Method for producing garnet-type oxide solid electrolyte

WO2024243870A1PCT designated stage expired Publication Date: 2024-12-05DIC CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097498
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-05

Smart Images

  • Figure PCTCN2023097498-FTAPPB-I100001
    Figure PCTCN2023097498-FTAPPB-I100001
  • Figure 00000028_0000
    Figure 00000028_0000
  • Figure 00000029_0000
    Figure 00000029_0000
Patent Text Reader

Abstract

A method for producing a garnet-type oxide solid electrolyte is a method for producing an oxide solid electrolyte that includes an oxide that is based on a Li7La3Zr2O12 garnet-type oxide and has a Zr site partially substituted with Mo as represented by general formula (1) : Li(7-2x) La3Zr (2-x) MoxO12 (x is greater than 0 and less than or equal to 0.6). The method includes a first step of preparing raw material powders in a manner such that composition ratios (molar ratios) that satisfy general formula (1) are achieved; a second step of firing the prepared raw material powders at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, thereby synthesizing a fired powder; and a third step of pelletizing the synthesized fired powder to form a pellet and subsequently firing the pellet at a densification temperature of less than or equal to 800℃, thereby densifying the pellet.
Need to check novelty before this filing date? Find Prior Art

Description

METHOD FOR PRODUCING GARNET-TYPE OXIDE SOLID ELECTROLYTE[Technical Field]

[0001] The present invention relates to a method for producing a garnet-type oxide solid electrolyte.[Background Art]

[0002] Lithium ion secondary batteries have a high energy density and can be operated at a high electric potential and are, therefore, used, for example, in small information devices, such as mobile phones and laptop computers, and electric vehicles. For the sake of safety, research and development have been conducted on all-solid-state lithium ion secondary batteries, which do not use flammable electrolyte solutions. Solid electrolytes that are used in all-solid-state lithium ion secondary batteries are required to have a high lithium ion conductivity. An oxide that has been disclosed as having a high lithium ion conductivity is Li7La3Zr2O12, which has a cubic garnet-type crystal structure (see, for example, Patent Literature 1) .

[0003] Realizing a solid electrolyte having a high lithium ion conductivity requires a reduction in grain boundary resistance and interfacial resistance. Accordingly, a type of garnet-type oxide has been synthesized, and research has been conducted on the crystal structure and the lithium ion conductivity of the garnet-type oxide; this garnet-type oxide is an oxide based on the Li7La3Zr2O12 having a garnet-type crystal structure and in which the La site is partially substituted with an alkaline earth element, and the Zr site is partially substituted with Nb (see, for example, Non Patent Literature 1) . Non Patent Literature 1 discloses that the synthesis of the garnet-type oxide was carried out by a process in which starting material powders  were calcined at approximately 900℃, subsequently, the calcined powders were ground and formed to have a pellet shape, and the pellet was subjected to main sintering (also simply referred to as sintering) at 1200℃ to form a polycrystalline pellet. Furthermore, another type of garnet-type oxide has been synthesized with a solid-state reaction method, and research has been conducted on the crystal structure and the lithium ion conductivity of the garnet-type oxide; this garnet-type oxide is Li6.4La3Zr1.7M0.3O12 (M=Mo and Cr) , which is based on the Li7La3Zr2O12 having a garnet-type crystal structure and in which the Zr site is partially substituted with Mo and Cr (see, for example, Non Patent Literature 2) . Non Patent Literature 2 discloses that the synthesis of the garnet-type oxide was carried out by a process in which raw material powders were fired at approximately 1000℃, subsequently, the fired powder was ground and formed to have a pellet shape, and the pellet was sintered at ll00℃ to form a polycrystalline pellet.[Citation List][Patent Literature]

[0004] [PTL 1]

[0005] International Publication No. WO2016 / 017769[Non Patent Literature]

[0006] [NPL 1]

[0007] Ohta et al., Journal of Flux Growth Vol. 11, No. l, 2016, 10-14

[0008] [NPL 2]

[0009] Gao et al., Solid State Ionics Vol. 291, 2016, 1-7[Summary of Invention][Technical Problem]

[0010] Furthermore, realizing an enhanced performance of all-solid-state lithium ion secondary batteries requires a  reduction in interfacial resistance between the solid electrolyte and electrodes, in addition to the development of a solid electrolyte having a high lithium ion conductivity. An effective way to reduce the interfacial resistance between the solid electrolyte and electrodes is to perform sintering in a state in which the positive electrode, the solid electrolyte, and the negative electrode are combined; such sintering is called co-sintering. However, in instances where the garnet-type oxide disclosed in Non Patent Literature 1 or Non Patent Literature 2 is to be used as a solid electrolyte, the co-sintering needs to be performed at greater than or equal to ll00℃, that is, at the sintering temperature disclosed in Non Patent Literature 1 or 2. Unfortunately, in instances where, for example, LiCoO2 or the like is used as an electrode material, a problem arises in that the performance of the electrode is degraded at temperatures greater than or equal to ll00℃. Performing the co-sintering without degrading the performance of electrodes requires composition designing and a production method that enable a garnet-type oxide solid electrolyte to be produced at less than or equal to 800℃. Unfortunately, neither Non Patent Literature 1 nor Non Patent Literature 2 discloses a composition of a garnet-type oxide and a production method therefor that address the need.

[0011] The present invention has been made to solve the problem described above, and an object of the present invention is to provide a method for producing a garnet-type oxide solid electrolyte, which is a method that enables co-sintering of the solid electrolyte and electrodes.[Solution to Problem]

[0012] The contents of the present disclosure include the following aspects [1] to [5] .

[0013] [1] A method for producing an oxide solid electrolyte that  includes a garnet-type oxide represented by general formula (1) below: Li(7-2x) La3Zr (2-x) MoxO12 (1)

[0014] where x is greater than 0 and less than or equal to 0.6, the method including:

[0015] a first step of preparing raw material powders in a manner such that composition ratios that satisfy general formula (1) are achieved, the composition ratios being molar ratios;

[0016] a second step of firing the prepared raw material powders at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, thereby synthesizing a fired powder; and

[0017] a third step of pelletizing the synthesized fired powder to form a pellet and subsequently firing the pellet at a densification temperature of less than or equal to 800℃, thereby densifying the pellet.

[0018] [2] The method for producing an oxide solid electrolyte according to [1] , wherein the garnet-type oxide represented by general formula (1) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo.

[0019] [3] A method for producing an oxide solid electrolyte that includes a garnet-type oxide represented by general formula (2) below: Li(7-2y-z) La3Zr (2-y-z) MoyTazO12  (2)

[0020] where y is greater than 0 and less than 0.6, z is greater than 0 and less than 0.6, and y+z is less than or equal to 0.6,

[0021] the method including:

[0022] a first step of preparing raw material powders in a manner such that composition ratios that satisfy general formula (2) are achieved, the composition ratios being molar ratios;

[0023] a second step of firing the prepared raw material powders at a firing temperature of less than or equal to 800℃ with  a solid-state reaction method, thereby synthesizing a fired powder; and

[0024] a third step of pelletizing the synthesized fired powder to form a pellet and subsequently firing the pellet at a densification temperature of less than or equal to 800℃, thereby densifying the pellet.

[0025] [4] The method for producing an oxide solid electrolyte according to [3] , wherein the garnet-type oxide represented by general formula (2) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo and Ta.

[0026] [5] The method for producing an oxide solid electrolyte according to any one of [1] to [4] , wherein the firing temperature in the second step is 700℃ to 800℃, and the densification temperature in the third step is 700℃ to 800℃.[Advantageous Effects of Invention]

[0027] The present invention can provide a method for producing a garnet-type oxide solid electrolyte, which is a method that enables co-sintering of the solid electrolyte and electrodes.[Brief Description of Drawings]

[0028] [Fig. 1]

[0029] Fig. 1 is a diagram illustrating a method for producing a garnet-type oxide solid electrolyte according to a first embodiment.

[0030] [Fig. 2]

[0031] Fig. 2 is a diagram illustrating a method for producing a garnet-type oxide solid electrolyte according to a second embodiment.

[0032] [Fig. 3]

[0033] Fig. 3 is an XRD pattern of a garnet-type oxide solid electrolyte produced by a production method of Example 3.

[0034] [Fig. 4]

[0035] Fig. 4 is an XRD pattern of a garnet-type oxide solid electrolyte produced by a production method of Example 14.

[0036] [Fig. 5]

[0037] Fig. 5 is an XRD pattern of a garnet-type oxide solid electrolyte produced by a production method of Comparative Example 1.[Description of Embodiments]

[0038] The present disclosure will be described in more detail below with reference to a first embodiment and a second embodiment. Note that the present invention is not limited to the embodiments described below.

[0039] When "to" is used to indicate a numerical range, the numerical range includes the numbers preceding and following "to" as the minimum and maximum numbers.

[0040] [First Embodiment]

[0041] [Method for Producing Mo-substituted Garnet-type Oxide Solid Electrolyte]

[0042] A method of this embodiment for producing an oxide solid electrolyte (which may also be referred to as a "production method of this embodiment" ) is a method for producing an oxide solid electrolyte that includes a garnet-type oxide represented by general formula (1) below. Preferably, the garnet-type oxide represented by general formula (1) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo. Li(7-2x) La3Zr (2-x) MoxO12  (1)

[0043] In formula 1) , x is greater than 0 and less than or equal to 0.6.

[0044] The production method of this embodiment includes first to third steps, described below.

[0045] First step: raw material powders are prepared in a manner  such that composition ratios (molar ratios) that satisfy general formula (1) are achieved.

[0046] Second step: the prepared raw material powders are fired at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, to synthesize a fired powder. Third step: the synthesized fired powder is pelletized to form a pellet, and subsequently, the pellet is fired at a densification temperature of less than or equal to 800℃ to be densified.

[0047] [Mo-substituted Garnet-type Oxide Solid Electrolyte]

[0048] The oxide solid electrolyte represented by the chemical formula of general formula (1) , which is the product to be synthesized by the production method of this embodiment, is a solid electrolyte (which may also be referred to as a "Mo-substituted garnet-type oxide solid electrolyte" ) formed of an oxide (which may also be referred to as a "Mo-substituted garnet-type oxide" ) represented by the chemical formula of general formula (1) . In general formula (1) , preferably, x is greater than or equal to 0.1 and less than or equal to 0.6, more preferably, greater than or equal to 0.2 and less than or equal to 0.6, and even more preferably, greater than or equal to 0.4 and less than or equal to 0.6. Specific examples of the Mo-substituted garnet-type oxide include Li6.4La3Zr1.7Mo0.3O12 (in general formula (1) , x=0.3) of Example 3 and Li5.8La3Zr1.4Mo0.6O12 (in general formula (1) , x=0.6) of Example 6.

[0049] Preferably, the Mo-substituted garnet-type oxide of this embodiment has a cubic crystal structure. Regarding methods for evaluating the crystal structure, a powder X-ray diffraction (XRD) method, which will be described later, can be used for determination. The Mo-substituted garnet-type oxide solid electrolyte of this embodiment may include one or more other components, in addition to the Mo-substituted garnet-type oxide, to an extent in which the  ability of the solid electrolyte is not impaired. Examples of the other components include impurities derived from raw materials. Preferably, the Mo-substituted garnet-type oxide solid electrolyte of this embodiment consists essentially only of the Mo-substituted garnet-type oxide. The expression "consists essentially only of the Mo-substituted garnet-type oxide" means that, in the Mo-substituted garnet-type oxide solid electrolyte of this embodiment, a content of the Mo-substituted garnet-type oxide may be 95%or greater and 100%or less, 98%or greater and 100%or less, or 99%or greater and 100%or less.

[0050] [First Step]

[0051] For the production of the garnet-type oxide represented by general formula (1) , the raw material powders are prepared in a manner such that composition ratios (molar ratios) that satisfy general formula (1) are achieved, and the raw material powders are then mixed together. In the instance where the raw material powders are prepared in a manner such that the composition ratios satisfy the value of x of greater than 0 and less than or equal to 0.6 as specified in general formula (1) , the firing temperature and the densification temperature in the subsequent steps can be lower than those typically employed, and in addition, a reduction in the composition ratio of Li can be inhibited; consequently, the cubic crystal structure is maintained, which results in a high lithium ion conductivity. On the other hand, if the composition ratio of Mo is greater than 0.6, the composition ratio of Li is reduced, and, consequently, forming a cubic crystal structure becomes difficult. As a result, the lithium ion conductivity is significantly reduced, and reproducibility for the production is reduced. For example, when the composition ratio of Mo is 0.6, the composition ratio of Li is 5.8, and these composition ratios of Mo and Li are the upper limit  of the composition ratio of Mo and the lower limit of the composition ratio of Li for forming a cubic crystal structure with good reproducibility. Furthermore, the reduction in the composition ratio of Li during the production of the garnet-type oxide, with respect to the composition ratio that satisfies general formula (1) , can be inhibited as follows: for example, in instances where a Li raw material such as LiNO3 that tends to volatilize in the second step is used, the Li raw material may be used in a 10%excess amount with respect to the amount corresponding to the composition ratio that satisfies general formula (1) .

[0052] Examples of the raw material from which the lithium is derived include nitrate salts, such as lithium nitrate, and include lithium hydroxide and lithium carbonate. Examples of the raw material from which the lanthanum is derived include oxides, such as lanthanum oxide, and include lanthanum nitrate. Examples of the raw material from which the zirconium is derived include oxides, such as zirconium oxide. Examples of the raw material from which the molybdenum is derived include oxides, such as molybdenum oxide, and include ammonium molybdate tetrahydrate.

[0053] Preferably, the raw materials of the constituent components of formula (1) are powders. An average particle size of the powders is preferably less than or equal to 200 μm, more preferably less than or equal to 100 μm, and even more preferably less than or equal to 50 μm. The average particle size may be greater than or equal to 1 μm. Note that the average particle size of the powders can be measured with a known method, and examples of the method include length measurement by SEM observation, wet particle-size distribution measurement, and dry particle-size distribution measurement.

[0054] The first step of the production method of this embodiment may include a sub-step la and a sub-step lb. In the sub-step la, the raw materials necessary for the components are selected based on the composition of the Mo-substituted garnet-type oxide that is to be synthesized. In the sub-step lb, the selected raw materials are mixed together. Furthermore, if necessary, the first step may further include a sub-step ic, in which grinding is performed. The sub-step ic may be performed between the sub-step la and the sub-step lb or after the sub-step lb. The methods to be used for the mixing and the grinding are not particularly limited and may be known methods.

[0055] [Second Step]

[0056] In the second step of the production method of this embodiment, the firing temperature is less than or equal to 800℃ and preferably 600 to 800℃. The firing temperature is more preferably 700 to 800℃. For example, in Examples, which will be described later, the firing temperature was 700℃ or 800℃.

[0057] The solid-state reaction method (apparatus) to be used for the firing is not particularly limited and may be a known method. For example, a muffle furnace, an electric furnace, or the like may be used.

[0058] Preferably, an atmosphere for the firing is air, for example. A firing time is preferably greater than or equal to 6 hours and more preferably greater than or equal to 12 hours. The firing time may be less than or equal to 20 hours. For example, in the Examples described later, the firing time was 12 hours.

[0059] A heating rate and a cooling rate during the time from the start to the end of the firing are not particularly limited. For example, the heating rate is preferably  10℃ / min, more preferably 8℃ / min, and even more preferably 5℃ / min. The cooling rate is preferably 5℃ / min, more preferably 3℃ / min, and even more preferably l℃ / min. A pressure for the firing is not particularly limited. The heating may be performed at atmospheric pressure.

[0060] Furthermore, from the standpoint of improving the lithium ion conductivity of the oxide solid electrolyte of this embodiment, it is possible to perform the heating at a pressure greater than atmospheric pressure.

[0061] The second step may further include a sub-step in which, after the raw material powders prepared in the first step are fired, the fired product is ground. The fired powder obtained in the second step may have a cubic crystal structure. Not that the firing performed in the second step may be referred to by various terms. For example, the term "calcine" is used in Non Patent Literature 1.

[0062] [Third Step]

[0063] The method to be used to pelletize the fired powder obtained in the second step is not particularly limited and may be a known method. Examples of the method for pelletization include a method in which the fired product obtained in the second step is pelletized with an isostatic press at 10 MPa or greater. The pressure may be 15 MPa or greater or 20 MPa or greater. The pressure may be 100 MPa or less. Specific examples of the method for pelletization include a method in which the fired powder is isostatically pressed at 20 MPa, as described in Example 3, which will be described later. A temperature for the pelletization is not particularly limited and is preferably less than or equal to 800℃. The pelletization may be carried out without performing heating (e.g., at 25℃) .

[0064] In the third step of the production method of this embodiment, the obtained pellet is sintered at the  densification temperature of less than or equal to 800℃and preferably 600 to 800℃. The densification temperature is more preferably 700 to 800℃. For example, in the Examples described later, the densification temperature was 700℃ or 800℃. Before the pellet is sintered for densification, a periphery of the pellet may be covered with the fired powder obtained in the second step (the description of Fig. 1 states "PORTION OF FIRED POWDER IS USED" ) , and the resulting pellet may be sintered at less than or equal to 800℃ for 12 hours for densification.

[0065] The apparatus to be used for the sintering for densification is not particularly limited and may be a known apparatus. For example, a muffle furnace, an electric furnace, a hot press, or the like may be used.

[0066] Preferably, the atmosphere for the sintering is air, for example. The sintering time is preferably greater than or equal to 6 hours and more preferably greater than or equal to 12 hours. The sintering time may be less than or equal to 20 hours. For example, in the Examples described later, the sintering time was 12 hours.

[0067] The heating rate and the cooling rate during the time from the start to the end of the sintering are not particularly limited. For example, the heating rate is preferably 10℃ / min, more preferably 8℃ / min, and even more preferably 5℃ / min. The cooling rate is preferably 5℃ / min, more preferably 3℃ / min, and even more preferably l℃ / min. Note that the "sintering" performed in the third step may be referred to by various names. For example, the term "main sintering" is used in Non Patent Literature 1. In the present invention, "densification" , "densification sintering" , or simply "sintering" is used.

[0068] As illustrated in Fig. 1, the production method of this  embodiment may be, for example, a production method that includes composition designing and raw material powder preparation and mixing steps, which correspond to the first step, a raw material powder firing step, which corresponds to the second step, and pelletization and densification sintering steps, which correspond to the third step. In addition, if necessary, an XRD measurement step, which is an inspection step, may be included.

[0069] [Composition Designing Step]

[0070] Composition designing is performed for designing a composition in which the Zr site of the garnet-type oxide having the fundamental composition of Li7La3Zr2O12 is partially substituted (doped) with Mo. The composition designing is carried out such that general formula (1) is satisfied.

[0071] [Raw Material Powder Preparation and Mixing Step]

[0072] Raw material powders are prepared in accordance with the composition designed in the composition designing step, and then the raw material powders are mixed together. For example, only a Li raw material, such as LiNO3, may be used in a 10%excess amount with respect to the amount of the designed composition.

[0073] [Raw Material Powder Firing Step]

[0074] The raw material powders prepared and mixed in the raw material powder preparation and mixing step are fired at less than or equal to 800℃ for 12 hours with a solid-state reaction method, to give a fired powder. Specific examples of the powder firing temperature include 700℃ and 800℃.

[0075] [Pelletization Step]

[0076] The fired powder obtained in the raw material powder firing step is isostatically pressed at 20 MPa.

[0077] [Densification Sintering Step]

[0078] A periphery of the pellet obtained in the pelletization step is covered with the fired powder and fired at less than or equal to 800℃ for 12 hours for densification.

[0079] Specific examples of the densification temperature include 700℃ and 800℃.

[0080] [XRD Measurement Step]

[0081] The densification-treated pellet obtained in the densification sintering step (which may also be referred to as a "dense pellet" ) is ground to a powder, and the powder is examined with an XRD method to confirm that the formation of a garnet-type (cubic) oxide solid electrolyte, which is the target product, has been achieved. The verification can be made, for example, with either of the methods described in Patent Literature A and Non Patent Literature A, listed below. The verification of the presence of the garnet-type (cubic) oxide solid electrolyte with an XRD method is carried out by comparing an XRD pattern obtained in the measurement, against a standard pattern of a cubic oxide. In instances where the patterns match each other, a verification can be made that a cubic crystal structure has been formed.

[0082] Patent Literature A: Japanese Unexamined Patent Application Publication No. 2021-174767

[0083] Non Patent Literature A: Rettenwander et al., Inorganic Chemistry Vol. 54, 2015, 10440-10449

[0084] [Second Embodiment]

[0085] [Method for Producing Mo-and Ta-substituted Garnet-type Oxide Solid Electrolyte]

[0086] A method of this embodiment for producing an oxide solid electrolyte (which may also be referred to as a "production method of this embodiment" ) is a method for producing an oxide solid electrolyte that includes a garnet-type oxide represented by general formula (2) below. Preferably, the  garnet-type oxide represented by general formula (2) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo and Ta. Li (7-2y-z) La3Zr (2-y-z) MoyTazO12  (2)

[0087] In formula (2) , y is greater than 0 and less than 0.6, z is greater than 0 and less than 0.6, and y+z is less than or equal to 0.6.

[0088] The production method of this embodiment includes first to third steps, described below.

[0089] First step: raw material powders are prepared in a manner such that composition ratios (molar ratios) that satisfy general formula (2) are achieved.

[0090] Second step: the prepared raw material powders are fired at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, to synthesize a fired powder. Third step: the synthesized fired powder is pelletized to form a pellet, and subsequently, the pellet is fired at a densification temperature of less than or equal to 800℃ to be densified.

[0091] [Mo-and Ta-substituted Garnet-type Oxide Solid Electrolyte]

[0092] The oxide solid electrolyte represented by the chemical formula of general formula (2) , which is the product to be synthesized by the production method of this embodiment, is a solid electrolyte (which may also be referred to as a "Mo-and Ta-substituted garnet-type oxide solid electrolyte" ) formed of an oxide (which may also be referred to as a "Mo-and Ta-substituted garnet-type oxide" ) represented by the chemical formula of general formula (2) . In general formula (2) , preferably, y is greater than or equal to 0.1 and less than or equal to 0.5, z is greater than or equal to 0.1 and less than or equal to 0.5, and y+z is greater than or equal to 0.2 and less than  or equal to 0.6, and more preferably, y is greater than or equal to 0.2 and less than or equal to 0.4, z is greater than or equal to 0.2 and less than or equal to 0.4, and y+z is greater than or equal to 0.4 and less than or equal to 0.6. Alternatively, y may be greater than or equal to 0.4 and less than 0.6, z may be greater than 0 and less than or equal to 0.2, and y+z may be greater than 0.4 and less than or equal to 0.6. Specific examples of the Mo-and Ta-substituted garnet-type oxide include Li6.1La3Zr1.4Mo0.3Ta0.3O12 (in general formula (2) , y=0.3, z=0.3) of Example 14 and Li5.9La3Zr1.4Mo0.5Ta0.1O12 (in general formula (2) , y=0.5, z=0.1) of Example 15.

[0093] Preferably, the Mo-and Ta-substituted garnet-type oxide of this embodiment has a cubic crystal structure. Regarding methods for evaluating the crystal structure, the powder X-ray diffraction (XRD) method described above can be used for determination. The Mo-and Ta-substituted garnet-type oxide solid electrolyte of this embodiment may include one or more other components, in addition to the Mo-and Ta-substituted garnet-type oxide, to an extent in which the ability of the solid electrolyte is not impaired. Examples of the other components include impurities derived from raw materials. Preferably, the Mo-and Ta-substituted garnet-type oxide solid electrolyte of this embodiment consists essentially only of the Mo-and Ta-substituted garnet-type oxide. The expression "consists essentially only of the Mo-and Ta-substituted garnet-type oxide" means that, in the Mo-and Ta-substituted garnet-type oxide solid electrolyte of this embodiment, a content of the Mo-and Ta-substituted garnet-type oxide may be 95%or greater and 100%or less, 98%or greater and 100%or less, or 99%or greater and 100%or less.

[0094] [First Step]

[0095] For the production of the garnet-type oxide represented by  general formula (2) , the raw material powders are prepared in a manner such that composition ratios (molar ratios) that satisfy general formula (2) are achieved, and the raw material powders are then mixed together. In the instance where the raw material powders are prepared in a manner such that the composition ratios (molar ratios) satisfy the value of y of less than 0.6, the value of z of less than 0.6, and the value of y+z of less than or equal to 0.6, the firing temperature and the densification temperature in the subsequent steps can be lower than those typically employed, and in addition, a reduction in the composition ratio of Li can be inhibited; consequently, the cubic crystal structure is maintained, which results in a high lithium ion conductivity. On the other hand, if the composition ratio of Mo+Ta is greater than 0.6, the composition ratio of Li is reduced, and, consequently, forming a cubic crystal structure becomes difficult. As a result, the lithium ion conductivity is significantly reduced, and reproducibility for the production is reduced. For example, when the composition ratio of Mo is 0.5, and the composition ratio of Ta is 0.1, which means that the composition ratio of Mo+Ta is 0.6, the composition ratio of Li is 5.9, and furthermore, when the composition ratio of Mo is 0.599, and the composition ratio of Ta is 0.001, which means that the composition ratio of Mo+Ta is 0.6, the composition ratio of Li is 5.801. These composition ratios of Mo+Ta and Li are the upper limit of the composition ratio of Mo+Ta (composition ratio of Mo+Ta of less than or equal to 0.6) and the lower limit of the composition ratio of Li (composition ratio of Li of greater than 5.8) for forming a cubic crystal structure with good reproducibility. Furthermore, the reduction in the composition ratio of Li during the production of the garnet-type oxide, with respect to the composition ratio that satisfies general formula (2) , can be inhibited as follows: for example, in instances where a Li raw material  such as LiNO3 that tends to volatilize in the second step is used, the Li raw material may be used in a 10%excess amount with respect to the amount corresponding to the composition ratio that satisfies general formula (2) .

[0096] The raw materials from which the lithium, the lanthanum, the zirconium, and the molybdenum are derived may be the same as those of the first embodiment. Examples of the raw material from which the tantalum is derived include oxides, such as tantalum oxide.

[0097] Preferably, the raw materials of the constituent components of formula (2) are powders. The average particle size of the powders is preferably less than or equal to 200 μm, more preferably less than or equal to 100 μm, and even more preferably less than or equal to 50 μm. The average particle size may be greater than or equal to 1 μm. Note that the average particle size of the powders can be measured with a known method, and examples of the method include length measurement by SEM observation, wet particle-size distribution measurement, and dry particle-size distribution measurement.

[0098] The first step of the production method of this embodiment may include a sub-step la and a sub-step lb. In the sub-step la, the raw materials necessary for the components are selected based on the composition of the Mo-and Ta-substituted garnet-type oxide that is to be synthesized. In the sub-step lb, the selected raw materials are mixed together. Furthermore, if necessary, the first step may further include a sub-step 1c, in which grinding is performed. The sub-step ic may be performed between the sub-step 1a and the sub-step lb or after the sub-step lb. The methods to be used for the mixing and the grinding are not particularly limited and may be known methods.

[0099] [Second Step]

[0100] The second step of the production method of this embodiment is the same as the second step of the first embodiment.

[0101] [Third Step]

[0102] The third step of the production method of this embodiment is the same as the third step of the first embodiment.

[0103] As illustrated in Fig. 2, the production method of this embodiment may be, for example, a production method that includes composition designing and raw material powder preparation and mixing steps, which correspond to the first step, a raw material powder firing step, which corresponds to the second step, and pelletization and densification sintering steps, which correspond to the third step. In addition, if necessary, an XRD measurement step, which is an inspection step, may be included.

[0104] [Composition Designing Step]

[0105] Composition designing is performed for designing a composition in which the Zr site of the garnet-type oxide having the fundamental composition of Li7La3Zr2O12 is partially substituted (doped) with Mo and Ta. For example, the composition designing is carried out such that general formula (2) is satisfied.

[0106] [Raw Material Powder Preparation and Mixing Step]

[0107] Raw material powders are prepared in accordance with the composition designed in the composition designing step, and then the raw material powders are mixed together. For example, only a Li raw material, such as LiNO3, may be used in a 10%excess amount with respect to the amount of the designed composition.

[0108] The raw material powder firing step, the pelletization step, the densification sintering step, and the XRD  measurement step of this embodiment are the same as the raw material powder firing step, the pelletization step, the densification sintering step, and the XRD measurement step of the first embodiment described above.

[0109] In the production methods of the present disclosure, the oxide solid electrolyte composition that enables the use of the firing temperature of less than or equal to 800℃ for the second step and the densification temperature of less than or equal to 800℃ for the third step is determined in the first step. Consequently, the production of a garnet crystal oxide solid electrolyte that can be co-sintered with an electrode made of, for example, LiCoO2 is made possible.

[0110] [EXAMPLES]

[0111] The present invention will now be described in more detail with reference to Examples. It should be noted that the present invention is not limited to the Examples.

[0112] [Raw Materials]

[0113] Lithium nitrate: LiNO3, manufactured by Kanto Chemical Co., Inc.

[0114] Lanthanum oxide: La2O3, manufactured by Kanto Chemical Co., Inc.

[0115] Zirconium oxide: ZrO2, manufactured by Kanto Chemical Co., Inc.

[0116] Molybdenum oxide: MoO3, manufactured by Kanto Chemical Co., Inc.

[0117] Tantalum oxide: Ta2O5, manufactured by Kanto Chemical Co., Inc.

[0118] [XRD Measurement]

[0119] Each of the pellets obtained in Examples and Comparative Examples was ground to a powder, which was then measured by XRD. The measurement system used was an Ultima IV,  manufactured by Rigaku Corporation, which was used with parallel beam optics, a scintillation counter detector, and a rotation stage. Each of the samples was loaded into a measurement sample holder having a depth of 0.5 mm, the measurement sample holder was then placed into the X-ray diffractometer (for XRD) , and the measurement was performed. The measurement conditions were as follows: Cu-Kα radiation; 40 kV and 40 mA; a scanning speed (2θ) of 2° / min; a step size (2θ) of 0.02°; and a scanning range (2θ) of 10° to 70°

[0120] (Examples 1 to 18 and Comparative Examples 1 to 3)

[0121] [First Step]

[0122] The compositions of the Examples and the Comparative Examples were designed as shown in Table 1. In accordance with each of the designed compositions, the raw materials shown in Table 1 (lithium nitrate, lanthanum oxide, zirconium oxide, molybdenum oxide, and tantalum oxide, listed above) were weighed according to the amounts shown in Table 1 and mixed together. In this manner, the raw material powders were prepared.

[0123] [Second Step]

[0124] The prepared raw material powders were fired at the powder firing temperature shown in Table 1 for 12 hours with a solid-state reaction method, to give fired powders.

[0125] [Third Step]

[0126] Each of the obtained fired powders was isostatically pressed at a pelletization pressure of 20 MPa to give a pellet. A periphery of the pellet was covered with the fired powder and fired at the densification temperature shown in Table 1 for 12 hours.

[0127] [Inspection Step]

[0128] The densified pellet was ground to a powder, and structural  analysis was performed on the powder with the XRD method described above. Figs. 3 to 5 are XRD patterns of the garnet-type oxide solid electrolytes obtained with the production methods of Example 3, Example 14, and Comparative Example 1, respectively. The results shown in Figs. 3 to 5 confirm that the formation of a garnet-type (cubic) oxide solid electrolyte, which is the target product, was achieved in the Examples.

[0129] The "Composition" , denoted by *1, represents the composition ratios (molar ratios) of the elements. Since the composition ratio (molar ratio) of the Zr site is 2, the composition ratio (molar ratio) of Zr+Mo (or Zr+Mo+Ta) is 2. Furthermore, since the Zr ion is tetravalent (Zr4+) , the Mo ion is hexavalent (Mo6+) , and the Ta ion is pentavalent (Ta5+) , if the composition ratio (molar ratio) of Mo increases by 0.1, and the composition ratio (molar ratio) of Zr decreases by 0.1, the composition ratio (molar ratio) of Li decreases by 0.2. Likewise, if the composition ratio (molar ratio) of Ta increases by 0.1, and the composition ratio (molar ratio) of Zr decreases by 0.1, the composition ratio (molar ratio) of Li decreases by 0.1. For example, in Example 3, since the composition ratio (molar ratio) of Mo is 0.3, the composition ratio (molar ratio) of Zr is 1.7, and the composition ratio (molar ratio) of Li is 6.4; therefore, the formula is Li6.4La3Zr1.7Mo0.3O12, according to general formula (1) . Furthermore, in Example 14, since the composition ratio (molar ratio) of Mo is 0.3, and the composition ratio (molar ratio) of Ta is 0.3, the composition ratio (molar ratio) of Zr is 1.4, and the composition ratio (molar ratio) of Li is 6.1; therefore, the formula is Li6.1La3Zr1.4Mo0.3Ta0.3O12, according to general formula (1) . The symbol "N" , denoted by *2, means "not a cubic single phase" . "Not a cubic single phase" means "having a crystal structure other than the cubic structure" or "including the cubic structure and a different crystal structure" .

[0130] [Discussion]

[0131] Based on the results shown in Table 1 and Figs. 3 to 5, the following conclusion can be made. In Examples 1 to 18, the methods for producing an oxide solid electrolyte represented by general formula (1) or (2) included the second step involving the use of the powder firing  temperature of less than or equal to 800℃ and the third step involving the use of the densification temperature of less than or equal to 800℃, and in this regard, the methods are different from those of Comparative Examples 1 to 3. As a result, in the instances where any of the production methods of Examples 1 to 18 was used, the production of a garnet crystal oxide solid electrolyte that can be co-sintered with an electrode made of LiCoO2 was made possible.[Industrial Applicability]

[0132] The methods of the present embodiments (e.g., the first embodiment and the second embodiment) for producing a garnet crystal oxide solid electrolyte enable the production of a garnet crystal oxide solid electrolyte that can be co-sintered with an electrode made of LiCoO2. The garnet crystal oxide solid electrolytes produced by the production methods of the present embodiments are expected to be used in applications such as those in solid electrolytes that are used in all-solid-state lithium ion secondary batteries.

Claims

1.A method for producing an oxide solid electrolyte that includes a garnet-type oxide represented by general formula (1) below: Li (7-2x) La3Zr (2-x) MoxO12    (1)where x is greater than 0 and less than or equal to 0.6, the method comprising:a first step of preparing raw material powders in a manner such that composition ratios that satisfy general formula (1) are achieved, the composition ratios being molar ratios;a second step of firing the prepared raw material powders at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, thereby synthesizing a fired powder; anda third step of pelletizing the synthesized fired powder to form a pellet and subsequently firing the pellet at a densification temperature of less than or equal to 800℃, thereby densifying the pellet.2.The method for producing an oxide solid electrolyte according to Claim 1, wherein the garnet-type oxide represented by general formula (1) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo.3.A method for producing an oxide solid electrolyte that includes a garnet-type oxide represented by general formula (2) below: Li (7-2y-z) La3Zr (2-y-z) MoyTazO12    (2)where y is greater than 0 and less than 0.6, z is greater than 0 and less than 0.6, and y+z is less than or equal to 0.6,the method comprising:a first step of preparing raw material powders in a manner such that composition ratios that satisfy general formula (2) are achieved, the composition ratios being molar ratios;a second step of firing the prepared raw material powders at a firing temperature of less than or equal to 800℃ with a solid-state reaction method, thereby synthesizing a fired powder; anda third step of pelletizing the synthesized fired powder to form a pellet and subsequently firing the pellet at a densification temperature of less than or equal to 800℃, thereby densifying the pellet.4.The method for producing an oxide solid electrolyte according to Claim 3, wherein the garnet-type oxide represented by general formula (2) is an oxide based on a Li7La3Zr2O12 garnet-type oxide and having a Zr site partially substituted with Mo and Ta.5.The method for producing an oxide solid electrolyte according to any one of Claims 1 to 4, wherein the firing temperature in the second step is 700℃ to 800℃, and the densification temperature in the third step is 700℃ to 800℃.

Citation Information

Patent Citations

  • Gallium and molybdenum co-doped garnet type lithium ion solid electrolyte and preparation method thereof

    CN108832173A

  • Solid electrolyte and all-solid-state battery

    CN109830740A

  • Preparation method of high-conductivity solid-state battery electrolyte for energy storage charging system battery

    CN113161607A

  • Ta element doped LLZO composite solid electrolyte and low-temperature preparation method and application thereof

    CN115149091A