloalkenyloxy, haloalkynyloxy, haloaryloxy, halocarbocyclyloxy, haloaralkyloxy, haloheteroaryloxy, haloheterocyclyloxy, haloacyloxy, nitro, nitroalkyl, nitroalkenyl, nitroalkynyl, nitroaryl, nitroheterocyclyl, nitroheteroayl, nitrocarbocyclyl, nitroacyl, nitroaralkyl, amino (NH2), alkylamino, dialkylamino, alkenylamino, alkynylamino, arylamino, diarylamino, aralkylamino, diaralkylamino, acylamino, diacylamino, heterocyclamino, heteroarylamino, carboxy, carboxyester, amido, alkylsulphonyloxy, arylsulphenyloxy, alkylsulphenyl, arylsulphenyl, thio, alkylthio, alkenylthio, alkynylthio, arylthio, aralkylthio, carbocyclylthio, heterocyclylthio, heteroarylthio, acylthio, sulfoxide, sulfonyl, sulfonamide, aminoalkyl, aminoalkenyl, aminoalkynyl, aminocarbocyclyl, aminoaryl, aminoheterocyclyl, aminoheteroaryl, aminoacyl, aminoaralkyl, thioalkyl, thioalkenyl, thioalkynyl, thiocarbocyclyl, thioaryl, thioheterocyclyl, thioheteroaryl, thioacyl, thioaralkyl, carboxyalkyl, carboxyalkenyl, carboxyalkynyl, carboxycarbocyclyl, carboxyaryl, carboxyheterocyclyl, carboxyheteroaryl, carboxyacyl, carboxyaralkyl, carboxyesteralkyl, carboxyesteralkenyl, carboxyesteralkynyl, carboxyestercarbocyclyl, carboxyesteraryl, carboxyesterheterocyclyl, carboxyesterheteroaryl, carboxyesteracyl, carboxyesteraralkyl, amidoalkyl, amidoalkenyl, amidoalkynyl, amidocarbocyclyl, amidoaryl, amidoheterocyclyl, amidoheteroaryl, amidoacyl, amidoaralkyl, formylalkyl, formylalkenyl, formylalkynyl, formylcarbocyclyl, formylaryl, formylheterocyclyl, formylheteroaryl, formylacyl, formylaralkyl, acylalkyl, acylalkenyl, acylalkynyl, acylcarbocyclyl, acylaryl, acylheterocyclyl, acylheteroaryl, acylacyl, acylaralkyl, sulfoxidealkyl, sulfoxidealkenyl, sulfoxidealkynyl, sulfoxidecarbocyclyl, sulfoxidearyl, sulfoxideheterocyclyl, sulfoxideheteroaryl, sulfoxideacyl, sulfoxidearalkyl, sulfonylalkyl, sulfonylalkenyl, sulfonylalkynyl, sulfonylcarbocyclyl, sulfonylaryl, sulfonylheterocyclyl, sulfonylheteroaryl, sulfonylacyl, sulfonylaralkyl, sulfonamidoalkyl, sulfonamidoalkenyl, sulfonamidoalkynyl, sulfonamidocarbocyclyl, sulfonamidoaryl, sulfonamidoheterocyclyl, sulfonamidoheteroaryl, sulfonamidoacyl, sulfonamidoaralkyl, nitroalkyl, nitroalkenyl, nitroalkynyl, nitrocarbocyclyl, nitroaryl, nitroheterocyclyl, nitroheteroaryl, nitroacyl, nitroaralkyl, cyano, sulfate and phosphate groups. Optional substitution may also be taken to refer to where a -CH2- group in a chain or ring is replaced by a group selected from -O-, -S-, -NRa-, -C(O)- (i.e. carbonyl), -C(O)O- (i.e. ester), and -C(O)NRa- (i.e. amide), where Rais as defined herein.

[0200] Preferred optional substituents include alkyl, (e.g. C1-6 alkyl such as methyl, ethyl, propyl, butyl, cyclopropyl, cyclobutyl, cyclopentyl or cyclohexyl), hydroxyalkyl (e.g. hydroxymethyl, hydroxyethyl, hydroxypropyl), alkoxyalkyl (e.g. methoxymethyl, methoxyethyl, methoxypropyl, ethoxymethyl, ethoxyethyl, ethoxypropyl etc) alkoxy (e.g. C1-6 alkoxy such as methoxy, ethoxy, propoxy, butoxy, cyclopropoxy, cyclobutoxy), halo, trifluoromethyl, trichloromethyl, tribromomethyl, hydroxy, phenyl (which itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyCi-6 alkyl, C1-6 alkoxy, haloCi -ealkyl, cyano, nitro OC(O)C 1-6 alkyl, and amino), benzyl (wherein benzyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyCnsalkyl, C1-6 alkoxy, haloCi-6 alkyl, cyano, nitro OC(O)Ci-6 alkyl, and amino), phenoxy (wherein phenyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyCi-6 alkyl, C1-6 alkoxy, haloC 1-6 alkyl, cyano, nitro OC(O)Ci-6 alkyl, and amino), benzyloxy (wherein benzyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyCi-6 alkyl, Ci-6 alkoxy, haloCi-6 alkyl, cyano, nitro OC(O)Ci-6 alkyl, and amino), amino, alkylamino (e.g. Ci-6 alkyl, such as methylamino, ethylamino, propylamino etc), dialkylamino (e.g. Ci-6 alkyl, such as dimethylamino, diethylamino, dipropylamino), acylamino (e.g. NHC(O)CH3), phenylamino (wherein phenyl itself may be further substituted e.g., by Ci-6 alkyl, halo, hydroxy, hydroxyCi-6 alkyl, Ci-6 alkoxy, haloCi-6 alkyl, cyano, nitro OC(O)Ci-6 alkyl, and amino), nitro, formyl, -C(O)-alkyl (e.g. Ci-6 alkyl, such as acetyl), O-C(O)-alkyl (e.g. Ci-6alkyl, such as acetyloxy), benzoyl (wherein the phenyl group itself may be further substituted e.g., by Ci-6 alkyl, halo, hydroxy hydroxyCi-6 alkyl, Ci-6 alkoxy, haloCi-6 alkyl, cyano, nitro OC(O)Ci-6alkyl, and amino), replacement of CH2 with C=O, CO2H, CCfalkyl (e.g. C1-6 alkyl such as methyl ester, ethyl ester, propyl ester, butyl ester), CChphenyl (wherein phenyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyl C1-6 alkyl, Ci- 6 alkoxy, halo C1-6 alkyl, cyano, nitro OC(O)Ci-6 alkyl, and amino), CONH2, CONHphenyl (wherein phenyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy, hydroxyl C1-6 alkyl, Ci -6 alkoxy, halo C1-6 alkyl, cyano, nitro OC(O)C 1-6 alkyl, and amino), CONHbenzyl (wherein benzyl itself may be further substituted e.g., by C1-6 alkyl, halo, hydroxy hydroxyl C1-6 alkyl, Ci -6 alkoxy, halo C1-6 alkyl, cyano, nitro OC(O)C 1-6 alkyl, and amino), CONHalkyl (e.g. C1-6 alkyl such as methyl ester, ethyl ester, propyl ester, butyl amide) CONHdialkyl (e.g. C1-6 alkyl) aminoalkyl (e.g., HN C1-6 alkyl-, Ci-6alkylHN-Ci-6 alkyl- and (Ci-6 alkyl)2N-Ci-6 alkyl-), thioalkyl (e.g., HS C1-6 alkyl-), carboxyalkyl (e.g., HO2CC1-6 alkyl-), carboxyesteralkyl (e.g., Ci- 6 alkylCfCCi , alkyl-), amidoalkyl (e.g., H2N(O)CCI-6 alkyl-, H(Ci^ alkyl)N(O)CCi-6 alkyl-), formylalkyl (e.g., OHCCusalkyl-), acylalkyl (e.g., Ci-6 alkyl(O)CCi-6 alkyl-), nitroalkyl (e.g., O2NC1-6 alkyl-), sulfoxidealkyl (e.g., R(O)SCI-6 alkyl, such as C1-6 alkyl(O)SCi-6 alkyl-), sulfonylalkyl (e.g., R(O)2SCI-6 alkyl- such as Ci-6 alkyl(O)2SCi-6 alkyl-), sulfonamidoalkyl (e.g.,2HRN(O)SCI-6alkyl, H(Cu alkyl)N(O)SCi-6alkyl-).

[0201] The term "heteroatom" or "hetero" as used herein in its broadest sense refers to any atom other than a carbon atom which may be a member of a cyclic organic group. Particular examples of heteroatoms include nitrogen, oxygen, sulfur, phosphorous, boron, silicon, selenium and tellurium, more particularly nitrogen, oxygen and sulfur.

[0202] For monovalent substituents, terms written as " [groupA] [group B]" refer to group A when linked by a divalent form of group B. For example, "[group A] [alkyl]" refers to a particular group A (such as hydroxy, amino, etc.) when linked by divalent alkyl, i.e. alkylene (e.g. hydroxyethyl is intended to denote HO-CH2-CH-). Thus, terms written as "oxy [group | " refer to a particular group when linked by oxygen, for example, the terms "oxyalkyl", "oxyalkenyl", oxyalkynyl", "oxyaryl" and "oxyacyl", respectively, denote alkyl, alkenyl, alkynyl, aryl and acyl groups as hereinbefore defined when linked by oxygen. Similarly, terms written as "thio[group]" refer to a particular group when linked by sulfur, for example, the terms "thioalkyl", "thioalkenyl", thioalkynyl" and "thioaryl", respectively, denote alkyl, alkenyl, alkynyl and aryl groups as hereinbefore defined when linked by sulfur.

[0203] The following invention will hereinafter be described with reference to the following nonlimiting examples.

[0204] EXAMPLES

[0205] Example 1 : Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n] } macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m « 120, n « 60 and t ~80.

[0206] A solution of dibenzyl trithiocarbonate (diBenT) (1.24 g, 4.2 mmol), 2,2’-azobisisobutyronitrile (AIBN) (0.20 g, 1.2 mmol), acrylic acid (AA) (18.4 g, 255 mmol), butyl acrylate (BA) (65.24 g, 509 mmol) in dioxane (80 g) was prepared in a 500 mL round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. At the end of the heating, styrene (St) (35.4 g, 340 mmol), AIBN (0.2 g, 1.2 mmol) was added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 53.8% solids.

[0207] Example 2: Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in Example 1 as a stabiliser.

[0208] A solution of St (315 g), AIBN (2.52 g) and macro-RAFT solution from Example 1 (105 g) was prepared. To this solution, sodium hydroxide (NaOH) solution (5.39 g NaOH in 126 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. 280 g of water was slowly added while the stirring was maintained to produce a white emulsion. A final 392 g of water was further added to the emulsion under stirring for another 5 minutes. After being deoxygenated for 10 minutes, the mixture was heated at 80°C with a stirring rate of 150 rpm over 1.5 hours. Electron microscopy (TEM) showed that the final product (approximately 1.2 kg) contained 33.3 wt. % solids, about 42 wt. % of which exhibited fibre morphology, and polymer fibres having an average diameter of about 70 nm.

[0209] The diameters of polymer fibres exemplified herein were measured from SEM and TEM micrographs using Image J analysis software. Reported values are the average of 10 measurements, with an uncertainty equal to the standard deviation of the data, both rounded up to the nearest 10 nm

[0210] Example 3: Polymer fibre synthesis with poly(tert-butyl acrylate) core using the macro- RAFT agent prepared in Example 1 as a stabiliser.

[0211] A solution of tert-butyl acrylate (t-BA) (22.5 g), AIBN (0. 18 g) and macro-RAFT solution from Example 1 (8.5 g) was prepared in a 500 mL glass container. To this solution, sodium hydroxide (NaOH) solution (0.43 g NaOH in 9 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. 20 g of water was slowly added into the beaker while the stirring was maintained to produce white emulsion. A final 28 g of water was further added to the emulsion under stirring for another 5 minutes. After being deoxygenated for 10 minutes, the jar was sealed and immersed in an oil bath with a temperature setting of 80°C. The reaction was carried out for 2 hours with magnetic stirring. Electron microscopy (SEM) showed that the final product contained 30.6 wt. % solids and polymer fibres having an average diameter of about 90 nm.

[0212] Example 4: Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n]} macro-RAFT agent with a non-symmetrical trithiocarbonate RAFT agent and monomer molar ratio m « 120, n « 60 and t «80.

[0213] A solution of 2- {[(butylsulfanyl)carbonothioyl] sulfanyl} propanoic acid (BuPAT) (0.51 g, 2.1 mmol), AIBN (0.07 g, 0.4 mmol), AA (9.17 g, 127.3 mmol), n-BA (32.64 g, 254.6 mmol) in dioxane (40 g) was prepared in a 250 mL round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2 hours under constant stirring. At the end of the heating, St (17.70 g, 170 mmol) and AIBN (0.07 g, 0.4 mmol) were added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 40.7% solids. Example 5: Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in example 4 as a stabiliser.

[0214] A solution of St (21.2 g), AIBN (0. 18 g) and macro-RAFT solution from example 4 (8.5 g) was prepared in a 500 mL glass container. To this solution, sodium hydroxide (NaOH) solution (0.4 g NaOH in 9 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. 20 g of water was slowly added into the beaker while the stirring was maintained to produce white emulsion. A final 28 g of water was further added to the emulsion under stirring for another 5 minutes. After being deoxygenated for 10 minutes, the jar was sealed and immersed in an oil bath with a temperature setting of 80°C. The reaction was carried out for 2 hours with magnetic stirring. Electron microscopy (SEM) showed that the final product contained 29.2 wt. % solids, about 55 wt. % of which exhibited fibre morphology, and polymer fibres having an average diameter of about 120 nm.

[0215] Example 6: Preparation of a poly[(butyl acrylate)m-co-(acrylic acid)n] macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m « 120 and n « 60. A solution of dibenzyl trithiocarbonate (diBenT) (0.61 g, 2.1 mmol), AIBN (0.10 g, 0.6 mmol), AA (9.15 g, 126.9 mmol), BA (32.62 g, 255.3 mmol) in dioxane (40 g) was prepared in a 250 mL round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. The final copolymer solution had 51.9% solids.

[0216] Example 7: Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in example 4a as a stabiliser.

[0217] A macro-RAFT solution from example 6 (7 g) was prepared in a 200 mL glass container with 5 g water and ammonium hydroxide (NH4OH) (2.0 g, 25%) under stirring at 1000 rpm using an overhead mixer (Labortechnik, IKA) to produce a yellow mixture. To this mixture, St (20 g), AIBN (0.2 g) and then 40 g of water was sequentially added into while the stirring was maintained at 2000 rpm to produce white emulsion. After being deoxygenated for 5 minutes, the jar was sealed and immersed in an oil bath with a temperature setting of 80°C. The reaction was carried out for 2 hours with magnetic stirring. Electron microscopy (TEM) showed that the final product contained 30.5 wt. % solids, about 74 wt. % of which exhibited fibre morphology, and polymer fibres having an average diameter of about 80 nm. Example 8: Preparation of low sheen white coatings using polymer fibres and measurement of hiding power of the coating relative to conventional paints.

[0218] Titanium dioxide rich intermediates were prepared with high speed dispersion equipment common to the paint development industry according to ingredients listed in Table 1.

[0219] The intermediates were formulated into paints (8a-f) with post adjustment of latex, Texanol, water and polymer fibre (where applicable) to provide low sheen white coatings with PVC of 36-37 and volume solids of 38-40%, with a final coating composition as per Table 1.

[0220] Incorporation of the post adjustment ingredients were conducted with a dispersion blade on a bench stirrer for 20 minutes at 1500 rpm.

[0221] Table 1: Paint formula compositions

[0222] Measurement of the Instrumental Opacity of the prepared coatings: The parameter that was tested was the hiding power of the coating, which is indicative of the opacity of the paints.

[0223] Preparation of the coatings for testing: 1. Coatings were drawn down on pieces of 45 pm polyester film (Melinex), which had been cleaned with ethanol and placed on a glass board with an ethanol seal, using a 175 pm doctor blade.

[0224] 2. The films were allowed to dry, in constant conditions of 25°C and 50% humidity, for 24 hours. Films were then moved to a 50°C oven and left overnight.

[0225] 3. The films were taken out of the oven, and 2 sections cut out of each film in areas free from visible defects, of roughly dimensions 6 cm x 6 cm. The precise area of the testing section was measured.

[0226] Testing the opacity of the film:

[0227] 1. Each testing section was weighed to 0.1 mg. This is the weight of the coating plus the substrate.

[0228] 2. Using a spectrophotometer, the reflectance of the paint against a black and a white tile was measured, ensuring complete contact between the film and the tiles by using a small amount of water between the Melinex and the tile.

[0229] 3. The reflectance of the black and white tiles was also measured.

[0230] 4. The coating was completely removed from the Melinex using acetone. Once dry, the bare Melinex sections were reweighed on the same balance. This is the weight of the bare substrate.

[0231] Testing the NVC of the coatings:

[0232] 1. Aluminium dishes were prepared by placing in a 150°C oven for 30 minutes.

[0233] 2. The aluminium trays were accurately weighed to 0. Img.

[0234] 3. Approximately 0.6 g of coating material was added to the tray and weighed accurately.

[0235] 4. The trays were then placed in a 150°C oven for 1 hour.

[0236] 5. The samples were reweighed.

[0237] 6. Using this information, the NVC was calculated. Calculating the hiding power:

[0238] 1. The wet film thickness is calculated using the following equation:

[0239] Where T=wet film thickness

[0240] U=weight of coating contained on a square

[0241] A=area of square

[0242] 2. The scatter co-efficient is calculated using the following equation:

[0243] Where:

[0244] Where S = scatter co-efficient

[0245] T = wet film thickness

[0246] Rb = reflectance of the film against the black tile

[0247] Rw= reflectance of the film against the white tile

[0248] W = reflectance of white tile

[0249] 3. The Hiding Power (HP) is calculated using the following formula:

[0250] This number is an indication of the opacity of the coating. References:

[0251] “Standard Test Method for Hiding Power of Paints by Reflectometry” ASTM D2805-96a.

[0252] Mitton PB “Opacity, Hiding Power, and Tinting Strength”. In Pigment Handbook, Vol 3, Characterization and Physical relationships, pp 301-303 (1973).

[0253] The dry hiding power values of the coatings (8a-f) were subsequently measured and the results can be found in Table 2 and Figure 1.

[0254] Table 2: Dry hiding power test results

[0255] As the above data indicates, the inventive examples that contain polymer fibres have higher dry opacities than the conventional paints that do not contain polymer fibres.

[0256] Measurement of the Wet Opacity of the prepared coatings:

[0257] The parameter that was tested was the wet hiding power of the coating, which is indicative of the wet opacity of the paints.

[0258] Process for measuring the wet opacity of the coatings using cryptometer:

[0259] 1. Apply a small pool of the material to be tested (approx. 1-2 mb) on the centre of the black and white junction and place the 0.002 top plate on the wet paint.

[0260] 2. Pressing firmly down on its four comers, move the top plate back and forth several times to force out the surplus material and then slowly move it to the right until the black and white junction disappears completely over the entire width of the wedge of material. Record the scale reading from the black scale where the edge of the top plate makes contact with the base plate.

[0261] 3. Repeat steps 1 and 2 twice, thus obtaining three readings in each direction. The wet hiding power values of the coatings (8a-f) were subsequently measured and the results can be found in Table 3 and Figure 2.

[0262] Table 3: Wet hiding power test results

[0263] As the above data indicates, the inventive examples that contain polymer fibres have higher wet opacities than the conventional paints that do not contain polymer fibres.

[0264] Example 9: High nanofibre content example

[0265] Example 9 (a): Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n]} macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m re 60, n re 120 and t «80.

[0266] A solution of dibenzyl trithiocarbonate (diBenT) (1.40 g, 4.8 mmol), 2,2’-azobisisobutyronitrile (AIBN) (0.20 g, 1.2 mmol), acrylic acid (AA) (41.60 g, 577 mmol), butyl acrylate (BA) (36.97 g, 288 mmol) in dioxane (80 g) was prepared in a 500 mb round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. At the end of the heating, styrene (St) (40.05 g, 385 mmol), AIBN (0.2 g, 1.2 mmol) was added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 51.8% solids.

[0267] Example 9 (b): Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in Example 9 (a) as a stabiliser.

[0268] Macro-RAFT solution (96 g) from example 9 (a) was added in a base solution containing 500 g water and 12.9 g NaOH under stirring. The yellow dispersion was then transferred to the 2 L reactor with an additional 64 g water. While under stirring, a monomer solution containing Styrene (264 g) and AIBN (2.16 g) was added to the reactor and was emulsified for 10 minutes. After being deoxygenated for 10 minutes, the mixture was heated at 80°C with a stirring rate of 150 rpm over 2 hours. The final product (approximately 1.0 kg) contained 36.6 wt. % solids. The fractionation method by centrifugation was used to estimate nanofibre content. The sample (2 g) was dispersed in water (38 g) by an overhead mixer. The diluted sample was centrifuged at 14 thousand rpm for 60 minutes to mostly separate nanofibres from the dispersion. The solids of the dispersion before and after centrifugation was determined by gravimetry. The two solid contents were used to calculate the nanofibre content of 95 wt. % in the final sample. By SEM, the fibres had an average diameter of about 80 nm and length of about 7 microns (Figure 3).

[0269] Example 9 (c): Crosslinked nanofibres with divinyl benzene (DVB).

[0270] Nanofibres from example 9 (b) (10 g) was dispersed in water (90 g). A solution containing 0.02 g DVB, 0.01 g AIBN and 1 g ethanol was added to the nanofibre dispersion and thoroughly mixed by a mechanical stirring. After being deoxygenated for 5 minutes, the mixture was heated 80°C for over 2 hours. The final product was found to contain nanofibres by SEM and had solids of 3.5%.

[0271] Example 10: nanofibres from macro-RAFT containing sulfoethyl methacrylate (SEM) Example 10 (a): Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n-co-(sulfoethyl methacrylate)o] } macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m « 60, n « 120, o~ 5 and t «80.

[0272] A solution of dibenzyl trithiocarbonate (diBenT) (0.67 g, 2.3 mmol), 2,2’-azobisisobutyronitrile (AIBN) (0.10 g, 0.6 mmol), acrylic acid (AA) (20.00 g, 277 mmol), butyl acrylate (BA) (17.8 g, 139 mmol) and sulfoethyl methacrylate (SEM) (2.00 g, 10 mmol) in dioxane (60 g) was prepared in a 500 mL round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. At the end of the heating, styrene (St) (19.15 g, 184 mmol), AIBN (0. 1 g, 0.6 mmol) was added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 47.3% solids.

[0273] Example 10 (b): Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in Example 10 (a) as a stabiliser.

[0274] A solution of St (44 g), AIBN (0.36 g) and macro-RAFT solution from Example 10 (a) (15 g) was prepared. To this solution, sodium hydroxide (NaOH) solution (1.44 g NaOH in 94 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. After being deoxygenated for 10 minutes, the mixture was heated at 80°C for over 2 hours. The final product contained 35 wt. % solids. By fractionation method (as in example 9 (b)), the sample was found to contain 87 wt. % nanofibres with an average diameter of about 100 nm and an average length of 1 micron.

[0275] Example 11: Nanofibres (~250K g / mole) from high molecular weight macro-RAFT agent (~ 40K g / mole) in the presence of sodium dodecyl sulphate (SDS)

[0276] Example 11 (a): Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n]} macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m « 240, n « 120 and t «160.

[0277] A solution of dibenzyl trithiocarbonate (diBenT) (0.62 g, 2.1 mmol), 2,2’-azobisisobutyronitrile (AIBN) (0.10 g, 0.6 mmol), acrylic acid (AA) (18.40 g, 255 mmol), butyl acrylate (BA) (65.50 g, 511 mmol) in dioxane (80 g) was prepared in a 500 mb round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. At the end of the heating, styrene (St) (35.50 g, 341 mmol), AIBN (0.1 g, 0.6 mmol) was added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 47.9% solids.

[0278] Example 11 (b): Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in Example 11 (a) as a stabiliser and SDS as a co-stabilizer.

[0279] A solution of St (45 g), AIBN (0.36 g) and macro-RAFT solution from Example 11 (a) (19 g) was prepared. To this solution, sodium hydroxide (NaOH) solution (0.98 g NaOH in 18 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. 40 g of water was slowly added while the stirring was maintained to produce a white emulsion. A final 36 g of water and 0.48 g SDS was further added to the emulsion under stirring for another 5 minutes. After being deoxygenated for 10 minutes, the mixture was heated at 80°C for 3 hours. The final product had 38 wt. % solids with fibres having an average diameter of about 100 nm and length of 4 microns. By fractionation method (as in example 9 (b)), the sample was found to contain 60 wt. % nanofibres. Example 12: Nanofibres (~66K g / mole) from low molecular weight macro-RAFT agent (~ 14K g / mole)

[0280] Example 12 (a): Preparation of a poly{(styrene)t -block- [(butyl acrylate)m-co-(acrylic acid)n]} macro-RAFT agent with dibenzyl trithiocarbonate RAFT agent and monomer molar ratio m « 60, n ® 30 and t « 40.

[0281] A solution of dibenzyl trithiocarbonate (diBenT) (2.44 g, 8.4 mmol), 2,2’-azobisisobutyronitrile (AIBN) (0.28 g, 1.7 mmol), acrylic acid (AA) (18.15 g, 252 mmol), butyl acrylate (BA) (64.50 g, 503 mmol) in dioxane (80 g) was prepared in a 500 mL round bottom flask. After being sealed and sparged with nitrogen for 10 minutes, the flask was heated at 70°C for 2.5 hours under constant stirring. At the end of the heating, styrene (St) (34.94 g, 335 mmol), AIBN (0.28 g, 1.7 mmol) was added to the copolymer solution. The flask was sealed, deoxygenated with nitrogen for 10 minutes and then maintained at 70°C for another 12 hours under constant stirring. The final copolymer solution had 53.5% solids.

[0282] Example 12 (b): Polymer fibre synthesis with polystyrene core using the macro-RAFT agent prepared in Example 12 (a) as a stabiliser.

[0283] A solution of St (45 g), AIBN (0.36 g) and macro-RAFT solution from Example 12 (a) (20 g) was prepared. To this solution, sodium hydroxide (NaOH) solution (1.0 g NaOH in 18 g water) was added in drop wise while the solution was stirred at 1500 rpm using an overhead mixer (Labortechnik, IKA) to produce a viscous white mixture. 76 g of water was slowly added while the stirring was maintained to produce a white emulsion. After being deoxygenated for 10 minutes, the mixture was heated at 80°C for 3 hours. The final product had 36.5 wt. % solids with fibres having an average diameter of about 50 run and length of 2 microns. By fractionation method (as in example 9 (b)), the sample was found to contain 57 wt. % nanofibres.

[0284] The reference in this specification to any prior publication (or information derived from it), or to any matter which is known, is not, and should not be taken as an acknowledgment or admission or any form of suggestion that that prior publication (or information derived from it) or known matter forms part of the common general knowledge in the field of endeavour to which this specification relates.

[0285] Throughout this specification and the claims which follow, unless the context requires otherwise, the word "comprise", and variations such as "comprises" and "comprising", will be understood to imply the inclusion of a stated integer or step or group of integers or steps but not the exclusion of any other integer or step or group of integers or steps.

Claims

THE CLAIMS DEFINING THE INVENTION ARE AS FOLLOWS1. An aqueous coating composition comprising a polymer binder, opacifier particles and polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles.

2. The aqueous coating composition according to claim 1, wherein the polymer binder is present in an amount of about 10 wt. % to about 80 wt. %.

3. The aqueous coating composition according to claim 1 or 2, wherein the polymer binder comprises polymerised residues of one or more crosslinking monomers.

4. The aqueous coating composition according to any one of claims 1 to 3, wherein the opacifier particles are selected from particles of metal oxide, carbon black, cobalt silicates, dibromanthrone, arylamide, copper phthalocyanine and combinations thereof.

5. The aqueous coating composition according to claim 4, wherein the particles of metal oxide are selected from titanium oxide, zinc oxide, iron oxide and combinations thereof.

6. The aqueous coating composition according to any one of claims 1 to 5, wherein the opacifier particles have an average diameter ranging from about 100 nm to about 600 nm.

7. The aqueous coating composition according to any one of claims 1 to 6, wherein the opacifier particles are present in an amount of about 5 wt. % to about 40 wt. %.

8. The aqueous coating composition according to any one of claims 1 to 7, wherein the polymer fibres have an average diameter of less than 100 nm.

9. The aqueous coating composition according to any one of claims 1 to 8, wherein the polymer fibres have an aspect ratio of greater than 60.

10. The aqueous coating composition according to any one of claims 1 to 9, wherein thepolymer fibres are provided in the form of a polymer mass and that polymer mass is present in an amount ranging from about 0.1 wt. % to about 30 wt. %, relative to a dry mass of a polymer film derived from the aqueous coating composition.

11. The aqueous coating composition according to any one of claims 1 to 10, wherein the block copolymer comprises a hydrophobic polymer block and a hydrophilic polymer block and the hydrophobic polymer block to hydrophilic polymer block molecular weight ratio ranges from about 0.5 to about 10.

12. The aqueous coating composition according to any one of claims 1 to 11, wherein the block copolymer is a reversible addition fragmentation chain transfer (RAFT) block copolymer.

13. The aqueous coating composition according to any one of claims 1 to 12, wherein the block copolymer comprises polymerised residues of one or more crosslinking monomers.

14. The aqueous coating composition according to any one of claims 1 to 13, wherein the block copolymer comprises a hydrophobic polymer block comprising about 50 to about 10,000 polymerised monomer repeat units.

15. The aqueous coating composition according to any one of claims 1 to 14, wherein the block copolymer comprises a hydrophilic polymer block comprising 5 to about 1,000 polymerised monomer repeat units.

16. A method of producing an aqueous coating composition, the method comprising blending together a polymer binder, opacifier particles and polymer fibres having (i) an average diameter of less than 200 nm, and (ii) a composition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles.

17. A method for increasing opacity of an aqueous coating composition comprising polymer binder and opacifier particles, wherein the opacifier particles are not vesiculated polymer particles or contained within vesiculated polymer particles, the method comprising including in the composition polymer fibres having (i) an average diameter of less than 200 nm, and (ii) acomposition formed from a block copolymer arranged so as to provide the polymer fibres with a hydrophobic core and a hydrophilic shell structure, the increased opacity being relative to the composition absent the polymer fibres.