Gel polymer electrolyte, battery and electric device

By introducing thermally conductive particles into the electrolyte of lithium-ion batteries, the problem of uneven thermal conductivity of gel polymer electrolyte during in-situ curing is solved, the dynamic performance and curing uniformity of the battery are improved, and the risk of self-discharge is reduced.

WO2024244313A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/131060
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2023-11-10
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

In traditional lithium-ion batteries, gel polymers are prone to thermal conductivity during in-situ curing, resulting in uneven in-situ polymerization reactions, increasing the problem of decreasing battery internal resistance, polarization and cycle capacity retention.

Method used

The thermally conductive particles are introduced into the electrolyte. The thermal conductivity coefficient of the thermally conductive particles is greater than or equal to 400W/mK. By controlling the conductivity, type, composition, particle size and dispersion concentration of the thermally conductive particles, the curing uniformity and battery of the gel polymer matrix are improved. kinetic properties.

Benefits of technology

The temperature uniformity and curing uniformity of gel polymer electrolyte are improved, the impedance of the battery is reduced, the kinetic performance is improved, and the probability of self-discharge problems is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023131060_05122024_PF_FP_ABST
    Figure CN2023131060_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a gel polymer electrolyte, a battery and an electric device. The gel polymer electrolyte comprises: an electrolyte, wherein heat-conducting particles are dispersed in the electrolyte, and the heat conductivity coefficient of the heat conducting particles at 25ºC is greater than or equal to 400 W / mK.
Need to check novelty before this filing date? Find Prior Art

Description

Gel polymer electrolyte, battery and electrical device Technical Field

[0001] The present application belongs to the field of batteries, and in particular, relates to gel polymer electrolytes, batteries and electrical devices. Background Art

[0002] Lithium-ion batteries, known for their green, environmentally friendly, high-energy, and low-carbon nature, are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. With the development of society, the demand for lithium-ion batteries is increasing, and research on semi-solid-state batteries is also on the rise.

[0003] Public content

[0004] In view of the technical problems existing in the background technology, the present application provides a gel polymer electrolyte, aiming to improve the curing uniformity of the gel polymer matrix.

[0005] To achieve the above objectives, the first aspect of the present application provides a gel polymer electrolyte, comprising: an electrolyte, in which heat-conductive particles are dispersed, and the thermal conductivity of the heat-conductive particles at 25° C. is greater than or equal to 400 W / mK.

[0006] The gel polymer electrolyte of the present application has at least the following beneficial effects: the introduction of thermally conductive particles into the electrolyte can improve the temperature uniformity of the electrolyte, thereby improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction, improving the impedance and elastic modulus of the gel polymer electrolyte matrix, and the dynamic performance of the battery.

[0007] In some embodiments of the present application, the electrical conductivity of the thermally conductive particles at 25° C. is not greater than 10 -7 S / cm, optional 10 -16 S / cm~10 -7 S / cm. Controlling the conductivity of the thermally conductive particles within the given range will neither increase the electronic conductivity of the electrolyte nor significantly change the ionic conductivity of the electrolyte.

[0008] In some embodiments of the present application, the thermal conductivity is 400W / mK to 2000W / mK.

[0009] In some embodiments of the present application, the thermally conductive particles include diamond-like carbon. Meeting this condition facilitates the thermally conductive particles to have a high thermal conductivity and a low electrical conductivity, thereby improving the uniformity of curing of the polymer matrix during the in-situ polymerization reaction while minimizing the likelihood of battery self-discharge, thereby improving the battery's dynamic performance.

[0010] In some embodiments of the present application, based on the total number of atoms of the diamond-like carbon, the atomic percentage of hydrogen in the diamond-like carbon is less than or equal to 50 at%, optionally less than or equal to 20 at%, and further optionally less than or equal to 10 at%. Controlling the hydrogen content in the diamond-like carbon within the given range not only helps improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also reduces the probability of self-discharge of the battery, thereby improving the dynamic performance of the battery.

[0011] In some embodiments of the present application, based on the total number of carbon atoms in the diamond-like carbon, the sp 3 The atomic percentage of bonded carbon is 20 at% to 85 at%, and can be 70 at% to 85 at%. 3 The content of bonded carbon is within the given range, which is beneficial to improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction, and is not easy to increase the probability of self-discharge problems in the battery, which is beneficial to improving the kinetic performance of the battery, while taking into account the difficulty and cost of preparing diamond-like carbon.

[0012] In some embodiments of the present application, the particle size of the thermally conductive particles is less than or equal to 10 μm. By controlling the particle size of the thermally conductive particles within the given range, it is beneficial to improve the temperature uniformity of the electrolyte and the curing uniformity of the gel polymer matrix, and it is also beneficial to improve the electrochemical performance of the battery.

[0013] In some embodiments of the present application, the concentration of the thermally conductive particles is 0.1 wt% to 5 wt%, and optionally 0.5 wt% to 2 wt%, based on the total mass of the gel polymer electrolyte. Controlling the concentration of the thermally conductive particles in the electrolyte within this range not only improves the curing uniformity of the gel polymer matrix with the thermally conductive particles, but also facilitates achieving better active ion transport.

[0014] In some embodiments of the present application, the gel polymer electrolyte further includes: a gel polymer matrix, on which the thermally conductive particles are dispersed.

[0015] The second aspect of the present application provides a battery comprising the gel polymer electrolyte of the first aspect of the present application. The battery of the present application has the characteristics and effects described for the gel polymer electrolyte of the first aspect of the present application. Generally speaking, the battery has good kinetic performance.

[0016] In some embodiments of the present application, the battery further comprises: a positive electrode sheet, a negative electrode sheet, and a separator, and at least one of the positive electrode sheet, the negative electrode sheet, and the separator comprises the thermally conductive particles. Meeting this condition further improves the temperature uniformity of the electrolyte and the uniformity of curing of the polymer matrix during the in-situ polymerization reaction.

[0017] In some embodiments of the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer includes the thermally conductive particles. Providing the thermally conductive particles in the positive electrode active material layer not only further improves the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also improves the heat dissipation and temperature uniformity of the battery during use.

[0018] In some embodiments of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes the thermally conductive particles; or the negative electrode plate includes a negative electrode current collector and a thermally conductive layer disposed on the negative electrode current collector, wherein the thermally conductive layer includes the thermally conductive particles. Including thermally conductive particles in the negative electrode plate not only further improves the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also improves the heat dissipation and temperature uniformity of the battery during use.

[0019] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the positive electrode active material layer is 0.1 wt% to 2 wt%. Controlling the mass proportion of the thermally conductive particles in the positive electrode active material layer within the given range not only helps further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, but also helps to balance the conductivity of the positive electrode sheet and the energy density of the battery.

[0020] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the negative electrode active material layer is 0.1 wt% to 4 wt%. Controlling the mass proportion of the thermally conductive particles in the negative electrode active material layer within the given range not only helps further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, but also helps to balance the conductivity of the negative electrode sheet and the energy density of the battery.

[0021] In some embodiments of the present application, the negative electrode active material layer includes a silicon material, and the mass fraction of silicon in the negative electrode active material layer is greater than or equal to 10 wt %. Controlling the mass fraction of silicon in the negative electrode active material layer to fall within the given range is beneficial for improving the energy density of the negative electrode sheet and the battery.

[0022] In some embodiments of the present application, the thickness of the thermally conductive layer is 50 nm to 5 μm; and / or the mass proportion of the thermally conductive particles in the thermally conductive layer is greater than or equal to 50 wt%. Meeting these conditions not only further improves the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, but also helps to balance the conductivity of the negative electrode sheet and the energy density of the battery.

[0023] In some embodiments of the present application, the thermally conductive layer further comprises: a conductive agent and / or a binder, wherein the conductive agent accounts for 0.1 wt% to 40 wt% of the thermally conductive layer, and optionally 5 wt% to 15 wt% of the thermally conductive layer; and the binder accounts for 0.01 wt% to 5 wt% of the thermally conductive layer. Controlling the content of the conductive agent and / or binder in the thermally conductive layer within the given range not only further improves the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, but also helps to balance the conductivity of the negative electrode sheet and the adhesion of the conductive layer.

[0024] In some embodiments of the present application, the mass fraction of the thermally conductive particles in the electrolyte is greater than or equal to the mass fraction of the thermally conductive particles in the negative electrode active material layer. Meeting this condition further improves the curing uniformity of the gel polymer matrix and the heat dissipation of the battery, while also balancing the energy density of the battery.

[0025] In some embodiments of the present application, the mass fraction of the thermally conductive particles in the negative electrode active material layer is greater than or equal to the mass fraction of the thermally conductive particles in the positive electrode active material layer. Meeting this condition further improves the curing uniformity of the gel polymer matrix and the heat dissipation of the battery.

[0026] The third aspect of the present application provides an electrical device, which includes: the battery of the second aspect of the present application.

[0027] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0029] FIG1 is a schematic structural diagram of a battery according to an embodiment of the present application.

[0030] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application.

[0031] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application.

[0032] FIG4 is an exploded view of a battery pack according to one embodiment of the present application.

[0033] FIG5 is a schematic diagram of an embodiment of an electric device using a battery as a power source according to an embodiment of the present application.

[0034] Reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION

[0035] The present application will be further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.

[0036] References to "embodiments" in this application mean that a particular feature, structure, or characteristic described in connection with the embodiment may be included in at least one embodiment of the application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described in this application may be combined with other embodiments.

[0037] " Scope " disclosed in the present application is limited in the form of lower limit and / or upper limit, and given range is limited by selecting a lower limit and / or an upper limit, and the selected lower limit and / or the rear upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form the scope of not clearly recording, and any lower limit can be combined with other lower limits to form the scope of not clearly recording, and any upper limit can be combined with any other upper limit to form the scope of not clearly recording. In addition, each separately disclosed point or single numerical value itself can be used as lower limit or upper limit and any other point or single numerical value combination or with other lower limit or upper limit combination to form the scope of not clearly recording.

[0038] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.

[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.

[0040] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or comprised, or may mean that only the listed components are included or comprised. Furthermore, as used in this application, the terms "plurality" and "multiple" refer to two or more components.

[0041] Unless otherwise specified, the term "and / or" in this application simply describes an association between related objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Furthermore, the character " / " in this document generally indicates that the related objects are in an "or" relationship.

[0042] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned description of the drawings and any variations thereof are intended to cover non-exclusive inclusions. Unless otherwise specified, the terms used in this application have the well-known meanings commonly understood by those skilled in the art. Unless otherwise specified, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).

[0043] With the continued advancement of green environmental protection, the application of lithium-ion batteries has penetrated into all aspects of life, including vehicles, electronic devices, and energy storage devices. However, as their application continues to expand, potential problems have also attracted increasing attention. Traditional liquid electrolytes have a low boiling point and are prone to leakage, which can easily cause problems such as lithium dendrite growth and leakage. Gel polymer electrolytes have a state between liquid and solid electrolytes, which can help to alleviate problems such as electrolyte leakage and lithium dendrite growth.

[0044] Currently, when gel polymer electrolytes are used in batteries, the monomers and / or prepolymers of the gel polymer matrix are typically mixed with a solvent, lithium salt, initiator, etc. to form a liquid solution. The liquid solution is then injected into a battery housing equipped with an electrode assembly, encapsulated, and subjected to an in-situ polymerization reaction at high temperature, solidifying to form a gel-like three-dimensional network structure. However, the in-situ curing process of gel polymers is prone to uneven thermal conductivity, which can lead to uneven in-situ polymerization. This can result in some areas with very high polymerization degrees while others have low or almost no polymerization. This can lead to increased internal resistance, increased polarization, and decreased cycle capacity retention and cycle life, impacting the battery's dynamic performance.

[0045] In this application, by introducing thermally conductive particles into the electrolyte, the uniformity of the gel polymer matrix during the in-situ curing process can be improved. At the same time, by controlling the thermal conductivity of the thermally conductive particles at 25°C to be greater than or equal to 400W / mK, it is beneficial to obtain better improvement effects.

[0046] The gel polymer electrolyte disclosed in the embodiments of the present application is suitable for gel-state batteries, i.e., semi-solid batteries, and the batteries disclosed in the embodiments of the present application can be used in electrical devices that use batteries as power sources or various energy storage systems that use batteries as energy storage elements. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like.

[0047] A first aspect of the present application provides a gel polymer electrolyte comprising: an electrolyte, in which heat-conducting particles are dispersed, and the heat-conducting particles have a thermal conductivity greater than or equal to 400 W / mK at 25° C.

[0048] The thermal conductivity of the thermally conductive particles can be tested using a transient plane heat source method, which can be performed with reference to GB / T 32064-2015. Specifically, the test can be performed at 25°C, and the test environment can be normal pressure. As some specific examples, the thermal conductivity of the thermally conductive particles at 25°C can be greater than or equal to 400 W / mK, greater than or equal to 700 W / mK, greater than or equal to 1000 W / mK, greater than or equal to 1300 W / mK, greater than or equal to 1600 W / mK, greater than or equal to 2000 W / mK, greater than or equal to 2500 W / mK, etc., or can be a range consisting of any of the above values. In actual operation, when testing the thermal conductivity of the thermally conductive particles in the electrolyte in the battery, the thermally conductive particles can be obtained by the following method: disassembling the battery to obtain a gel polymer electrolyte, separating the electrolyte and the gel polymer matrix (such as by centrifugation), filtering, and drying to separate the solid particles therein.

[0049] Introducing thermally conductive particles into the electrolyte helps improve the temperature uniformity of the electrolyte across different regions within the battery housing, thereby improving the uniformity of the in-situ polymerization reaction of the monomers and / or prepolymers used to form the gel polymer matrix at different locations. This improves the thickness uniformity and structural consistency of the gel polymer matrix located between the positive and negative electrodes, reduces the impedance of the gel polymer matrix, and improves battery kinetic performance. Furthermore, the increased thermal conductivity of the thermally conductive particles also helps improve the uniformity of the gel polymer matrix's curing.

[0050] As some specific examples, the curing uniformity of the gel polymer matrix can be tested by the mechanical mode and electrochemical mode of the atomic force microscope. For example, the following operations may be included: disassembling the battery containing the gel polymer electrolyte, removing the isolation membrane containing the cured gel polymer electrolyte, placing the isolation membrane on a stainless steel plate, and connecting the stainless steel to the counter electrode of the electrochemical mode of the atomic force microscope to form a test path. The atomic force microscope can be used to take points in a 10×10 matrix in the 5cm×5cm area of ​​the isolation membrane. The elastic modulus E of each test point can be obtained by the atomic force microscope test in the mechanical mode, and the local AC impedance Z can be measured by the impedance test in the electrochemical mode. The uniformity of the distribution of the elastic modulus and the electrochemical impedance can reflect the uniformity of the curing of the gel polymer electrolyte. Among them, the uniformity of the distribution of the elastic modulus A E The distribution uniformity of electrochemical impedance spectroscopy Z They can be evaluated by the following formulas:

[0051] Among them, σ EIt is the square average of the difference between the elastic modulus at different test points on the isolation membrane and the arithmetic average elastic modulus of all test points; is the average elastic modulus of 100 test points selected on the isolation membrane; E i is the elastic modulus of the i-th test point selected on the isolation membrane; E i , σ E 、 and E i The units are the same as σ. Z It is the square average of the difference between the impedance of different test points on the isolation membrane and the arithmetic average impedance of all test points; is the arithmetic mean of the impedance of 100 test points selected on the isolation membrane; Z i is the elastic modulus of the i-th test point selected on the isolation membrane; σ Z 、 Z i The units are the same. E and A Z When both are less than 0.2, it is determined that the gel polymer electrolyte matrix is ​​uniformly solidified, and when A E and A Z When at least one of the above is greater than 0.2, it is determined that the gel polymer electrolyte matrix is ​​non-uniformly cured.

[0052] The gel polymer electrolyte of the present application has at least the following beneficial effects: the introduction of thermally conductive particles into the electrolyte can improve the temperature uniformity of the electrolyte, thereby improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction, improving the impedance and elastic modulus of the gel polymer electrolyte matrix, and the dynamic performance of the battery; in addition, on the basis of improving the temperature uniformity of the electrolyte, it is also beneficial to improve the heat dissipation uniformity of the battery during use.

[0053] Furthermore, the gel polymer electrolyte of the first aspect of the present application, while satisfying the aforementioned conditions, can further optimize the performance of the gel polymer electrolyte by controlling the electrical conductivity range and thermal conductivity coefficient range of the thermally conductive particles, as well as the type, composition, particle size, and dispersion concentration of the thermally conductive particles in the gel polymer electrolyte. That is, in addition to satisfying the aforementioned conditions, one or more of the following conditions can also be optionally satisfied.

[0054] In some embodiments of the present application, the thermal conductivity of the thermally conductive particles may be 400 W / mK to 2000 W / mK.

[0055] For example, the thermal conductivity of the thermally conductive particles can be 400 W / mK, 500 W / mK, 700 W / mK, 900 W / mK, 1100 W / mK, 1300 W / mK, 1500 W / mK, 1700 W / mK, 1900 W / mK, or 2000 W / mK, or any range thereof. Increasing the thermal conductivity of the thermally conductive particles can improve the uniformity of curing of the gel polymer matrix. However, the thermal conductivity of the thermally conductive particles depends primarily on their material and structure. As the thermal conductivity increases, the cost and / or difficulty of material selection also increase accordingly.

[0056] By controlling the thermal conductivity of the thermally conductive particles within a given range, it is beneficial to improve the curing uniformity of the gel polymer matrix and also to reduce the cost and / or material selection difficulty of the thermally conductive particles.

[0057] In some embodiments of the present application, the conductivity of the thermally conductive particles at 25° C. is not greater than 10 -7 S / cm, optional 10 -16 S / cm~10 -7 S / cm.

[0058] For example, the electrical conductivity of the thermally conductive particles at 25°C may be less than or equal to 10 -7 S / cm, less than or equal to 10 -8 S / cm, less than or equal to 10 -9 S / cm, less than or equal to 10 -10 S / cm, less than or equal to 10 -11 S / cm, less than or equal to 10 -12 S / cm, less than or equal to 10 -16S / cm, etc., or it can be a range consisting of any of the above values. The conductivity of the thermally conductive particles can be tested with reference to the test method for volume conductivity in GB / T 1410-2006. Specifically, the test can be carried out at 25°C, and the test environment can be normal pressure. In actual operation, when testing the thermal conductivity of the thermally conductive particles in the electrolyte in the battery, the battery can be disassembled to obtain the gel polymer electrolyte and separate the thermally conductive particles. The specific separation method has been described in the previous section and will not be repeated here. In the battery system, it is expected that the electrolyte has a high ionic conductivity and as low an electronic conductivity as possible. In order to reduce the probability of self-discharge problems in the battery, it is expected that the additives in the electrolyte system are non-conductive and will not increase the electronic conductivity of the electrolyte. For the thermally conductive particles, the lower their conductivity, the worse their electrical conductivity. After adding thermally conductive particles to the electrolyte, the circuit in the battery will be short-circuited, and the probability of self-discharge problems will be lower. By controlling the conductivity of the thermally conductive particles to meet the given range, the electronic conductivity of the electrolyte is not easily increased, and the probability of the battery self-discharge problem is low; at the same time, the thermally conductive particles that meet this condition are not easily lithiated during the charge and discharge process, and the ionic conductivity of the electrolyte will not change significantly after the thermally conductive particles are added.

[0059] Optionally, the conductivity of the thermally conductive particles at 25°C may be 10 -16 S / cm~10 -7 S / cm, for example, it can be 10 -7 S / cm, 5×10 -8 S / cm, 5×10 -9 S / cm, 5×10 -10 S / cm, 5×10 -11 S / cm, 5×10 -12 S / cm, 5×10 -13 S / cm, 5×10 -14 S / cm, 5×10 -15 S / cm, 5×10 -16 S / cm, etc., or a range consisting of any of the above values. The lower the conductivity of the thermally conductive particles, the better their insulation properties. When introduced into the electrolyte, they are less likely to increase the electronic conductivity of the electrolyte, and the probability of battery self-discharge is relatively low. However, as the conductivity of the thermally conductive particles increases, the cost of the thermally conductive particles and / or the difficulty of selecting the materials also increase accordingly.

[0060] By controlling the conductivity of the thermally conductive particles within a given range, it is beneficial to reduce the probability of battery self-discharge caused by the introduction of the thermally conductive particles, and also to reduce the cost and / or difficulty of material selection of the thermally conductive particles.

[0061] In some embodiments of the present application, the thermally conductive particles include diamond-like carbon.

[0062] Carbon in diamond is in sp 3 The carbon in graphite is bonded in the form of sp 2 The diamond-like carbon is amorphous carbon, the main component of which is carbon, including sp 3 and sp 2 Two types of hybrid bonds are categorized as hydrogenated diamond-like carbon (DLC) and hydrogen-free DLC. Hydrogenated DLC also includes carbon-hydrogen groups. DLC has excellent thermal conductivity and electrical insulation properties. Introducing it into the electrolyte as a thermally conductive particle improves the temperature uniformity of the electrolyte, enhances the uniformity of the gel polymer matrix during in-situ polymerization, improves the uniformity of the impedance and elastic modulus of the gel polymer electrolyte matrix, and improves the dynamic performance of the battery. It also reduces the likelihood of self-discharge. The characteristic peaks of carbon in different types of carbon materials are different. In actual operation, the battery can be disassembled to collect the solid thermal conductive particle particles in the gel polymer electrolyte, and the obtained solid particle sample can be subjected to XRD testing. The presence of diamond-like carbon can be determined based on the characteristic peaks of carbon in the XRD spectrum. For example, the solid particle sample can be placed on the XRD sample stage and tested by an XRD device with a Cu target as the X-ray source. If the sample shows a diffraction peak in the range of 2θ=43°~45° and 74°~76°, it means that the solid particle sample contains characteristic diffraction peaks of diamond-like carbon, and the electrolyte of the gel polymer electrolyte contains diamond-like carbon material. It is understood that the thermally conductive particles may comprise only diamond-like carbon or may comprise both diamond-like carbon and other thermally conductive material particles that meet the thermal conductivity and electrical conductivity requirements of the thermally conductive particles. Furthermore, the diamond-like carbon in the thermally conductive particles may comprise hydrogenated diamond-like carbon and / or hydrogen-free diamond-like carbon, and the hydrogenated diamond-like carbon and hydrogen-free diamond-like carbon may each independently comprise one or more different diamond-like carbons. Alternatively, the thermally conductive particles may comprise only diamond-like carbon.

[0063] By using thermally conductive particles including diamond-like carbon, the thermally conductive particles can be further helped to have a higher thermal conductivity coefficient and a lower electrical conductivity, which is beneficial for improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction, and is not easy to increase the probability of self-discharge problems in the battery, which is beneficial for improving the dynamic performance of the battery.

[0064] In some embodiments of the present application, based on the total number of atoms of the diamond-like carbon, the atomic percentage of hydrogen in the diamond-like carbon may be less than or equal to 50 at %, optionally less than or equal to 20 at %, and further optionally less than or equal to 10 at %.

[0065] For example, the atomic percentage of hydrogen in the diamond-like carbon can be 50 at%, 45 at%, 40 at%, 35 at%, 30 at%, 25 at%, 20 at%, 15 at%, 10 at%, 5 at%, 3 at%, or the like, or any range thereof. The total number of atoms in the diamond-like carbon can be understood as the sum of the molar numbers of all elements included in the diamond-like carbon. For example, assuming that the diamond-like carbon includes only hydrogen and carbon, with the total molar number of hydrogen being n1 and the total molar number of carbon being n2, the total number of atoms in the diamond-like carbon is n1+n2, and the atomic percentage of hydrogen in the diamond-like carbon is n1 / (n1+n2)×100%. In actual operation, solid particles in the electrolyte of a gel polymer electrolyte can be collected and subjected to XRD testing. If the solid particle sample only contains characteristic peaks of diamond-like carbon, it indicates that the solid particles are diamond-like carbon materials. At this time, the solid particle sample can be sent to an elemental analyzer, and then completely combusted and decomposed in an environment with a small amount of pure oxygen. The CO2 and H2O produced by the combustion are quantitatively analyzed to determine the hydrogen content in the diamond-like carbon. The lower the hydrogen content in the diamond-like carbon, the closer its performance is to that of diamond, and its thermal conductivity and electrical insulation properties are also better. Using it as a thermally conductive particle in the electrolyte can further help improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, while also reducing the probability of self-discharge problems in the battery. It should be noted that the diamond-like carbon can include only hydrogenated diamond-like carbon or a combination of hydrogenated diamond-like carbon and hydrogen-free diamond-like carbon, as long as its hydrogen content meets the requirements of the given range. To further improve the thermal conductivity and electrical insulation properties of the thermally conductive particles, the hydrogen content in the diamond-like carbon may be less than or equal to 20 at %, or less than or equal to 10 at %.

[0066] By controlling the hydrogen content in diamond-like carbon within a given range, it is beneficial to improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, and it is not easy to increase the probability of self-discharge problems in the battery, which is beneficial to improving the battery's kinetic performance.

[0067] In some embodiments of the present application, based on the total number of carbon atoms in diamond-like carbon, the number of sp atoms in diamond-like carbon is 3 The atomic percentage of bonded carbon may be 20 at % to 85 at %, and may be optionally 70 at % to 85 at %.

[0068] For example, sp 3The atomic percentage of bonded carbon can be 20at%, 25at%, 30at%, 35at%, 40at%, 45at%, 50at%, 55at%, 60at%, 65at%, 70at%, 75at%, 80at%, 85at%, etc., or can be a range consisting of any of the above values. The total number of carbon atoms in the diamond-like carbon can be understood as the total molar number of carbon elements in the diamond-like carbon. In actual operation, the solid particles in the electrolyte of the gel polymer electrolyte can be collected and subjected to XRD testing. If there are only characteristic peaks of diamond-like carbon in the solid particle sample, it means that the solid particle is a diamond-like carbon material. At this time, the solid particle sample can be loaded and XPS testing can be performed. Through the XPS test of the carbon element, the sp 2 With sp 3 The different characteristic peaks contributed by different hybrid bond energies are 284.4eV and 285.2eV respectively. By splitting the XPS test peaks, the corresponding area ratio of the characteristic peaks of 284.4eV and 285.2eV can be used to determine the sp 3 The content ratio of bonded carbon. 3 The higher the content of bonded carbon, the closer its performance is to diamond, and the better its thermal conductivity and electrical insulation are. Using it as a thermal conductive particle in the electrolyte can not only further improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also not easily increase the probability of self-discharge problems in the battery. However, with the sp 3 As the content of bonded carbon increases, the difficulty and cost of its preparation will also increase accordingly. It should be noted that the diamond-like carbon can include only hydrogenated diamond-like carbon or both hydrogenated diamond-like carbon and hydrogen-free diamond-like carbon. 3 The content of bonded carbon can meet the requirements of the given range. In order to further improve the thermal conductivity and electrical insulation properties of the thermally conductive particles, the sp 3 The atomic percentage of bonded carbon is 70 at% to 85 at%.

[0069] By controlling the sp 3 The content of bonded carbon is within the given range, which is beneficial to improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction, and is not easy to increase the probability of self-discharge problems in the battery, which is beneficial to improving the kinetic performance of the battery, while taking into account the difficulty and cost of preparing diamond-like carbon.

[0070] In some embodiments of the present application, the particle size of the thermally conductive particles may be less than or equal to 10 μm.

[0071] For example, the particle size of the thermally conductive particles can be less than or equal to 10 μm, less than or equal to 8 μm, less than or equal to 6 μm, less than or equal to 4 μm, less than or equal to 2 μm, less than or equal to 1 μm, less than or equal to 500 nm, less than or equal to 100 nm, less than or equal to 50 nm, etc., or can be a range consisting of any of the above values. The particle size of the thermally conductive particles can be measured using a laser particle size analyzer (such as Malvern Master Size 3000) with reference to the standard GB / T 19077.1-2016. The particle size of the thermally conductive particles may affect their dispersion uniformity in the electrolyte and the transmission path of active ions (such as lithium ions), affecting the electrochemical performance of the battery. Optionally, the particle size of the thermally conductive particles can be 50nm~10μm; further optionally, the thermally conductive particles can include primary particles with a particle size of 5nm~1μm and secondary particles with a particle size of 50nm~10μm. The secondary particles can be formed by agglomeration of primary particles. Thermally conductive particles with smaller particle sizes may agglomerate in the electrolyte. By controlling the particle sizes of the primary particles and the secondary particles to meet the given range, it is beneficial to improve the dispersion uniformity of the thermally conductive particles in the electrolyte and obtain better active ion transmission effect.

[0072] By controlling the particle size of the thermally conductive particles within a given range, it is beneficial to improve the temperature uniformity of the electrolyte, enhance the solidification uniformity of the gel polymer matrix, and also help the battery have better electrochemical performance.

[0073] In some embodiments of the present application, based on the total mass of the gel polymer electrolyte, the mass proportion of the thermally conductive particles may be 0.1 wt % to 5 wt %, and may be optionally 0.5 wt % to 2 wt %.

[0074] For example, based on the total mass of the gel polymer electrolyte, the mass proportion of the thermally conductive particles can be 0.1 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.2 wt%, 1.5 wt%, 1.8 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, or the like, or a range thereof. Alternatively, the thermally conductive particles in the electrolyte can be diamond-like carbon (DLC). The DLC content in the gel polymer electrolyte can be confirmed by thermogravimetric-mass spectrometry (TG-MS). DLC has an extremely high thermal stability temperature and, due to its excellent thermal conductivity, is immune to localized overheating. The TG-MS test can include separating the electrolyte and the gel polymer matrix in the gel polymer electrolyte, filtering, and washing to obtain a solid sample. The solid sample is then heated to 500°C at 20°C / min in an oxygen environment to completely remove any residual components of the polymer electrolyte matrix, leaving only the DLC component. The mass ratio of the diamond-like carbon thermally conductive particles can be calculated by adding the mass of the other components measured by TG-MS to the total mass of the gel polymer electrolyte sample. Increasing the mass concentration of thermally conductive particles in the gel polymer electrolyte can improve the temperature uniformity of the electrolyte. However, if the concentration of thermally conductive particles in the electrolyte increases too high, the transmission path of active ions (such as lithium ions) may be affected to a certain extent.

[0075] By controlling the mass concentration of the thermally conductive particles in the gel polymer electrolyte within a given range, it is beneficial to improve the effect of the thermally conductive particles on improving the curing uniformity of the gel polymer matrix and also to obtain a better active ion transmission effect.

[0076] In some embodiments of the present application, the gel polymer electrolyte further includes: a gel polymer matrix, and heat-conducting particles may be dispersed on the gel polymer matrix.

[0077] A gel polymer electrolyte comprises a gel polymer matrix and an electrolyte. The gel polymer matrix is ​​a three-dimensional network structure formed by crosslinking and curing, and the electrolyte fills the pores of this three-dimensional network structure. During the in-situ curing of the gel polymer matrix or the charge-discharge cycle of the battery, some thermally conductive particles may adhere to the gel polymer matrix. The thermally conductive particles may include diamond-like carbon, and the presence of diamond-like carbon dispersed in the gel polymer matrix can be confirmed by combining one or more conventional methods such as TG-MS testing, thermogravimetric analysis, and XRD testing.

[0078] The fact that thermally conductive particles may be dispersed on the gel polymer matrix can be used to further confirm whether the gel polymer electrolyte contains thermally conductive particles.

[0079] It is understood that the electrolyte of the gel polymer electrolyte may include a solvent and an active metal salt (for example, for lithium batteries, the active metal salt may be a lithium salt). The solvent may be a non-aqueous solvent. Optionally, the solvent may include a primary solvent and an auxiliary solvent. The primary solvent may dissolve the lithium salt and improve the electrochemical stability of the electrolyte, and the auxiliary solvent may reduce the viscosity of the electrolyte and further improve the ionic conductivity. The types of the auxiliary solvent, auxiliary solvent, and lithium salt are not particularly limited, and those skilled in the art may flexibly select them according to actual needs.

[0080] In some embodiments of the present application, the main solvent in the electrolyte may include, but is not limited to, at least one of an ester solvent, an ether solvent, a sulfone solvent, a nitrile solvent, and an ionic liquid solvent. Among them, the ester solvent may include, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), ethylene sulfite (ES), propylene sulfite (PS), dimethyl sulfite (DMS), diethyl sulfite (DES), γ-butyrolactone (BL), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methylpropyl carbonate (MPC), methyl formate (MF), ethyl formate (EF), methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), ethyl butyrate (EB), and at least one of their fluorinated derivatives. Ether solvents may include but are not limited to dimethoxymethane (DMM), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (DEE), 1,2-dimethoxypropane (DMP), diethylene glycol dimethyl ether (DGM), tetrahydrofuran (THF), tetrahydropyran (THP), 1,3-dioxolane (DOL), 1,3-dioxane (1,3-DXA), 1,4-dioxane (1,4-DXA), and at least one of their fluorinated derivatives. Sulfone solvents include but are not limited to dimethyl sulfone, dimethyl sulfoxide, sulfolane, ethyl methyl sulfone, tetramethylene sulfoxide, ethyl methyl sulfoxide, diethyl sulfone, diethyl sulfoxide, methyl phenyl sulfone, methyl phenyl sulfoxide, ethyl phenyl sulfone, ethyl phenyl sulfoxide, vinyl phenyl sulfone, vinyl phenyl sulfoxide, and at least one of their fluorinated derivatives. Using the main solvent within the above-mentioned range is beneficial to promoting the dissolution of active metal salts and making the electrolyte have good ion transport properties.

[0081] In some embodiments of the present application, the auxiliary solvent in the electrolyte can be a solvent that does not dissolve the active metal salt but is well miscible with the main solvent. Generally speaking, electrolytes with low active metal salt concentrations have low viscosity and high conductivity, but slightly poor electrochemical stability. High-concentration electrolytes have a high electrochemical stability because most solvent molecules can react with active metal ions (such as Li +) are combined to form a solvated shell structure, which has high electrochemical stability. However, the high viscosity and low ion mobility caused by high concentration will lead to a decrease in the electrical performance of the electrolyte. The auxiliary solvent that does not dissolve the active metal salt but is well miscible with the main solvent is regarded as a diluent. By adding the diluent to the high-concentration electrolyte to form a local high-concentration electrolyte, the characteristics of the high-concentration electrolyte can be retained, and the advantages of low viscosity and high ionic conductivity of the low-concentration electrolyte can be obtained. That is, the electrolyte can combine the advantages of low-concentration electrolyte and high-concentration electrolyte, so that it has both high ion mobility rate and good electrochemical stability, thereby further improving the kinetic performance of the battery.

[0082] In some embodiments of the present application, the auxiliary solvent in the electrolyte may include but is not limited to fluoroethylene carbonate, cyclohexane, benzene, toluene, p-xylene, m-xylene, o-xylene, fluorobenzene, p-difluorobenzene, m-difluorobenzene, o-difluorobenzene, trifluorotoluene, trifluoromethoxybenzene, decafluoropentane, perfluoropentanone, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, bis(2,2,2-trifluoroethyl)ether, 1,1,2,3,3,3-hexafluoro At least one of propyl ethyl ether, 1H,1H,5H octafluoropentyl 1,1,2,2-tetrafluoroethyl ether, ethyl trifluoromethyl ether, difluoromethyl-2,2,3,3,3-pentafluoropropyl ether, heptafluoropropyl-1,2,2,2-tetrafluoroethyl ether, difluoromethyl 2,2,3,3-tetrafluoropropyl ether, perfluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, ethyl-1,1,2,2-tetrafluoroethyl ether, ethyl-2,2,2-tetrafluoroethyl ether, bis(1,1,2,2-tetrafluoroethyl) ether, etc. Optionally, the auxiliary solvent in the electrolyte may include at least one of trifluoromethoxybenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane. The auxiliary solvent within the given range has a high electrochemical window, good compatibility, and good ability to promote the formation of fluorine-rich SEI. Combining it with the main solvent can not only improve the ionic conductivity and electrochemical stability of the electrolyte, but also help reduce the side reactions between the electrolyte and the negative electrode.

[0083] In some embodiments of the present application, the type of active metal salt can be selected based on the type of battery to which the gel polymer electrolyte is applicable. Taking lithium batteries as an example, the active metal salt can be a lithium salt. The lithium salt in the electrolyte can include but is not limited to lithium bis(fluorosulfonyl)imide (LiFSI), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiOTF), lithium difluorophosphate (LiDFP), lithium dioxalatoborate (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate. For example, lithium bis(fluorosulfonyl)imide can be selected. The above lithium salts can decompose on the surface of the battery negative electrode to form an SEI component rich in inorganic fluorine. At the same time, they have good dissociation ability, which is conducive to achieving higher electrolyte ion conductivity and lower electrolyte viscosity, thereby improving the electrochemical performance of the battery.

[0084] In some embodiments of the present application, the polymerized monomers and / or prepolymers of the gel polymer matrix, an initiator, an active metal salt, and thermally conductive particles can be dispersed together in an electrolyte. After the electrolyte is injected into a housing containing an electrode assembly, the temperature is increased and polymerization is carried out to cause the polymerized monomers and / or prepolymers to undergo an in-situ polymerization reaction to form a gel polymer matrix. The initiator is used to initiate the polymerization of the polymerized monomers and / or prepolymers to form a gel polymer matrix. Optionally, additives can be added to the electrolyte according to actual needs to achieve the desired effect. For example, additives that inhibit the dissolution of transition metals can be added, and / or additives that promote film formation can be added. Among them, the additives that promote film formation may include but are not limited to at least one of propane sultone, vinyl sulfate, vinyl sulfite, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trifluoroethyl) phosphate, tris(trifluoroethyl) phosphite, tris(trimethylsilane) borate, dimethylmaleic anhydride and 1,4-diisocyanate. Selecting additives within the given range is beneficial to improving the stability of the positive and negative electrodes of the battery and extending the life of the battery.

[0085] The second aspect of the present application provides a battery comprising the gel polymer electrolyte of the first aspect of the present application. The battery of the present application has the characteristics and effects described for the gel polymer electrolyte of the first aspect of the present application. Generally speaking, the battery has good kinetic performance. Optionally, the battery can be a secondary battery, for example, a lithium metal secondary battery or a lithium-ion battery.

[0086] In some embodiments of the present application, the battery may further include: a positive electrode sheet, a negative electrode sheet, and a separator, and at least one of the positive electrode sheet, the negative electrode sheet, and the separator may include thermally conductive particles.

[0087] The gel polymer electrolyte is distributed between the electrode and the separator. Distributing thermally conductive particles on at least one of the positive electrode, negative electrode, and separator improves the uniformity of the positive electrode, negative electrode, and separator, thereby improving the temperature uniformity of the electrolyte and enhancing the curing uniformity of the polymer matrix during the in-situ polymerization reaction. Optionally, the thermally conductive particles may include diamond-like carbon. XRD testing can be used to determine whether the positive electrode, negative electrode, or separator contains diamond-like carbon. For example, the battery can be disassembled to obtain the positive and negative electrode sheets or separators. For example, the surface material (such as the active material layer) on the positive electrode or negative electrode sheet can be scraped off after cleaning to produce a powder. The powder sample is then subjected to XRD testing. The presence of thermally conductive particles in the electrode sheet can be determined based on the characteristic peaks of the XRD test spectrum. The specific operation and determination method can be referred to the description in the previous section. It should be noted that silicon and other commonly used carbon-containing negative electrode active materials do not have diffraction peaks corresponding to the peaks of diamond-like carbon.

[0088] Distributing thermally conductive particles on at least one of the positive electrode sheet, the negative electrode sheet, and the separator is beneficial for further improving the temperature uniformity of the electrolyte and improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction.

[0089] In some embodiments of the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector, and the positive electrode active material layer may include thermally conductive particles.

[0090] For example, thermally conductive particles can be dispersed in the positive electrode active material layer. Alternatively, the thermally conductive particles can be dispersed in an active slurry of the positive electrode active material layer, and the active slurry can be coated on at least one layer of the positive electrode current collector to obtain a positive electrode active material layer comprising thermally conductive particles. In a battery, the positive electrode active material layer can be in direct contact with the electrolyte. The inclusion of thermally conductive particles in the positive electrode active material layer can, on the one hand, further improve the temperature uniformity of the electrolyte, thereby improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction; on the other hand, it can also improve the heat dissipation of the battery during use, reducing the probability of heat concentration within the battery.

[0091] By providing thermally conductive particles in the positive electrode active material layer, it is not only beneficial to further improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also beneficial to improve the heat dissipation effect and temperature uniformity of the battery during use.

[0092] In some embodiments of the present application, the positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be arranged on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be aluminum foil. The positive electrode active material layer includes a positive electrode active material, wherein the specific type of the positive electrode active material is not limited, and active materials that can be used for the positive electrode of the battery known in the art can be used, and those skilled in the art can select according to actual needs. For example, for lithium batteries, the positive electrode active material may include but is not limited to lithium transition metal oxides and / or olivine-structured lithium phosphate-containing positive electrode active materials, the lithium transition metal oxides may include undoped and / or optionally doped-modified lithium transition metal oxides, uncoated and / or coated-modified lithium transition metal oxides, the olivine-structured lithium phosphates may include undoped and / or optionally doped-modified lithium phosphates of olivine structure, uncoated and / or coated-modified lithium phosphates of olivine structure. As some specific examples, lithium transition metal oxides may include but are not limited to lithium cobalt oxide (such as LiCoO2, etc.), lithium nickel oxide (such as LiNiO2, etc.), lithium manganese oxide (such as LiMnO2, LiMn2O4, etc.), lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.5 Co 0.25 Mn 0.25 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.96 Co 0.02 Mn 0.02 O2, etc.), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2, etc.) and their modified compounds. As some specific examples, olivine-structured lithium-containing phosphates include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. The positive electrode active materials within the given range can be prepared or obtained through commercial channels.

[0093] In some specific embodiments of the present application, the positive electrode active material layer may further optionally include a binder, a conductive agent and other optional auxiliary agents. As an example, the conductive agent may include but is not limited to one or more of acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene and carbon nanofibers. As an example, the binder may include but is not limited to one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0094] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the positive electrode active material layer may be 0.1 wt % to 2 wt %.

[0095] For example, the mass proportion of the thermally conductive particles in the positive electrode active material layer can be 0.1wt%, 0.3wt%, 0.5wt%, 0.7wt%, 0.9wt%, 1.1wt%, 1.3wt%, 1.5wt%, 1.7wt%, 1.9wt%, 2wt%, etc., or can be a range consisting of any of the above values. When testing the content of thermally conductive particles in the positive electrode active material layer, the battery can be disassembled to obtain the positive electrode sheet. After cleaning, the positive electrode active material layer on the positive electrode sheet can be scraped off and weighed; by adding excess hydrochloric acid solution, the positive electrode active material in the positive electrode active material layer can be completely dissolved, and the remaining binder, thermally conductive particles and conductive agent are left; then the remaining material is rinsed with N-methylpyrrolidone (NMP) until the binder is completely removed, and dried to obtain a powder mixture of the conductive agent and the thermally conductive particles; conventional methods such as XRD testing are used to confirm the components of the powder mixture, and based on the difference in decomposition temperature of the thermally conductive particles and the conductive agent, the content of the thermally conductive particles is confirmed in combination with TG-MS testing, and then the content of the thermally conductive particles in the positive electrode active material layer is obtained. For example, assuming that the thermally conductive particles and conductive agent in the powder mixture are diamond-like carbon and carbon black, respectively, the powder mixture can be loaded into a TG-MS for thermogravimetric testing. The mixture is heated to 550 degrees Celsius at a rate of 20 degrees per minute in an oxygen environment and kept warm for 30 minutes to completely decompose the carbon black and confirm the mass proportion of the conductive agent. The temperature is then raised to above 800 degrees Celsius to measure the mass of the diamond-like carbon, thereby confirming the mass proportion of the diamond-like carbon in the positive electrode active material layer. Among them, increasing the mass proportion of the thermally conductive particles in the positive electrode active material layer is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery. However, as the content of thermally conductive particles in the positive electrode active material layer increases, the relative content of the positive electrode active material in the positive electrode sheet will decrease, and the conductivity of the positive electrode active material layer will also decrease.

[0096] By controlling the mass proportion of the thermally conductive particles in the positive electrode active material layer within a given range, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, and it is also beneficial to take into account the conductivity of the positive electrode sheet and the energy density of the battery.

[0097] In some embodiments of the present application, the negative electrode plate may include a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, and the negative electrode active material layer may include thermally conductive particles; or, the negative electrode plate may include a negative electrode current collector and a thermally conductive layer provided on the negative electrode current collector, and the thermally conductive layer may include thermally conductive particles.

[0098] In a battery, the negative electrode plate typically includes a current collector and a negative electrode active material layer. When the negative electrode plate includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode active material. The negative electrode current collector can be a conventional metal foil or a composite current collector (for example, a metal material can be disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector can be copper foil. In this case, thermally conductive particles can be dispersed in the negative electrode active material layer.

[0099] Furthermore, the negative electrode sheet may not contain a negative active material layer. In this case, the negative electrode current collector may be a metal current collector, including but not limited to a single metal. For example, for lithium batteries, the negative electrode current collector may be made of metallic lithium or an alloy of metallic lithium with various other metal or non-metal elements. Optionally, the metal elements may include but are not limited to tin (Sn), zinc (Zn), aluminum (Al), magnesium (Mg), silver (Ag), gold (Au), gallium (Ga), indium (In), and platinum foil (Pt). Alternatively, the non-metallic elements may include but are not limited to boron (B), carbon (C), and silicon (Si). As an example, the negative electrode current collector may be lithium foil. When the negative electrode sheet does not contain a negative active material layer, only the lithium in the positive electrode is used during cycling, precipitating and stripping off as lithium metal on the negative electrode side. In this case, a thermally conductive layer may be provided on the surface of the negative electrode current collector, comprising thermally conductive particles. It is understood that the thermally conductive layer may include only thermally conductive particles or other components, including but not limited to a binder.

[0100] In the battery, the negative electrode plate can also be in direct contact with the electrolyte. Dispersing heat-conductive particles in the negative active material layer or providing a heat-conductive layer containing heat-conductive particles on the surface of the negative electrode plate can, on the one hand, further improve the temperature uniformity of the electrolyte, thereby improving the curing uniformity of the polymer matrix during the in-situ polymerization reaction; on the other hand, it can also help improve the heat dissipation effect of the battery during use and reduce the probability of heat concentration inside the battery.

[0101] By arranging heat-conducting particles in the negative electrode active material layer or arranging a heat-conducting layer containing heat-conducting particles on the surface of the negative electrode current collector, it is not only beneficial to further improve the curing uniformity of the polymer matrix during the in-situ polymerization reaction, but also beneficial to improve the heat dissipation effect and temperature uniformity of the battery during use.

[0102] In some embodiments of the present application, the negative electrode active material may include silicon material, such as a composite negative electrode active material doped with silicon-based material and carbon material, etc. Using silicon material in the negative electrode active material layer is beneficial to further improve the energy density of the battery.

[0103] In some embodiments of the present application, the negative electrode active material layer may also optionally include a binder, a conductive agent and other optional additives. As an example, the conductive agent may include but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. As an example, the binder may include but is not limited to one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB). As an example, other optional additives may include but are not limited to thickeners and dispersants (such as sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials.

[0104] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the negative electrode active material layer may be 0.1 wt % to 4 wt %.

[0105] For example, the mass percentage of the thermally conductive particles in the negative electrode active material layer can be 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, etc., or can be a range consisting of any of the above values. Among them, increasing the mass percentage of the thermally conductive particles in the negative electrode active material layer is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery. However, as the content of the thermally conductive particles in the negative electrode active material layer increases, the relative content of the negative electrode active material in the negative electrode sheet will decrease, and the conductivity of the negative electrode active material layer will also decrease.

[0106] By controlling the mass proportion of the thermally conductive particles in the negative electrode active material layer within a given range, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, and it is also beneficial to take into account the conductivity of the negative electrode sheet and the energy density of the battery.

[0107] In some embodiments of the present application, the negative electrode active material layer may further include silicon material, and the mass proportion of silicon element in the negative electrode active material layer may be greater than or equal to 10 wt %.

[0108] For example, the mass proportion of silicon element in the negative electrode active material layer can be greater than or equal to 10wt%, greater than or equal to 15wt%, greater than or equal to 20wt%, greater than or equal to 25wt%, greater than or equal to 30wt%, greater than or equal to 35wt%, etc., or can be a range composed of any of the above values. Silicon has a high theoretical specific capacity and a low lithium insertion potential. The use of silicon material as a negative electrode active material is beneficial to further improve the energy density of the negative electrode sheet and the battery. Optionally, silicon material and carbon material can be composited as a negative electrode active material. Optionally, the negative electrode active material layer can include both silicon material and thermally conductive particles. The thermal conductivity of silicon material is relatively poor. Using silicon material and thermally conductive particles together in the negative electrode active material layer is beneficial to simultaneously improve the charge and discharge specific capacity and thermal conductivity uniformity of the negative electrode sheet.

[0109] By controlling the mass proportion of silicon in the negative electrode active material layer to meet the given range, it is beneficial to improve the energy density of the negative electrode sheet and the battery.

[0110] In some embodiments of the present application, the thickness of the heat conductive layer may be 50 nm to 5 μm.

[0111] When a heat-conducting layer is provided on the negative electrode current collector, the thickness of the heat-conducting layer can be 50nm, 60nm, 70nm, 80nm, 100nm, 200nm, 500nm, 800nm, 1μm, 2μm, 3μm, 4μm, 5μm, etc., or can be a range composed of any of the above values. When testing the thickness of the heat-conducting layer, the negative electrode pole piece can be prepared into a cross section under cryo-ion beam polishing (Cryo-CP) and observed in SEM. The average particle size of the heat-conducting particles in the heat-conducting layer is lower than that of the active material in the negative electrode layer. This can be used to distinguish the spatial distribution of the heat-conducting layer and perform thickness measurement in SEM. Alternatively, a heat-conducting layer can be formed on the surface of the negative electrode current collector by vapor deposition, and the heat-conducting layer can be made to have a porous structure by adjusting the vapor deposition. The heat-conducting layer with a porous structure is beneficial to improving the uniform deposition of active ions of the battery on the surface of the negative electrode pole piece and the effective contact between the negative electrode pole piece and the electrolyte. Increasing the thickness of the thermal conductive layer is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery. However, as the thickness of the thermal conductive layer increases, the energy density of the battery will decrease. In addition, the conductivity of the negative electrode may also decrease.

[0112] By controlling the thickness of the thermal conductive layer within a given range, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, and it is also beneficial to take into account the conductivity of the negative electrode sheet and the energy density of the battery.

[0113] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the thermally conductive layer may be greater than or equal to 50 wt %.

[0114] When a thermally conductive layer is provided on the negative electrode current collector, the mass proportion of the thermally conductive particles in the thermally conductive layer may be greater than or equal to 50 wt%, greater than or equal to 55 wt%, greater than or equal to 60 wt%, greater than or equal to 65 wt%, greater than or equal to 70 wt%, greater than or equal to 75 wt%, etc., or may be a range consisting of any of the above values. When testing the mass proportion of the thermally conductive particles in the thermally conductive layer, the thermally conductive layer may be scraped off, and other components in the thermally conductive layer may be removed by conventional methods such as solvent method and / or ultrasonic method, and the weight change of the test sample before and after the removal of other components is obtained. Increasing the mass proportion of the thermally conductive particles in the thermally conductive layer is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, but the electrical conductivity of the thermally conductive layer and the negative electrode plate may decrease.

[0115] By controlling the content of the heat-conducting particles in the heat-conducting layer within a given range, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, and it is also beneficial to take into account the conductivity of the negative electrode.

[0116] In some embodiments of the present application, the thermal conductive layer further includes: a conductive agent and / or an adhesive. The mass proportion of the conductive agent in the thermal conductive layer can be 0.1wt% to 40wt%, optionally 5wt% to 15wt%, and the mass proportion of the adhesive in the thermal conductive layer can be 0.01wt% to 5wt%.

[0117] For example, the weight percentage of the conductive agent in the thermally conductive layer can be 0.1wt%, 1wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, etc., or can be any range consisting of the above values. The weight percentage of the binder in the thermally conductive layer can be 0.01wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, etc., or can be any range consisting of the above values. When testing the binder content in the thermally conductive layer, the thermally conductive layer can be scraped off and ground into powder and weighed. The powder can then be rinsed with N-methylpyrrolidone and deionized water respectively until the binder is fully dissolved. The powder can then be thoroughly dried and weighed. The difference between the two weights is the weight percentage of the binder in the thermally conductive layer. When the thermal conductive layer also includes a conductive agent, conventional methods such as ultrasonic method can be combined to separate the thermal conductive particles and the conductive agent. For example, if the conductive agent is conductive carbon black and the thermal conductive particles are diamond-like carbon, the density of diamond-like carbon is greater than 3g / cm3 , the density of conductive carbon black is less than 3g / cm 3 The characteristics of the conductive agent and thermal conductive particles are mixed powder at a density of 3g / cm 3 Ultrasonication is performed in a solvent. After sonication, the particles disperse and separate into layers in the solvent. The upper conductive agent layer is sampled, dried, and weighed to determine the mass percentage of the conductive agent in the thermally conductive layer. Optionally, the mass percentage of the thermally conductive particles in the thermally conductive layer can be further determined by measuring the mass percentage of the lower thermally conductive particles by drying and weighing, and / or by combining the mass percentage of the conductive agent and / or binder.

[0118] The electrical conductivity of the thermally conductive particles is low. An appropriate amount of conductive agent can be added to the thermally conductive layer to improve the conductivity of the negative electrode sheet, and an appropriate amount of binder can be added to the thermally conductive layer to improve the adhesion of the thermally conductive layer to the surface of the negative electrode current collector. However, the amount of the two added will have a certain impact on the thermal conductivity of the thermally conductive layer.

[0119] By controlling the content of the conductive agent and / or binder in the thermal conductive layer within a given range, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery, and it is also beneficial to take into account the conductivity of the negative electrode sheet and the adhesion of the conductive layer.

[0120] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the electrolyte may be greater than or equal to the mass proportion of the thermally conductive particles in the negative electrode active material layer.

[0121] As some specific examples, thermally conductive particles can be dispersed in the electrolyte and the negative electrode active material layer at the same time. Compared with dispersing the thermally conductive particles in the negative electrode active material layer, dispersing the thermally conductive particles in the electrolyte is beneficial to improving the curing uniformity of the gel polymer matrix and the heat dissipation of the battery, and will not affect the amount of negative electrode active material in the negative electrode sheet.

[0122] By making the mass proportion of the thermally conductive particles in the electrolyte greater than or equal to the mass proportion of the thermally conductive particles in the negative electrode active material layer, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation of the battery, while also taking into account the energy density of the battery.

[0123] In some embodiments of the present application, the mass proportion of the thermally conductive particles in the negative electrode active material layer may be greater than or equal to the mass proportion of the thermally conductive particles in the positive electrode active material layer.

[0124] In order to improve the charge and discharge capacity of the negative electrode plate, the negative electrode active material may include a silicon material with low thermal conductivity. By making the content of thermally conductive particles in the negative electrode active material layer higher than that in the positive electrode active material layer, it is beneficial to improve the thermal conductivity uniformity of the negative electrode plate and the consistency of the overall thermal conductivity effect inside the battery, and improve the thermal conductivity of the negative electrode plate containing silicon material and the curing uniformity of the gel polymer matrix.

[0125] By making the mass proportion of the thermally conductive particles in the negative electrode active material layer greater than or equal to the mass proportion of the thermally conductive particles in the positive electrode active material layer, it is beneficial to further improve the curing uniformity of the gel polymer matrix and the heat dissipation effect of the battery.

[0126] In some embodiments of the present application, the battery may further include a separator, which may include but is not limited to a polyethylene porous membrane, a polypropylene porous membrane, a polyimide porous membrane, and a porous membrane formed by a composite of multiple polymers.

[0127] In some embodiments of the present application, the shape of the battery in the second aspect of the present application is not particularly limited, and those skilled in the art can flexibly select it according to actual needs. For example, it can be cylindrical, square (refer to Figure 1 for understanding) or any other shape.

[0128] In some embodiments of the present application, the battery may include an outer package for encapsulating a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte.

[0129] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a base plate and side plates connected to the base plate, with the base plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover plate may be positioned over the opening to seal the receiving cavity.

[0130] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The electrolyte in the gel polymer electrolyte is infiltrated into the electrode assembly. The number of electrode assemblies in a battery can be one or more, and can be adjusted based on demand.

[0131] In some embodiments, the outer packaging of the battery may be a hard shell, which may be a metal shell or a non-metal shell, for example, a hard plastic shell, an aluminum shell, a steel shell, etc.

[0132] In some embodiments, the outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may include plastic, for example, one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc., and may also be an aluminum-plastic film.

[0133] In some embodiments of the present application, the battery may be either a battery cell 1 (refer to FIG1 for understanding), or a battery module 2 (refer to FIG2 for understanding) or a battery pack 3 (refer to FIG3 for understanding) composed of battery cells 1 .

[0134] In some embodiments, the battery may be a battery module, and the number of battery cells contained in the battery module may be one or more, and the specific number may be adjusted according to the application and capacity of the battery module. Figure 2 is a battery module 2 as an example. Referring to Figure 2, in the battery module 2, a plurality of battery cells 1 may be arranged in sequence along the length direction of the battery module 2. Of course, they may also be arranged in any other manner. The plurality of battery cells 1 may further be fixed by fasteners. Optionally, the battery module 2 may further include a housing having a housing space, and the plurality of battery cells 1 are accommodated in the housing space.

[0135] In some embodiments, the battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack. Referring to Figure 3 or Figure 4 (Figures 3 and 4 are battery packs 3 as an example), the battery pack 3 may include a battery box and a plurality of battery modules 2 disposed in the battery box. The battery box may include an upper box body 4 and a lower box body 5. The upper box body 4 can be covered on the lower box body 5 and form an enclosed space for accommodating the battery modules 2. The plurality of battery modules 2 can be arranged in the battery box in any manner.

[0136] In addition, the present application also provides an electric device, which includes: the battery of the second aspect of the present application. The battery, such as a battery cell, a battery module or a battery pack, can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include but is not limited to mobile devices (such as mobile phones, laptops), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, and energy storage systems. With reference to Figure 5, as a specific example, the electric device can be a vehicle. The electric device can select the specific type of battery according to its usage requirements, such as a battery cell, a battery module or a battery pack.

[0137] As an example, the electric device may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the electric device's requirements for high power and high energy density of the battery, a battery pack or battery module may be used.

[0138] As another example, the electrical device may be a mobile phone, a tablet computer, or a laptop computer. The electrical device is generally required to be lightweight and thin, and may use a battery cell as a power source.

[0139] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0140] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0141] Example 1

[0142] (1) Preparation of positive electrode sheet

[0143] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black, and binder PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 96:2:2, and solvent N-methylpyrrolidone (NMP) was added and stirred until the system became uniform to obtain a positive electrode slurry (solid content of 40wt%); the positive electrode slurry was prepared with a solid content of about 20mg / cm 2 The positive electrode sheet was evenly coated on both sides of the positive electrode current collector aluminum foil, dried at room temperature, and then transferred to an oven for further drying. It was then cut into 40mm×50mm rectangles as positive electrode sheets. The positive electrode surface capacity was 4mAh / cm 2 .

[0144] (2) Preparation of negative electrode sheet

[0145] A 20 μm lithium foil was rolled onto a 12 μm copper foil and then cut into a 41 mm × 51 mm rectangle for use as a negative electrode.

[0146] Alternatively, the negative electrode active material 20wt% Si-Graphite silicon carbon, the conductive agent carbon nanotubes, and the binder SBR (styrene-butadiene rubber) were mixed in a mass ratio of 96.9:0.1:3, and the solvent NMP was added and stirred until the system became uniform to obtain a negative electrode slurry (solid content of 30wt%); the negative electrode slurry was prepared with a solid content of about 3.9mg / cm 2 The loading amount is evenly coated on both sides of the negative electrode current collector copper foil, dried at room temperature, transferred to the oven for further drying, and then cut into 41mm×51mm rectangles as positive electrode sheets. The negative electrode surface capacity is 4.4mAh / cm 2 .

[0147] (3) Preparation of gel polymer electrolyte precursor solution:

[0148] 115g of the main solvent (made by mixing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1), 6g of the auxiliary solvent fluoroethylene carbonate (FEC), 15g of the lithium salt LiPF6, and diamond-like carbon were mixed to form a 1M concentration electrolyte. 20g of the polymer monomer vinylene carbonate, 6.67g of the cross-linking agent polyethylene glycol diacrylate, and 0.53g of the initiator azobisisobutyronitrile were then added. The thermal conductivity of diamond-like carbon is 1000W / mK and the electrical conductivity is 3.9×10 -12 S / cm, and its mass proportion in the gel polymer electrolyte precursor solution is 2 wt%.

[0149] (4) Preparation of isolation membrane

[0150] A polyethylene porous film with a thickness of 10 μm was selected as the separator and cut into a rectangle of 45 mm×55 mm for standby use.

[0151] (5) Preparation of secondary batteries

[0152] Battery Assembly: 12 pre-cut positive electrode sheets are matched with 13 pre-cut negative electrode sheets, separated by the aforementioned separator film. The cells are then wrapped in an aluminum-plastic film bag to form a laminated dry cell. 4.5g of the prepared electrolyte is injected, and the aluminum-plastic film bag is sealed by vacuum hot pressing. Curing is performed at 70°C for 6 hours, followed by at least 12 hours at room temperature before testing. The laminated battery prepared in this manner has a rated capacity of 2376mAh.

[0153] Examples 2 to 20 and Comparative Example 1

[0154] The difference between Comparative Example 1 and Example 1 is that in step (3), no diamond-like carbon is added when preparing the gel polymer electrolyte precursor solution.

[0155] The difference between Examples 2 to 7 and Example 1 is that the thermal conductivity of diamond-like carbon is different.

[0156] The difference between Examples 8 to 11 and Example 1 is that the mass proportion of diamond-like carbon in the gel polymer electrolyte is different.

[0157] The difference between Examples 12 to 14 and Example 1 is that the particle size ranges of the diamond-like carbon are different.

[0158] The difference between Examples 15 to 19 and Example 2 is that the hydrogen content and sp 3 Different bonded carbon contents result in different thermal and electrical conductivities.

[0159] The difference between Examples 20 to 24 and Example 2 is that the electrical conductivity and thermal conductivity of the diamond-like carbon are different. The thermal conductivity of the diamond-like carbon in Examples 20 to 24 at 25° C. is greater than 400 W / mK.

[0160] Performance testing:

[0161] The curing uniformity of the diamond-like carbon and the gel polymer electrolyte of the secondary battery prepared in the above-mentioned embodiments and comparative examples was tested. The testing method includes:

[0162] 1. Electrical conductivity and thermal conductivity test of diamond-like carbon

[0163] Conduct conductivity test at room temperature and pressure with reference to the test method for volume conductivity in GB / T 1410-2006;

[0164] Thermal conductivity test was carried out at room temperature and pressure with reference to GB / T 32064-2015.

[0165] 2. Hydrogen content and sp of diamond-like carbon 3 Test of bonded carbon content

[0166] The hydrogen content in diamond-like carbon is determined by completely burning and decomposing the diamond-like carbon and quantitatively analyzing the CO2 and H2O produced by the combustion.

[0167] By performing XPS testing on diamond-like carbon, the sp 2 With sp 3 The different characteristic peaks contributed by different hybrid bond energies are 284.4eV and 285.2eV respectively. By splitting the XPS test peaks, the corresponding area ratio of the characteristic peaks of 284.4eV and 285.2eV can be used to determine the sp 3 The proportion of bonded carbon.

[0168] 3. Test of curing uniformity of gel polymer electrolyte

[0169] The prepared battery cell was disassembled, and the separator containing the solidified gel polymer electrolyte was removed. The separator was placed on a stainless steel plate, and the stainless steel was connected to the counter electrode of the atomic force microscope electrochemical mode to form a test path. The atomic force microscope was used to select points in a 10×10 matrix in the separator area with a length and width of 5cm×5cm. The elastic modulus E of each test point was obtained by atomic force microscope testing in the mechanical mode. i At the same time, the AC impedance Z of each test point is obtained through the impedance test in electrochemical mode. iThe uniformity of the gel polymer electrolyte curing was evaluated based on the elastic modulus and AC impedance measured at each test point, where the uniformity of the elastic modulus distribution A E The distribution uniformity of electrochemical impedance spectroscopy Z They are evaluated by the following formulas:

[0170] 4. Ionic conductivity and electronic conductivity test of gel polymer electrolyte

[0171] The battery cell was disassembled, the gel polymer electrolyte membrane was taken out, and the ionic conductivity and electronic conductivity of the gel polymer electrolyte membrane were tested: the test method of ionic conductivity was carried out in accordance with the standard HG / T 4067-2015, and the resistance of the gel polymer electrolyte was tested using a conductivity meter at a constant temperature of 25±0.1°C and an AC impedance of 1kHz to calculate its conductivity; the electronic conductivity of the gel polymer electrolyte can be measured using the resistance value obtained by the DC two-probe method, where the contact area between the probe and the gel polymer electrolyte membrane can be set to 49πmm 2 For example, the resistance R of the gel polymer electrolyte membrane can be tested using a Hioki BT23562 internal resistance tester. The specific operation is as follows: the upper and lower sides of the gel polymer electrolyte membrane are clamped between two conductive terminals of the tester and pressure is applied to secure it. The diameter of the conductive terminals is 14 mm, and the applied pressure is 15 MPa to 27 MPa. The resistance R of the gel polymer electrolyte membrane is measured, and the electronic conductivity σ of the gel polymer electrolyte is calculated according to the formula σ = d / S × (1 / R), where S is the detection area, which in this test is equal to the area of ​​the conductive terminals. d is the thickness of the test sample located between the two conductive terminals, that is, the thickness of the gel polymer electrolyte membrane.

[0172] The test results of Examples 1 to 24 and Comparative Example 1 are detailed in Table 1.

[0173] Table 1 Differences and test results of Examples 1 to 14 and Comparative Example 1

[0174] Table 2 Differences and test results of Examples 2, 15 to 19

[0175] Table 3 Differences and test results of Examples 2, 20-24

[0176] Results and Conclusions:

[0177] Combining Examples 1 to 24 and Comparative Example 1, it can be seen that dispersing diamond-like carbon as thermally conductive particles in the electrolyte of the gel polymer electrolyte is beneficial to improving the curing uniformity of the gel polymer matrix during the in-situ curing process. At the same time, the amount of diamond-like carbon added to the gel polymer electrolyte, as well as the thermal conductivity, hydrogen content, and sp 3 The changes in bonded carbon content and particle size have a certain impact on improving the curing uniformity of the gel polymer matrix during the in situ curing process. The improvement effect can be further improved by further optimizing the selection of various parameters.

[0178] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A gel polymer electrolyte, wherein: include: An electrolyte having thermally conductive particles dispersed therein, wherein the thermal conductivity of the thermally conductive particles at 25° C. is greater than or equal to 400 W / mK.

2. The gel polymer electrolyte according to claim 1, wherein The conductivity of the thermally conductive particles at 25°C is not greater than 10 -7 S / cm, optional 10 -16 S / cm~10 -7 S / cm.

3. The gel polymer electrolyte according to claim 1 or 2, wherein: The thermal conductivity is 400W / mK to 2000W / mK.

4. The gel polymer electrolyte according to any one of claims 1 to 3, wherein The thermally conductive particles include diamond-like carbon.

5. The gel polymer electrolyte according to claim 4, wherein Based on the total number of atoms of the diamond-like carbon, the atomic percentage of hydrogen in the diamond-like carbon is less than or equal to 50 at%, optionally less than or equal to 20 at%, and further optionally less than or equal to 10 at%; and / or, Based on the total number of carbon atoms in the diamond-like carbon, the number of sp 3 The atomic percentage of bonded carbon is 20 at% to 85 at%, and may be 70 at% to 85 at%.

6. The gel polymer electrolyte according to any one of claims 1 to 5, wherein The particle size of the thermally conductive particles is less than or equal to 10 μm.

7. The gel polymer electrolyte according to any one of claims 1 to 6, wherein Based on the total mass of the gel polymer electrolyte, the mass proportion of the thermally conductive particles is 0.1 wt% to 5 wt%, and may be 0.5 wt% to 2 wt%.

8. The gel polymer electrolyte according to any one of claims 1 to 7, wherein It also includes: a gel polymer matrix, on which the thermally conductive particles are dispersed.

9. A battery, wherein: The invention comprises the gel polymer electrolyte according to any one of claims 1 to 8.

10. The battery according to claim 9, wherein It also includes: a positive electrode sheet, a negative electrode sheet and a separator, and at least one of the positive electrode sheet, the negative electrode sheet and the separator includes the thermally conductive particles.

11. The battery according to claim 10, wherein The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer comprises the thermally conductive particles; and / or, The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes the thermally conductive particles; or, the negative electrode plate includes a negative electrode current collector and a thermally conductive layer disposed on the negative electrode current collector, wherein the thermally conductive layer includes the thermally conductive particles.

12. The battery according to claim 11, wherein The mass proportion of the thermally conductive particles in the positive electrode active material layer is 0.1 wt % to 2 wt %.

13. The battery according to claim 11 or 12, wherein The mass percentage of the thermally conductive particles in the negative electrode active material layer is 0.1wt% to 4wt%; and / or the negative electrode active material layer comprises silicon material, and the mass percentage of silicon in the negative electrode active material layer is greater than or equal to 10wt%.

14. The battery according to any one of claims 11 to 13, wherein The thickness of the heat-conducting layer is 50 nm to 5 μm; and / or the mass proportion of the heat-conducting particles in the heat-conducting layer is greater than or equal to 50 wt %.

15. The battery according to any one of claims 11 to 14, wherein The thermal conductive layer further comprises: a conductive agent and / or a binder, wherein the conductive agent accounts for 0.1wt% to 40wt% by weight of the thermal conductive layer, and may be 5wt% to 15wt% by weight, and the binder accounts for 0.01wt% to 5wt% by weight of the thermal conductive layer.

16. The battery according to any one of claims 11 to 15, wherein The mass proportion of the thermally conductive particles in the electrolyte is greater than or equal to the mass proportion of the thermally conductive particles in the negative electrode active material layer; and / or the mass proportion of the thermally conductive particles in the negative electrode active material layer is greater than or equal to the mass proportion of the thermally conductive particles in the positive electrode active material layer.

17. An electrical device, wherein: A battery comprising the battery according to any one of claims 9 to 16.

Citation Information

Patent Citations

  • Patterning on surface with high thermal conductivity materials

    CN101460678A

  • Separator, battery, battery pack, electronic apparatus, electric vehicle, power storage device, and power system

    CN105051941A

  • Battery, electrolyte layer, battery pack, electronic apparatus, electric vehicle, power storage device, and power system

    CN105051963A

  • Thermally conductive lithium ion electrodes and batteries

    US20160308263A1