Easy-to-identify tensile type b1-class metro rail transit cable and preparation method therefor
By using nylon material and special mold extrusion technology, combined with braided soft copper tape and copper shielding, the problem of insufficient performance of the outer skin material of the traffic cable is solved, and the improvement of conductor and insulation performance and mechanical performance are achieved to ensure the thermal of the cable Stability and wear resistance.
Patent Information
- Application Number
- PCT/CN2023/102569
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-06-27
- Publication Date
- 2024-12-05
AI Technical Summary
The performance of the existing transportation cable outer skin material is poor, the conductor DC resistance, insulation resistance and voltage resistance test performance are insufficient, and the problems of depression, scratches and difficulty in temperature control are prone to occur during the preparation process.
Use nylon material as cable jacket and extruded through a special mold and extruder. Combined with braided soft copper tape, steel armor and copper shielding, the extrusion temperature and cooling process are controlled to ensure uniform molding and tightness of the nylon sheath Cover to avoid depressions and scratches while using filler and copper shields to improve the mechanical and electrical properties of the cable.
It improves the conductor DC resistance, insulation resistance and voltage resistance of the cable, prevents bending, depression and scratches of the nylon sheath, ensures the thermal stability and wear resistance of the discharge, and enhances the overall performance of the cable.
Smart Images

Figure CN2023102569_05122024_PF_FP_ABST
Abstract
Description
An easily identifiable tensile-resistant B1-grade subway rail transit cable and its preparation method Technical Field
[0001] The present invention relates to the field of cables, and in particular to an easily identifiable tensile-resistant B1-level subway rail transit cable and a preparation method thereof. Background Art
[0002] A cable is a device for transmitting electrical energy or signals, usually composed of several or several groups of wires. Cables include power cables, control cables, compensation cables, shielded cables, high-temperature cables, computer cables, signal cables, coaxial cables, fire-resistant cables, marine cables, mining cables, aluminum alloy cables, etc. They are all composed of single or multiple wires and an insulation layer, and are used to connect circuits, electrical appliances, etc.
[0003] Most of the existing transportation cable sheath materials have poor performance. The performance of their conductor DC resistance, insulation resistance and voltage withstand test is mediocre and cannot be further improved. In addition, they are prone to dents and scratches during their preparation. There is a lack of better means of temperature control when the sheath is discharged, and they are prone to being unable to stretch, yellowing and thinning.
[0004] Therefore, it is necessary to propose an easily identifiable tensile-resistant B1-level subway rail transit cable and a preparation method thereof to solve the above problems.
[0005] Summary of the Invention
[0006] The main purpose of the present invention is to provide an easily identifiable tensile-resistant B1-level subway rail transit cable and a preparation method thereof, which can effectively solve the problems in the background technology.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] A readily identifiable tensile-resistant B1-grade subway rail transit cable comprises a cable body, the inner wall of the cable body being fixedly connected to a nylon sleeve, the inner wall of the nylon sleeve being fixedly connected to a braided soft copper belt, the inner wall of the braided soft copper belt being fixedly connected to a steel armor, the inner wall of the steel armor being filled with a filling glue, the inner wall of the filling glue being fixedly connected to a copper shielding layer, and the inner cavity of the copper shielding layer being fixedly connected to a wire core.
[0009] A method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable comprises nylon material, a braided soft copper tape, steel armor, a filling rubber, and a copper shielding layer, and includes the following steps:
[0010] S1: Dry the nylon material and preheat the wire core: Test the moisture content of the nylon material and perform subsequent work based on the moisture content. If the moisture content is high, use a vacuum drying suction machine to transport the nylon material. If the moisture content is normal, directly suck it into the hopper for extrusion. When the nylon sheath is extruded, preheat the wire core online, and the preheating temperature is controlled at 60-90 degrees.
[0011] S2: Mould selection: Use a special mould. In the selection of the mould, in order to adapt to the thin-wall extrusion of the nylon sheath, the matching requirements of the mould core and the mould sleeve must be strictly implemented. During production, the mould core and the diverter should be kept in close fit, otherwise the glue will leak from the thread gap. The aperture size of the nylon extrusion mould is mainly determined by the diameter of the wire and the thickness of the nylon. The specific calculation of the mould size is calculated according to the formula: d = d1 + 1-2, D = d + 2t + 3e + 2, where d = inner diameter of the mould core (mm), d1 = outer diameter of the insulation (mm), D = inner diameter of the mould sleeve (mm), t = wall thickness of the mould core (mm), and e = thickness of the nylon sheath (mm).
[0012] S3: Extrusion screw: When performing screw extrusion, the screw parameters are: screw diameter is less than 60mm, aspect ratio is between 20:1 and 25:1, compression ratio range is 3.5:1 to 4:1. During extrusion, the temperature is controlled, and the temperature is controlled in different intervals, where zone 1 is 180 degrees, zone 2 is 200 degrees, zone 3 is 200 degrees, zone 4 is 215 degrees, zone 5 is 220 degrees, and zone 6 is 250 degrees. According to the above requirements, the nylon material is placed in the extruder for extrusion;
[0013] S4: Extrusion: To ensure uniform nylon extrusion and establish a stable melt pressure in the barrel, a diverter is required, as well as a sieve plate and screen at the connection between the neck and the head. The sieve plate and screen convert the rotational motion of the nylon flow in the screw into linear motion, while filtering out particles and impurities. The screen requirements are: 20 mesh + 80 mesh + 20 mesh, a total of three layers;
[0014] S5: Molding cooling: After the nylon material is extruded, it is cooled. During molding, the shrinkage rate of nylon is large and the directionality is obvious. It is easy to produce defects such as shrinkage holes, dents, and deformation. The molding process conditions must be strictly controlled. The melting point of nylon material is 215 degrees. At the melting point, it is amorphous and has no crystalline components. However, as the temperature decreases, nylon crystals will gradually form. The starting temperature of crystal formation is 185 degrees and the termination temperature is 71 degrees. During production, the extruded nylon forms crystals in the air or cooling water. The size of the crystals depends on the cooling temperature and cooling time. Only sufficient cooling can increase the shrinkage rate of the nylon sheath, make it tightly wrapped, and increase wear resistance. Nylon extrusion molding cooling is divided into three parts, including natural air cooling, warm water cooling, and cold water cooling. The air cooling length is about half a meter, the hot water cooling temperature is 43-60 degrees, and the water tank length is about 1-3.5 meters.
[0015] S6: Make the cable ends and install the cables: including the following steps:
[0016] A: Split one end of the braided soft copper tape into three equal parts in advance, re-weave them and wrap them around each phase shield layer respectively. Tie them tightly and then weld them to the copper tape. Tie the other braided wire with a tie wire and weld it to the steel armor.
[0017] B: Install the branch finger sleeve: Wrap the filling glue around the three-phase bifurcation and the root to make the appearance flat and slightly apple-shaped. The maximum diameter should be about 15mm larger than the outer diameter of the cable. Clean the nylon sleeve and put it into the branch finger sleeve, making it as close to the root of the core wire as possible. Then, use a slow fire ring to heat and shrink it from the root of the finger sleeve to both ends, first downward and then upward. After it is completely shrunk, a small amount of glue should be squeezed out from the end.
[0018] C: Stripping and cutting the phase shield and semi-conductive layer: From the finger end of the branch glove upwards 55mm copper shield, tie with copper wire, cut the shielding tape, the fracture should be neat, strip the outer semi-conductive layer, and retain the outer semi-conductive layer 20mm away from the copper shield opening. The stripping should be clean, but the core insulation should not be damaged. The remaining outer semi-conductive layer can be cleaned with a detergent or polished with fine sandpaper;
[0019] D: Install the stress control tube: Clean the insulation shield and copper tape shield surface, clean the core insulation surface, make sure there is no carbon trace on the insulation surface, insert the stress control tube, overlap the lower part of the stress control tube with the copper shield by more than 20mm, and heat the stress control tube with a low flame from top to bottom to shrink it;
[0020] E: Crimping terminals: Determine the lead length, strip the main insulation, and cut the stripped end into a "pencil head" shape. Crimping the terminal, use emery cloth or a wood file to smooth out any unevenness, clean the surface, and fill the gaps between the insulation and the terminal as well as the pressure pits with filler tape. The filler tape should overlap the wire core insulation and the terminal by 5-10mm to ensure a smooth transition.
[0021] F: Install the insulating tube: clean the surface of the wire core insulation, stress tube and branch glove, put the insulating tube on the root of the three-pronged fork, the upper end of the tube should be overfilled with glue by more than 510mm, heat and shrink from the root upwards and cut off the excess insulating tube of the terminal after heating, install the auxiliary tube and phase color tube, put the auxiliary tube on the terminal connecting pipe, preheat the terminal first, heat and shrink from the top end, then put the phase color tube on the terminal connecting pipe or heat and shrink a little further down, and now the cable head is installed.
[0022] Preferably, when the water content of the nylon material is higher than 3%, it needs to be dried. At the same time, the unpacked nylon material cannot be exposed to the air for too long, not more than forty-five minutes.
[0023] Preferably, the surface finish of the mold is very important for the extrusion of the nylon sheath, especially the mating area between the mold core and the mold sleeve. Any defects will cause dents or scratches on the nylon sheath. Therefore, the surface finish should be checked before and after each use of the mold. In addition, during the mold replacement process, the inner cavity and related components of the machine head should be cleaned to remove the glue, impurities and burnt particles attached to it.
[0024] Preferably, the nylon is in a viscous flow state when melted, so an extruder with a small gap between the cylinder and the screw should be selected, the gap being about 0.15 mm, and the temperature deviation of each interval being controlled within ±2 degrees. During extrusion, attention should be paid to the temperature of the extruder neck to make it equal to the melting point of the nylon material, and the temperature of the mold core should not be lower than the crystallization temperature of 181 degrees.
[0025] Preferably, in order to make the sheath tightly extruded, reduce the tensile stress of nylon during the extrusion process, and improve the mechanical properties of the finished product, the nylon sheath is extruded by vacuum extrusion, and the vacuum pressure is based on not causing the nylon to fall back.
[0026] Preferably, when preparing the nylon sheath, attention should be paid to moisture-proofing of the material, accurate adjustment of the mold concentricity before starting the machine, and the insulation time should be maintained within fifteen minutes after the temperature reaches the set value. The mold core temperature should be greater than 181 degrees during vacuuming, the stretching ratio of nylon extrusion is 8:1-14:1, the stretching length should be greater than 6.35mm, and the entire part should be immersed in water during cooling. Beneficial effects
[0027] Compared with the prior art, the present invention provides an easily identifiable tensile-resistant B1-level subway rail transit cable and a preparation method thereof, which has the following beneficial effects:
[0028] 1. The easily identifiable tensile-resistant B1-class subway rail transit cable and its preparation method. In the present invention, nylon is used as the outer jacket of the transportation cable, so that the cable has good electrical properties, including good performance in the conductor DC resistance, insulation resistance and withstand voltage test, and its mechanical properties are also good. During preparation, the outer jacket can be prevented from bending and wrinkling, and the nylon sheath can be prevented from being dented and scratched. By controlling the extrusion temperature of the nylon, the yellowing, thinning, and inability to stretch the material due to excessively high temperature can be prevented. It can also be avoided that the temperature is too low and the material is crystallized prematurely, causing the material to be difficult to discharge. In this way, the thermal stability of the nylon in the molten state is improved, and it is not easy to degrade and reduce the performance of the sheath. At the same time, during production, when the extruded nylon forms crystals in the air or cooling water, ensuring the cooling temperature and cooling time can effectively increase the shrinkage rate of the nylon sheath, making it tightly coated and increasing the wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] FIG1 is a schematic structural diagram of a cable body according to the present invention;
[0030] FIG2 is an enlarged view of point A in FIG1 of the present invention.
[0031] In the figure: 1. Cable body; 2. Nylon sleeve; 3. Braided soft copper tape; 4. Steel armor; 5. Filling glue; 6. Copper shielding layer; 7. Wire core. DETAILED DESCRIPTION
[0032] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is further described below in conjunction with specific implementation methods.
[0033] Specific embodiment one:
[0034] As shown in Figure 1-2, an easily identifiable tensile-resistant B1-level subway rail transit cable includes a cable body 1, a nylon sleeve 2 is fixedly connected to the inner wall of the cable body 1, a braided soft copper tape 3 is fixedly connected to the inner wall of the nylon sleeve 2, a steel armor 4 is fixedly connected to the inner wall of the braided soft copper tape 3, the inner wall of the steel armor 4 is filled with filling glue 5, the inner wall of the filling glue 5 is fixedly connected to a copper shielding layer 6, and a wire core 7 is fixedly connected to the inner cavity of the copper shielding layer 6.
[0035] A method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable comprises a nylon material, a braided soft copper tape 3, a steel armor 4, a filling glue 5, and a copper shielding layer 6, and includes the following steps:
[0036] S1: Drying the nylon material and preheating the core 7: Test the moisture content of the nylon material and perform subsequent work based on the moisture content. When the moisture content is high, use a vacuum drying and suction machine to transport the nylon material. If the moisture content is normal, directly suck it into the hopper for extrusion. When the core 7 is extruded into the nylon sheath, it is preheated online. The preheating temperature is controlled at 60-90 degrees. When the moisture content of the nylon material is higher than 3%, it needs to be dried. At the same time, the unpacked nylon material cannot be exposed to the air for too long, and cannot exceed 45 minutes.
[0037] S2: Mold selection: Use a special mold. In the selection of the mold, in order to adapt to the thin-wall extrusion of the nylon sheath, the matching requirements of the mold core and the mold sleeve must be strictly implemented. During production, the mold core and the diverter should be kept closely matched, otherwise the glue will leak from the thread gap. The aperture size of the nylon extrusion mold is mainly determined by the diameter of the wire and the thickness of the nylon. The specific calculation of the mold size is calculated according to the formula: d = d1 + 1-2, D = d + 2t + 3e + 2, where d = the inner diameter of the mold core mm, d1 = insulation outer diameter (mm), D = mold sleeve inner diameter (mm), t = mold core wall thickness (mm), e = nylon sheath thickness (mm). The surface finish of the mold is very important for the extrusion of the nylon sheath, especially the mold core and mold sleeve matching area. Any defects will cause dents or scratches on the nylon sheath. Therefore, the surface finish should be checked before and after each use of the mold. In addition, when the mold is replaced, the inner cavity and related components of the die head should be cleaned to remove the glue, impurities and burnt particles attached to it.
[0038] S3: Extrusion screw: When performing screw extrusion, the parameters of the screw are: screw diameter is less than 60mm, aspect ratio is between 20:1 and 25:1, compression ratio range is 3.5:1 to 4:1, and the temperature is controlled during extrusion. The temperature is controlled in intervals, where zone 1 is 180 degrees, zone 2 is 200 degrees, zone 3 is 200 degrees, zone 4 is 215 degrees, zone 5 is 220 degrees, and zone 6 is 250 degrees. According to the above requirements, the nylon material is placed in the extruder for extrusion. Nylon is in a viscous flow state when melted, so an extruder with a smaller gap between the machine shell and the screw should be selected, with a gap of about 0.15mm. The temperature deviation of each interval is controlled within ±2 degrees. During extrusion, attention should be paid to the temperature of the extruder neck to make it equal to the melting point of the nylon material, and the temperature of the mold core should not be lower than the crystallization temperature of 181 degrees.
[0039] S4: Extrusion: To ensure uniform nylon extrusion and establish a stable melt pressure in the barrel, a diverter is required, as well as a sieve plate and screen at the connection between the neck and the head. The sieve plate and screen convert the rotational motion of the nylon flow in the screw into linear motion, while filtering out particles and impurities. The screen requirements are: 20 mesh + 80 mesh + 20 mesh, a total of three layers. In order to make the sheath tightly extruded, reduce the tensile stress of the nylon during the extrusion process, and improve the mechanical properties of the finished product, the nylon sheath is extruded by vacuum extrusion. The vacuum pressure is based on the principle of not causing the nylon to fall back.
[0040] S5: Molding cooling: After the nylon material is extruded, it is cooled. During molding, the shrinkage rate of nylon is large and the directionality is obvious. It is easy to produce defects such as shrinkage holes, dents, and deformation. The molding process conditions must be strictly controlled. The melting point of nylon material is 215 degrees. At the melting point, it is amorphous and has no crystalline components. However, as the temperature decreases, nylon crystals will gradually form. The starting temperature of crystal formation is 185 degrees and the termination temperature is 71 degrees. During production, the extruded nylon forms crystals in the air or cooling water. The size of the crystals depends on the cooling temperature and cooling time. Only by sufficient cooling can the shrinkage rate of the nylon sheath be increased to make it wrap. The coverage is tight and the wear resistance is increased. The cooling process of nylon extrusion molding is divided into three parts, including natural air cooling, warm water cooling and cold water cooling. The air cooling length is about half a meter, the hot water cooling temperature is 43-60 degrees, and the water tank length is about 1-3.5 meters. When preparing the nylon sheath, attention should be paid to moisture-proofing of the material, accurate adjustment of the mold concentricity before starting the machine, and after the temperature reaches the set value, the insulation time should be maintained within fifteen minutes. The core temperature should be greater than 181°C during vacuuming. The stretch ratio of nylon extrusion is 8:1-14:1, and the stretch length should be greater than 6.35mm. At the same time, it should be fully immersed in water during cooling.
[0041] S6: Make the cable ends and install the cables: including the following steps:
[0042] A: Split one end of the braided soft copper tape 3 into three equal parts in advance, re-weave them around each phase shield layer and tie them tightly, then weld them to the copper tape. Tie the other braided wire with a tie wire and weld it to the steel armor 4.
[0043] B: Install the branch finger sleeve: Wrap the filling glue 5 at the three-phase bifurcation and the root to make the appearance flat and slightly apple-shaped. The maximum diameter should be about 15mm larger than the outer diameter of the cable. Clean the nylon sleeve 2 and put it into the branch finger sleeve, making it as close to the root of the core wire as possible. Then, use a slow fire ring to heat and shrink it from the root of the finger sleeve to both ends, first downward and then upward. After it is completely shrunk, a small amount of glue should be squeezed out from the end.
[0044] C: Stripping and cutting the phase shield and semi-conductive layer: From the fingertip of the branch glove upward 55mm, tie with copper wire 6 times, cut the shielding tape, and make sure the cut is neat. Strip the outer semi-conductive layer, leaving the outer semi-conductive layer 20mm away from the copper shield opening. Strip cleanly, but do not damage the insulation of the core 7. The remaining outer semi-conductive layer can be cleaned with a detergent or polished with fine sandpaper.
[0045] D: Install the stress control tube: Clean the insulation shield and copper tape shield surface, clean the insulation surface of core 7, make sure there is no carbon trace on the insulation surface, insert the stress control tube, overlap the lower part of the stress control tube with the copper shield by more than 20mm, and heat the stress control tube with a low flame from top to bottom to shrink it;
[0046] E: Crimping terminals: Determine the lead length, strip the main insulation, and cut the stripped end into a "pencil head" shape. Crimping the terminal, use emery cloth or a wood file to smooth out any unevenness, clean the surface, and fill the gap between the insulation and the terminal and the pressure pit with filler tape 5. The filler tape should overlap the wire core 7 insulation and the terminal by 5-10mm to make a smooth transition.
[0047] F: Install the insulating tube: clean the insulating surface of the wire core 7, the stress tube and the branch glove surface, put the insulating tube on the root of the three-pronged fork, the upper end of the tube should be filled with glue for more than 510mm, heat and shrink from the root upwards and cut off the excess insulating tube of the terminal after heating, install the auxiliary tube and the phase color tube, put the auxiliary tube on the terminal connecting pipe, preheat the terminal first, heat and shrink from the top end, then put the phase color tube on the terminal connecting pipe or heat and shrink a little further down, and now the cable head is installed.
[0048] Specific embodiment two:
[0049] The following table shows the performance test data of the traffic cable prepared by the present invention.
[0050] This is a graph showing the test results, from which it can be seen that the traffic cable prepared by the present invention has good performance in deformation performance, flame retardancy, wear resistance and oil immersion test.
[0051] The present invention uses nylon as the outer jacket of the transportation cable, so that the cable has good electrical properties, including good performance in the conductor DC resistance, insulation resistance and withstand voltage test, and its mechanical properties are also good. During preparation, the outer jacket can be prevented from bending and wrinkling, and the nylon sheath can be prevented from being dented and scratched. By controlling the extrusion temperature of the nylon, the yellowing, thinning and inability to stretch the output material due to excessively high temperature can be prevented, and the premature crystallization due to excessively low temperature, which causes the output material to be difficult, can be avoided. In this way, the thermal stability of the nylon in the molten state can be improved, and it is not easy to degrade and cause the performance of the sheath to deteriorate. At the same time, during production, when the extruded nylon forms crystals in the air or cooling water, ensuring the cooling temperature and cooling time can effectively increase the shrinkage rate of the nylon sheath, make it tightly coated, and increase the wear resistance.
[0052] The basic principles, main features, and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.
Claims
1. An easily identifiable tensile-resistant B1-level subway rail transit cable, comprising a cable body (1), characterized in that: The inner wall of the cable body (1) is fixedly connected to a nylon sleeve (2), the inner wall of the nylon sleeve (2) is fixedly connected to a braided soft copper belt (3), the inner wall of the braided soft copper belt (3) is fixedly connected to a steel armor (4), the inner wall of the steel armor (4) is filled with a filling glue (5), the inner wall of the filling glue (5) is fixedly connected to a copper shielding layer (6), and the inner cavity of the copper shielding layer (6) is fixedly connected to a wire core (7).
2. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 1 comprises nylon material, a braided soft copper tape (3), a steel armor (4), a filling glue (5), and a copper shielding layer (6), characterized in that: The steps include: S1: Drying the nylon material and preheating the wire core (7): Testing the moisture content of the nylon material, and performing subsequent work according to the moisture content. When the moisture content is high, a vacuum drying suction machine is used to transport the nylon material. If the moisture content is normal, the nylon material is directly sucked into the hopper for extrusion. When the nylon sheath is extruded, the wire core (7) is preheated online, and the preheating temperature is controlled at 60 to 90 degrees. S2: Mold selection: Use special molds. In the selection of molds, in order to adapt to the thin-wall extrusion of nylon sheaths, the matching requirements of the mold core and the mold sleeve must be strictly implemented. During production, the mold core and the diverter should be kept in close cooperation, otherwise the stored glue will leak from the thread gap. The aperture size of the nylon extrusion mold is mainly determined by the diameter of the wire and the thickness of nylon. The specific calculation of the mold size is calculated according to the formula: d = d1 + (1-2), D = d + 2t + 3e + 2, where d = mold core inner diameter (mm), d1 = insulation outer diameter (mm), D = mold sleeve inner diameter (mm), t = mold core wall thickness (mm), e = nylon sheath thickness (mm); S3: Extrusion screw: When the screw is extruded, the parameters of the screw are: the screw diameter is less than 60mm, the aspect ratio is between 20:1 and 25:1, and the compression ratio is between 3.5:1 and 4:
1. When the extrusion is carried out, the temperature is controlled, and the temperature is controlled in different intervals, where the first zone is 180 degrees, the second zone is 200 degrees, the third zone is 200 degrees, the fourth zone is 215 degrees, the fifth zone is 220 degrees, and the sixth zone is 250 degrees. According to the above requirements, the nylon material is placed in the extruder for extrusion; S4: Extrusion: To ensure uniform nylon extrusion, a stable melt pressure is established in the barrel. It is necessary to equip a flow divider, as well as a sieve plate and a screen at the connection between the machine neck and the machine head. The sieve plate and the screen transform the rotational motion of the nylon flow in the screw into a linear motion, and filter out particles and impurities at the same time. The requirements for the screen are: 20 mesh + 80 mesh + 20 mesh, a total of three layers; S5: Molding cooling: After the nylon material is extruded, it is cooled. During molding, the shrinkage rate of nylon is large and the directionality is obvious. It is easy to produce defects such as shrinkage holes, dents, and deformation. The molding process conditions must be strictly controlled. The melting point of nylon material is 215 degrees. At the melting point temperature, it is amorphous and has no crystalline components. However, as the temperature decreases, nylon crystals will gradually form. The starting temperature of crystal formation is 185 degrees and the termination temperature is 71 degrees. In production, the extruded nylon forms crystals in the air or cooling water. The size of the crystals depends on the cooling temperature and cooling time. Only when the cooling is sufficient can the shrinkage rate of the nylon sheath be increased, so that it can be tightly wrapped and the wear resistance can be increased. The cooling of nylon extrusion molding is divided into three parts, including natural air cooling, warm water cooling, and cold water cooling. The air cooling length is about half a meter, the hot water cooling temperature is 43 to 60 degrees, and the water tank length is about 1 to 3.5 meters. S6: Make the cable ends and install the cables: including the following steps: A: Split one end of the braided soft copper tape (3) in advance and divide it into three equal parts. After re-braiding, wrap them around the shielding layers of each phase respectively and tie them tightly. Then weld them to the copper tape. Tie the other braided wires with a tie wire and weld them to the steel armor (4). B: Install the branch finger sleeve: Wrap the filling glue (5) around the three-phase bifurcation and the root to make it smooth and slightly apple-shaped, with a maximum diameter about 15mm larger than the outer diameter of the cable. Clean the nylon sleeve (2) and put it into the branch finger sleeve, making it as close to the root of the core wire as possible. Then use a slow fire ring to heat from the root of the finger sleeve to both ends, first downward and then upward to shrink and fix it. After it is completely shrunk, a small amount of glue should be squeezed out from the end; C: Stripping and cutting the phase shield and semi-conductive layer: From the finger tip of the branch glove, 55mm above the copper shield layer (6), tie with copper wire, cut the shield tape, and make sure the cut is neat. Strip the outer semi-conductive layer, leaving 20mm of the outer semi-conductive layer away from the copper shield opening. Strip cleanly, but do not damage the insulation of the wire core (7). The remaining outer semi-conductive layer can be wiped clean with a cleaning agent or polished with fine sandpaper; D: Install the stress control tube: Clean the insulation shield and copper tape shield surface, clean the insulation of the wire core (7) Insulate the surface, make sure there is no carbon trace on the insulating surface, insert the stress tube, overlap the lower part of the stress tube with the copper shield by more than 20mm, and heat the stress tube from top to bottom with a low flame to shrink it; E: Crimping the terminal: Determine the lead length, strip the main insulation, and cut the stripped end into a "pencil head" shape. Crimping the terminal, use sandpaper or a wood file to file the uneven parts, clean the surface, and use filling glue (5) to fill the space between the insulation and the terminal and the pressure pit. The filling tape and the wire core (7) insulation and the terminal should overlap by 5-10mm to make a smooth transition; F: Install the insulating tube: Clean the insulating surface of the wire core (7), the stress tube and the branch glove surface, and put the insulating tube on the root of the three-pronged fork. The upper end of the tube should be more than 10mm beyond the filling glue (5). Heat and shrink from the root upwards and cut off the excess insulating tube of the terminal after heating. Install the auxiliary tube and phase color tube. Put the auxiliary tube on the terminal connection part, preheat the terminal first, heat and shrink from the upper end, and then put the phase color tube on the terminal connection or a little lower to heat and shrink. At this point, the cable head is installed.
3. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 2, characterized in that: When the water content of the nylon material is higher than 3%, it needs to be dried. At the same time, the unpacked nylon material cannot be exposed to the air for too long, not more than forty-five minutes.
4. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 2, characterized in that: The surface finish of the mold is very important for the extrusion of the nylon sheath, especially the matching area between the mold core and the mold sleeve. Any defects will cause dents or scratches on the nylon sheath. Therefore, the surface finish should be checked before and after each use of the mold. In addition, during the mold replacement process, the inner cavity and related components of the machine head should be cleaned to remove the glue, impurities and coke particles attached to it.
5. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 2, characterized in that: The nylon is in a viscous flow state when melted, so an extruder with a smaller gap between the cylinder and the screw should be selected, the gap is about 0.15mm, and the temperature deviation of each interval is controlled within ±2 degrees. During extrusion, attention should be paid to the temperature of the extruder neck to make it equal to the melting point of the nylon material, and the temperature of the mold core should not be lower than the crystallization temperature of 181 degrees.
6. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 2, characterized in that: In order to make the sheath tightly extruded, reduce the tensile stress of nylon during the extrusion process, and improve the mechanical properties of the finished product, the nylon sheath is extruded by vacuum tube extrusion, and the vacuum pressure is based on not causing the nylon to fall back.
7. The method for preparing an easily identifiable tensile-resistant B1-level subway rail transit cable according to claim 2, characterized in that: When preparing the nylon sheath, attention should be paid to moisture-proofing of the material, accurate adjustment of the mold concentricity before starting the machine, and the insulation time should be maintained within fifteen minutes after the temperature reaches the set value. The mold core temperature should be greater than 181 degrees during vacuuming. The stretching ratio of nylon extrusion is 8:1-14:1, and the stretching length should be greater than 6.35mm. At the same time, it should be fully immersed in water during cooling.
Citation Information
Patent Citations
High-temperature resistant and shock-absorption rail traffic locomotive cable
CN108648865A
High-strength anti-friction type rail traffic locomotive cable
CN108666024A
Physical rat-proof and termite-proof cable
CN115631885A
Technology for producing PVC insulated nylon flexible wire using double machine extruding method
CN1595547A
Electromagnetically screened electrical data communications cable
DE19535305A1
Cited By
Heat-dissipation joint device of fireproof cable
CN119627475A