Coated lithium manganate lithium-ion sieve, preparation method therefor, and use thereof
By covering the surface of lithium manganese lithium manganese sieve with aluminum-based adsorbent, the problems of manganese dissolution and reduction of adsorption capacity during use of lithium manganese lithium manganese sieve are solved, and higher adsorption capacity and lithium extraction purity are achieved. Suitable for lithium extraction of salt lake brine.
Patent Information
- Application Number
- PCT/CN2023/097372
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
During the use of existing lithium manganate lithium ion sieve, there are problems of manganese dissolution loss and decreased adsorption capacity, resulting in poor circulation performance and failure to be used on a large scale.
The surface of lithium manganate lithium ion sieve is coated with aluminum-based adsorbent by co-precipitation method. By adjusting the pH value and adding surfactant, uniform coating of aluminum-based adsorbent is achieved, forming a protective film to reduce manganese dissolution and improve adsorption. capacity.
The first adsorption capacity of lithium manganate lithium ion sieve is significantly improved and the adsorption capacity after recycling is reduced, manganese dissolution loss is improved, and the purity and efficiency in the lithium extraction process are improved.
Smart Images

Figure CN2023097372_05122024_PF_FP_ABST
Abstract
Description
A coated lithium manganate lithium ion sieve and its preparation method and application Technical Field
[0001] The present disclosure relates to the technical field of lithium extraction from brine, and in particular to a coated lithium manganate lithium ion sieve and a preparation method and application thereof. Background Art
[0002] Lithium is a critical strategic resource and one of the most ideal materials for new energy development. With the increasing scarcity and depletion of mineral resources like spodumene in recent years, lithium extraction from salt lake brine has risen to over 90% of global lithium salt production. Salt lake brine has a complex composition, containing significant amounts of ions such as Li, Na, K, Ca, Mg, and B, and its composition varies significantly from location to location. Furthermore, brine contains significant amounts of alkali and alkaline earth metals, whose chemical properties are similar to those of lithium ions, increasing the difficulty of extracting lithium from liquid form. The effective separation of lithium from these metals has become a global technical challenge.
[0003] Through the unremitting efforts of scholars in the field, several methods for extracting liquid lithium resources have been developed, including evaporation crystallization, precipitation, solvent extraction and ion exchange adsorption. Among them, the lithium ion sieve exchange method is the most practical method for extracting lithium from dilute solutions. Lithium ion sieve is a general term for a class of adsorbents that can selectively adsorb lithium from solutions. It has a unique chemical structure. Lithium ion sieve can selectively and efficiently adsorb lithium from complex systems where multiple metal ions coexist. Moreover, the adsorption and extraction process of lithium is simple, energy-efficient and environmentally friendly. Therefore, lithium ion sieve technology was once considered the most promising solution lithium extraction technology. Among them, a certain degree of metal dissolution will occur during the desorption process of lithium manganese oxide lithium ion sieve, resulting in poor cycle performance. Therefore, since the invention of lithium ion sieve in the 1980s, it has not been used on a large scale in industry.
[0004] Lithium manganate ion sieves commonly used in related technologies suffer from severe manganese dissolution and a significant decrease in adsorption capacity after repeated use. Therefore, developing a new type of lithium ion sieve that effectively improves its lithium ion adsorption capacity is of great significance.
[0005] In view of this, the present disclosure is proposed.
[0006] Summary of the Invention
[0007] The purpose of the present disclosure includes providing a coated lithium manganate lithium ion sieve, which can alleviate the problem of easy dissolution of manganese in the lithium ion sieve during use. At the same time, the aluminum-based adsorbent coated on the surface of the lithium manganate lithium ion sieve can also play a role of selective filtration, which has a certain effect on the removal of cationic impurities in the lithium extraction process.
[0008] The present disclosure also aims to provide a method for preparing a coated lithium manganate lithium ion sieve, which is simple and easy to operate, and can achieve uniform coating of the aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve.
[0009] The purpose of the present disclosure also includes providing an application of a coated lithium manganate lithium ion sieve in lithium extraction from solution.
[0010] The present invention also aims to provide a method for extracting lithium from salt lake brine.
[0011] In order to achieve at least one of the above-mentioned objectives of the present disclosure, the following technical solutions may be adopted:
[0012] In a first aspect, the present disclosure provides a coated lithium manganate lithium ion sieve, which includes a lithium manganate lithium ion sieve and an aluminum-based adsorbent, wherein the molecular formula of the lithium manganate lithium ion sieve is LiMn2O4, and the molecular formula of the aluminum-based adsorbent is LiCl·2Al(OH)3·3H2O, the lithium manganate lithium ion sieve is a carrier, and the aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve.
[0013] In some embodiments of the present disclosure, the mass of the aluminum-based adsorbent accounts for 5%-10% of the mass of the lithium manganate lithium ion sieve.
[0014] In some embodiments of the present disclosure, the mass of the aluminum-based adsorbent accounts for 6%-9% of the mass of the lithium manganate lithium ion sieve.
[0015] In some embodiments of the present disclosure, the initial adsorption capacity of the coated lithium manganate lithium ion sieve is greater than or equal to 44 mg / g, the adsorption capacity after 100 cycles is greater than or equal to 36 mg / g, and the manganese dissolution loss is less than or equal to 1.46%.
[0016] In a second aspect, the present disclosure provides a method for preparing a coated lithium manganate lithium ion sieve, comprising:
[0017] Under alkaline conditions, an aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve to obtain an intermediate product;
[0018] The intermediate product is subjected to acid elution to remove lithium;
[0019] Wherein, the molecular formula of the lithium manganate lithium ion sieve is LiMn2O4, and the molecular formula of the aluminum-based adsorbent is LiCl·2Al(OH)3·3H2O.
[0020] In some embodiments of the present disclosure, the step of coating the surface of the lithium manganate lithium ion sieve with an aluminum-based adsorbent under alkaline conditions comprises: mixing an aluminum salt and a lithium salt with water, adjusting the pH to 6.5-7.5, to obtain a mixed solution;
[0021] The mixed solution and the lithium manganate lithium ion sieve are mixed in water, the pH of the reaction system is adjusted to 9-10, and a coprecipitation reaction is performed to obtain a precipitate as an intermediate product.
[0022] In some embodiments of the present disclosure, the mass ratio of the aluminum salt to the lithium salt is 4-6:1.
[0023] In some embodiments of the present disclosure, the aluminum salt comprises aluminum chloride.
[0024] In some embodiments of the present disclosure, the lithium salt includes lithium chloride.
[0025] In some embodiments of the present disclosure, the molar ratio of the mixed solution to the lithium manganate lithium ion sieve is 0.03-0.06:1.
[0026] In some embodiments of the present disclosure, the coprecipitation reaction is carried out at a stirring speed of 700-1000 r / min and a temperature of 70-100° C. for 4-5 hours.
[0027] In some embodiments of the present disclosure, sodium hydroxide is used to adjust the pH value of the mixed solution and the reaction system.
[0028] In some embodiments of the present disclosure, when adjusting the pH value of the reaction system, the feeding rate of the sodium hydroxide is 3-5 ml / min.
[0029] In some embodiments of the present disclosure, when the mixed solution and the lithium manganate lithium ion sieve are mixed, a surfactant is further added to the system.
[0030] In some embodiments of the present disclosure, the surfactant includes at least one of an alkyl glucoside and a fatty acid glyceride.
[0031] In some embodiments of the present disclosure, the added amount of the surfactant accounts for 1-3% by volume of the base liquid in the system.
[0032] In some embodiments of the present disclosure, the acid elution of lithium includes: placing the dried intermediate product in an acid solution for soaking treatment to obtain an acidified product, and washing and drying the acidified product to obtain the coated lithium manganate lithium ion sieve.
[0033] In some embodiments of the present disclosure, the acid solution is hydrochloric acid or sulfuric acid.
[0034] In some embodiments of the present disclosure, the concentration of the acid solution is 0.25-0.5 mol / L.
[0035] In some embodiments of the present disclosure, the soaking time is 12-48 hours.
[0036] In some embodiments of the present disclosure, before the acid elution of lithium from the intermediate product, the intermediate product is further dried at 20-80° C. for 10-14 hours.
[0037] In a third aspect, the present disclosure provides the use of the coated lithium manganate lithium ion sieve described in any one of the aforementioned embodiments or the coated lithium manganate lithium ion sieve prepared by the preparation method of the coated lithium manganate lithium ion sieve described in the aforementioned embodiments in solution lithium extraction.
[0038] In a fourth aspect, the present disclosure provides an electrode for extracting lithium from salt lake brine, which comprises a coated lithium manganate lithium ion sieve prepared by the coated lithium manganate lithium ion sieve described in any one of the aforementioned embodiments or the method for preparing the coated lithium manganate lithium ion sieve described in the aforementioned embodiments.
[0039] In a fifth aspect, the present disclosure provides a method for extracting lithium from salt lake brine, which includes using an anion exchange membrane to vertically divide an electrolytic cell into a cathode chamber and an anode chamber, brine is added to the cathode chamber, and a supporting electrolyte is added to the anode chamber. The electrode for extracting lithium from salt lake brine described in any of the aforementioned embodiments is placed as a cathode in the brine, and an inert electrode is placed as an anode in the supporting electrolyte, and voltage is applied to the cathode and the anode to extract lithium.
[0040] Compared with the prior art, the advantages of the present invention include:
[0041] The preparation method of the coated lithium manganate lithium ion sieve provided by the present disclosure uses a coprecipitation method to coat an aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve. The aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve can act as a layer of cationic impurity filter membrane, thereby enabling the lithium ion sieve to have a certain degree of automatic impurity removal process during the lithium ion absorption process, thereby improving the purity of the extracted lithium. In addition, the aluminum-based adsorbent has strong water absorption and can have a good hydrophilic effect. Moreover, the aluminum-based adsorbent has an octahedral pore structure, which can enable brine to better penetrate into the interior of the lithium ion sieve through the aluminum-based adsorbent. Coating the aluminum-based adsorbent on the surface of the lithium ion sieve is equivalent to coating the surface of the lithium ion sieve with a protective film, thereby protecting the lithium ion sieve from corrosion. The lithium ion sieve in the present disclosure can serve as a carrier during the use of the aluminum-based adsorbent, playing a certain role in fixing the aluminum-based adsorbent. During the lithium extraction process, the aluminum-based adsorbent and the lithium manganate lithium ion sieve can cooperate to achieve a synergistic effect, thereby significantly improving the initial adsorption capacity. The coated lithium manganate lithium ion sieve disclosed in the present disclosure can be widely used in solution lithium extraction. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0043] FIG1 is an SEM image of the coated lithium manganate lithium ion sieve of Example 1 of the present disclosure. DETAILED DESCRIPTION
[0044] The embodiments of the present disclosure will be described in detail below with reference to the examples. However, those skilled in the art will appreciate that the following examples are intended only to illustrate the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, the experiments were performed under conventional conditions or the conditions recommended by the manufacturer. Where the manufacturer of the reagents or instruments is not specified, all are commercially available conventional products.
[0045] The endpoints of the ranges and any values disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered to be specifically disclosed herein.
[0046] In the first aspect, the present disclosure provides a coated lithium manganate lithium ion sieve, which includes a lithium manganate lithium ion sieve and an aluminum-based adsorbent. The molecular formula of the lithium manganate lithium ion sieve is LiMn2O4, and the molecular formula of the aluminum-based adsorbent is LiCl·2Al(OH)3·3H2O. The lithium manganate lithium ion sieve is a carrier, and the aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve.
[0047] The mass of the aluminum-based adsorbent accounts for 5%-10% of the mass of the lithium manganate lithium ion sieve. In some embodiments, the mass of the aluminum-based adsorbent accounts for 6%-9% of the mass of the lithium manganate lithium ion sieve. In some embodiments, the mass of the aluminum-based adsorbent accounts for 6%-8% of the mass of the lithium manganate lithium ion sieve. The coated lithium manganate lithium ion sieve has an initial adsorption capacity of greater than or equal to 44 mg / g, an adsorption capacity of greater than or equal to 36 mg / g after 100 cycles of use, and a manganese dissolution loss of less than or equal to 1.46%.
[0048] In a second aspect, the present disclosure provides a method for preparing a coated lithium manganate lithium ion sieve, which comprises the following steps:
[0049] S1. Prepare lithium manganate lithium ion sieve.
[0050] The lithium manganate lithium ion sieve disclosed in the present invention can be independently prepared or purchased commercially.
[0051] S2. Under alkaline conditions, an aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve to obtain an intermediate product.
[0052] (1) Mixing an aluminum salt and a lithium salt in a mass ratio of 4-6:1 with water, and adjusting the pH to 6.5-7.5 to obtain a mixed solution. Optionally, the aluminum salt includes aluminum chloride; and the lithium salt includes lithium chloride.
[0053] (2) Add an appropriate amount of deionized water as a base liquid into the reactor, add the mixed solution and lithium manganate lithium ion sieve into the reactor at a molar ratio of 0.03-0.06:1, then add an appropriate amount of surfactant into the system, adjust the pH of the reaction system to 9-10, and carry out a coprecipitation reaction for 4-5 hours at a stirring speed of 700-1000 r / min and a temperature of 70-100°C to obtain a precipitate as an intermediate product.
[0054] In the present disclosure, an acid or base is used to adjust the pH value of the mixed solution and the reaction system, and sodium hydroxide can be optionally used to achieve pH adjustment. When adjusting the pH of the mixed solution, the addition rate of sodium hydroxide is not limited, and it only needs to be adjusted to a preset pH. When adjusting the pH value of the reaction system, the feeding rate of sodium hydroxide is 3-5 ml / min. Since the mixed solution and the lithium manganate lithium ion sieve are undergoing a co-precipitation reaction at this time, the mixed solution is precipitated on the surface of the lithium manganate lithium ion sieve and coated on the surface of the lithium manganate lithium ion sieve, it is necessary to control the pH in real time within an appropriate range. In the present disclosure, by limiting the feeding rate of sodium hydroxide, the pH of the reaction system can be slowly adjusted, making the reaction more gentle and more complete.
[0055] In the present disclosure, the addition of a surfactant can control the agglomeration state of the precipitate, thereby achieving more uniform coating. The surfactant includes, but is not limited to, at least one of an alkyl glucoside and a fatty acid glyceride. The amount of surfactant added is 1-3% by volume of the base solution in the system.
[0056] S3. Post-processing.
[0057] (1) Dry the intermediate product at 20-80°C for 10-14 hours.
[0058] (2) Acid removal of lithium.
[0059] The dried intermediate product is immersed in an acid solution to obtain an acidified product. In the present disclosure, the acid solution is hydrochloric acid or sulfuric acid, and the concentration of the acid solution is 0.25-0.5 mol / L. The acidification immersion time must be carefully controlled. If the immersion time is too short, the lithium ion leaching is insufficient, while if the leaching time is too long, the product will be over-acidified and cause Mn dissolution. Therefore, the immersion time in the present disclosure is 12-48 hours.
[0060] (3) The acidified product is washed and dried to obtain a coated lithium manganate lithium ion sieve.
[0061] The acidified product is filtered, washed with deionized water, and then dried in an oven at 50-70°C for 10-14 hours. The resulting powder material is the coated lithium ion sieve disclosed herein. The coated lithium manganate lithium ion sieve comprises an inner layer of lithium manganate lithium ion sieve LiMn2O4 and a coating layer of an aluminum-based adsorbent, LiCl·2Al(OH)3·3H2O.
[0062] The preparation method of the coated lithium manganate lithium ion sieve provided by the present disclosure adopts a co-precipitation method to coat the aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve. The aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve can act as a layer of cationic impurity filter membrane, so that the lithium ion sieve has a certain automatic impurity removal process in the process of absorbing lithium ions, thereby improving the purity of lithium extraction. In addition, the aluminum-based adsorbent has strong water absorption and can play a good hydrophilic effect. Moreover, the aluminum-based adsorbent has an octahedral pore structure, which can enable brine to better penetrate into the interior of the lithium ion sieve through the aluminum-based adsorbent. In the present disclosure, by adding a small amount of surfactant during the co-precipitation process, the agglomeration state of the precipitate can be controlled, so that the coating is more uniform. Coating the aluminum-based adsorbent on the surface of the lithium ion sieve is equivalent to coating the surface of the lithium ion sieve with a protective film, thereby protecting the lithium ion sieve from corrosion. The lithium ion sieve in the present disclosure can serve as a carrier during the use of the aluminum-based adsorbent, playing a certain role in fixing the aluminum-based adsorbent.
[0063] The coated lithium manganate lithium ion sieve provided by the present disclosure can be widely used in solution lithium extraction. In this regard, the present disclosure also provides an electrode for lithium extraction from salt lake brine, which is prepared using the above-mentioned coated lithium manganate lithium ion sieve. The specific preparation method is to directly coat the coated lithium manganate lithium ion sieve on the surface of the electrode. The present disclosure also provides a method for extracting lithium from salt lake brine, which includes using an anion exchange membrane to vertically divide the electrolytic cell into a cathode chamber and an anode chamber, brine is added to the cathode chamber, and a supporting electrolyte is added to the anode chamber, the electrode for lithium extraction from salt lake brine is placed in the brine as a cathode, and an inert electrode is placed in the supporting electrolyte as an anode, and voltage is applied to the cathode and anode to extract lithium.
[0064] The features and performance of the present disclosure are further described in detail below with reference to the embodiments.
[0065] Example 1
[0066] This embodiment provides a coated lithium manganate lithium ion sieve, wherein the mass of the aluminum-based adsorbent accounts for 5% of the mass of the lithium manganate lithium ion sieve.
[0067] The preparation method comprises the following steps:
[0068] S1. Prepare lithium manganate lithium ion sieve.
[0069] (1) Dissolve 0.1 g of potassium permanganate in 20 mL of 10 g / L carboxymethyl cellulose solution. After complete dissolution, transfer the solution to a 35 mL reactor and react at 140 °C for 6 hours. Centrifuge and dry the sample to obtain Mn3O4.
[0070] (2) Mn3O4 and lithium hydroxide were added to a mortar in a molar ratio of lithium to manganese of 1:2 and fully ground, and then calcined in a muffle furnace at a heating rate of 5°C / min and kept at 700°C for 10 hours to obtain lithium manganate;
[0071] S2. Prepare a lithium manganate lithium ion sieve with a surface coated aluminum-based adsorbent.
[0072] (1) Weigh 1 g of aluminum chloride and 0.2 g of lithium chloride, add them to sufficient distilled water (50 mL), stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0073] (2) Add an appropriate amount of deionized water (100 mL) as the base liquid to the reactor at a molar ratio of 0.03:1. Take the above mixed solution and the prepared lithium ion sieve and add them to the reactor. Then add a small amount of alkyl glucoside (2 mL) to the reactor. By adjusting the feeding rate of sodium hydroxide to 4 ml / min, the pH of the solution in the reactor is controlled to be around 9 to obtain a precipitate. The reaction temperature is 80°C and the stirring speed is 800 r / min; the reaction is carried out for 4 hours.
[0074] S3. Post-processing.
[0075] (1) The product in S2 is dried at 50°C for 12 hours to obtain a lithium manganate lithium ion sieve with an aluminum-based adsorbent coated on the surface.
[0076] (2) The coated lithium manganate lithium ion adsorbent was placed in 20 mL of 0.5 mol / L dilute hydrochloric acid and shaken at room temperature for 12 hours to complete the delithiation.
[0077] (3) The obtained product was filtered, washed, and then placed in an oven and dried at 60° C. for 12 h. The obtained powder material was the coated lithium ion sieve in this embodiment.
[0078] The coated lithium ion sieve obtained in this example was characterized by SEM. As can be seen from FIG1 , the coated lithium manganate lithium ion sieve was effectively synthesized in this example.
[0079] Example 2
[0080] This embodiment provides a coated lithium manganate lithium ion sieve, wherein the mass of the aluminum-based adsorbent accounts for 7% of the mass of the lithium manganate lithium ion sieve.
[0081] The preparation method comprises the following steps:
[0082] S1. Prepare lithium manganate lithium ion sieve according to the method of Example 1.
[0083] S2. Prepare a lithium manganate lithium ion sieve with a surface coated aluminum-based adsorbent.
[0084] (1) Weigh 1 g of aluminum chloride and 0.2 g of lithium chloride, add them to 50 mL of distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0085] (2) Add 100 mL of deionized water as the base liquid to the reactor at a molar ratio of 0.045:1. Take the above mixed solution and the prepared lithium ion sieve and add them to the reactor. Then add a small amount of fatty acid glyceride (2 mL) to the reactor. By adjusting the feeding rate of sodium hydroxide to 4 ml / min, the pH of the solution in the reactor is controlled to be around 9 to obtain a precipitate. The reaction temperature is 80°C and the stirring speed is 800 r / min; the reaction is carried out for 4.5 hours.
[0086] S3. Post-processing.
[0087] (1) The product in S2 is dried at 50°C for 12 hours to obtain a lithium manganate lithium ion sieve with an aluminum-based adsorbent coated on the surface.
[0088] (2) The coated lithium manganate lithium ion adsorbent was placed in 20 mL of 0.5 mol / L dilute hydrochloric acid and shaken at room temperature for 24 h to complete the delithiation.
[0089] (3) The obtained product was filtered, washed, and then placed in an oven and dried at 60° C. for 12 h. The obtained powder material was the coated lithium ion sieve in this embodiment.
[0090] Example 3
[0091] This embodiment provides a coated lithium manganate lithium ion sieve, wherein the mass of the aluminum-based adsorbent accounts for 10% of the mass of the lithium manganate lithium ion sieve.
[0092] The preparation method comprises the following steps:
[0093] S1. Prepare lithium manganate lithium ion sieve according to the method of Example 1.
[0094] S2. Prepare a lithium manganate lithium ion sieve with a surface coated aluminum-based adsorbent.
[0095] (1) Weigh 1 g of aluminum chloride and 0.2 g of lithium chloride, add them to 50 mL of distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0096] (2) Add 100 mL of deionized water as a base liquid to the reactor at a molar ratio of 0.06:1. Take the above mixed solution and the prepared lithium ion sieve and add them to the reactor. Then add a small amount of alkyl glucoside (2 mL) to the reactor. By adjusting the feeding rate of sodium hydroxide to 4 ml / min, the pH of the solution in the reactor is controlled to be around 9 to obtain a precipitate. The reaction temperature is 80°C, the stirring speed is 800 r / min, and the reaction is carried out for 5 hours.
[0097] S3. Post-processing.
[0098] (1) The product in S2 is dried at 50°C for 12 hours to obtain a lithium manganate lithium ion sieve with an aluminum-based adsorbent coated on the surface.
[0099] (2) The coated lithium manganate lithium ion adsorbent was placed in 20 mL of 0.5 mol / L dilute hydrochloric acid and shaken at room temperature for 48 hours to complete the delithiation.
[0100] (3) The obtained product was filtered, washed, and then placed in an oven and dried at 60° C. for 12 h. The obtained powder material was the coated lithium ion sieve in this embodiment.
[0101] Example 4
[0102] This embodiment provides a coated lithium manganate lithium ion sieve, wherein the mass of the aluminum-based adsorbent accounts for 6% of the mass of the lithium manganate lithium ion sieve.
[0103] The preparation method comprises the following steps:
[0104] S1. Prepare lithium manganate lithium ion sieve according to the method of Example 1.
[0105] S2. Prepare a lithium manganate lithium ion sieve with a surface coated aluminum-based adsorbent.
[0106] (1) Weigh 1.2 g of aluminum chloride and 0.2 g of lithium chloride, add them to sufficient distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0107] (2) Add an appropriate amount of deionized water as the base liquid to the reactor at a molar ratio of 0.036:1. Take the above mixed solution and the prepared lithium ion sieve and add them to the reactor. Then add a small amount of alkyl glucoside (2 mL) to the reactor. By adjusting the feeding rate of sodium hydroxide to 3 ml / min, the pH of the solution in the reactor is controlled to be around 9 to obtain a precipitate. The reaction temperature is 70 ° C, the stirring speed is 1000 r / min, and the reaction is carried out for 4 hours.
[0108] S3. Post-processing.
[0109] (1) The product in S2 was dried at 20°C for 14 h to obtain a lithium manganate lithium ion sieve with a surface coated with an aluminum-based adsorbent.
[0110] (2) The coated lithium manganate lithium ion adsorbent was placed in 20 mL of dilute hydrochloric acid with a concentration of 0.25 mol / L, and the delithiation was completed after shaking at room temperature for 48 hours.
[0111] (3) The obtained product was filtered, washed, and then placed in an oven and dried at 50° C. for 14 h. The obtained powder material was the coated lithium ion sieve in this embodiment.
[0112] Example 5
[0113] This embodiment provides a coated lithium manganate lithium ion sieve, wherein the mass of the aluminum-based adsorbent accounts for 9% of the mass of the lithium manganate lithium ion sieve.
[0114] The preparation method comprises the following steps:
[0115] S1. Prepare lithium manganate lithium ion sieve according to the method of Example 1.
[0116] S2. Prepare a lithium manganate lithium ion sieve with a surface coated aluminum-based adsorbent.
[0117] (1) Weigh 0.8 g of aluminum chloride and 0.2 g of lithium chloride, add them to sufficient distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0118] (2) Add an appropriate amount of deionized water as the base liquid to the reactor at a molar ratio of 0.054:1. Take the above mixed solution and the prepared lithium ion sieve and add them to the reactor. Then add a small amount of alkyl glucoside (2 mL) to the reactor. By adjusting the feeding rate of sodium hydroxide to 5 ml / min, the pH of the solution in the reactor is controlled to be around 9 to obtain a precipitate. The reaction temperature is 100 ° C, the stirring speed is 700 r / min, and the reaction is carried out for 4 hours.
[0119] S3. Post-processing.
[0120] (1) The product in S2 is dried at 80°C for 10 h to obtain a lithium manganate lithium ion sieve with a surface coated with an aluminum-based adsorbent.
[0121] (2) The coated lithium manganate lithium ion adsorbent was placed in 20 mL of 0.4 mol / L dilute hydrochloric acid and shaken at room temperature for 48 hours to complete the delithiation.
[0122] (3) The obtained product was filtered, washed, and then placed in an oven and dried at 70° C. for 10 h. The obtained powder material was the coated lithium ion sieve in this embodiment.
[0123] Comparative Example 1
[0124] The difference between this comparative example and Example 1 is that this comparative example is an uncoated lithium manganate lithium ion sieve.
[0125] S1. The lithium manganate lithium ion sieve prepared in Example 1 was placed in 20 mL of dilute hydrochloric acid with a concentration of 0.5 mol / L, and the lithium was removed after shaking at room temperature for 24 hours. The obtained product was filtered and washed, and then placed in an oven and dried at 60°C for 12 hours. The obtained powder material is the lithium manganate lithium ion sieve in this comparative example.
[0126] Comparative Example 2
[0127] The difference between this comparative example and Example 1 is that this comparative example uses an aluminum-based adsorbent.
[0128] S1. Weigh 1 g of aluminum chloride and 0.2 g of lithium chloride, add them to sufficient distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0129] S2. Add an appropriate amount of deionized water as a base liquid to the reactor, take the above mixed solution and add it to the reactor, then add a small amount of alkyl glucoside to the reactor, and adjust the feeding rate of sodium hydroxide to 4 ml / min to control the pH of the solution in the reactor to about 9 to obtain a precipitate. The reaction temperature is 80° C. and the stirring speed is 800 r / min.
[0130] S3. Dry the product in S2 at 50° C. to obtain an aluminum-based adsorbent precursor.
[0131] S4. Place the aluminum-based adsorbent precursor in 20 mL of 0.5 mol / L dilute hydrochloric acid and shake at room temperature for 12 hours to complete the delithiation. Filter and wash the resulting product, then dry it in an oven at 60°C for 12 hours. The resulting powder material is the aluminum-based adsorbent in this comparative example.
[0132] Comparative Example 3
[0133] The difference between this comparative example and Example 1 is that the carrier in this comparative example is a titanium oxide lithium ion sieve adsorbent.
[0134] S1. Weigh 1 g of aluminum chloride and 0.2 g of lithium chloride, add them to sufficient distilled water, stir and dissolve, and add sodium hydroxide solution to adjust the pH to 7 to obtain a mixed solution;
[0135] S2. Add an appropriate amount of deionized water as a base liquid to the reactor at a molar ratio of 0.05:1; add the above mixed solution and titanium oxide powder to the reactor; then add a small amount of alkyl glucoside to the reactor; and adjust the feeding rate of sodium hydroxide to 4 ml / min to control the pH of the solution in the reactor to about 9 to obtain a precipitate. The reaction temperature is 80° C. and the stirring speed is 800 r / min;
[0136] S3. Dry the product in S2 at 50° C. to obtain a titanium oxide lithium ion sieve adsorbent with an aluminum-based adsorbent coated on its surface.
[0137] S4. Place the coated titanium oxide adsorbent in 20 mL of 0.5 mol / L dilute hydrochloric acid, shake at room temperature for 12 hours to complete the delithiation, filter the obtained product, wash it, and place it in an oven at 60°C for 12 hours to dry it. The obtained powder material is the coated lithium ion sieve adsorbent in this embodiment.
[0138] Comparative Example 4
[0139] The difference between this comparative example and Example 1 is that the mass of the aluminum-based adsorbent in this comparative example accounts for 15% of the mass of the lithium manganate lithium ion sieve. Among them, the preparation method of this comparative example is different from that of Example 1 only in step S2 (2):
[0140] An appropriate amount of deionized water was added to the reactor as a base liquid at a molar ratio of 0.09:1. The above mixed solution and the prepared lithium ion sieve were added to the reactor, and a small amount of alkyl glucoside was added to the reactor. The pH of the solution in the reactor was controlled at about 9 by adjusting the feeding rate of sodium hydroxide to 4 ml / min to obtain a precipitate. The reaction temperature was 80°C and the stirring speed was 800 r / min.
[0141] Comparative Example 5
[0142] The difference between this comparative example and Example 1 is that the surfactant (alkyl glucoside) in Example 1 is omitted in this comparative example.
[0143] Experimental Example 1
[0144] First adsorption capacity test: initial lithium ion concentration is 165mg / L, Mg 2+20 mL of brine with a concentration of 5 g / L and a solution pH of 12.0 were added, and 0.1 g of the lithium ion sieve prepared in Examples 1-3 and Comparative Examples 1-2 were respectively coated on the surface of the electrode to form an electrode for lithium extraction from salt lake brine. The electrolytic cell was vertically divided into a cathode chamber and an anode chamber using an anion exchange membrane. Brine was added to the cathode chamber, and a supporting electrolyte (50 mmol / L) was added to the anode chamber. The electrode for lithium extraction from salt lake brine was placed as a cathode in the brine, and an inert electrode (activated carbon electrode) was placed as an anode in the supporting electrolyte. A voltage of 1.2 V was applied to the cathode and anode to extract lithium. Under the conditions of 25 ° C and a reaction time of 12 h, the adsorption capacity was measured as shown in Table 1 for the first adsorption capacity;
[0145] The test method for adsorption capacity after 100 cycles is the same as the test method for the first adsorption capacity;
[0146] Mg in lithium-rich solution 2+ The concentration test method is based on HJ776-2015 "Determination of 32 elements in water quality - Inductively coupled plasma optical emission spectrometry" to detect its concentration;
[0147] The test results are shown in Table 1.
[0148] As can be seen from the above table, the initial adsorption capacity of the coated lithium manganate lithium ion sieve provided by Examples 1-5 of the present disclosure is significantly better than that of Comparative Examples 1-5, and the adsorption capacity after 100 cycles provided by Examples 1-5 is also significantly better than that of Comparative Examples 1-5, and the Mg in the lithium-rich solution of Examples 1-5 of the present disclosure is significantly better than that of Comparative Examples 1-5. 2+ The concentration is significantly lower than that of comparative examples 1-5, which fully proves that the coated lithium manganate lithium ion sieve provided by the present disclosure not only has a specific adsorption effect on lithium ions, but also has a filtering effect on other impurity ions besides lithium ions, such as magnesium ions. It can be seen from comparative examples 1 and 2 that the coated lithium manganate lithium ion sieve provided by the present disclosure has a synergistic effect and has a certain inhibitory effect on the dissolution of manganese metal. It can be seen from the experimental data of comparative example 3 that the effect of using titanium oxide lithium ion sieve as a carrier is worse than that of Example 1. The possible reason is that the lithium manganate lithium ion sieve in the present disclosure is not a conventional carrier. When the lithium manganate lithium ion sieve is not powered, only the aluminum-based adsorbent coated on the surface absorbs lithium, and the lithium manganate material basically does not absorb lithium. When powered, the lithium manganate lithium ion sieve and the aluminum-based adsorbent can both achieve lithium adsorption, which can achieve a synergistic effect of lithium absorption. It can be seen from the experimental data of comparative example 4 that when the proportion of the aluminum-based adsorbent in the coating layer is large, it will affect the adsorption capacity. It can be seen from Comparative Example 5 that when the surfactant is omitted, the precipitate will easily agglomerate during coprecipitation, resulting in uneven coating, thereby affecting the initial adsorption capacity and the manganese dissolution loss.
[0149] In summary, the preparation method of the coated lithium manganate lithium ion sieve provided by the present disclosure adopts a co-precipitation method to coat the aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve. The aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve can act as a layer of cationic impurity filter membrane, so that the lithium ion sieve has a certain automatic impurity removal process in the process of absorbing lithium ions, thereby improving the purity of lithium extraction. In addition, the aluminum-based adsorbent has strong water absorption and can play a good hydrophilic effect. Moreover, the aluminum-based adsorbent has an octahedral pore structure, which can enable brine to better penetrate into the interior of the lithium ion sieve through the aluminum-based adsorbent. In the present disclosure, by adding a small amount of surfactant during the co-precipitation process, the agglomeration state of the precipitate can be controlled, so that the coating is more uniform. Coating the aluminum-based adsorbent on the surface of the lithium ion sieve is equivalent to coating the surface of the lithium ion sieve with a protective film, thereby protecting the lithium ion sieve from corrosion. The lithium ion sieve in the present disclosure can act as a carrier during the use of the aluminum-based adsorbent, and play a certain role in fixing the aluminum-based adsorbent. The combination of the aluminum-based adsorbent and the lithium manganate lithium ion sieve can achieve a synergistic effect, thereby significantly improving the initial adsorption capacity. The coated lithium manganate lithium ion sieve disclosed in the present invention can be widely used in solution lithium extraction.
[0150] The above describes in detail the optional embodiments of the present disclosure, but the present disclosure is not limited thereto. Within the technical concept of the present disclosure, various simple variations of the technical solution of the present disclosure can be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as the contents disclosed by the present disclosure and fall within the scope of protection of the present disclosure. Industrial Applicability
[0151] The preparation method of the coated lithium manganate lithium ion sieve provided by the present disclosure adopts a co-precipitation method to coat the aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve. The aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve can act as a layer of cationic impurity filter membrane, so that the lithium ion sieve has a certain automatic impurity removal process in the process of absorbing lithium ions, thereby improving the purity of lithium extraction. In addition, the aluminum-based adsorbent has strong water absorption and can play a good hydrophilic effect. Moreover, the aluminum-based adsorbent has an octahedral pore structure, which can enable brine to better penetrate into the interior of the lithium ion sieve through the aluminum-based adsorbent. In the present disclosure, by adding a small amount of surfactant during the co-precipitation process, the agglomeration state of the precipitate can be controlled, so that the coating is more uniform. Coating the aluminum-based adsorbent on the surface of the lithium ion sieve is equivalent to coating the surface of the lithium ion sieve with a protective film, thereby protecting the lithium ion sieve from corrosion. The lithium ion sieve in the present disclosure can serve as a carrier during the use of the aluminum-based adsorbent, playing a certain role in fixing the aluminum-based adsorbent. The combination of the aluminum-based adsorbent and the lithium manganate lithium ion sieve can achieve a synergistic effect, thereby significantly improving the initial adsorption capacity. The coated lithium manganate lithium ion sieve disclosed in the present invention can be widely used in solution lithium extraction.
Claims
1. A coated lithium manganate lithium ion sieve, characterized in that: It includes a lithium manganate lithium ion sieve and an aluminum-based adsorbent, the molecular formula of the lithium manganate lithium ion sieve is LiMn2O4, the molecular formula of the aluminum-based adsorbent is LiCl·2Al(OH)3·3H2O, the lithium manganate lithium ion sieve is a carrier, and the aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve.
2. The coated lithium manganate lithium ion sieve according to claim 1, characterized in that: The mass of the aluminum-based adsorbent accounts for 5%-10% of the mass of the lithium manganate lithium ion sieve.
3. The coated lithium manganate lithium ion sieve according to claim 1, characterized in that: The mass of the aluminum-based adsorbent accounts for 6%-9% of the mass of the lithium manganate lithium ion sieve.
4. The coated lithium manganate lithium ion sieve according to any one of claims 1 to 3, characterized in that: The first adsorption capacity of the coated lithium manganate lithium ion sieve is greater than or equal to 44 mg / g, the adsorption capacity after 100 cycles of use is greater than or equal to 36 mg / g, and the manganese dissolution loss is less than or equal to 1.46%.
5. A method for preparing a coated lithium manganate lithium ion sieve, characterized in that: It includes: Under alkaline conditions, an aluminum-based adsorbent is coated on the surface of the lithium manganate lithium ion sieve to obtain an intermediate product; The intermediate product is subjected to acid elution to remove lithium; Wherein, the molecular formula of the lithium manganate lithium ion sieve is LiMn2O4, and the molecular formula of the aluminum-based adsorbent is LiCl·2Al(OH)3·3H2O.
6. The method for preparing the coated lithium manganate lithium ion sieve according to claim 5, characterized in that: The step of coating the aluminum-based adsorbent on the surface of the lithium manganate lithium ion sieve under alkaline conditions comprises: mixing aluminum salt and lithium salt with water, adjusting the pH to 6.5-7.5, and obtaining a mixed solution; The mixed solution and the lithium manganate lithium ion sieve are mixed in water, the pH of the reaction system is adjusted to 9-10, and a coprecipitation reaction is performed to obtain a precipitate as an intermediate product.
7. The method for preparing the coated lithium manganate lithium ion sieve according to claim 6, characterized in that: The mass ratio of the aluminum salt to the lithium salt is 4-6:
1.
8. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 7, characterized in that: The aluminum salt includes aluminum chloride.
9. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 8, characterized in that: The lithium salt includes lithium chloride.
10. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 9, characterized in that: The molar ratio of the mixed solution to the lithium manganate lithium ion sieve is 0.03-0.06:
1.
11. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 10, characterized in that: The coprecipitation reaction is carried out at a stirring speed of 700-1000 r / min and a temperature of 70-100° C. for 4-5 hours.
12. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 11, characterized in that: Sodium hydroxide is used to adjust the pH value of the mixed solution and the reaction system; when adjusting the pH value of the reaction system, the feeding rate of the sodium hydroxide is 3-5 ml / min.
13. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 6 to 12, characterized in that: When the mixed solution and the lithium manganate lithium ion sieve are mixed, a surfactant is also added into the system.
14. The method for preparing the coated lithium manganate lithium ion sieve according to claim 13, characterized in that: The surfactant includes at least one of an alkyl glucoside and a fatty acid glyceride.
15. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 13 to 14, characterized in that: The added amount of the surfactant is 1-3% by volume of the base liquid in the system.
16. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 5 to 15, characterized in that: The acid elution of lithium comprises: placing the dried intermediate product in an acid solution for immersion treatment to obtain an acidified product, and washing and drying the acidified product to obtain the coated lithium manganate lithium ion sieve.
17. The method for preparing the coated lithium manganate lithium ion sieve according to claim 16, characterized in that: The acid solution is hydrochloric acid or sulfuric acid.
18. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 16 to 17, characterized in that: The concentration of the acid solution is 0.25-0.5 mol / L.
19. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 16 to 18, characterized in that: The soaking time is 12-48h.
20. The method for preparing the coated lithium manganate lithium ion sieve according to any one of claims 5 to 19, characterized in that: Before the acid elution of lithium from the intermediate product, the method further comprises drying the intermediate product at 20-80° C. for 10-14 hours.
21. Use of the coated lithium manganate lithium ion sieve as claimed in any one of claims 1 to 4 or the coated lithium manganate lithium ion sieve prepared by the preparation method of the coated lithium manganate lithium ion sieve as claimed in any one of claims 5 to 20 in lithium extraction from solution.
22. An electrode for extracting lithium from salt lake brine, characterized in that: The coated lithium manganate lithium ion sieve prepared by the method for preparing the coated lithium manganate lithium ion sieve described in any one of claims 1 to 4 and any one of claims 5 to 20 is coated on the surface of the electrode substrate.
23. A method for extracting lithium from salt lake brine, characterized in that: It includes using an anion exchange membrane to vertically divide the electrolytic cell into a cathode chamber and an anode chamber, brine is added to the cathode chamber, a supporting electrolyte is added to the anode chamber, the electrode for lithium extraction from salt lake brine as claimed in claim 22 is placed in the brine as a cathode, an inert electrode is placed in the supporting electrolyte as an anode, and voltage is applied to the cathode and the anode to extract lithium.
Citation Information
Patent Citations
Composite adsorbing material for removing lithium ions in natural water and preparation method thereof
CN102872792A
Method for doping and cladding double modifying for lithium manganate in one step
CN105576218A
Microcrystalline property aluminum salt lithium ion adsorbent particles coated with macro-porous silica gel and loaded with lightweight glass material and preparation method thereof
CN108043358A
Crystalline aluminium-salt lithium-ion adsorbent particles and preparation method thereof
CN108187608A
Aluminum salt lithium adsorbent, and preparation method and application thereof
CN108993376A