Electrochemical apparatus and electronic apparatus
By setting the protrusion of the recessed accommodating electrode assembly on the housing encapsulation layer of the electrochemical device, uniform stress and fixation are achieved, and the electrode interface deterioration and safety problems caused by uneven surface of the bare core are solved, and the cycle life and Energy density.
Patent Information
- Application Number
- PCT/CN2023/096914
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-12-05
AI Technical Summary
The surface of the bare battery cell is uneven due to the welding of the electrode ears and the uneven force is applied when the pressure is applied, which can easily lead to deterioration of the electrode interface, precipitation of lithium dendrites and explosive fire, which is difficult to effectively solve the problem in the existing technology.
The housing encapsulation layer of the electrochemical device is provided with depressions to accommodate the protrusions on the surface of the electrode assembly to ensure uniform stress, and through the bonding strength and structural design of the encapsulation layer, the electrode assembly is fixed to prevent twitching and breaking.
It improves the cycle life and safety of the electrochemical device, avoids the risk of electrode interface deterioration and fire explosion, and at the same time improves the energy density and reduces the dependence on the additional buffer structure.
Smart Images

Figure CN2023096914_05122024_PF_FP_ABST
Abstract
Description
Electrochemical device and electronic device Technical Field
[0001] The present application relates to the field of energy storage technology, and in particular to an electrochemical device and an electronic device. Background Art
[0002] Secondary batteries are widely used in consumer electronics, and in recent years, the end market has increasingly demanded higher lifespans and higher energy density. Currently, there are two mainstream packaging formats for secondary batteries: soft-pack and metal-shell packaging. Soft-pack secondary batteries are widely used due to their safety, high specific energy, and flexible design.
[0003] Before use, secondary batteries (such as lithium-ion batteries) require a formation treatment. This involves the initial charge and discharge of the secondary battery to form an electrolyte interface film on the surface of the electrode material. This electrolyte interface film effectively prevents further loss of electrolyte and provides excellent ionic conductivity, electronic insulation, thermal stability, and chemical stability, significantly impacting the subsequent performance of the secondary battery. Applying pressure during the formation treatment is an effective means of improving production efficiency and enhancing the performance of the electrode interface.
[0004] Summary of the Invention
[0005] However, the inventors of this application have discovered that the surface of a bare cell is uneven and has a concave-convex morphology due to the presence of structures such as tab welding. When pressure is applied for a formation process, the surface of the bare cell is subjected to uneven force, which can easily lead to deterioration of the electrode interface, precipitation of lithium dendrites, and even fire and explosion. In view of the above-mentioned problems in the prior art, this application provides an electrochemical device and an electronic device to improve the flatness of the surface of the electrochemical device, thereby improving the electrode interface formed by the electrochemical device during the pressurized formation process, and improving the cycle life and safety of the electrochemical device.
[0006] In a first aspect of the present application, an electrochemical device is provided, comprising an electrode assembly and a shell, wherein the electrode assembly is accommodated in the shell, the shell comprising a packaging layer, a side surface of the electrode assembly having a protrusion, a side surface of the packaging layer adjacent to the electrode assembly having a recess, and the protrusion being at least partially accommodated in the recess.
[0007] The present application provides a depression in the packaging layer of the electrochemical device shell, and the depression accommodates the protrusions on the surface of the electrode assembly, so that when the electrochemical device is subjected to a pressurized formation treatment, each position on the surface of the electrode assembly can be uniformly stressed, thereby avoiding the deterioration of the electrode interface due to the concentration of pressure on the protruding parts of the electrode assembly surface, and further causing the precipitation of lithium dendrites and fire and explosion. On the other hand, the depression of the packaging layer can also limit and fix the electrode assembly in the shell, and when the electrochemical device falls or is hit, it can effectively suppress the movement of the electrode assembly and reduce the risk of the shell being broken. In summary, the solution of the present application is conducive to improving the cycle life and safety performance of the electrochemical device. In addition, since the electrochemical device of the present application does not require the addition of an additional buffer structure, such as a silicone pad, it can achieve uniform force on the electrode assembly during pressurized formation, and therefore, it is also conducive to improving the energy density of the electrochemical device.
[0008] In some embodiments, the protrusion is completely contained within the depression. This can further promote uniform stress on the surface of the electrode assembly during pressurized formation treatment, improve the electrode interface, and thus increase the cycle life and safety of the electrochemical device.
[0009] In some embodiments, the surface of the encapsulation layer facing away from the electrode assembly is flat. This can further promote uniform stress distribution across the surface of the electrode assembly during pressurized formation of the electrochemical device, improve the electrode interface, and thus enhance the cycle life and safety of the electrochemical device.
[0010] In some embodiments, the melting point of the encapsulation layer is 80° C. to 150° C. This is beneficial for encapsulating the housing and forming a recess on the inner surface of the encapsulation layer.
[0011] In some embodiments, the material of the encapsulation layer includes a thermoplastic polymer.
[0012] In some embodiments, the material of the encapsulation layer includes at least one of polyethylene, polypropylene, ethylene-propylene copolymer, anhydride-modified polypropylene, polyvinyl chloride, polyvinyl acetate, polyvinylidene fluoride, or derivatives thereof.
[0013] In some embodiments, the depth of the recess is 3 μm to 150 μm.
[0014] In some embodiments, the thickness of the packaging layer in the recess is 15 μm to 200 μm, thereby increasing the structural strength of the packaging layer in the recess and improving the reliability of the housing.
[0015] In some embodiments, the encapsulation layer further includes a body region adjacent to the recess, and the body region has a thickness of 20 μm to 250 μm.
[0016] In some embodiments, the bond strength between the encapsulation layer and the electrode assembly is greater than or equal to 2 N / m. This further enhances the securing effect of the housing on the electrode assembly, inhibiting movement of the electrode assembly when the electrochemical device is dropped or impacted, reducing the risk of the housing being breached, and improving the safety of the electrochemical device.
[0017] In some embodiments, the electrode assembly includes a pole piece and a pole tab, the electrode assembly includes a pole tab connection area, the pole tab is connected to the pole piece in the pole tab connection area, and the protrusion is located in the pole tab connection area.
[0018] In some embodiments, the electrode assembly is a wound structure including a main body and corner portions, and a maximum thickness difference of the electrochemical device at the main body is less than or equal to 20 μm.
[0019] In some embodiments, the casing further includes a barrier layer, and the barrier layer is located on a surface of the packaging layer facing away from the electrode assembly.
[0020] In some embodiments, the barrier layer has a thickness of 0.1 μm to 50 μm.
[0021] In some embodiments, the material of the barrier layer includes at least one of metal, inorganic oxide, or inorganic nitride.
[0022] In some embodiments, the housing further includes a protective layer, and the protective layer is located on a surface of the barrier layer facing away from the encapsulation layer.
[0023] In some embodiments, the protective layer has a thickness of 2 μm to 50 μm.
[0024] In some embodiments, the protective layer includes at least one of a polymer or a fiber.
[0025] In some embodiments, the metal includes at least one of aluminum, copper, iron, titanium, or nickel.
[0026] In some embodiments, the inorganic oxide includes at least one of titanium dioxide, aluminum oxide, hafnium dioxide, silicon dioxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, zinc oxide, tin oxide, zirconium titanium oxide, or vanadium oxide.
[0027] In some embodiments, the inorganic nitride includes at least one of silicon nitride, silicon oxynitride, boron nitride, titanium nitride, or aluminum nitride.
[0028] A second aspect of the present application provides an electronic device comprising the aforementioned electrochemical device. Thus, the electronic device of the present application has a good service life and safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] FIG1 shows a cross-sectional view of the electrochemical device of the present application.
[0030] FIG2 shows an enlarged view of area A in FIG1 . DETAILED DESCRIPTION
[0031] To make the purpose, technical solutions, and advantages of this application more clear, the technical solutions of this application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of this application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of this application. The embodiments of this application should not be interpreted as limiting this application.
[0032] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0033] In the description herein, unless otherwise specified, “above” and “below” include the number itself.
[0034] Unless otherwise specified, the terms used in this application have the commonly understood meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0035] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0036] 1. Electrochemical Device
[0037] An embodiment of the present application provides an electrochemical device, comprising an electrode assembly and a shell, wherein the electrode assembly is accommodated in the shell, the shell comprising a packaging layer, a side surface of the electrode assembly having a protrusion, a side surface of the packaging layer adjacent to the electrode assembly having a recess, and the protrusion being at least partially accommodated in the recess.
[0038] In the electrochemical device of the present application, the depression can accommodate the protrusions on the surface of the electrode assembly, so that when the electrochemical device is subjected to a pressurized formation treatment, each position on the surface of the electrode assembly can be uniformly stressed, thereby avoiding the deterioration of the electrode interface due to the concentration of pressure on the protruding parts of the surface of the electrode assembly, thereby causing lithium dendrite precipitation and fire and explosion. On the other hand, the depression of the encapsulation layer can also play a limiting and fixing role on the electrode assembly in the shell, and when the electrochemical device falls or is hit, it can effectively suppress the movement of the electrode assembly and reduce the risk of the shell being broken. In summary, the solution of the present application is conducive to improving the cycle life and safety performance of the electrochemical device. In addition, since the electrochemical device of the present application does not require the addition of an additional buffer structure, such as a silicone pad, it can achieve uniform force on the electrode assembly during pressurized formation, and therefore, it is also conducive to improving the energy density of the electrochemical device.
[0039] In some embodiments, the protrusion is completely contained within the depression. This can further promote uniform stress on the surface of the electrode assembly during pressurized formation treatment, improve the electrode interface, and thus enhance the cycle life and safety of the electrochemical device.
[0040] In some embodiments, the surface of the encapsulation layer facing away from the electrode assembly is flat. This further promotes uniform stress distribution across the surface of the electrode assembly during pressurized formation of the electrochemical device, improves the electrode interface, and thereby enhances the cycle life and safety of the electrochemical device.
[0041] In some embodiments, the encapsulation layer is made of a thermoplastic polymer. When the housing is thermally encapsulated, the encapsulation layer can be heated and melted to form a connection, thereby sealing the electrode assembly in the housing to form an electrochemical device. At the same time, by subjecting the surface of the electrochemical device to a heat-pressing treatment, the encapsulation layer can be softened by the heat. Under the action of pressure, the surface of the encapsulation layer in contact with the protrusion forms a depression, thereby accommodating the protrusion in the depression, thereby improving the uniformity of force applied to the surface of the electrode assembly during the pressurized formation treatment of the electrochemical device. Furthermore, the softened encapsulation layer can be tightly bonded to the surface of the electrode assembly, inhibiting the movement of the electrode assembly when the electrochemical device is dropped or impacted, reducing the risk of the housing being ruptured, and further improving the safety of the electrochemical device.
[0042] In some embodiments, the material of the encapsulation layer includes at least one of polyethylene, polypropylene, ethylene-propylene copolymer, anhydride-modified polypropylene, polyvinyl chloride, polyvinyl acetate, polyvinylidene fluoride, or derivatives thereof.
[0043] In some embodiments, the melting point of the encapsulation layer is 80°C to 150°C. This facilitates encapsulation of the housing and formation of a recessed inner surface of the encapsulation layer. Exemplarily, the melting point of the encapsulation layer is 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or a range consisting of any two of the foregoing values.
[0044] In some embodiments, the depth of the recess is 3 μm to 150 μm. For example, the depth of the recess is 3 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, or a range consisting of any two of the foregoing values.
[0045] It is understood that the depth of the depression is related to the height of the protrusion on the surface of the electrode assembly. For example, if the height of the protrusion on the surface of the electrode assembly is h and the depth of the depression is d, then the following condition is satisfied: 0.5h≤d≤h.
[0046] In some embodiments, the thickness of the packaging layer in the recess is 15μm to 200μm. It is understandable that the thickness of the packaging layer in the recess is within the above range. On the one hand, it can ensure the structural strength of the packaging layer in the recess and the reliability of the shell; on the other hand, it is also conducive to forming a lightweight electrochemical device and improving the energy density of the electrochemical device. Exemplarily, the thickness of the packaging layer in the recess is 15μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm or a range consisting of any two of the above values.
[0047] In some embodiments, the encapsulation layer further includes a body region adjacent to the recess, and the body region has a thickness of 20 μm to 250 μm. Exemplarily, the body region has a thickness of 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, or a range consisting of any two of the foregoing values.
[0048] It is understood that in some embodiments, the thickness of the main region is equal to the sum of the depth of the recess and the thickness of the encapsulation layer in the recess. This can further improve the uniformity of force applied to the electrode assembly surface during pressurized formation processing of the electrochemical device, improve the electrode interface, and thus enhance the cycle life and safety of the electrochemical device.
[0049] In some embodiments, the bond strength between the encapsulation layer and the electrode assembly is greater than or equal to 2 N / m. It is understood that the bond between the encapsulation layer and the electrode assembly can further enhance the securing effect of the housing on the electrode assembly, thereby suppressing movement of the electrode assembly when the electrochemical device is dropped or impacted, reducing the risk of the housing being breached, and further improving the safety of the electrochemical device.
[0050] In some embodiments, the electrode assembly includes a pole piece and a pole tab, the electrode assembly includes a pole tab connection area, the pole tab is connected to the pole piece in the pole tab connection area, and the protrusion is located in the pole tab connection area.
[0051] In some embodiments, the electrode assembly has a wound structure including a main body and corner portions, and the maximum thickness difference of the electrochemical device in the main body is less than or equal to 20 μm. It is understood that a thickness difference in the main body of the electrochemical device within the above range is beneficial for improving the uniformity of force applied to the surface of the electrode assembly during pressurized formation processing of the electrochemical device, thereby improving the electrode interface and enhancing the cycle life and safety of the electrochemical device.
[0052] In some embodiments, the housing further comprises a barrier layer, the barrier layer being located on a surface of the encapsulation layer facing away from the electrode assembly, and the thickness of the barrier layer being 0.1 μm to 50 μm. Exemplarily, the thickness of the barrier layer is 0.1 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, or a range consisting of any two of the foregoing values. It is understood that the thickness of the barrier layer within the foregoing range is beneficial in preventing water vapor and the like from penetrating into the housing and affecting the normal use of the electrochemical device.
[0053] In some embodiments, the material of the barrier layer includes at least one of metal, inorganic oxide, or inorganic nitride.
[0054] In some embodiments, the metal material includes, but is not limited to, at least one of aluminum, copper, iron, titanium, or nickel.
[0055] In some embodiments, the inorganic oxide material includes at least one of titanium dioxide, aluminum oxide, hafnium dioxide, silicon dioxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, zinc oxide, tin oxide, zirconium titanium oxide, or vanadium oxide.
[0056] In some embodiments, the inorganic nitride material includes at least one of silicon nitride, silicon oxynitride, boron nitride, titanium nitride, or aluminum nitride.
[0057] In some embodiments, the housing further includes a protective layer, and the protective layer is located on a surface of the barrier layer facing away from the encapsulation layer.
[0058] In some embodiments, the thickness of the protective layer is 2 μm to 50 μm. Exemplarily, the thickness of the protective layer is 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, or a range consisting of any two of the foregoing values. It is understood that the thickness of the protective layer within the foregoing range is beneficial for preventing external structures from damaging the housing and affecting the normal use of the electrochemical device.
[0059] In some embodiments, the protective layer includes at least one of a polymer or a fiber.
[0060] The electrochemical devices of the present application include, but are not limited to, all types of primary or secondary batteries. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0061] 2. Electronic Devices
[0062] An embodiment of the present application further provides an electronic device comprising the electrochemical device of the aforementioned embodiment.
[0063] The electronic devices of this application include but are not limited to: mobile phones, laptops, tablet computers, drones, smart watches, smart bracelets, VR glasses, electric cars or power tools, etc.
[0064] 3. Preparation Method of Electrochemical Device
[0065] An embodiment of the present application also provides a method for preparing an electrochemical device, which is used to prepare the electrochemical device of the aforementioned embodiment, including: step 1, preparing an electrode assembly; step 2, wrapping the electrode assembly with a packaging layer, and heat-sealing the openings of the packaging layer; step 3, using a heating mold with a flat surface, heating and pressurizing the packaging layer on the surface of the electrode assembly to form depressions on the protrusions of the packaging layer facing the surface of the electrode assembly; step 4, injecting electrolyte, and obtaining the electrochemical device of the present application through processes such as standing, pressurized formation, and degassing.
[0066] In some embodiments, the heat sealing temperature in step 2 is 80° C. to 150° C. Exemplarily, the heat sealing temperature is 80° C., 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., 115° C., 120° C., 125° C., 130° C., 135° C., 140° C., 145° C., 150° C., or a range consisting of any two of the foregoing values.
[0067] It is understood that the heating temperature of the heating and pressurizing treatment in step 3 can soften the encapsulation layer. In some embodiments, the heating temperature of the heating and pressurizing treatment in step 3 is less than the melting point of the encapsulation layer, so that the risk of local film rupture when the encapsulation layer is subjected to heating and pressurizing treatment can be reduced. In some embodiments, the heating temperature of the heating and pressurizing treatment in step 3 is 80°C to 150°C. In some embodiments, the pressure of the heating and pressurizing treatment in step 3 is 0.1MPa to 1MPa. Exemplarily, the heating temperature of the heating and pressurizing treatment is 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C or a range consisting of any two of the above values. The pressure of the heating and pressurizing treatment is 0.1MPa, 0.2MPa, 0.4MPa, 0.5MPa, 0.7MPa, 0.9MPa, 1MPa or a range consisting of any two of the above values.
[0068] In some embodiments, the method for preparing an electrochemical device further includes: step 5, forming a barrier layer on a surface of the encapsulation layer facing away from the electrode assembly. The barrier layer may be formed by at least one of coating, spraying, deposition, evaporation, or vapor deposition.
[0069] In some embodiments, the method for preparing an electrochemical device further includes: step 6, forming a protective layer on a surface of the barrier layer facing away from the encapsulation layer. The process of forming the protective layer includes at least one of coating, spraying, dipping, or winding.
[0070] Hereinafter, the electrochemical device of the present application will be further described with reference to specific embodiments and comparative examples, taking a lithium-ion battery as an example.
[0071] Examples and Comparative Examples
[0072] Example 1
[0073] 1. Preparation of negative electrode sheet: Mix the negative electrode active material graphite, conductive carbon black (Super P), and styrene-butadiene rubber (SBR) in a weight ratio of 96:1.5:2.5, add deionized water as a solvent, and prepare a slurry with a solid content of 0.7, and stir evenly. The slurry is evenly coated on the negative electrode current collector copper foil. The weight of the active material on the sheet is 95g / m 2 . Dry at 110℃ to obtain a negative electrode sheet coated on one side. Then, complete these steps on the back of the sheet in exactly the same way to obtain a negative electrode sheet coated on both sides. Then, cold press the negative electrode sheet to 1.7g / cm 3 The compaction density is achieved by cutting and welding the tabs to obtain the negative electrode sheet.
[0074] 2. Preparation of positive electrode sheet: Mix the positive electrode active material lithium cobalt oxide, conductive carbon black (Super P), and polyvinylidene fluoride (PVDF) in a weight ratio of 97.5:1.0:1.5, add N-methylpyrrolidone (NMP) as a solvent, and prepare a slurry with a solid content of 0.75, and stir evenly. The slurry is evenly coated on the positive electrode current collector aluminum foil. The weight of the active material on the sheet is 180g / m 2 . Dry at 90℃ to obtain a single-sided coated positive electrode sheet. Then, complete these steps on the back of the sheet in exactly the same way to obtain a double-sided coated positive electrode sheet. Then, cold press the positive electrode sheet to 4.1g / cm 3 The compaction density is achieved by cutting and welding the tabs to obtain the positive electrode sheet.
[0075] 3. Preparation of electrolyte: In a dry argon atmosphere, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were first mixed in a mass ratio of EC:EMC:DEC = 30:50:20 to obtain an organic solvent. Then, lithium salt lithium hexafluorophosphate (LiPF6) was added to the organic solvent to dissolve and mix well to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.
[0076] 4. Preparation of Bare Cells: The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in sequence to form a bare cell with a wound structure. The positive and negative electrode tabs are located on the outside of the wound structure. The separator is a 9μm thick porous polyethylene film. The bare cell dimensions are 4.0mm (thickness) × 19mm (width) × 24mm (length). The end face of the bare cell is shown in Figures 1 and 2. The enlarged surface of the bare cell shows a concave and convex surface, with the tabs 60μm higher than the adjacent positions.
[0077] 5. Pre-packaging: Wrap the electrode assembly with a packaging film with a thickness of 110 μm (three-layer co-extruded polyethylene film, the middle layer is a high-density polyethylene layer, and the two sides are low-density polyethylene layers, and the melting point of the low-density polyethylene layers on both sides is 114°C), and perform hot pressing packaging at the opening at a hot pressing temperature of 110°C.
[0078] 6. Hot pressing and shaping: Use a heated mold with a flat surface to hot press the surfaces of the bare cell and the packaging film. Maintain the temperature at 115°C and a pressure of 0.1 MPa for 10 seconds. The low-density polyethylene layer in the packaging film melts and flows due to the heat, forming a complementary morphology with the surface of the bare cell, as shown in Figure 2. The inner surface of the packaging film at the tab is 60 μm recessed compared to the adjacent position. At the same time, when the low-density polyethylene layer in the packaging film is heated and melted, it forms a bond with the diaphragm on the outer surface of the bare cell, with a bonding strength of 3 N / m. The outer surface flatness of the main body is consistent with that of the mold, and the thickness difference does not exceed 3 μm.
[0079] 8. Liquid injection and packaging: The above electrolyte is injected into the unpackaged open area and then packaged. After standing, pressurized formation, degassing and other processes, the lithium-ion battery is obtained.
[0080] Comparative Example 1
[0081] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses an aluminum-plastic film with a thickness of 100 μm for packaging, places the bare battery cell in an aluminum-plastic film packaging bag, heat-seales the four sides, leaves a liquid injection port, and seals the liquid injection port after liquid injection. Subsequently, a lithium-ion battery is obtained through processes such as standing, pressurized formation, and degassing.
[0082] Test Method
[0083] 1. Energy density test: At room temperature (25°C ± 2°C), allow the lithium-ion battery to rest for no less than 30 minutes. Charge the battery at a constant current of 0.5C to 4.25V, then charge the battery at a constant voltage of 4.25V to a current of 0.05C until the battery is fully charged. Discharge the battery at a constant current of 0.5C to 3.0V, and measure the discharge energy E (in Wh). Use a micrometer to measure the maximum length, width, and height of the lithium-ion battery, and measure the volume V (in L). The volume energy density of the discharged lithium-ion battery, VED (Wh / L), is calculated as E / V.
[0084] 2. Micro-drop test: The experiment used 10 sets of lithium-ion batteries, secured with double-sided tape and assembled into the battery compartment of a watch model. The test was performed at a height of 7 cm. The battery was dropped head-down and tail-down 20,000 times at a rate of 20 drops per minute. Each of the four sides was dropped 500 times at a rate of 50 drops per minute, for a total of 42,000 drops. Any cases of package edge rupture or leakage were recorded. A failure was considered if the battery had ruptured or leaked. The micro-drop test pass rate = number of passes / 10.
[0085] 3. Hot Box Safety Test after 300 Cycles: The experiment used three sets of lithium-ion batteries. The lithium-ion batteries were allowed to rest at 25±3°C for 30 minutes, then charged at a constant current of 0.5C to 4.25V. They were then charged at a constant voltage of 4.25V to a current of 0.05C, and then discharged at a constant current of 0.5C to 3.0V. This process was repeated 300 times. The batteries that had undergone 300 cycles were then charged at a constant current of 0.5C to 4.25V, and then charged at a constant voltage of 4.25V to a current of 0.05C. This fully charged state was then subjected to the hot box test. The test process involved placing the fully charged lithium-ion batteries in an oven, heating the oven at 5°C / min, raising the temperature to 140°C and holding it for 1 hour, and observing the battery's condition. Fire or explosion were considered a failure; no fire or explosion was considered a pass. The pass rate of the hot box safety test after 300 cycles = number of passes / 3.
[0086] 4. Bond Strength Test between Encapsulation Layer and Bare Cell: Cut a strip of the bond area between the encapsulation layer and the bare cell (20mm wide x 60mm long) of a certain size. Place the strip in a tensile testing machine, clamping both ends with a clamp. Test and obtain a curve of force versus distance. Once the force stabilizes, read the corresponding value, f (N). The bond strength is F = f / 0.02 (N / m).
[0087] Table 1
[0088] As can be seen from Table 1, in Comparative Example 1, since aluminum-plastic film is used for packaging and no hot pressing shaping is performed, there is no depression in the packaging layer on the inside, which cannot effectively accommodate the protrusions in the tab connection area of the bare cell, resulting in a large difference in the thickness of the battery body, which in turn leads to poor electrode interface formation during the pressurized formation of the lithium-ion battery, making it easy to form lithium dendrites in the subsequent cycle process, and lithium dendrites are relatively unstable and easily cause battery thermal runaway under heating conditions. Therefore, the pass rate of the hot box safety test of the lithium-ion battery after 300 cycles in Comparative Example 1 is low. In contrast, since Example 1 of the present application uses a polyethylene packaging film for packaging and performs hot pressing shaping, a depression is formed at the place corresponding to the protrusion of the packaging film and the tab connection area, thereby better accommodating the protrusions on the surface of the bare cell, making the surface of the battery body smoother, and then improving the electrode interface during the pressurized formation process, so that the pass rate of the hot box safety test of the lithium-ion battery after 300 cycles is significantly improved, which greatly improves the safety of the lithium-ion battery.
[0089] At the same time, the presence of depressions in the encapsulation layer and the bonding between the encapsulation layer and the outer surface of the bare cell can further improve the mechanical safety of the lithium-ion battery. In Comparative Example 1, there is no depression in the encapsulation layer on the inside of the aluminum-plastic film, and there is no bonding with the bare cell. During the micro-drop test, the bare cell will repeatedly impact the encapsulation edge of the aluminum-plastic film due to inertia, resulting in a low micro-drop test pass rate for the lithium-ion battery. In Example 1, since the depression in the encapsulation layer can limit the protrusions on the surface of the bare cell, and there is bonding with the bare cell, the inertia of the bare cell is greatly weakened, and the impact of the bare cell on the encapsulation edge is weakened, so the micro-drop test pass rate of the lithium-ion battery is significantly improved.
[0090] In addition, since the depression of the packaging layer can accommodate the protrusions on the surface of the bare battery cell, the maximum thickness of the lithium-ion battery can be reduced, thereby further improving the volume energy density of the lithium-ion battery.
[0091] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements, and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. An electrochemical device, comprising an electrode assembly and a shell, wherein the electrode assembly is accommodated in the shell, the shell comprises a packaging layer, one side surface of the electrode assembly has a protrusion, and one side surface of the packaging layer adjacent to the electrode assembly has a depression, and the protrusion is at least partially accommodated in the depression.
2. The electrochemical device according to claim 1, wherein: At least one of the following conditions is met: (1) The protrusion is completely accommodated in the depression; (2) A surface of the packaging layer facing away from the electrode assembly is a flat surface; (3) The melting point of the encapsulation layer is 80°C to 150°C; (4) The material of the encapsulation layer includes a thermoplastic polymer; (5) The material of the encapsulation layer includes at least one of polyethylene, polypropylene, ethylene-propylene copolymer, anhydride-modified polypropylene, polyvinyl chloride, polyvinyl acetate, polyvinylidene fluoride or derivatives thereof.
3. The electrochemical device according to claim 1, wherein The depth of the recess is 3 μm to 150 μm.
4. The electrochemical device according to claim 1, wherein At least one of the following conditions is met: (1) The thickness of the encapsulation layer in the recess is 15 μm to 200 μm; (2) The encapsulation layer further includes a main body region adjacent to the recess, and the thickness of the main body region is 20 μm to 250 μm.
5. The electrochemical device according to claim 1, wherein The bonding strength between the encapsulation layer and the electrode assembly is greater than or equal to 2 N / m.
6. The electrochemical device according to claim 1, wherein The electrode assembly includes a pole piece and a pole lug, the electrode assembly includes a pole lug connection area, the pole lug is connected to the pole piece in the pole lug connection area, and the protrusion is located in the pole lug connection area.
7. The electrochemical device according to claim 1, wherein: The electrode assembly is a wound structure, the wound structure includes a main body and a corner portion, and the maximum value of the thickness difference of the electrochemical device at the main body is less than or equal to 20 μm.
8. The electrochemical device according to any one of claims 1 to 7, wherein: The shell further includes a barrier layer, which is located on a surface of the packaging layer facing away from the electrode assembly and satisfies at least one of the following conditions: (1) The thickness of the barrier layer is 0.1 μm to 50 μm; (2) The material of the barrier layer includes at least one of metal, inorganic oxide or inorganic nitride; (3) The shell further includes a protective layer, and the protective layer is located on a surface of the barrier layer facing away from the encapsulation layer.
9. The electrochemical device according to claim 8, wherein: At least one of the following conditions is met: (1) The thickness of the protective layer is 2 μm to 50 μm; (2) The protective layer comprises at least one of a polymer or a fiber; (3) The metal includes at least one of aluminum, copper, iron, titanium or nickel; (4) The inorganic oxide comprises at least one of titanium dioxide, aluminum oxide, hafnium dioxide, silicon dioxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, zinc oxide, tin oxide, zirconium titanium oxide or vanadium oxide; (5) The inorganic nitride includes at least one of silicon nitride, silicon oxynitride, boron nitride, titanium nitride or aluminum nitride.
10. An electronic device comprising the electrochemical device according to any one of claims 1 to 9.
Citation Information
Patent Citations
Flexible lithium ion battery
CN106252737A
Edge sealing method of cylindrical soft package battery and cylindrical soft package battery
CN113113703A
Electrochemical device and electronic device comprising same
CN115485922A
Lithium ion battery
CN203733894U
Soft package power supply device and electronic equipment with same
CN211654922U