Antistatic polyester film and preparation method therefor

By using aluminum-doped zinc oxide to coat nanobarium sulfate antistatic coating on polyester films on the online coating method, the problem that polyester films are difficult to have long-lasting antistatic while maintaining mechanical and optical properties is solved, and the polyester films are realized. The long-lasting anti-static and smooth properties of polyester films avoid adhesion and maintain the optical and mechanical properties of the film.

WO2024244269A1PCT designated stage expired Publication Date: 2024-12-05NINGBO CHANGYANG TECH +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/127060
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-10-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing anti-static polyester films are difficult to have long-lasting anti-static properties while maintaining mechanical and optical properties, and are prone to adhesion during the production process, affecting transparency and adhesion.

Method used

The polyester film is coated with an antistatic coating containing aluminum-doped zinc oxide coated nanobarium sulfate on the surface of the polyester film by online coating. The aluminum-doped zinc oxide coated nanobarium sulfate particles are prepared by hydrothermal method to form a core-shell structure. The antistatic agent avoids the influence on transparency and mechanical properties, and plays an opening role through tiny protrusions to prevent adhesion.

Benefits of technology

The long-lasting antistatic properties and smoothness of polyester films are achieved, which avoids adhesion phenomena, while maintaining the optical and mechanical properties of the films, and the process is environmentally friendly and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023127060-FTAPPB-I100001
    Figure PCTCN2023127060-FTAPPB-I100001
  • Figure PCTCN2023127060-FTAPPB-I100002
    Figure PCTCN2023127060-FTAPPB-I100002
  • Figure PCTCN2023127060-FTAPPB-I100003
    Figure PCTCN2023127060-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention relates to the field of plastic material forming and processing. Disclosed are an antistatic polyester film and a preparation method therefor. The antistatic polyester film comprises a polyester base film and an antistatic coating. The antistatic coating solution forming the antistatic coating comprises: 10-15 wt% of water-based resin, 0.1-3 wt% of a cross-linking agent, 0.01-2 wt% of an aluminum-doped zinc oxide coated nano-barium sulfate antistatic agent, 0.002-0.3 wt% of a wetting agent, and 0.002-0.2 wt% of a pH regulator, the balance being water. According to the present invention, an antistatic coating containing an aluminum-doped zinc oxide coated nano-barium sulfate antistatic agent is coated on the surface of a polyester base film by using an in-line coating method, which can enable the polyester base film to have lasting excellent antistatic performance while maintaining the original optical performance and mechanical performance. In addition, the polyester film is provided an excellent opening effect, thereby effectively preventing adhesion during the rolling process.
Need to check novelty before this filing date? Find Prior Art

Description

Antistatic polyester film and preparation method thereof Technical Field

[0001] The invention relates to the field of plastic material forming and processing, in particular to an antistatic polyester film and a preparation method thereof. Background Art

[0002] Biaxially oriented polyester film, due to its high transparency, high tensile strength, excellent stiffness, and superior dimensional stability, temperature resistance, electrical properties, gas barrier properties, and chemical resistance, has found widespread application in the electrical, insulation, packaging, transfer printing, display, and window film industries. However, as an insulating material, polyester has a high surface resistivity, making it susceptible to static electricity during production and use due to friction with itself or other materials. This static electricity causes polyester film to easily absorb dust, affecting product properties such as light transmittance and haze. It can also lead to a range of problems, such as reduced adhesion and poor bonding of subsequent functional layers. Therefore, imparting antistatic properties to polyester film is crucial.

[0003] In view of the above-mentioned shortcomings of polyester film, the method of adding antistatic agents is generally used to give polyester film antistatic properties. There are mainly two methods: internal addition method (the antistatic agent is mixed and evenly melted with polyester chips to make polyester film) and coating method (the liquid containing the antistatic agent is applied to the surface of the polyester film).

[0004] Because the internal addition method involves melting polyester chips, the antistatic agent must be heat-resistant, resulting in a limited selection. Unfortunately, existing high-temperature-resistant antistatic agents are generally colored, which can reduce the transparency of the polyester film and negatively impact its mechanical properties. Furthermore, the antistatic agent added in this manner must migrate to the surface of the polyester film to achieve its antistatic properties, resulting in unstable static values ​​that are easily affected by environmental factors and become ineffective.

[0005] Coating methods include offline coating and online coating. Offline coating is prone to surface defects such as scratches and contamination due to the mechanical and environmental contact of the polyester film substrate during repeated winding, unwinding, slitting, and transportation. In addition, the glue used in offline coating is an organic solvent, which is highly polluting and adds a process step, which also increases costs. Online coating is a process in which the film is biaxially stretched and coated simultaneously. After stretching and heating, a thinner, more uniform, and better-adhesive coating can be produced. It has the advantages of fast production speed, high efficiency, and low cost. Existing antistatic coating solutions are all water-based coating solutions containing conductive substances such as conductive polymers or conductive carbon nanotubes, which will also affect the optical properties of the film. In addition, the static value is easily invalidated when the film is subjected to high temperature, corona, and ultraviolet treatment during film preparation.

[0006] Therefore, it is of great significance to develop an antistatic polyester film that can maintain its antistatic properties for a long time while not affecting the mechanical properties, optical properties and stability of the polyester film.

[0007] Summary of the Invention

[0008] To address the above-mentioned technical problems, the present invention provides an antistatic polyester film and a method for preparing the same. This invention utilizes an in-line coating method to apply an antistatic coating comprising an aluminum-doped zinc oxide-coated nano-barium sulfate antistatic agent to the surface of a polyester base film. This coating imparts long-lasting, excellent antistatic properties to the polyester base film while maintaining its original optical and mechanical properties. Furthermore, the coating imparts an excellent opening effect to the polyester film, effectively preventing film sticking during the winding process.

[0009] The specific technical solutions of the present invention are:

[0010] In a first aspect, the present invention provides an antistatic polyester film having a three-layer composite structure, comprising a polyester base film and an antistatic coating attached to at least one surface of the polyester base film.

[0011] The antistatic coating is formed by curing an antistatic coating liquid; the antistatic coating liquid includes the following components: 10-15wt% water-based resin, 0.1-3wt% crosslinking agent, 0.01-2wt% antistatic agent, 0.002-0.3wt% wetting agent, 0.002-0.2wt% pH regulator, and water.

[0012] The present invention forms an antistatic coating by coating an antistatic coating liquid on the surface of a polyester base film and curing the coating. The antistatic coating contains aluminum-doped zinc oxide-coated nano-barium sulfate particles. The particles have a core-shell structure, with nano-barium sulfate as the core and aluminum-doped zinc oxide as the shell. Aluminum-doped zinc oxide is a doped semiconductor with excellent conductivity, making it an ideal antistatic agent. Furthermore, the present invention coats the nano-barium sulfate particles before adding them, which, compared to conventional carbon-based antistatic agents (carbon nanotubes, graphene, etc.) or the direct addition of aluminum-doped zinc oxide particles, does not affect the light transmittance and color of the film.

[0013] In addition, in the scheme of the present invention, the aluminum-doped zinc oxide-coated nano-barium sulfate also has an opening function: after the antistatic coating liquid is solidified to form an antistatic coating, the aluminum-doped zinc oxide-coated nano-barium sulfate will form a large number of tiny protrusions on the coating surface, which can give the film smoothness and play an opening role, and can effectively prevent the film from sticking during the winding process. There is no need to add other opening agents such as silica sol to the coating liquid, which can improve the adhesion of the coating (too many types and amounts of additives can easily lead to poor coating adhesion).

[0014] Specifically, the antistatic agent is aluminum-doped zinc oxide-coated nano-barium sulfate, and its preparation method includes: dispersing nano-barium sulfate with a particle size of 40-60 nanometers, aluminum nitrate and zinc nitrate in a solvent at a mass ratio of (88-92):1:(11-7) at room temperature, stirring evenly, transferring the resulting dispersion into a reactor, and reacting at a constant temperature of 140-160°C for 8-12 hours; after the reaction is completed, cooling, centrifuging, washing and drying to obtain aluminum-doped zinc oxide-coated nano-barium sulfate with a particle size of 60-90 nm, which has nano-barium sulfate as a core and aluminum-doped zinc oxide as a shell.

[0015] The present invention uses a high-pressure hydrothermal method to prepare aluminum-doped zinc oxide-coated nanobarium sulfate. This method can produce an aluminum-doped zinc oxide coating with good crystallinity and high purity. It is also relatively simple to manufacture. Compared with methods such as coprecipitation, the hydrothermal method can directly form a highly crystalline aluminum-doped zinc oxide coating on the surface of the nanobarium sulfate after the hydrothermal reaction, eliminating the need for subsequent high-temperature calcination.

[0016] Among them, it should be noted that the time and temperature of the hydrothermal reaction are crucial, which will significantly affect the doping effect of antimony and the crystal form of the aluminum-doped zinc oxide coating layer, thereby affecting the antistatic effect. In addition, in order to highlight the opening effect of aluminum-doped zinc oxide coated nano-barium sulfate, it is necessary to have a suitable particle size range. Its ideal particle size is slightly smaller than the coating thickness (the particle size accounts for about 45-75% of the thickness), so that the antistatic agent nanoparticles can be partially exposed on the coating surface to form small protrusions. If the particle size is too small, it is easy to cause the antistatic agent nanoparticles to be completely wrapped in the coating. If the particle size is too large, it will cause the antistatic agent nanoparticles to be excessively exposed, thus easily falling off, that is, the coating has poor adhesion. Therefore, in order to obtain the ideal particle size, it is necessary to strictly limit the particle size of nano-barium sulfate and the feed ratio between nano-barium sulfate and zinc nitrate and aluminum nitrate. The present invention has found through research that under the above-mentioned specific conditions, aluminum-doped zinc oxide can be uniformly coated on the surface of nano-barium sulfate, and the thickness of the coating layer and the particle size of the nanoparticles can be controlled (60-90nm), which is conducive to the opening effect.

[0017] Preferably, the water-based resin is selected from at least one of a water-based polyester resin, a water-based polyurethane resin and a water-based acrylate resin.

[0018] Preferably, the cross-linking agent is at least one selected from the group consisting of isocyanate compounds, melamine compounds, oxazoline compounds, aziridine compounds, epoxy compounds and carbodiimide compounds.

[0019] Preferably, the wetting agent is selected from one or more of alkylaryl polyether alcohols, modified polysiloxanes, organic fluorocarbon compounds and polyoxyalkyl ether compounds.

[0020] Preferably, the pH regulator is selected from one or more of 2-amino-2-methyl-1-propanol, aqueous ammonia, diethanolamine and triethanolamine.

[0021] Preferably, in the preparation process of the antistatic agent: the solvent is anhydrous ethanol; the stirring time is 0.5-1.5 hours; the drying temperature is 70-90° C. and the drying time is 10-15 hours.

[0022] Preferably, the thickness of the antistatic coating is 120-160 nanometers, and the thickness of the antistatic polyester film is 50-250 micrometers.

[0023] In a second aspect, the present invention provides a method for preparing an antistatic polyester film, comprising the following steps:

[0024] S1 Preparation of antistatic coating liquid.

[0025] Preparation of S2 polyester film: Polyester chips are added to a twin-screw extruder and heated to melt to obtain a polyester melt, which is then cooled on a casting roller to form a thick polyester base film sheet.

[0026] S3 online coating: firstly, the polyester base film thick sheet is longitudinally stretched, and the antistatic coating liquid is scraped onto one or both sides of the longitudinally stretched film, and then transversely stretched and heat-set to obtain the antistatic polyester film.

[0027] The antistatic coating liquid of the present invention is a water-based system, which is not only VOC-free and environmentally friendly, but also has a low viscosity and is not prone to generating bubbles during the preparation process. At the same time, the antistatic coating liquid is evenly coated on the membrane by an online scraping method. Compared with the internal addition method, it not only does not affect the mechanical properties of the film, but also has good coating adhesion. It can also further eliminate bubbles generated in the process in a timely manner, thereby reducing the apparent defects of the antistatic coating.

[0028] Preferably, S1 comprises: adding water-based resin to water, stirring at a speed of 400-600 r / min for 20-40 min, then adding pH regulator, wetting agent, crosslinking agent and antistatic agent in sequence, maintaining the speed and stirring for 20-40 min to obtain an antistatic coating liquid.

[0029] In S1, the present invention can uniformly disperse the antistatic agent in the water-based resin by controlling the adding order of the antistatic agent, the water-based resin and other additives, thereby avoiding agglomeration of the antistatic agent and achieving an ideal antistatic effect for the film.

[0030] Preferably, in S3: the stretching ratio of the longitudinal stretching is 2.8-3.5 times, the stretching ratio of the transverse stretching is 3-4 times, and the heat setting temperature is 225-240°C.

[0031] Compared with the prior art, the present invention has the following technical effects:

[0032] (1) The antistatic coating on the surface of the polyester base film of the present invention contains aluminum-doped zinc oxide coated nano-barium sulfate particles with a core-shell structure, which can make the polyester film have a long-lasting and stable antistatic performance (resistance value is 10 6 -10 9 In addition, it can also give the film smoothness and play the role of opening, which can effectively prevent the film from sticking during the winding process.

[0033] (2) The present invention uses a hydrothermal method to prepare aluminum-doped zinc oxide-coated nano-barium sulfate. This method can obtain an aluminum-doped zinc oxide coating with good crystallinity and high purity. In addition, this method is relatively simple to manufacture. Compared with coprecipitation methods, the aluminum-doped zinc oxide coating with good crystallinity can be directly formed on the surface of the nano-barium sulfate without the need for subsequent high-temperature calcination. The present invention further enhances the antistatic effect and opening effect of the antistatic agent by optimizing the hydrothermal reaction time / temperature and the raw material ratio.

[0034] (3) The antistatic coating liquid of the present invention is a water-based system, which is not only free of VOC emissions and environmentally friendly, but also has a low viscosity and is not prone to generating bubbles during the preparation process. At the same time, the antistatic coating liquid is evenly coated on the membrane by an online scraping method. Compared with the internal addition method, it not only does not affect the mechanical properties of the film, but also has good coating adhesion. It can also further eliminate the bubbles generated in the process in a timely manner, thereby reducing the apparent defects of the antistatic coating. DETAILED DESCRIPTION

[0035] The present invention will be further described below with reference to the embodiments.

[0036] Overall embodiment

[0037] In a first aspect, the present invention provides an antistatic polyester film having a three-layer composite structure, comprising a polyester base film (preferably having a thickness of 50-250 microns) and an antistatic coating (preferably having a thickness of 120-160 nanometers) attached to at least one surface of the polyester base film. The antistatic coating is formed by curing an antistatic coating solution; the antistatic coating solution comprises the following components: 10-15 wt% of a water-based resin, 0.1-3 wt% of a cross-linking agent, 0.01-2 wt% of an antistatic agent, 0.002-0.3 wt% of a wetting agent, 0.002-0.2 wt% of a pH regulator, and the balance being water.

[0038] The antistatic agent is aluminum-doped zinc oxide-coated nano-barium sulfate. The preparation method thereof comprises the following steps: dispersing nano-barium sulfate with a particle size of 40-60 nm, aluminum nitrate and zinc nitrate in a solvent (preferably anhydrous ethanol) at a mass ratio of (88-92):1:(11-7) at room temperature, stirring evenly (preferably for 0.5-1.5 hours), and then subjecting the obtained dispersion to a constant temperature reaction at 140-160° C. for 8-12 hours; after the reaction is completed, cooling, centrifuging, washing and drying (preferably at 70-90° C. for 10-15 hours) to obtain aluminum-doped zinc oxide-coated nano-barium sulfate with a particle size of 60-90 nm, which has nano-barium sulfate as a core and aluminum-doped zinc oxide as a shell.

[0039] Preferably, the water-based resin is selected from at least one of a water-based polyester resin, a water-based polyurethane resin, and a water-based acrylate resin. The cross-linking agent is selected from at least one of an isocyanate compound, a melamine compound, an oxazoline compound, an aziridine compound, an epoxy compound, and a carbodiimide compound. The wetting agent is selected from at least one of an alkylaryl polyether alcohol, a modified polysiloxane, an organic fluorocarbon compound, and a polyoxyalkyl ether compound. The pH adjusting agent is selected from at least one of 2-amino-2-methyl-1-propanol, aqueous ammonia, diethanolamine, and triethanolamine.

[0040] A method for preparing an antistatic polyester film comprises the following steps:

[0041] Preparation of S1 antistatic coating liquid: add water-based resin to water, stir at a speed of 400-600r / min for 20-40min, then add pH regulator, wetting agent, crosslinking agent and antistatic agent in sequence, maintain the speed and continue stirring for 20-40min to obtain antistatic coating liquid.

[0042] Preparation of S2 polyester film: Polyester chips are added to a twin-screw extruder and heated to melt to obtain a polyester melt, which is then cooled on a casting roller to form a thick polyester base film sheet.

[0043] S3 online coating: first, the polyester base film thick sheet is longitudinally stretched 2.8-3.5 times, the antistatic coating liquid is scraped on one or both sides of the longitudinally stretched film, and then transversely stretched 3-4 times, and heat-set (225℃-240℃) to obtain the antistatic polyester film.

[0044] Specific embodiments

[0045] Example 1

[0046] The invention discloses an antistatic polyester film with a three-layer composite structure, comprising a PET polyester base film (100 microns thick) and antistatic coatings (130-150 nanometers thick) attached to both sides of the PET polyester base film.

[0047] The antistatic coating liquid for forming the antistatic coating comprises the following components: 12 wt % aqueous polyurethane resin, 1.5 wt % polycarbodiimide, 0.5 wt % antistatic agent, 0.1 wt % modified dimethylpolysiloxane, 0.02 wt % 2-amino-2-methyl-1-propanol, and the balance water.

[0048] The preparation method of the above-mentioned antistatic polyester film is:

[0049] (1) Preparation of antistatic agent: At room temperature, nano-barium sulfate, aluminum nitrate and zinc nitrate with a particle size of 40-60 nm were dispersed in anhydrous ethanol in a mass ratio of 90:1:9. After stirring for 1 hour, the resulting dispersion was transferred to the inner container of a reactor and reacted at a constant temperature of 150°C for 10 hours. After the reaction, the mixture was cooled, centrifuged, washed with anhydrous ethanol, and dried at 80°C for 12 hours to obtain aluminum-doped zinc oxide-coated nano-barium sulfate with a particle size of 70-90 nm.

[0050] (2) Preparation of antistatic coating liquid: Add water-based resin to water and stir at a speed of 500 r / min for 30 min. Then add pH regulator, wetting agent, crosslinking agent and antistatic agent in sequence and continue stirring at the same speed for 30 min to obtain antistatic coating liquid.

[0051] (3) Preparation of polyester film: Polyester chips are added to a twin-screw extruder and heated to melt to obtain a polyester melt. The polyester melt is cooled on a casting roll to form a polyester base film sheet with a thickness of 100 μm.

[0052] (4) Online coating: First, the polyester base film thick sheet is longitudinally stretched 3.1 times, and the antistatic coating liquid is applied to both sides of the longitudinally stretched film through a wire rod, and then the film is transversely stretched 3.4 times, heat-set at 235°C, and rolled up to obtain the antistatic polyester film.

[0053] Examples 2-5 and Comparative Examples 1-6

[0054] The differences between Examples 2-5 and Comparative Examples 1-6 and Example 1 are shown in the following table (“ / ” indicates the same as Example 1):

[0055] Performance Testing

[0056] The polyester films prepared in each embodiment and each comparative example were tested for performance, including surface resistance (Ω), adhesion (0B-5B), light transmittance (%), haze (%), and smoothness. The test methods are as follows:

[0057] Surface resistivity: GB / T33398-2016.

[0058] Light transmittance and haze: GB / T2410-2008.

[0059] Adhesion: GB / T9286-199. The width of the cutter blade is approximately 10 mm, with 10 cuts spaced 1 mm apart. The adhesive tape used is 3M Transparent Tape 600. Evaluation is based on the number of cuts removed during the 100-cut test, with 5B being the best and 0B being the worst.

[0060] Slipperiness: ●: Good slipperiness, can be cut, no sticking; ○: Poor slipperiness, sticking. ● means acceptable, ○ means unacceptable.

[0061] The test results are shown in the following table.

[0062] From the data in the above table, we can see that:

[0063] The antistatic polyester films prepared in Examples 1-5 all have excellent surface properties in terms of surface resistance, light transmittance, haze, adhesion, and smoothness.

[0064] Comparative Example 1 differs from Example 1 in that it lacks an antistatic coating, resulting in the highest surface resistance and a lack of an opening effect, resulting in poor slip. Furthermore, the antistatic coating provided in Example 1, due to its suitable coating thickness and refractive index, can, according to the law of refraction, increase the light transmittance of the polyester film and reduce surface reflection. However, Comparative Document 1 lacks a coating, resulting in lower light transmittance and haze than Example 1.

[0065] Compared with Example 1, Comparative Examples 2 and 3 differ in that the antistatic agents used are carbon nanotubes and aluminum-doped zinc oxide, respectively. Although the antistatic effect is excellent, the light transmittance of the film decreases significantly, the haze increases sharply, and there is no opening effect, and the smoothness is poor.

[0066] Compared with Example 1, the difference between Comparative Example 4 is that the surface of the antistatic agent is coated with less aluminum-doped zinc oxide, the conductive effect is slightly lower than that of Example 1, the antistatic effect is poor, and the ratio of the antistatic agent particle size to the thickness of the antistatic coating is too small, which easily causes the antistatic agent particles to be completely wrapped in the coating, thereby failing to achieve the opening effect.

[0067] Comparative Examples 5 and 6 differ from Example 1 in that the degree of hydrothermal reaction is respectively too high or too low, resulting in reduced conductivity of the resulting aluminum-doped zinc oxide. This is because the reaction temperature affects the crystal form of the aluminum-doped zinc oxide layer, and poor crystal form leads to poor conductivity. Furthermore, the antistatic agent particle size in Comparative Example 5 is too large relative to the coating thickness, resulting in reduced adhesion.

[0068] Unless otherwise specified, the raw materials and equipment used in the present invention are commonly used in the art; the methods used in the present invention are conventional methods in the art unless otherwise specified.

[0069] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still fall within the scope of protection of the technical solution of the present invention.

Claims

1. An antistatic polyester film, characterized in that: It has a three-layer composite structure, including a polyester base film and an antistatic coating attached to at least one side of the polyester base film; The antistatic coating is formed by curing an antistatic coating liquid; the antistatic coating liquid comprises the following components: 10-15wt% of an aqueous resin, 0.1-3wt% of a crosslinking agent, 0.01-2wt% of an antistatic agent, 0.002-0.3wt% of a wetting agent, 0.002-0.2wt% of a pH regulator, and water; The antistatic agent is aluminum-doped zinc oxide-coated nano-barium sulfate with a particle size of 60-90 nanometers, nano-barium sulfate as a core and aluminum-doped zinc oxide as a shell.

2. The antistatic polyester film according to claim 1, characterized in that: The preparation method of aluminum-doped zinc oxide-coated nano-barium sulfate comprises: dispersing nano-barium sulfate with a particle size of 40-60 nanometers, aluminum nitrate and zinc nitrate in a solvent in a mass ratio of (88-92):1:(11-7), stirring evenly, and reacting the obtained dispersion in a reactor at 140-160° C. at a constant temperature for 8-12 hours; after the reaction is completed, cooling, centrifuging, washing and drying to obtain aluminum-doped zinc oxide-coated nano-barium sulfate with a particle size of 60-90 nanometers, nano-barium sulfate as a core and aluminum-doped zinc oxide as a shell.

3. The antistatic polyester film according to claim 2, characterized in that: In the preparation process of aluminum-doped zinc oxide coated nano-barium sulfate: The solvent is anhydrous ethanol; The stirring time is 0.5-1.5h; The drying temperature is 70-90° C. and the drying time is 10-15 hours.

4. The antistatic polyester film according to claim 1 or 2, characterized in that: The water-based resin is selected from at least one of a water-based polyester resin, a water-based polyurethane resin and a water-based acrylate resin.

5. The antistatic polyester film according to claim 1 or 2, characterized in that: The cross-linking agent is selected from at least one of isocyanate compounds, melamine compounds, oxazoline compounds, aziridine compounds, epoxy compounds and carbodiimide compounds.

6. The antistatic polyester film according to claim 1 or 2, characterized in that: The wetting agent is selected from one or more of alkylaryl polyether alcohols, modified polysiloxanes, organic fluorocarbon compounds and polyoxyalkyl ether compounds; The pH regulator is selected from one or more of 2-amino-2-methyl-1-propanol, aqueous ammonia, diethanolamine and triethanolamine.

7. The antistatic polyester film according to claim 1 or 2, characterized in that: The thickness of the antistatic coating is 120-160 nanometers, and the thickness of the antistatic polyester film is 50-250 micrometers.

8. A method for preparing an antistatic polyester film as claimed in any one of claims 1 to 7, characterized in that The following steps are involved: S1 Preparation of antistatic coating liquid; Preparation of S2 polyester film: adding polyester chips into a twin-screw extruder and heating and melting them to obtain a polyester melt, which is then cooled on a casting roll to form a polyester base film thick sheet; S3 online coating: firstly, the polyester base film thick sheet is longitudinally stretched, and the antistatic coating liquid is scraped on one side or both sides of the longitudinally stretched film, and then transversely stretched and heat-set to obtain the antistatic polyester film.

9. The preparation method according to claim 8, characterized in that: S1 includes: Add the water-based resin into water, stir at a speed of 400-600 r / min for 20-40 min, then add the pH adjuster, wetting agent, cross-linking agent and antistatic agent in sequence, maintain the speed and continue stirring for 20-40 min to obtain an antistatic coating liquid.

10. The preparation method according to claim 8, characterized in that: In S3: the stretching ratio of the longitudinal stretching is 2.8-3.5 times, the stretching ratio of the transverse stretching is 3-4 times, and the temperature of the heat setting is 225-240°C.

Citation Information

Patent Citations

  • Anti-adhesion antistatic polyester film

    CN111040219A

  • Antistatic polyester film and preparation method thereof

    CN116426020A

  • High transparent Anti-static polyester film and method for manufacturing the same

    KR1020160093422A

  • Polyester film and manufacturing method thereof

    KR1020170019675A