Ultrathin glass with low periphery-to-center breakage ratio

WO2024243755A1PCT designated stage expired Publication Date: 2024-12-05SCHOTT GLASS TECH (SUZHOU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/096696
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-05

Smart Images

  • Figure CN2023096696_05122024_PF_FP_ABST
    Figure CN2023096696_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a foldable glass article having a thickness of at most 200 μm and to a method of manufacturing the glass article. The glass article has a lower thickness in a peripheral region as compared to a center region. The glass article has a low periphery-to-cen-ter breakage ratio. In particular, in a 2-point-bending test more breakage origins stem from the center of the glass article than from its periphery. The invention also relates to the use of the glass article, in particular in consumer electronics such as foldable handheld devices including smartphones.
Need to check novelty before this filing date? Find Prior Art

Description

Ultrathin glass with low periphery-to-center breakage ratio

[0001] The present invention relates to a foldable glass article having a thickness of at most 200 μm and to a method of manufacturing the glass article. The glass article has a lower thickness in a peripheral region as compared to the center region. The glass article has a low periphery-to-center breakage ratio. In particular, in a 2-point-bending test more breakage origins stem from the center of the glass article than from its periphery. The disclosure also relates to the use of the glass article, in particular in consumer electronics such as foldable handheld devices includ-ing smartphones.Background

[0002] Due to the unique properties of being flexible, high modulus and transparent, ultrathin glasses have large potential in applications for consumer electronics and optics. However, while being highly flexible, breakage from the edges under bending stress still poses a high risk for failure. Common approaches (for example edge grinding and polishing) to increase the edge strength of thick glass are hardly applicable for ultrathin glasses. Therefore, ultrathin glasses with low edge strength could lead to breakage of the glasses in their later application (such as cover glasses for foldable electronic devices) upon repetitive bending and lead to failure of the final (usually expensive) devices.

[0003] Usually, glass processors focus a lot on improving the flexural strength of foldable glasses to enable a smaller and smaller minimum bending radius. While surface treatments like chemical toughening and slight etching could be applicable for ultrathin glasses to easily improve the flex-ural strength, quality of the edges could more often be the limiting factor. An approach to in-crease the edge quality of ultrathin glasses is by edge processing, including creating a chamfer structure. However, previous edge processing methods leave room for further improvements.

[0004] WO 2022 / 232996 A1 discloses ultrathin glass with high edge impact resistance when tested in a swing arm test. However, in the respective disclosure all etching steps occur prior to chemical toughening. Thus, a “post-etching” step is neither disclosed nor suggested. The peripheral re-gions of the present disclosure are not obtained.

[0005] KR 10-1620375 B1 describes a UTG stack processing method, wherein UTG glasses are stacked into a laminated stack, cut to size and edge ground and polished followed by an etching step, wherein the stack is rotated within the etchant. However, here not the individual glasses are rotated inside the etchant post-toughening, but the stack prior to toughening. The peripheral  regions of the present disclosure are not obtained.

[0006] WO 2019 / 218155 A1 discloses ultrathin glass with special chamfer shape. The peripheral re-gions of the present disclosure are not disclosed.

[0007] Details of Invention

[0008] The inventors of the present invention have found that an optimized thinning of the peripheral region can improve bendability and reduce failure of such glasses due to breakage from the pe-riphery drastically. In particular, it was found that bending strength can be improved so much that the glasses tend to rather break from the center of the glass than from its periphery. In the commonly used 2-Point Bending (2PB) test, glasses produced by the present method show a ratio of breakage initiated from the periphery of <50 %, in particular at most 45%.

[0009] It was found that a width of a thinned peripheral region of about 3 to 5 mm (measured from the edge) and a peripheral thickness of the glass of about at most 99%, at least 75%, at least 85%, or at least 90%in relation to the center thickness (in particular 1-10 or 1-3 μm thinner) shows optimal edge strength in the 2PB test.

[0010] In one aspect, the present disclosure relates to a chemically toughened glass article comprising a first main surface and a second main surface and at least one edge surface connecting the first main surface and the second main surface,

[0011] ● wherein the glass article has a center region and a peripheral region, wherein first and second main surface are essentially parallel to each other in the center region,

[0012] ○ wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,

[0013] ○ wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface,

[0014] ● wherein the average thickness of the center region is at most 200 μm,

[0015] ● wherein the average thickness of the peripheral region is lower than the average thick-ness of the center region by 1.0 μm to 10.0 μm, such as 1.0 to 7.0 μm, 1.0 to 5.0 μm or 1.0 to 3.0 μm,

[0016] ● wherein the average thickness of the peripheral region is measured as the average thickness along the perimeter line having a distance of 2.5 mm to the edge surface measured parallel to the first or second main surface.

[0017] The length and the width of the first main surface are in particular essentially identical to the length and the width of the second main surface.

[0018] The average thickness of the peripheral region in a closest distance of 2.5 mm to the edge sur-face measured parallel to the first or second main surface is for example lower than the average thickness of the center region by 1.0 to 10.0 μm, 1.0 to 7.0 μm, 1.0 to 5.0 μm, 1.0 to 3.0 μm, 1.2 μm to 2.8 μm, by 1.5 μm to 2.5 μm, or by 1.7 μm to 2.3 μm. The average thickness of the pe-ripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface is for example lower than the average thickness of the center region by at least 1.0 μm, at least 1.2 μm, at least 1.5 μm, or at least 1.7 μm. The average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface is for example lower than the average thickness of the center region by at most 10.0 μm, at most 7.0 μm, at most 5.0 μm, at most 3.0 μm, at most 2.8 μm, at most 2.5 μm, or at most 2.3 μm.

[0019] The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the center region may in particular be in a range of from 75%to 99%, from 80%to 99%, from 85%to 99%, from 90%to 98%, or from 91%to 97%. The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the center region may in particular be at least 75%, at least 80%, at least 85%, at least 90%, or at least 91%. The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the center region may in particular be at most 99%, at most 98%, or at most 97%.

[0020] In one aspect, the present disclosure relates to a chemically toughened glass article comprising a first main surface and a second main surface and at least one edge surface connecting the first main surface and the second main surface,

[0021] ● wherein the glass article has a center region and a peripheral region, wherein first and second main surface are essentially parallel to each other in the center region,

[0022] ○ wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to  the first or second main surface,

[0023] ○ wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface,

[0024] ● wherein the average thickness of the center region is at most 200 μm,

[0025] ● wherein the ratio of the average thickness of the peripheral region and the average thickness of the center region is in a range of from 75%to 99%, from 80%to 99%, or from 85%to 99%,

[0026] ● wherein the average thickness of the peripheral region is measured as the average thickness along the perimeter line having a distance of 2.5 mm to the edge surface measured parallel to the first or second main surface.

[0027] The length and the width of the first main surface are in particular essentially identical to the length and the width of the second main surface.

[0028] The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the center region may in particular be in a range of from 90%to 98%, or from 91%to 97%. The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the center region may in particular be at least 75%, at least 80%, at least 85%, at least 90%, or at least 91%. The ratio of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the aver-age thickness of the center region may in particular be at most 99%, at most 98%, or at most 97%.

[0029] The average thickness of the peripheral region in a closest distance of 2.5 mm to the edge sur-face measured parallel to the first or second main surface may be lower than the average thick-ness of the center region by 1.0 to 10.0 μm, 1.0 to 7.0 μm, 1.0 to 5.0 μm, 1.0 μm to 3.0 μm, 1.2 μm to 2.8 μm, by 1.5 μm to 2.5 μm, or by 1.7 μm to 2.3 μm. The average thickness of the pe-ripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface may be lower than the average thickness of the center region by at least 1.0 μm, at least 1.2 μm, at least 1.5 μm, or at least 1.7 μm. The average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface may be lower than the average thickness of the center region by at  most 10.0 μm, at most 7.0 μm, at most 5.0 μm, at most 3.0 μm, at most 2.8 μm, at most 2.5 μm, or at most 2.3 μm.

[0030] The average thickness of the center region and the average thickness of the peripheral region are in particular determined as follows.

[0031] Peripheral region: micrometer is used to measure the thickness along the line 2.5 mm away from the outline towards the center. One measurement is done for every 1 cm length of the out-line. Then the average thickness is calculated based on the measurements. The average thick-ness at a distance of 2.5 mm from the edge is a reasonable measure for the average thickness of the edge region because the increase in thickness may in particular be approximately linear throughout the peripheral region towards the center region.

[0032] Center region: micrometer is used to measure the thickness within the area more than 5 mm away from the outline towards the center. One measurement is done for every 1 cm2 of the area. Then the average thickness is calculated based on the measurements.

[0033] The chemically toughened glass article of the present disclosure is in particular a foldable glass article. Thus, optionally the glass article of the disclosure can be folded around a folding axis.

[0034] In the present disclosure, the indication “measured parallel to the first or second main surface” refers to a direction parallel to those parts of the first or second main surface in which first and second main surface are essentially parallel to each other.

[0035] That first and second main surface are essentially parallel to each other in the center region does not exclude that the center region may also contain areas in which there are minor devia-tions from the parallel orientation of the first and second main surface. In particular, the present disclosure also comprises locally slimmed glass (LSG) . Locally slimmed glasses are glasses that have a thinned area around their folding axis and thicker non-folding areas. In such glasses, first and second main surface are essentially parallel to each other in particular in the thicker non-folding area and in the part of the thinned area that correspond to the minimum thickness. However, between these areas there is an area in which the thickness gets lower from the periphery towards the center. In this transitional area between the thicker non-folding area and the minimum thickness of the thinned area first and second main surface are less par-allel to each other as compared to the remaining parts of the center region.

[0036] The average thickness of the center region is in particular in a range of from 15 μm to 200 μm, from 15 μm to 150 μm, from 15 μm to 120 μm, from 15 μm to 100 μm, from 20 μm to 80 μm, from 25 μm to 75 μm, or from 30 μm to 70 μm. The average thickness of the center region is in  particular at least 15 μm, at least 20 μm, at least 25 μm, or at least 30 μm. The average thick-ness of the center region is in particular at most 200 μm, at most 150 μm, at most 120 μm, at most 100 μm, at most 80 μm, at most 75 μm, or at most 70 μm.

[0037] The glass article of the present disclosure is a chemically toughened glass article. The surface compressive stress at the first and / or second main surface is in particular in a range of from 300 to 1500 MPa, such as from 400 to 1200 MPa, from 500 to 1000 MPa, from 600 to 900 MPa, or from 700 to 850 MPa. The surface compressive stress at the first and / or second main surface is in particular at least 300 MPa, at least 400 MPa, at least 500 MPa, at least 600 MPa, or at least 700 MPa. The surface compressive stress at the first and / or second main surface is in particular at most 1500 MPa, at most 1200 MPa, at most 1000 MPa, at most 900 MPa, at most 800 MPa, or at most 750 MPa.

[0038] The depth of layer at the first and / or second main surface is in particular in a range of from 0.5 to 40 μm, such as from 1.0 to 20 μm, from 2.0 to 15 μm, or from 5.0 to 10 μm. The depth of layer at the first and / or second main surface is in particular at least 0.5 μm, at least 1.0 μm, at least 2.0 μm, or at least 5.0 μm. The depth of layer at the first and / or second main surface is in particular at most 40 μm, at most 20 μm, at most 15 μm, or at most 10 μm.

[0039] The depth of layer at the first and / or second main surface is in particular in a range of from 1.0%to 40%as compared to the average thickness of the center region, such as from 2.0%to 20%, or from 5.0%to 10%. The depth of layer at the first and / or second main surface is in particular at least 1.0%, at least 2.0%or at least 5.0%as compared to the average thickness of the center region. The depth of layer at the first and / or second main surface is in particular at most 40%, at most 20%, or at most 10%as compared to the average thickness of the center region.

[0040] In some embodiments, the center region may comprise a folding area and a non-folding area, wherein the average thickness of the center region in the folding area is lower than the average thickness of the center region in the non-folding area. Likewise, the peripheral region may com-prise a folding area and a non-folding area, wherein the average thickness of the peripheral re-gion in the folding area is lower than the average thickness of the peripheral region in the non-folding area. In such embodiments, the average thickness of the folding area of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or sec-ond main surface may for example be lower than the average thickness of folding area of the center region by 1.0 μm to 3.0 μm such as from 1.2 μm to 2.8 μm, from 1.5 μm to 2.5 μm, or from 1.7 μm to 2.3 μm. Likewise, the ratio of the average thickness of the folding area of the pe-ripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the folding area of the center region may  be in a range of from 85%to 99%such as from 90%to 98%, or from 91%to 97%.

[0041] In some embodiments, the reduced thickness of the peripheral region as compared to the cen-ter region of the glass is homogeneously distributed around the entire peripheral region. In par-ticular, the deviation of the thickness of the peripheral region at any given position in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface from the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface may be less than 2.0%, less than 1.0%, less than 0.5%, or less than 0.2%of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface. For example, if the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface is 50 μm, and the thickness of the peripheral region at any given position in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface is in a range of from >49 μm to <51 μm, the above-described deviation would be less than 2%. Even in embodiments with homogeneous distribution of thickness reduction of the peripheral region, the deviation of the thickness of the peripheral region at any given position in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface from the average thick-ness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured par-allel to the first or second main surface may be at least 0.01%, at least 0.02%, or at least 0.05%of the average thickness of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface.

[0042] In some embodiments, the reduced thickness of the peripheral region as compared to the cen-ter region of the glass is inhomogeneously distributed around the entire peripheral region. For example, in some embodiments the peripheral region of the glass may include one or more ar-eas having a reduced thickness as compared to the center region and one or more areas not having a reduced thickness as compared to the center region. In some embodiments, the seg-ments of the peripheral region being parallel to the longitudinal axis of the glass article may have a reduced thickness as compared to the center region, whereas the segments of the pe-ripheral region being orthogonal to the longitudinal axis do not have a reduced thickness as compared to the center region.

[0043] Segments that are parallel to the longitudinal axis may also be referred to as the long sides of the glass article. Generally, it is these long sides that are bent during the folding of the glass ar-ticle. In contrast, the short sides are generally not bent during the folding. Therefore, it is of par-ticular advantage that the segments of the peripheral region being parallel to the longitudinal axis of the glass article have a reduced thickness as compared to the center region.

[0044] The glass article of the present disclosure optionally is axially symmetric. In other words, the glass article optionally comprises one axis of symmetry or more than one axis of symmetry. Thus, the glass article may comprise one axis of symmetry or two axes of symmetry. For exam-ple, if the glass article has a rectangular shape (length y being larger than width z of the glass article) , there may be a first axis of symmetry being parallel to the long sides of the glass article and a second axis of symmetry being parallel to the short sides of the glass article. In embodi-ments in which the glass article has a squared shape (length y being equal to width z) , there may be a first axis of symmetry being parallel to two opposing sides of the glass article and a second axis of symmetry being parallel to the two other sides of the glass article. In such em-bodiments, the term “long sides” of the glass article may refer to two opposing sides of the glass articles, whereas the term “short sides” of the glass article may refer to the two remaining sides which are orthogonal to the long sides.

[0045] Thus, even though long sides and short sides have the same length in square shaped glass ar-ticles, the respective terms are nevertheless used in the present disclosure to refer not only to glass articles of rectangular shape but also to glass articles having a squared shape, in order to differentiate between two opposing sides on the one hand and two sides being orthogonal thereto on the other hand. Of course, in embodiments of glass articles having a rectangular shape, the long sides are actually longer than the short sides of the glass article. In particular, the long sides have a length being identical to the length y of the glass article, whereas the short sides have a length being identical to the width z of the glass article.

[0046] In any case, in particular irrespective of whether the glass article has a rectangular shape or a squared shape, the first axis of symmetry is in particular orthogonal to the second axis of sym-metry.

[0047] The folding axis of the glass article may be one of its axes of symmetry. In particular, the folding axis may be the axis of symmetry of the glass article that is parallel to the short sides of the glass article.

[0048] In the 2PB test, the glass article is placed as a U-shape between two parallel plates. The two plates are big enough to cover the whole glass article. Then one of the plate moves towards the other one while remaining parallel with a speed of 60 mm / min until the designed folding dis-tance of fifty times the center thickness is reached. The folding distance is defined as the dis-tance of the two plates. In case the foldable article survived when the folding distance is reached, it is considered as passing the test. For ultrathin glass (UTG) , the center thickness of the glass article corresponds to the average thickness of the center region of the glass article.

[0049] For locally slimmed glass (LSG) , the center thickness of the glass article corresponds to the av-erage thickness in the folding area of the center region. The passing rate is the number of sam-ples passed divided by the number of total measured samples.

[0050] The glass articles of the present disclosure may in particular have a passing rate in the 2PB test of at least 65%, such as at least 70%, at least 75%, at least 80%, at least 85%, or at least 90%. The passing rate in the 2PB test may for example be at most 99.9%, at most 99%, at most 98%, at most 97%, at most 96%, or at most 95%. The passing rate in the 2PB test may for example be in a range of from 65%to 99.9%, from 70%to 99%, from 75%to 98%, from 80%to 97%, from 85%to 96%, or from 90%to 95%. The 2PB test is in particular performed with a sample size of at least 50 pieces, for example 50 pieces.

[0051] To evaluate the breakage origin of the glasses in the 2PB test, test glasses are double-side laminated with polymer films that are 5 mm bigger than the glass in terms of length and width. The adhesion between the glass and the polymer films is electrostatic. The material of the film is PE (polyethylene) to have a smaller modulus of elasticity. Each side of the glass is laminated with a single layer of the polymer that is 50 μm thick. By doing so, fractures and shards are cap-tured in the polymer film and the point of origin can be analyzed by the weblike crack structure. In this analysis, it was found that glass articles of the disclosure show more breakage origins stemming from the center of the glass than from its edges. When calculated as periphery-to-center breakage ratio (P2C) , the glasses of invention in particular have a P2C of less than 50%, at most 45%, at most 40%, at most 35%, at most 30%, at most 25%, at most 20%, or at most 15%. The P2C ratio may for example be at least 0.1%, at least 0.2%, at least 0.5%, at least 1.0%, at least 2.0%, at least 3.0%, at least 4.0%, or at least 5.0%. The P2C ratio may for exam-ple be in a range of from 0.1%to <50%, from 0.2%to 45%, from 0.5%to 40%, from 1.0%to 35%, from 2.0%to 30%, from 3.0%to 25%, from 4.0%to 20%, or from 5.0%to 15.0%. The P2C ratio is in particular determined based on a sample size of at least 50 pieces, for example 50 pieces.

[0052] The P2C ratio indicates the percentage of breakage origins stemming from the peripheral region as compared to the total number of breakages. The P2C ratio is calculated based on the follow-ing formula:

[0053] In this respect, the term “periphery” refers to the peripheral region of the glass article which is constituted by the parts of the glass article having a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface. Likewise, the term “center”  refers to the center region of the glass article which is constituted by the parts of the glass arti-cle having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface.

[0054] The glass articles of the disclosure are in particular able to pass a sliding test with a folding dis-tance equal to 50 times center thickness (referring to the center thickness, as above) of the glass article. In this test the foldable glass article is placed as a U-shape between two parallel plates. The two plates are big enough to cover the whole article. Then one of the plates moves towards the other one while remaining parallel with a speed of 60 mm / min until the designed distance is reached. The folding distance is defined as the distance of the two plates. Then the moving plate starts to move back and forth along the article length direction with a speed of 10 mm / sand a travel distance of 10 mm. The glass article surviving 10 times of sliding without glass breakage is considered passing the test. The setup of the sliding test is schematically shown in Figure 5.

[0055] The glass articles of the disclosure in particular pass 10 repetitions without breakage in the slid-ing test with a folding distance of 50 times the center thickness of the glass article, with a plate speed of 10 mm / sand with a plate travel distance of 10 mm. The passing rate of the glass arti-cles of the disclosure in the sliding test with a folding distance of 50 times the center thickness of the glass article, with a plate speed of 10 mm / sand with a plate travel distance of 10 mm is in particular more than 50%, for example at least 55%, at least 60%, at least 65%, at least 70%, or at least 75%. The passing rate of the glass articles of the disclosure in the sliding test with a folding distance of 50 times the center thickness of the glass article, with a plate speed of 10 mm / sand with a plate travel distance of 10 mm may for example be 100%, at most 99%, at most 98%, at most 95%, at most 90%, or at most 87%. The passing rate of the glass articles of the disclosure in the sliding test with a folding distance of 50 times the center thickness of the glass article, with a plate speed of 10 mm / sand with a plate travel distance of 10 mm may for example be in a range of from >50%to 100%, from 55%to 99%, from 60%to 98%, from 65%to 95%, from 70%to 90%, or from 75%to 87%. The sample size is in particular at least 50 pieces, for example 50 pieces.

[0056] In some embodiments, the edge of the glass article of the present disclosure has a chamfer structure. When the angle of a tangent line to the first surface is defined as 0° and the angle of the tangent line to the second surface is defined as 180°, the chamfer structure in particular has an averaged chamfer surface with a profile such that the angle αxi of the tangent line to the aver-aged chamfer surface at any position xi of the averaged chamfer surface is in a range of from >0° to <180°. The chamfer structure in particular has a chamfer height H, defined as the projec-tion of the segment spanning from position xi of the averaged chamfer surface closest to the  first surface of the glass article with αxi = 45° to position xj of the averaged chamfer surface clos-est to the second surface of the glass article with αxj = 135° onto a line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second surface. The to-tal chamfer height variation TCHV of the chamfer height H in the direction of the length y and / or width z of the glass article is defined as the difference of the maximum chamfer height Hmax and the minimum chamfer height Hmin along at least a portion of the length y and / or width z of the article divided by the average chamfer height Havg along said portion of the length y and / or width z of the article, wherein the portion is at least 25%of the length y and / or width z. The ratio (t*Havg)  / TCHV may in particular be at least 250 μm2.

[0057] The averaged chamfer surface is obtained based on overlapping optical layers of a cross-sec-tion of the chamfer surface profile. In order to obtain such images, the glass article is observed with an optical microscope in transmitted light mode. A 200x magnification is used. The focus is on the top plane so that the edges look very sharp. The glass article is positioned such that the top plane is not tilted. Thus, the top plane is perpendicular to the direction of light. Images of particularly good quality are generally obtained with automatic white balance, automatic bright-ness and automatic contrast, in particular using Nikon Y-TV55 microscope. An averaged cham-fer surface is observed in such images due to the depth of field, which determines the depth of overlapping. Using above described method, the averaged chamfer structure is based on over-lapping optical layers over a depth of about 0.5 mm. For example, the sample has an extent of at least 1 mm in the direction of the observation so that there is sufficient depth for the overlap-ping.

[0058] In some embodiments, the chamfer structure has a chamfer width W, defined as the distance of a specific position on the averaged chamfer surface to the line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second surface, wherein the dis-tance is measured orthogonal to the respective line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second surface, wherein there is no other po-sition on the averaged chamfer surface having a larger distance to the respective line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second sur-face measured orthogonal to the respective line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second surface. In one aspect of the disclo-sure, the ratio of chamfer width W and average chamfer height Havg may be in a range of from 0.1: 1 to 10: 1, for example from 1: 1 to 10: 1, from 2: 1 to 7.5: 1, from 3: 1 to 6: 1, or from 3.5: 1 to 5: 1. The ratio of chamfer width W and average chamfer height Havg may for example be at least 0.1: 1, at least 1: 1, at least 2: 1, at least 3: 1, or at least 3.5: 1. The ratio of chamfer width W and average chamfer height Havg may for example be at most 10: 1, at most 7.5: 1, at most 6: 1, or at  most 5: 1.

[0059] In some embodiments, the ratio of thickness t and average chamfer height Havg may be in a range of from 1.2: 1 to 10: 1, for example from 1.3: 1 to 7.5: 1, from 1.5: 1 to 5: 1, from 1.75: 1 to 4: 1 or from 2.0: 1 to 3.25: 1. The ratio of thickness t and average chamfer height Havg may for exam-ple be at least 1.2: 1, at least 1.3: 1, at least 1.5: 1, at least 1.75: 1 or at least 2.0: 1. The ratio of thickness t and average chamfer height Havg may for example be at most 10: 1, at most 7.5: 1, at most 5: 1, at most 4: 1 or at most 3.25: 1.

[0060] The glass article can be of any size. For example it could be a long ultrathin glass ribbon that is rolled (glass roll) or a single smaller glass part cut out off a glass roll or a separate glass sheet or a single small glass article (like a fingerprint sensor (FPS) or display cover glass) etc. Option-ally, the glass article of the disclosure is a sheet or sheet-like article, in particular an article of rectangular or squared shape having a length y and a width z. Both length y and width z are preferably much larger as compared to the thickness t of the article. For example, length y and / or width z may be at least 1 mm, at least 2 mm, at least 5 mm, at least 10 mm, at least 15 mm, at least 20 mm, at least 25 mm, at least 30 mm, at least 40 mm, or at least 50 mm. For ex-ample, length y and / or width z may be at most 500 mm, at most 400 mm, at most 300 mm, at most 200 mm, at most 150 mm, at most 125 mm, at most 100 mm, or at most 70 mm. The ratio of length y and width z may be 1: 1 or more. In some embodiments, the glass article may have a notch, in particular for the front camera in smartphone applications.

[0061] In one embodiment of the present disclosure, the article has a length y in a range of from 10 mm to 500 mm and / or a width z in a range of from 5 mm to 400 mm, for example a length y and / or a width z in a range of from 10 to 400 mm, from 15 to 300 mm, from 20 to 200 mm, from 25 to 150 mm, from 30 to 125 mm, from 40 to 100 mm, or from 50 to 70 mm. The length y and / or the width z may for example be at least 5 mm, at least 10 mm, at least 15 mm, at least 20 mm, at least 25 mm, at least 30 mm, at least 40 mm, or at least 50 mm. The length y and / or the width z may for example be at most 500 mm, at most 400 mm, at most 300 mm, at most 200 mm, at most 150 mm, at most 125 mm, at most 100 mm, or at most 70 mm.

[0062] Optionally, the article has exactly one edge connecting first and second surface thereof. De-pending on the shape of the article, the edge may have different sides. For example, in case of a sheet or sheet-like article having rectangular or squared shape, the edge has four sides, wherein two opposite sides represent the length y of the article and the remaining two opposite sides represent the width z of the article. The positions connecting two adjacent sides of the edge are generally referred to as corners.

[0063] Compressive stress (CS) (also referred to as "Pressure stress" or "surface stress" ) is the stress that results from the displacement effect on the glass network through the glass surface after ion exchange, while no deformation occurs in the glass.

[0064] "Penetration depth" or "depth of ion exchanged layer" or "ion exchange depth" ( "depth of layer" or "depth of ion exchanged layer" , DoL) is the thickness of the glass surface layer in which ion exchange occurs and compressive stress is generated. The compressive stress CS and the penetration depth DoL can be measured optically (in particular by a waveguide mechanism) , us-ing the commercially available stress meter FSM6000 (for example company “Luceo Co., Ltd. ” , Japan, Tokyo) .

[0065] When CS is induced on one side or both sides of single glass sheet, to balance the stress ac-cording to the 3rd principle of Newton’s law, a tension stress must be induced in the center re-gion of glass, and it is called central tension (CT) . CT can be calculated from measured CS and DoL values.

[0066] Ion exchange means that the glass is hardened or chemically tempered (also called chemically toughened) by ion exchange processes, a process that is well known to the person skilled in the art in the field of glass making and processing. The toughening process may be done by im-mersing the glass layer into a salt bath which contains monovalent ions to exchange with alkali ions inside the glass. The monovalent ions in the salt bath have radii larger than alkali ions in-side the glass. A compressive stress to the glass is built up after ion-exchange due to larger ions squeezing into the glass network. After ion-exchange, the strength and flexibility of glass are significantly improved. In addition, the CS induced by chemical toughening improves the bending properties of the toughened glass layer and increases scratch resistance of the glass layer. The typical salt used for chemical tempering is, for example, K+-containing molten salt or mixtures of salts. Optional salt baths for chemical toughening are Na+-containing and / or K+-con-taining molten salt baths or mixtures thereof. Optional salts are NaNO3, KNO3, NaCl, KCl, Na2SO4, K2SO4, Na2CO3, K2CO3, and K2Si2O5. Additives such as NaOH, KOH and other sodium salts or potassium salts are also used to better control the rate of ion exchange for chemical tempering. Ion exchange may for example be done in KNO3 at temperatures in a range of from 300℃ to 480℃, in particular from 340℃ to 450℃ or from 390℃ to 450℃, for example for a time span of from 30 seconds to 48 hours, in particular for about 20 minutes. Chemical toughen-ing is not limited to a single step. It can include multi steps in one or more salt baths with alka-line metal ions of various concentrations to reach better toughening performance. Thus, the chemically toughened glass layer can be toughened in one step or in the course of several steps, e.g. two steps. Two-step chemical toughening is in particular applied to Li2O-containing glasses as lithium may be exchanged for both sodium and potassium ions.

[0067] In one embodiment of the disclosure, the averaged chamfer surface profile may be such that for any position xi of the averaged chamfer surface there is exactly one angle αxi of the tangent line to the averaged chamfer surface. For example, the averaged chamfer surface may be de-scribed by a continuous function. In another embodiment of the disclosure, more than one angle αxi may be attributed to one or more positions xi of the averaged chamfer surface, for example to two positions thereof. In particular, the averaged chamfer structure may comprise peaks or corners at a position xi connecting positions xh and xj, wherein the angle αxh of the tangent line to the averaged chamfer surface at a position xh of the averaged chamfer surface differs from the angle αxj of the tangent line to the averaged chamfer surface at position xj of the averaged chamfer surface by at least 1°, at least 2°, at least 5°, or at least 10°, for example 15° to 80°, 20° to 70°, or 30° to 60°. For example, the angle αxh of the tangent line to the averaged chamfer surface at a position xh of the averaged chamfer surface may be 30° and the angle αxj of the tangent line to the averaged chamfer surface at position xj of the averaged chamfer surface may be 90°. In such a case there is a rapid change of angles at the position xi that connects po-sitions xh and xj. In fact, any angle from 30° to 90° may be attributed to the angle αxi of the tan-gent line to the averaged chamfer surface at the position xi that connects position xh with αxh being 30° and position xj with angle αxj being 90°.

[0068] In one embodiment of the disclosure, the averaged chamfer surface profile is such that the an-gle αxi of the tangent line to the averaged chamfer surface at any position xi of the averaged chamfer surface is different from the angle αxj of the tangent line to the averaged chamfer sur-face at any other position xj of the averaged chamfer surface. In other words, the averaged chamfer surface profile may be represented as a strictly monotonous function. However, in an-other embodiment of the present disclosure, the averaged chamfer surface profile is such that the angle αxi of the tangent line to the averaged chamfer surface at a position xi of the averaged chamfer surface is the same as the angle αxj of the tangent line to the averaged chamfer surface at another position xj of the averaged chamfer surface. In one embodiment of the present dis-closure, the averaged chamfer surface profile is such that the angle αxi of the tangent line to the averaged chamfer surface is from >0° to <45°, from >135° to <180°, or from 89° to 91° for at least 90%, at least 95%, at least 99%, or at least 99.9%of positions xi of the averaged chamfer surface. In one embodiment of the present disclosure, the averaged chamfer surface profile is such that the angle αxi of the tangent line to the averaged chamfer surface is from 89° to 91° for at least 5%to 20%of positions xi of the averaged chamfer surface.

[0069] The chamfer structure has a chamfer height H, defined as the projection of the segment span-ning from position xi of the averaged chamfer surface closest to the first surface of the glass ar-ticle with αxi = 45° to position xj of the averaged chamfer surface closest to the second surface  of the glass article with αxj = 135° onto a line having an angle of 90° with both the tangent line to the first surface and the tangent line to the second surface.

[0070] The chamfer height is preferably determined by optical microscopy, in particular based on mi-croscope images having a direction of view facing the edge of the glass article. The chamfer height H can be visually determined as the height H of the chamfer structure based on such mi-croscope images, in particular in transmitted light mode. The magnification may for example be 200x. The focus is on the top plane. The glass article is positioned such that the top plane is not tilted. Thus, the top plane is perpendicular to the direction of light. Images of particularly good quality are generally obtained with automatic white balance, automatic brightness and automatic contrast, in particular using Nikon Y-TV55 microscope.

[0071] Notably, the chamfer height H may differ at different positions around the perimeter of the glass article. For example, there may be H (p1) = H1 at a position p1, and H (p2) = H2 at a position p2, with p1 ≠ p2 and H1 ≠ H2. The local chamfer height LH is defined herein as the average local chamfer height along a portion of the length y and / or width z of the article, wherein said portion has a length of from 300 μm to 600 μm, for example 350 μm or 500 μm. The local chamfer height LH can be determined by optical microscopy, in particular based on microscope images having a direction of view facing the edge of the glass article. For example, in such images the boundaries of the chamfer may be fitted with a box of 300 to 600 μm in length, for example 350 μm or 500 μm in length, and the height of the box may be recorded as the local chamfer height LH. The height of the box is chosen such that the top line and the bottom line fit best with the boundaries of the chamfer over the length of the box. Thus, the local chamfer height LH repre-sents an average over the length of the box. Determining the local chamfer height LH as an av-erage along a portion of from 300 to 600 μm, for example along a portion of 350 μm or 500 μm turned out to be particularly advantageous for characterizing the local chamfer height. If this portion is reduced, there is an increased risk of noise in the data. If the portion is increased, there is an increased risk of averaging out relevant chamfer height variations. The local chamfer height LH may for example be determined as an average along a portion of at least 300 μm, or at least 350 μm. The local chamfer height LH may for example be determined as an average along a portion of at most 600 μm, or at most 500 μm.

[0072] The total chamfer height variation TCHV of the chamfer height H in the direction of the length y and / or width z of the glass article is defined as the difference of the maximum chamfer height Hmax and the minimum chamfer height Hmin along at least a portion of the length y and / or width z of the article divided by the average chamfer height Havg along said portion of the length y and / or width z of the article, wherein the portion is at least 25%of the length y and / or width z. TCHV = (Hmax-Hmin)  / Havg        (Formula 1)

[0073] Optionally, the portion is at least 50%of the length y and / or width z, at least 75%of the length y and / or the width z, at least 90%of the length y and / or width z, at least 99%of the length y and / or width z, or 100%of the length y and / or width z. In one embodiment of the disclosure, the portion is at least 25%, at least 50%, at least 75%, at least 90%, at least 99%, or 100%of the length y and width z.

[0074] In one embodiment of the disclosure, TCHV is at most 0.75, at most 0.70, at most 0.65, at most 0.60, at most 0.55, at most 0.50, at most 0.45, at most 0.40, at most 0.35, at most 0.30, at most 0.25, or at most 0.20. TCHV may for example be 0.05 or more, or 0.10 or more, or 0.15 or more.

[0075] As described above, the local chamfer height LH is defined herein as the average local chamfer height along a portion of the length y and / or width z of the article, wherein said portion has a length of from 300 μm to 600 μm, for example 350 μm or 500 μm. Optionally, Hmax, Hmin and Havg are determined based on respective local chamfer heights LH at different positions of the perim-eter of the glass article. In particular, local chamfer heights LH may be determined every 10 mm around the entire perimeter of the glass article. Hmax may be defined as the highest LH, Hmin as the lowest LH, and Havg as the mean of all local chamfer heights LH determined around the pe-rimeter of the glass article. In turn, TCHV can be calculated (based on Formula 1) from Hmax, Hmin and Havg thus determined.

[0076] The corners connecting two adjacent sides of the edge may be excluded from determining local chamfer heights LH. For example, determining the local chamfer height every 10 mm may give rise to in total 20 different LH values for a glass article having a length y of 60 mm and a width z of 60 mm if the actual corners of the article are excluded so that measurements are done at length positions of y = 10 mm, 20 mm, 30 mm, 40 mm and 50 mm, and at width positions of z = 10 mm, 20 mm, 30 mm, 40 mm and 50 mm, respectively (y and z = 0 mm and y and z = 60 mm are excluded) . This resolution of 10 mm turned out to be sufficient for characterizing the cham-fer height variations of the glass article. However, if an increased resolution is desired, it is of course possible to determine the local chamfer height LH at more positions around the perime-ter of the glass article, for example every 5 mm, every 2 mm, every 1 mm, or every 0.5 mm.

[0077] As described above, determining the local chamfer height every 10 mm around the entire perim-eter of the glass article gives rise to in total 20 different LH values for a glass article having a length y of 60 mm and a width z of 60 mm if the actual corners of the article are excluded. In such a case, TCHV is determined as the difference of the maximum chamfer height Hmax and  the minimum chamfer height Hmin along 100%of the length y and width z of the article divided by the average chamfer height Havg along 100%of the length y and width z of the article. The reason is that local chamfer heights LH are determined around the entire perimeter of the glass article and thus along 100%of the length y and width z of the article. Determining local chamfer heights LH around the entire perimeter of the glass article (and thus along 100%of the length y and width z of the article) is often desirable.

[0078] However, in embodiments of the disclosure, the TCHV along particular portions of the length and / or width of the glass article may be particularly relevant. For example, in some cases partic-ular portions of the length and / or width of the glass article are in need of a particularly high edge impact resistance because such portions are exposed to particularly high forces, for example during handling and / or use. Therefore, TCHV of the chamfer height H in the direction of the length y and / or width z of the glass article is not necessarily determined along 100%of the length y and width z of the article. It may well be sufficient to determine TCHV along a portion being at least 25%of the length y and / or width z.

[0079] In some embodiments, the ratio (t*Havg)  / TCHV is at least 250 μm2, at least 500 μm2, at least 750 μm2, at least 1000 μm2, at least 1250 μm2, at least 1500 μm2, at least 1750 μm2, at least 2000 μm2, at least 2250 μm2, at least 2500 μm2, for example at least 2750 μm2, at least 3000 μm2, at least 3500 μm2, at least 4000 μm2, at least 4500 μm2, at least 5000 μm2, at least 6000 μm2, at least 7000 μm2 or at least 8000 μm2. The respective ratio is a good indicator for the edge impact resistance. The higher the ratio (t*Havg)  / TCHV is, the better is the edge impact resistance. The ratio (t*Havg)  / TCHV is also called “ratio R” or simply “R” herein. The ratio R may be below 20000 μm2, below 15000 μm2 or below 10000 μm2.

[0080] The glass articles of the present disclosure are not restricted to certain glass compositions. However, some glass compositions are particularly advantageous. In an embodiment, the glass may be a silicate glass, such as alumosilicate glass, lithium-aluminum-silicate glass, or borosili-cate glass. The glass may also be soda-lime glass. The glass may contain alkali metal oxides, for example Na2O, in particular in an amount sufficient to allow chemical tempering.

[0081] The glass may comprise the following components, in weight percent: SiO2 45.0 to 75.0 wt. -%, B2O3 0 to 8.5 wt. -%, Al2O3 2.5 to 25.0 wt. -%, Li2O 0 to 10.0 wt. -%, Na2O 5.0 to 20.0 wt. -%, K2O 0 to 10.0 wt. -%, MgO 0 to 15.0 wt. -%, CaO 0 to 10.0 wt. -%, BaO 0 to 5.0 wt. -%, ZnO 0 to 5.5 wt. -%, TiO2 0 to 5.0 wt. -%, ZrO2 0 to 5.0 wt. -%, P2O5 0 to 20.0 wt. -%. Optionally, the glass may comprise the following components, in weight percent: SiO2 45.0 to 75.0 wt. -%, B2O3 0 to 5.0 wt. -%, Al2O3 2.5 to 25.0 wt. -%, Li2O 0 to 10.0 wt. -%, Na2O 5.0 to 20.0 wt. -%, K2O 0 to 10.0 wt. -%, MgO 0 to 15.0 wt. -%, CaO 0 to 10.0 wt. -%, BaO 0 to 5.0 wt. -%, ZnO 0 to 5.0 wt. -%, TiO2 0 to  2.5 wt. -%, ZrO2 0 to 5.0 wt. -%, P2O5 0 to 20.0 wt. -%. In some embodiments, the glass consists of the components mentioned in the before-mentioned list to an extent of at least 95.0 wt. -%, at least 97.0 wt. -%, or at least 99.0 wt. -%.

[0082] The terms, , X-free “and, , free of component X “, respectively, as used herein, preferably refer to a glass, which essentially does not comprise said component X, i.e. such component may be pre-sent in the glass at most as an impurity or contamination, however, it is not added to the glass composition as an individual component. This means that the component X is not added in es-sential amounts. Non-essential amounts according to the present disclosure are amounts of less than 100 ppm (m / m) , less than 50 ppm or less than 10 ppm. Thereby “X “may refer to any component, such as lead cations or arsenic cations. Optionally, the glasses described herein do essentially not contain any components that are not mentioned in this disclosure.

[0083] In an embodiment, the glass may comprise the following components, in weight percent: SiO2 45.0 to 72.0 wt. -%, B2O3 0 to 4.7 wt. -%, Al2O3 4.0 to 24.0 wt. -%, Li2O 0 to 6.0 wt. -%, Na2O 8.0 to 18.0 wt. -%, K2O 0 to 8.0 wt. -%, MgO 0 to 10.0 wt. -%, CaO 0 to 3.0 wt. -%, BaO 0 to 2.0 wt. -%, ZnO 0 to 3.0 wt. -%, TiO2 0 to 1.0 wt. -%, ZrO2 0 to 4.6 wt. -%, P2O5 0 to 15.0 wt. -%.

[0084] In an embodiment, the glass may comprise the following components, in weight percent: SiO2 51.0 to 65.0 wt. -%, B2O3 0 to 4.7 wt. -%, Al2O3 11.0 to 24.0 wt. -%, Li2O 0 to 6.0 wt. -%, Na2O 8.0 to 18.0 wt. -%, K2O 0 to 8.0 wt. -%, MgO 0 to 5.5 wt. -%, CaO 0 to 1.0 wt. -%, BaO 0 to 1.0 wt. -%, ZnO 0 to 3.0 wt. -%, TiO2 0 to 1.0 wt. -%, ZrO2 0 to 4.6 wt. -%, P2O5 0 to 10.0 wt. -%.

[0085] In an embodiment, the glass may comprise the following components, in weight percent: SiO2 45.0 to 72.0 wt. -%, B2O3 0 to 4.7 wt. -%, Al2O3 4.0 to 24.0 wt. -%, Li2O 0 to 3.0 wt. -%, Na2O 8.0 to 18.0 wt. -%, K2O 0 to 8.0 wt. -%, MgO 0 to 5.5 wt. -%, CaO 0 to 1.0 wt. -%, BaO 0 to 2.0 wt. -%, ZnO 0 to 3.0 wt. -%, TiO2 0 to 1.0 wt. -%, ZrO2 0 to 3.0 wt. -%, P2O5 0 to 15.0 wt. -%.

[0086] Lower limits of the amount of SiO2 may for example be at least 45 wt. -%, at least 51 wt. -%, or at least 55 wt. -%. Upper limits of the amount of SiO2 may for example be at most 75 wt. -%, at most 72 wt. -%, or at most 65 wt. -%.

[0087] Lower limits of the amount of B2O3 may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of B2O3 may for example be at most 5 wt. -%, at most 2 wt. -%, or at most 1 wt. -%. The glass may for example be free of B2O3.

[0088] Lower limits of the amount of Al2O3 may for example be at least 2.5 wt. -%, at least 4 wt. -%, or at least 11 wt. -%. Upper limits of the amount of Al2O3 may for example be at most 25 wt. -%, at most 24 wt. -%, or at most 20 wt. -%.

[0089] Lower limits of the amount of Li2O may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of Li2O may for example be at most 10 wt. -%, at most 6 wt. -%, or at most 3 wt. -%. The glass may for example be free of Li2O.

[0090] Lower limits of the amount of Na2O may for example be at least 5 wt. -%, at least 8 wt. -%, or at least 10 wt. -%. Upper limits of the amount of Na2O may for example be at most 20 wt. -%, at most 18 wt. -%, or at most 16 wt. -%.

[0091] Lower limits of the amount of K2O may for example be at least 0.5 wt. -%, at least 1 wt. -%, or for some variants at least 2 wt. -%. Upper limits of the amount of K2O may for example be at most 10 wt. -%, at most 8 wt. -%, at most 5 wt. -%, at most 3 wt. -%, or for some variants at most 2 wt. -%or at most 1.5 wt. -%. The glass may for example be free of K2O.

[0092] Lower limits of the amount of MgO may for example be at least 0.5 wt. -%, at least 1 wt. -%, or at least 2 wt. -%. Upper limits of the amount of MgO may for example be at most 15 wt. -%, at most 10 wt. -%, or at most 5.5 wt. -%. The glass may for example be free of MgO.

[0093] Lower limits of the amount of CaO may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of CaO may for example be at most 10 wt. -%, at most 3 wt. -%, or at most 1 wt. -%. The glass may for example be free of CaO.

[0094] Lower limits of the amount of P2O5 may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of P2O5 may for example be at most 20 wt. -%, at most 15 wt. -%, or at most 10 wt. -%. The glass may for example be free of P2O5.

[0095] Lower limits of the amount of BaO may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of BaO may for example be at most 5 wt. -%, at most 2 wt. -%, or at most 1 wt. -%. The glass may for example be free of BaO.

[0096] Lower limits of the amount of ZnO may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of ZnO may for example be at most 5 wt. -%, at most 3 wt. -%, or at most 1 wt. -%. The glass may for example be free of ZnO.

[0097] Lower limits of the amount of ZrO2 may for example be at least 0.2 wt. -%, at least 0.5 wt. -%, or at least 1 wt. -%. Upper limits of the amount of ZrO2 may for example be at most 5 wt. -%, at most 4.6 wt. -%, or at most 3 wt. -%. The glass may for example be free of ZrO2.

[0098] Lower limits of the amount of TiO2 may for example be at least 0.1 wt. -%, at least 0.2 wt. -%, or at least 0.5 wt. -%. Upper limits of the amount of TiO2 may for example be at most 2.5 wt. -%, at most 1.5 wt. -%, or at most 1 wt. -%. The glass may for example be free of TiO2.

[0099] Optionally, the glass comprises the following components in the indicated amounts (in wt. -%) :

[0100] Optionally, the glass comprises the following components in the indicated amounts (in wt. -%) :

[0101] The present disclosure also relates to a method of producing a chemically toughened glass arti-cle, in particular a chemically toughened glass article of the present disclosure. The method in particular comprises the following steps in the indicated order:

[0102] ● Providing an (individual) glass article comprising a first main surface and a second main surface and at least one edge surface connecting the first main surface and the second main surface,

[0103] ● Chemically toughening the glass article, and subsequently

[0104] ● Contacting both a center region and a peripheral region of the glass article with an etch-ing solution, wherein the etch rate is higher in the peripheral region as compared to the center region of the article,

[0105] ○ wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,

[0106] ○ wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface.

[0107] In order for both the center region and the peripheral region of the glass article being contacted with an etching solution, the contacting step (etching step) of the present disclosure is per-formed on individual glass articles. “Individual glass articles” are in particular those glass articles that are not present in any kind of layer composite. The entire surface of the glass article should be available for being contacted with the etching solution. This includes in particular also both the first main surface and the second main surface of the glass article in their entirety.

[0108] The contacting step (etching step) being performed on individual glass articles distinguishes the present disclosure from prior art disclosures directed to etching of stacks of glass articles. Such stack etching is generally performed in order to obtain certain chamfer structures at the edge of glass articles. However, such chamfer structures are very different from the advantageous pe-ripheral regions of the present disclosure. While the glass articles of the present disclosure may include chamfer structures as well, they additionally or alternatively have the advantageous pe-ripheral regions described herein.

[0109] For obtaining chamfer structures, it is necessary to perform etching on layer composites. For ex-ample, even if a chamfer structure is to be introduced onto one single glass article only, the glass article has to be provided as part of a layer composite in order to obtain a chamfer struc-ture by etching. In such a case, the glass article is generally laminated between two thick dummy glasses for obtaining a chamfer structure by etching.

[0110] In contrast, for obtaining the glass article of the present disclosure having the advantageous pe-ripheral region as described herein, individual glass articles not part of any kind of layer compo-site are subjected to an etching step.

[0111] In the present disclosure, it was found that an accordingly modified etching and / or edge treat-ment step can benefit the edge strength. It was found that it is advantageous if the etch rate  around the edges is higher than for the center of the glass. The thinning of the etches can in particular be adjusted by finetuning the etching rates, by adjusting for instance etching media, temperature and etching duration. The etching duration may for example be in a range of from 5 seconds to 120 minutes, such as from 30 seconds to 60 minutes, from 1.0 to 30 minutes, from 2.0 to 15 minutes, or from 5.0 to 10 minutes. The etching duration may for example be at least 5 seconds, at least 30 seconds, at least 1.0 minute, at least 2.0 minutes, or at least 5.0 minutes. The etching duration may for example be at most 120 minutes, at most 60 minutes, at most 30 minutes, at most 15 minutes, or at most 10 minutes.

[0112] In some embodiments, the etch rate is higher in the peripheral region as compared to the center region of the glass article by at least 10%, at least 20%, at least 25%, at least 50%, at least 75%, at least 100%, at least 150%, at least 200%, at least 250%, at least 300%, or at least 400%. In some embodiments, the etch rate is higher in the peripheral region as compared to the center region of the glass article by at most 1000%, at most 950%, at most 900%, at most 850%, at most 800%, at most 750%, at most 700%, at most 650%, at most 600%, at most 550%, or at most 500%. In some embodiments, the etch rate is higher in the peripheral region as compared to the center region of the glass article by 10%to 1000%, by 20%to 950%, by 25%to 900%, by 50%to 850%, by 75%to 800%, by 100%to 750%, by 150%to 700%, by 200%to 650%, by 250%to 600%, by 300%to 550%, or by 400%to 500%.

[0113] In some embodiments, the step of contacting both the center region and the peripheral region of the glass article with the etching solution reduces the average thickness of the center region of the glass article by 0.5 to 4 μm and / or reduces the average thickness of the peripheral region of the glass article by 1.5 to 14 μm. In particular, if the etch rate is higher in the peripheral region as compared to the center region of the glass article, the step of contacting both the center re-gion and the peripheral region of the glass article with the etching solution reduces the average thickness of the center region of the glass article less as compared to the reduction of the aver-age thickness of the peripheral region of the glass article. For example, if the average thickness of the center region is reduced by 4 μm, the average thickness of the peripheral region is re-duced by more than 4 μm.

[0114] Optionally, the glasses can be rotated inside the etching solution. The rotation optionally occurs around a central rotation axis, ideally the glasses are placed vertically with the folding axis (of a single fold cover glass) being orthogonal to the rotation axis. By adjusting / matching the etching solution and process temperature (= etching speed or etch rate) and the rotational speed and / or direction the etch rates particularly in the edge regions of the glasses can be manipulated. By doing so, a thinning of the edge region is realized and also the width of the thinned region can be fine-tuned. Alternatively or additionally to rotating the glasses inside the etching solution, a  stirring of the etching solution is also an option to wash the etching solution around the edges of the glasses. Here the direction of rotation can be alternated as well, however, the reverse times are generally longer due to inertia of the etching solution.

[0115] The method may in particular comprise one or more measures selected from the group consist-ing of

[0116] ● Rotating the glass article inside the etching solution,

[0117] ● Bubbling the etching solution, wherein the bubbling is stronger at the peripheral region of the glass article as compared to the center region,

[0118] ● Stirring the etching solution so that the etch rate is higher in the peripheral region as compared to the center region of the article,

[0119] ● Directing a stream of etching solution onto the peripheral region of the glass article, in particular by at least one nozzle present in an etching tank comprising the etching solu-tion, and

[0120] ● Combination of two or more thereof.

[0121] Rotation of the glass article around the rotation axis may be either clockwise or counter-clock-wise or alternating clockwise and counter-clockwise.

[0122] The ratio of the duration of clockwise rotation and the duration of counter-clockwise rotation may for example be in a range of from 1: 3 to 3: 1 such as from 1: 2 to 2: 1, in particular about 1: 1. The ratio of the duration of clockwise rotation and the duration of counter-clockwise rotation may for example be at least 1: 3, at least 1: 2, or at least 1: 1. The ratio of the duration of clock-wise rotation and the duration of counter-clockwise rotation may for example be at most 3: 1, at most 2: 1, or at most 1: 1.

[0123] The rotational speed of the glass article may for example be in a range of from 0.1 to 10.0 rounds per minute (rpm) such as from 0.2 to 5.0 rpm or from 0.5 to 2.0 rpm. The rotational speed of the glass article may for example be at least 0.1 rpm, at least 0.2 rpm, or at least 0.5 rpm. The rotational speed of the glass article may for example be at most 10.0 rpm, at most 5.0 rpm, or at most 2.0 rpm.

[0124] Further, as for the optional rotation of the glasses inside the etching solution, by shifting the bal-ance of one rotational direction to the opposite rotational direction, an additional finetuning of  the process can be achieved in a way that a symmetric or asymmetric chamfer can be intro-duced (here, opposite edges show opposite chamfer directions) . Additionally, for locally slimmed glass (LSG) -glasses that have a thinned area around their folding axis and thicker non-folding areas -thinned edges can have additional benefits for their bending strength per-formance as well as a potential mitigation of wrinkle effects around the slimmed section that stem from uneven expansion upon chemical toughening. In the latter case, such LSG is prefera-bly rotated about its longitudinal axis (orthogonal to the folding axis) . Corresponding embodi-ments are schematically shown in Figure 6.

[0125] Moreover, rotation about the center axis that is orthogonal to the folding axis of the glass article is not only advantageous for LSG but for glass articles in general because the most crucial seg-ments of the peripheral region of the glass article are those being bent during the application. Therefore, it is advantageous to have increased etching at these segments of the peripheral re-gion as compared to segments of the peripheral region of the glass article not being bent during application. By rotating about the longitudinal axis, the segments of the peripheral regions paral-lel to the longitudinal axis are subjected to increased etching. The segments that are parallel to the longitudinal axis may also be referred to as the long sides of the glass article. Generally, it is these long sides that are being bent during the application. In contrast, the short sides are gen-erally not bent during the application.

[0126] In some embodiments, the rotating step comprises rotation of the glass article around a rotation axis, wherein the rotation axis is perpendicular to a folding axis of the glass article. In particular, the rotation axis may be parallel to the long sides of the glass article and the folding axis may be parallel to the short sides of the glass article, or the rotation axis may be parallel the short sides of the glass article and the folding axis may be parallel to the long sides of the glass article.

[0127] In some embodiments, the rotation axis is one of the axes of symmetry of the glass article. In particular, the rotation axis is the axis of symmetry of the glass article that is parallel to the long sides of the glass article.

[0128] In some embodiments, the etching solution is stirred such that it moves around a stirring axis which is parallel to the long sides of the glass article.

[0129] In some embodiments, a stream of etching solution is directed onto the peripheral region of the glass article. The stream of etching solution may be a stream of new etching solution or a stream of already present etching solution or a combination of both. The stream of etching solu-tion may be directed onto the peripheral region of the glass article in particular by at least one  nozzle. For example, new etching solution may be applied from one or more etching tanks com-prising the etching solution and directed onto the peripheral region of the glass article by at least one nozzle. A stream of already present etching solution may be directed onto the peripheral region of the glass article for example by creating a circulation of etching solution, in particular by at least one pump.

[0130] In some embodiments, the method comprises applying measures during etching such as mask-ing areas not to be etched, or dipping the glass article into the etching solution in a bent state. Dipping in a bend state means the glass article is folded and then only the folding area is dipped into the etching solution. The additional slimming of the folding area takes away some of the CS / DoL of the slimmed folding area and results in a more balanced strengthening and expan-sion of this region in comparison to the non-folding region. An additional advantage is the lower thickness of the slimmed areas which is advantageous for folding.

[0131] In some embodiments, the etching solution comprises HF and / or NH4HF2, and additionally an inorganic and / or organic acid. The inorganic acid is in particular selected from the group con-sisting of HCl, HNO3, H2SO4 and mixtures of two or more thereof.

[0132] In more detail, the etchant solution optionally comprises or consists of a mixture of HF and / or NH4HF2 with an inorganic acid (for example HCl, HNO3, H2SO4 or mixtures of two or more thereof) and / or with an organic acid (for example acetic acid) .

[0133] The total amount of HF and NH4HF2 may for example be in range of from 0.1 wt. -%to 10.0 wt. -%such as from 0.5 to 5.0 wt. -%or from 1.0 to 2.0 wt. -%. The total amount of HF and NH4HF2 may for example be at least 0.1 wt. -%, at least 0.5 wt. -%or at least 1.0 wt. -%. The total amount of HF and NH4HF2 may for example be at most 10.0 wt. -%, at most 5.0 wt. -%or at most 2.0 wt. -%.

[0134] The weight ratio of the total amount of inorganic acid to the total amount of HF and NH4HF2 may for example be in a range of from 0.1: 1 to 10: 1 such as from 0.2: 1 to 5: 1 or from 0.5: 1 to 2: 1. The weight ratio of the total amount of inorganic acid to the total amount of HF and NH4HF2 may for example be at least 0.1: 1, at least 0.2: 1 or at least 0.5: 1. The weight ratio of the total amount of inorganic acid to the total amount of HF and NH4HF2 may for example be at most 10: 1, at most 5: 1 or at most 2: 1.

[0135] The weight ratio of the total amount of organic acid to the total amount of HF and NH4HF2 may for example be in a range of from 0.1: 1 to 10: 1 such as from 0.2: 1 to 5: 1 or from 0.5: 1 to 2: 1. The weight ratio of the total amount of organic acid to the total amount of HF and NH4HF2 may for example be at least 0.1: 1, at least 0.2: 1 or at least 0.5: 1. The weight ratio of the total amount  of organic acid to the total amount of HF and NH4HF2 may for example be at most 10: 1, at most 5: 1 or at most 2: 1.

[0136] The etchant solution may for example comprise or consist of 3 wt. -%NH4HF2 and 3 wt. -%HNO3, or the etchant solution may comprise or consist of 2 wt. -%NH4HF2, 2 wt. -%HNO3 and 5 wt. -%acetic acid, or the etchant solution may comprise or consist of 1 wt. -%HF and 1 wt. -%HNO3. The etchant solution may comprise one or more surfactants, for example alkylphenol ethoxylate, or ammonium lauryl sulfate, or mixtures of alkylphenol ethoxylate and ammonium lauryl sulfate.

[0137] The temperature of the etching solution may for example be in a range of from 1℃ to 50℃, from 1℃ to 40℃ such as from 5℃ to 30℃ or from 15℃ to 25℃. The temperature of the etch-ing solution may for example be at least 1℃, at least 5℃, or at least 15℃. The temperature of the etching solution may for example be at most 50℃, at most 40℃, at most 30℃, or at most 25℃.

[0138] In some embodiments, the method further comprises the step of contacting both the center re-gion and the peripheral region of the glass article with an etching solution prior to chemical toughening. The etch rate may be higher in the peripheral region as compared to the center re-gion of the article in the etching step prior to chemical toughening.

[0139] The newly developed method of the invention may follow in its first steps UTG processing steps, including:

[0140] -Stacking of multiple UTG sheets with glue

[0141] -Cutting of blocks of “cells” (cut-to-size) by disc knife

[0142] -Edge grinding and / or polishing (optional)

[0143] -Edge etching (immersing the cut-to-size block into etching solution)

[0144] -Delamination of blocks to individual cells

[0145] -Chemical toughening of cells

[0146] -Washing / cleaning

[0147] In particular, the method of the disclosure may comprise the following steps in the indicated or-der prior to the step of chemical toughening:

[0148] ● Providing a layer composite comprising a plurality of glass articles,

[0149] ● Optionally cutting the layer composite to a desired size,

[0150] ● Optionally edge grinding and / or polishing,

[0151] ● Immersing the layer composite into an etching solution,

[0152] ● Delamination of the layer composite to obtain individual glass articles.

[0153] The layer composite may for example comprise 2 to 30 glass articles, such as 3 to 20 glass arti-cles or 5 to 15 glass articles. The number of glass articles in the layer composite may for exam-ple be at least 2, at least 3, or at least 5. The number of glass articles in the layer composite may for example be at most 30, at most 20, or at most 15.

[0154] In some embodiments, the method of the disclosure comprises the following steps, in particular in the indicated order:

[0155] ● Providing a layer composite comprising a plurality of the glass articles,

[0156] ● Optionally cutting the layer composite to a desired size,

[0157] ● Optionally edge grinding and / or polishing,

[0158] ● Immersing the layer composite into an etching solution,

[0159] ● Delamination of the layer composite to provide individual glass articles,

[0160] ● Optionally contacting both a center region and a peripheral region of the individual glass articles with an etching solution, wherein the etch rate is higher in the peripheral region as compared to the center region of the article

[0161] ○ wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,

[0162] ○ wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface,

[0163] ● Chemically toughening the individual glass articles, and subsequently

[0164] ● Contacting both a center region and a peripheral region of the individual glass articles with an etching solution, wherein the etch rate is higher in the peripheral region as com-pared to the center region of the article,

[0165] ○ wherein the center region is constituted by the parts of the glass article having a  closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,

[0166] ○ wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface.

[0167] The present disclosure also relates to the use of the glass article of the present disclosure, in particular in consumer electronics such as

[0168] ● foldable handheld devices including smartphones, tablets or wearables,

[0169] ● laptops,

[0170] ● monitors, or

[0171] ● display screens.

[0172] The invention in particular relates to the use of the glass article of the present invention in folda-ble smartphones and laptops.

[0173] Description of the Figures

[0174] Figures 1 schematically shows three embodiments of the method of the present disclosure as Figure 1A, 1B, and 1C, respectively. The etching solution is indicated by a dashed pattern throughout Figure 1.

[0175] Figure 1A schematically shows an embodiment of rotating the glass article 11 inside the etching solution. The rotational movement is indicated by two black arrows. The rotation axis 12 is shown as dashed line.

[0176] Figure 1B schematically shows an embodiment of directing a stream of etching solution onto the peripheral region of the glass article 11. This is indicated by black arrows originating from posi-tions of the etching tank in which nozzles 13 are present.

[0177] Figure 1C schematically shows an embodiment of stirring the etching solution. Stirring is indi-cated by two black arrows.

[0178] Figure 2A schematically shows an embodiment of rotating the glass article 21 inside the etching solution. The rotational movement is indicated by two black arrows. The rotation axis 22 is shown as dashed line.

[0179] Figure 2B schematically shows an enlarged depiction of the glass article, wherein the rotation axis 22 is shown as a dashed line and the folding axis 24 is shown as a dotted line. The rotation axis 22 is perpendicular to the folding axis 24 of the glass article.

[0180] Figure 2C also schematically shows an enlarged depiction of the glass article. Figure 2C indi-cates that the glass article has two parallel long sides 25, and two parallel short sides 26, wherein the long sides 25 are oriented perpendicular to the short sides 26. The length of the long sides 25 is larger than the length of the short sides 26.

[0181] Figures 2B and 2C schematically show that the rotation axis 22 is parallel to the long sides 25 of the glass article and the folding axis 24 is parallel to the short sides 26 of the glass article.

[0182] Figure 3 schematically shows a glass article of the disclosure having a center region 31 and a peripheral region 32. The average thickness of the peripheral region 32 is lower than the aver-age thickness of the center region 31 as indicated by the darker coloration of the peripheral re-gion 32 as compared to the center region 31.

[0183] Figure 4 shows an image of a glass article of the disclosure. The average thickness of the pe-ripheral region is lower than the average thickness of the center region. The image was taken with the glass lying flat under a uniform light source. The principal is same as Newton’s rings. It’s showing the interference fringes of the lights reflected by the top and bottom surface of the glass. The lines could be considered as thickness contour lines. Denser distributed lines are in-dicating a steeper change of thickness.

[0184] Figure 5 schematically shows the setup of the sliding test. A glass article 51 is tested in the slid-ing test with a folding distance 56 equal to fifty times the center thickness of the glass article 51. For ultrathin glass (UTG) , the center thickness of the glass article 51 corresponds to the aver-age thickness of the center region of the glass article 51. For locally slimmed glass (LSG) , the center thickness of the glass article 51 corresponds to the average thickness in the folding area of the center region. In the sliding test, the foldable glass is placed as a U-shape between two parallel plates 52, 53. The two plates 52, 53 are big enough to cover the whole article 51. Then one of the plates (here 53) moves towards the other one (here 52) while remaining parallel with a speed of 60 mm / min (movement indicated by arrow heads 55) until the designed folding dis-tance 56 of fifty times the center thickness is reached. The folding distance 56 is defined as the distance of the two plates 52, 53. When the folding distance 56 is reached, the moving plate (here 52) starts to move back and forth along the article length direction with a speed of 10 mm / sand a travel distance of 10 mm as indicated by double-arrow 54. In case the foldable arti-cle 51 survived 10 times of sliding without glass breakage, it is considered as passing the test.

[0185] Figure 6 schematically shows glass articles of the present invention, embodied as locally slimmed glass (LSG) in Figure 6A, or as ultrathin glass (UTG) in Figure 6B, respectively. The depiction is similar to the depiction of Figure 3. Thus, a lower thickness is indicated by darker coloration. In contrast to the embodiments depicted in Figure 3, the embodiments depicted in Figures 6A and 6B have a further reduced thickness of the peripheral regions in areas around the folding axis.

[0186] Figure 6A shows a glass article of the disclosure having a thinned area around its folding axis and thicker non-folding areas. In Figure 6A this holds true both for the central region and the pe-ripheral region of the glass article. The central region of the glass article has a thinned area 61b and thicker areas 61a. Likewise, the peripheral region of the glass article has thinned portions 62b and thicker portions 62a.

[0187] Figure 6B shows a glass article of the disclosure. The peripheral region of the glass article has a thinned area around its folding axis. In contrast to the embodiment of Figure 6A, the embodi-ment of Figure 6B does not include thinned areas of the central region 71. The central region 71 of the glass article does not have a thinned area. However, the peripheral region of the glass article has thinned portions 72b and thicker portions 72a.Examples

[0188] Preparation of the examples of the present disclosure included the following steps in the indi-cated order:

[0189] ● Providing glass articles,

[0190] ● Stacking of the glass articles to obtain a layer composite,

[0191] ● Dicing and CNC grinding to the target size,

[0192] ● Chamfer shaping by etching of the stack (i.e. the layer composite) ,

[0193] ● Delamination to obtain single (individual) glass articles,

[0194] ● Pre-etching of the single glass articles (Examples 2, 4, and 6 only) ,

[0195] ● Chemical strengthening,

[0196] ● Post-etching of the single glass articles (Examples 1-6 and 10 only) .

[0197] All examples were based on chemically toughened aluminosilicate glass. All samples had a  comparable chamfer structure including a chamfer height of 10-12 μm and a chamfer width of 40-60 μm.

[0198] Examples 7 to 9 were not etched. The etching of Examples 1 to 6 and 10 was done with a mix-ture of 1-5 wt. %HNO3 + 1-5 wt. %HF. The same mixture and setup were applied for pre-etching and post-etching. “Pre-Etching” refers to an etching step prior to chemical toughening. “Post-Etching” refers to an etching step subsequent to chemical toughening. Both pre-etching and post-etching were done on individual glass articles (not on stacks of glass articles) with in-creased etching speed in the peripheral region of the glass articles as compared to the center region thereof. For Examples 1 to 6, etching was done with an increased etching speed around the edges. In Example 10 there was no increased etching speed around the edges.

[0199] The sample size was n = 50. Thus, 50 samples were used for each test. 2PB, P2C and sliding are destructive tests. Therefore, different sets of 50 samples were used for each of these tests.

[0200] The results are shown in the following tables.

[0201] Table 1

[0202] Table 2

[0203] CS and DoL indicate final CS and DoL values subsequent to all etching steps applied.

[0204] The term “yes*” for post-etching of Example 10 indicates that post-etching was done, however, not with an increased etching speed around the edges in contrast to Examples 1 to 6. Conse-quently, the average thickness of the center region is equal to the average thickness of the pe-ripheral region for Example 10. In contrast, the average thickness of the peripheral region is smaller than the average thickness of the center region for Examples 1 to 6. The average thick-ness was determined as indicated further below.

[0205] The indicated properties of the examples were tested as indicated in the following.

[0206] Average thickness of center region and peripheral region

[0207] Average thickness of center region and average thickness of peripheral region were determined as follows.

[0208] Peripheral region: micrometer was used to measure the thickness along the line 2.5 mm away from the outline towards the center. One measurement was done for every 1 cm length of the outline. Then the average thickness was calculated based on the measurements.

[0209] Center region: micrometer was used to measure the thickness within the area more than 5 mm away from the outline towards the center. One measurement was done for every 1 cm2 of the area. Then the average thickness was calculated based on the measurements.

[0210] 2PB Test

[0211] The 2-point-bending (2PB) test was performed as follows.

[0212] In the test, the glass article was placed as a U-shape between two parallel plates. The two plates were big enough to cover the whole glass article. Then one of the plate moved towards the other one while remaining parallel with a speed of 60 mm / min until the designed folding dis-tance of fifty times the center thickness was reached. The folding distance is defined as the dis-tance of the two plates. In case the foldable article survived when the folding distance is reached, it was considered as passing the test. For ultrathin glass (UTG) , the center thickness of the glass article corresponds to the average thickness of the center region of the glass article. For locally slimmed glass (LSG) , the center thickness of the glass article corresponds to the av-erage thickness in the folding area of the center region. The passing rate is the number of sam-ples passed divided by the number of total measured samples.

[0213] P2C ratio

[0214] To evaluate the breakage origin of the glasses in the 2PB test, example glasses were double-side laminated with polymer films, that were 5 mm bigger than the glass in terms of length and width. The adhesion between the glass and the polymer films was electrostatic. The material of the film was PE. Each side of the glass was laminated with a single layer of the polymer that was 50 μm thick. By doing so, fractures and shards were captured in the coating and the point of origin could be analyzed by the weblike crack structure.

[0215] In this analysis, it was found that glasses processed by the method of the present invention show more breakage origins stemming from the center of the glass than from its edges. When calculated as periphery-to-center breakage ratio (P2C) , examples 1-6 had P2C ratios in a range of from 6%to 13%, whereas examples 7-10 had P2C ratios in a range of from 47%to 63%. The P2C ratio indicates the percentage of breakage origins stemming from the peripheral region as compared to the total number of breakages. The P2C ratio is calculated based on the following formula:

[0216] In this respect, the term “periphery” refers to the peripheral region of the glass article which is constituted by the parts of the glass article having a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface. Likewise, the term “center” refers to the center region of the glass article which is constituted by the parts of the glass arti-cle having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface.

[0217] Sliding Test

[0218] The glasses further were tested in a sliding test with a folding distance equal to 50 times the center thickness (referring to the center thickness, as above with respect to P2C ratio) of the glass article. In this test, the foldable glass is placed as a U-shape between two parallel plates. The two plates are big enough to cover the whole article. Then one of the plates moves towards the other one while remaining parallel with a speed of 60 mm / min until the designed folding dis-tance of 50 times the center thickness is reached. The folding distance is defined as the dis-tance of the two plates. When the folding distance is reached, the moving plate starts to move back and forth along the article length direction with a speed of 10 mm / sand a travel distance of 10 mm. In case the foldable article survived 10 times of sliding without glass breakage, it is con-sidered as passing the test.

Claims

1.Chemically toughened glass article comprising a first main surface and a second main sur-face and at least one edge surface connecting the first main surface and the second main surface,· wherein the glass article has a center region and a peripheral region, wherein first and second main surface are essentially parallel to each other in the center region,ο wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,ο wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface,· wherein the average thickness of the center region is at most 200 μm,· wherein the ratio of the average thickness of the peripheral region and the average thickness of the center region is in a range of from 75%to 99%,· wherein the average thickness of the peripheral region is measured as the average thickness along the perimeter line having a distance of 2.5 mm to the edge surface measured parallel to the first or second main surface.2.Chemically toughened glass article of claim 1, wherein the average thickness of the periph-eral region is lower than the average thickness of the center region by 1.0 μm to 10.0 μm, such as 1.0 to 7.0 μm, 1.0 to 5.0 μm or 1.0 to 3.0 μm.3.Chemically toughened glass article of at least one of the preceding claims, wherein the cen-ter region comprises a folding area and a non-folding area, wherein the average thickness of the center region in the folding area is lower than the average thickness of the center re-gion in the non-folding area.4.Chemically toughened glass article of at least one of the preceding claims, wherein the pe-ripheral region comprises a folding area and a non-folding area, wherein the average thick-ness of the peripheral region in the folding area is lower than the average thickness of the peripheral region in the non-folding area.5.Chemically toughened glass article of at least one of the preceding claims,· wherein the center region comprises a folding area and a non-folding area, wherein the average thickness of the center region in the folding area is lower than the average thickness of the center region in the non-folding area,· wherein the peripheral region comprises a folding area and a non-folding area, wherein the average thickness of the peripheral region in the folding area is lower than the aver-age thickness of the peripheral region in the non-folding area, and· wherein the average thickness of the folding area of the peripheral region is lower than the average thickness of the folding area of the center region by 1.0 μm to 10.0 μm.6.Chemically toughened glass article of at least one of the preceding claims,· wherein the center region comprises a folding area and a non-folding area, wherein the average thickness of the center region in the folding area is lower than the average thickness of the center region in the non-folding area,· wherein the peripheral region comprises a folding area and a non-folding area, wherein the average thickness of the peripheral region in the folding area is lower than average thickness of the peripheral region in the non-folding area, and· wherein the ratio of the average thickness of the folding area of the peripheral region in a closest distance of 2.5 mm to the edge surface measured parallel to the first or second main surface and the average thickness of the folding area of the center region is in a range of from 75%to 99%.7.Chemically toughened glass article of at least one of the preceding claims, wherein the glass article has a periphery-to-center breakage ratio of at most 45%.8.Chemically toughened glass article of at least one of the preceding claims, wherein the arti-cle is foldable.9.Chemically toughened glass article of at least one of the preceding claims, wherein the sur-face compressive stress at the first and / or second main surface is in a range of from 300 to 1500 MPa.10.Chemically toughened glass article of at least one of the preceding claims, wherein the depth of layer at the first and / or second main surface is in a range of from 0.5 to 40 μm.11.Chemically toughened glass article of at least one of the preceding claims, wherein the passing rate of the glass article in a sliding test with a folding distance of 50 times the cen-ter thickness of the glass article, with a plate speed of 10 mm / s and with a plate travel dis-tance of 10 mm is more than 50%, wherein the center thickness of the glass article corre-sponds to the average thickness of the center region of the glass article, or, if the center re-gion comprises a folding area and a non-folding area, to the average thickness of the fold-ing area of the center region.12.Chemically toughened glass article of at least one of the preceding claims, wherein the passing rate of the glass article in a 2-point-bending test of at least 65%with a folding dis-tance of 50 times the center thickness of the glass article, wherein the center thickness of the glass article corresponds to the average thickness of the center region of the glass arti-cle, or, if the center region comprises a folding area and a non-folding area, to the average thickness of the folding area of the center region.13.Chemically toughened glass article of at least one of the preceding claims, wherein the av-erage thickness of the center region is in a range of from 20 μm to 80 μm.14.Chemically toughened glass article of at least one of the preceding claims, wherein the arti-cle has a length y and a width z and wherein the ratio of length y and width z of the article is 1∶ 1 or more.15.Chemically toughened glass article of at least one of the preceding claims, wherein the glass article is axially symmetric.16.Chemically toughened glass article of at least one of the preceding claims, wherein the glass article comprises one axis of symmetry or more.17.Chemically toughened glass article of at least one of the preceding claims, wherein the glass comprises the following components in the indicated amounts (in wt.-%) : 18.Method of producing a chemically toughened glass article of at least one of the preceding claims, the method comprising the following steps in the indicated order:· Providing a glass article comprising a first main surface and a second main surface and at least one edge surface connecting the first main surface and the second main sur-face,· Chemically toughening the glass article, and subsequently· Contacting both a center region and a peripheral region of the glass article with an etch-ing solution, wherein the etch rate is higher in the peripheral region as compared to the center region of the article,ο wherein the center region is constituted by the parts of the glass article having a closest distance to the edge surface of more than 5.0 mm measured parallel to the first or second main surface,ο wherein the peripheral region is constituted by the parts of the glass article hav-ing a closest distance to the edge surface of at most 5.0 mm measured parallel to the first or second main surface.19.Method of claim 18, wherein the etch rate is higher in the peripheral region as compared to the center region of the glass article by at least 10%.20.Method of at least one of claims 18 and 19, wherein the step of contacting both the center region and the peripheral region of the glass article with the etching solution reduces the average thickness of the center region of the glass article by 0.5 to 4 μm and / or reduces the average thickness of the peripheral region of the glass article by 1.5 to 14 μm.21.Method of at least one of claims 18 to 20, wherein the method comprises one or more measures selected from the group consisting of · Rotating the glass article inside the etching solution,· Bubbling the etching solution, wherein the bubbling is stronger at the peripheral region of the glass article as compared to the center region,· Stirring the etching solution so that the etch rate is higher in the peripheral region as compared to the center region of the article,· Directing a stream of etching solution onto the peripheral region of the glass article, in particular by at least one nozzle present in an etching tank comprising the etching solu-tion, and· Combination of two or more thereof.22.Method of claim 21, wherein the rotating step comprises rotation of the glass article around a rotation axis, wherein the rotation axis is perpendicular to a folding axis of the glass arti-cle.23.Method of at least one of claims 21 and 22, wherein the rotation axis is parallel to the long sides of the glass article and the folding axis is parallel to the short sides of the glass article or wherein the rotation axis is parallel the short sides of the glass article and the folding axis is parallel to the long sides of the glass article.24.Method of at least one of claims 21 to 23, wherein the rotation axis is one of the axes of symmetry of the glass article.25.Method of at least one of claims 21 to 24, wherein the rotation axis is the axis of symmetry of the glass article that is parallel to the long sides of the glass article.26.Method of at least one of claims 21 to 25, wherein the rotation of the article around the rota-tion axis is either clockwise or counter-clockwise or alternating clockwise and counter-clock-wise.27.Method of claim 26, wherein the ratio of the duration of clockwise rotation and the duration of counter-clockwise rotation is in a range of from 1∶ 3 to 3∶ 1.28.Method of at least one of claims 21 to 27, wherein the rotational speed is in a range of from 0.1 to 10.0 rounds per minute.29.Method of at least one of claims 21 to 28, wherein the etching solution is stirred such that it moves around a stirring axis which is parallel to the long sides of the glass article.30.Method of at least one of claims 18 to 29, wherein the etching solution comprises HF and / or NH4HF2, and additionally an inorganic and / or organic acid.31.Method of claim 30, wherein the inorganic acid is selected from the group consisting of HCl, HNO3, H2SO4 and mixtures of two or more thereof.32.Method of at least one of claims 18 to 31, wherein the temperature of the etching solution is in a range of from 1℃ to 50℃.33.Method of at least one of claims 18 to 32, wherein the method further comprises the step of contacting both the center region and the peripheral region of the glass article with an etch-ing solution prior to chemical toughening.34.Method of claim 33, wherein in the etching step prior to chemical toughening the etch rate is higher in the peripheral region as compared to the center region of the article by at least 10%.35.Method of at least one of claims 18 to 34, wherein the method further comprises the follow-ing steps in the indicated order prior to the step of chemical toughening:· Providing a layer composite comprising a plurality of glass articles,· Optionally cutting the layer composite to a desired size,· Optionally edge grinding and / or polishing,· Immersing the layer composite into an etching solution,· Delamination of the layer composite to obtain individual glass articles.36.Method of claim 35, wherein the layer composite comprises 2 to 30 glass articles.37.Use of a glass article of at least one of claims 1 to 17 in consumer electronics such as· foldable handheld devices including smartphones, tablets or wearables,· laptops,· monitors, or· display screens.

Citation Information

Patent Citations

  • Visibility Improvement Flexible Cover Window

    CN111833735A

  • Slim fold-up type electromotive window with window frame which has only one machine devices guidehole opening

    KR1020220167458A

  • Prefabricated multifunctional fence system

    KR102620743B1

  • Positive electrode active material for secondary battery, and lithium secondary battery comprising the same

    KR102725846B1

  • Ultrathin glass with special chamfer shape and high strength

    US20210078899A1