Battery, battery pack, electronic device, and energy storage system

By doping the first inactive metal element into the positive electrode material of the sodium ion battery and using a phosphate coating layer, the cycle stability and metal element dissolution problems of layered oxide material are solved, and higher cycle stability and Battery safety.

WO2024244386A1PCT designated stage expired Publication Date: 2024-12-05HUAWEI DIGITAL POWER TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/138269
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-12-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Laminated oxide materials have poor cycle stability in actual applications, especially in high-temperature environments, severe cycle life attenuation, and metal element dissolution problems, affecting battery safety.

Method used

Using a positive electrode material doped with the first inactive metal element and a phosphate-based material, the structural stability is improved by doping the first inactive metal element into the core material, and the metal element is reduced by the phosphate coating layer. The risk of contact of electrolytes reduces interfacial side reactions.

Benefits of technology

It improves the cycle stability, cycle life and voltage of the cathode material, enhances the safety of battery use, and performs more significantly in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138269_05122024_PF_FP_ABST
    Figure CN2023138269_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A battery. A positive electrode sheet of the battery comprises a positive electrode active material layer; the positive electrode active material layer comprises a positive electrode material; the positive electrode material comprises a core material and a coating layer material with which the surface of the core material is coated, the core material is a metal oxide, the core material is doped with a first non-active metal element, and the coating layer material is phosphate. Also provided are a battery pack and an electronic device using the battery, and an energy storage system using the battery pack. The first non-active metal element is doped in the positive electrode material, and the surface of the positive electrode material is coated with a phosphate coating material, so that the positive electrode material has high structural stability and dissolution of the metal element is effectively reduced, and thus, the battery shows good cycle stability, long cycle life, and high voltage, and the use safety of the battery is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Batteries, battery packs, electronic devices and energy storage systems

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to a Chinese patent application filed with the Patent Office of China on May 30, 2023, with application number 202310628555.X and application name “Batteries, battery packs, electronic devices and energy storage systems,” the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of battery technology, and in particular to a battery, a battery pack and electronic equipment using the battery, and an energy storage system using the battery pack. Background Art

[0004] As a new generation of green energy storage devices, the commonly used positive electrode materials for sodium-ion batteries include layered oxides. Layered oxide materials are considered to be the first materials to be commercialized due to their advantages such as high gram capacity, simple synthesis process and high compaction density.

[0005] However, in practical applications, it is found that the cycle stability of layered oxide materials is poor, especially in high-temperature environments, where the cycle life is severely attenuated; in addition, layered oxide materials also have the problem of metal element dissolution, which poses a hidden danger to battery safety.

[0006] Summary of the Invention

[0007] In view of this, in order to solve at least one of the above defects, an embodiment of the present application provides a battery, the positive electrode plate of which can improve the cycle stability and voltage of the battery, extend the cycle life of the battery, and improve the safety of battery use.

[0008] In addition, embodiments of the present application also provide a battery pack and electronic device using the above-mentioned battery, and an energy storage system using the above-mentioned battery pack.

[0009] In a first aspect, an embodiment of the present application provides a battery comprising a positive electrode sheet, a negative electrode sheet, and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet comprising a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer comprising a positive electrode material. The positive electrode material comprises a core material and a coating material coated on the surface of the core material, wherein the core material is a metal oxide, the coating material is a phosphate, and the core material is doped with a first inactive metal element. The first inactive metal element is doped into the formed core material by doping. The core material comprises an active metal element and a second inactive metal element, wherein the concentration of the active metal element gradually increases from the surface layer of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface layer of the core material to the core of the core material.

[0010] By doping the core material with a first inactive metal element, the first inactive metal element does not participate in the charge and discharge reaction, and can play an effective structural support role, stabilizing the structure of the core material, thereby optimizing the layered structure of the positive electrode material, effectively inhibiting the harmful phase transformation of the positive electrode material during the cycle (especially at high voltage), and helping to improve the stability of the positive electrode material; in addition, by doping the core material with the first inactive metal element, the problem of uneven stress within the core material during the cycle can also be reduced, thereby reducing the formation of microcracks within the core material, and further improving the stability of the positive electrode material. Therefore, after doping the core material with the first inactive metal element, it is beneficial to improve the cycle stability, cycle life, and voltage of the positive electrode sheet, so that the battery has high cycle stability (especially high voltage cycle stability), long cycle life, and high voltage.

[0011] By coating the surface of the core material with a phosphate coating material, not only is the risk of contact between the metal elements in the core material and the electrolyte reduced, the dissolution of the metal elements is reduced, and the safety of the battery is improved, but also the interface side reactions between the positive electrode plate using the positive electrode material and the electrolyte are reduced, and the risk of a passivation layer being generated at the interface between the positive electrode plate and the electrolyte is reduced, thereby ensuring smooth ion transmission and improving the cycle stability and cycle life (especially the cycle life in a high temperature environment) of the battery using the positive electrode material; in addition, phosphate contains PO bonds with strong bond energy, is not easy to lose oxygen atoms in the electrolyte, and has higher structural stability, which is conducive to further reducing interface side reactions.

[0012] Specifically, the general formula of the core material can be: A ɑ X γ Y βO2, ɑ is 0.9 to 1.1, γ + β = 1, wherein A can be a sodium ion or a lithium ion, X is an active metal element, and Y is a second inactive metal element.

[0013] In the core material, the active metal element can participate in electrochemical reactions, increasing the specific capacity of the cathode material to meet the requirements of high energy density. The addition of the second inactive metal element can provide structural support within the layered metal oxide, delaying or inhibiting phase transitions and resulting in greater safety and structural stability for the cathode material. Furthermore, by gradually increasing the concentration of the active metal element from the surface to the core of the core material, while gradually decreasing the concentration of the second inactive metal element from the surface to the core of the core material, the core material has a lower concentration of the active metal element on the surface and a higher concentration of the second inactive metal element, further reducing the risk of active metal element dissolution.

[0014] Therefore, the positive electrode material of the embodiment of the present application has high structural stability and can reduce the dissolution of metal elements, so that the battery using the positive electrode material has good cycle stability, long cycle life, high voltage, and high safety in use.

[0015] Furthermore, the active metal element is at least one selected from the group consisting of iron, cobalt, nickel, vanadium, copper, and chromium. The second inactive metal element is at least one selected from the group consisting of manganese and niobium.

[0016] Furthermore, in the core material, the molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:4. For example, the molar ratio may be 9:1, 8:2, 7:3, or 6:4.

[0017] In combination with the first aspect, in some possible embodiments, the first inactive metal element is selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + and the like, and when the core material is a sodium-containing oxide, the first inactive metal element is not Na + When the core material is a lithium-containing oxide, the first inactive metal element is not Li + .

[0018] By using the first inactive metal element to dope the core material, since the ion radius of this type of inactive metal element is closer to the transport ions in the core material (such as Li + Or Na +) radius, such as the active metal elements listed above (such as Ni 2+ ) is more likely to occupy the position of transported ions, and the structural support is stronger, which is more conducive to limiting the transported ions in the core material (such as Li + Or Na + ) and active metal elements (such as Ni 2+ ) to improve the structural stability of the core material.

[0019] In combination with the first aspect, in some possible embodiments, the doping concentration of the first inactive metal element gradually decreases from the surface layer of the core material to the core of the core material.

[0020] By designing the doping concentration of the doping element to gradually decrease from the surface of the core material to the core of the core material, the first inactive metal element is distributed in a non-uniform gradient state, which can ensure that the first inactive metal element optimizes the layered structure of the core material and improves the stability of the core material structure. At the same time, it can effectively reduce the doping amount of the first inactive metal element, improve the purity of the core material, and reduce the impact of the doping of the first inactive metal element on the electrochemical properties of the core material.

[0021] In conjunction with the first aspect, in some possible embodiments, the molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04), further 1:(0.0001-0.01), further 1:(0.0001-0.005), and further 1:(0.0001-0.001). For example, the molar ratio of the core material to the first inactive metal element can be 1:0.001, 1:0.005, 1:0.01, and so on.

[0022] If the doping amount of the first inactive metal element is too low, it will not provide good structural support and will have a weak effect on optimizing the layered structure of the core material. If the doping amount of the first inactive metal element is too high, the excess first inactive metal element will reduce the purity of the core material, affect ion transport, and reduce the specific capacity of the positive electrode material. Therefore, the embodiments of the present application control the doping amount of the first inactive metal element in the core material within the above range. While achieving improved structural stability of the core material, it can also improve the purity of the core material, thereby reducing the impact of the doping of the first inactive metal element on the electrochemical performance of the positive electrode material.

[0023] In combination with the first aspect, in some possible embodiments, the phosphate contains at least two phosphate groups and / or at least one pyrophosphate group.

[0024] Phosphates containing at least two phosphate groups and / or at least one pyrophosphate group have a higher content of PO bonds, and the PO bond energy is relatively strong, and it is not easy to lose oxygen atoms, thereby making the structural stability of the coating layer material higher and less likely to react with the electrolyte, which is beneficial to further improve the stability of the positive electrode material.

[0025] In conjunction with the first aspect, in some possible embodiments, the molecular formula of the phosphate is: A x R y (PO4) a (P2O7) b , wherein A is a sodium ion or a lithium ion; R is selected from at least one of the elements Fe, V, Ti, Mn, Co, etc.; the values ​​of x, y, a and b can satisfy the algebraic sum of positive and negative valences in the molecular formula of phosphate to be zero.

[0026] Phosphate contains sodium or lithium elements, so the coating layer material is a sodium or lithium storage material. This type of coating layer material is used to modify the surface of sodium oxide-containing positive electrode materials or lithium oxide-containing positive electrode materials, which is beneficial to reduce interfacial side reactions while not sacrificing the capacity of the positive electrode material.

[0027] Furthermore, the core material is a sodium oxide, and the phosphate is selected from at least one of Na2FeP2O7, Na3Fe2(PO4)P2O7, Na3V2Fe(PO4)3, Na3VMn2Fe(PO4)3, Na3VTiFe(PO4)3, Na3Fe2Fe(PO4)3 and Na3MnTiFe(PO4)3.

[0028] In combination with the first aspect, in some possible embodiments, the average particle size of the particles of the coating layer material is 40nm~90nm, further 50~70. Exemplarily, the average particle size of the particles of the coating layer material can be 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm or a value between any two of the above values.

[0029] By controlling the particle size of the coating layer material, it is beneficial to form a coating layer with uniform thickness and uniform coating on the surface of the core material, so as to fully isolate the core material and the electrolyte.

[0030] In conjunction with the first aspect, in some possible embodiments, the mass ratio of the coating layer material to the positive electrode material is 1% to 40%, or further 5% to 20%. Exemplarily, the mass ratio of the coating layer material to the positive electrode material is 1%, 5%, 10%, 20%, 30%, or 40%.

[0031] When the content of the coating material is too much, the coating thickness is too thick, which affects the ion transmission and also reduces the proportion of the core material, thereby reducing the capacity of the positive electrode material; when the content of the coating material is too little, a uniform and effective coating layer cannot be formed, and the effect of reducing the interface side reaction is not obvious. Therefore, the embodiment of the present application controls the content of the coating material in the positive electrode material within the above range. On the one hand, a positive electrode material with excellent surface morphology can be obtained after coating. The coating thickness is moderate, which is conducive to reducing the interface side reaction while having a positive effect on the capacity and ion transmission of the positive electrode material. In addition, the metal element in the core material and the oxygen element in the coating material are bonded to form a chemical bond. Such chemical bond can be an ionic bond, a covalent bond, etc., for example: Mn-O. Since the core material and the coating material are combined together by solid phase grinding and microwave treatment to form a modified positive electrode material, it can promote the bonding reaction between the oxygen element in the coating material and the metal element in the core material, producing chemical bonds such as Mn-O, thereby enhancing the bonding force between the coating material and the core material.

[0032] A second aspect of the present application provides a battery pack comprising a plurality of batteries as described above, wherein the plurality of batteries are connected in series or in parallel with a separator. The positive electrode plates in the batteries described above are beneficial for improving the battery's cycle stability, overall cycle life, voltage, and safety, thereby improving the service life and safety of the battery pack incorporating the batteries.

[0033] A third aspect of the present application provides an electronic device comprising a housing and a battery as described above, the battery being mounted within the housing. The positive electrode plate in the battery improves the battery's cycle stability, overall cycle life, voltage, and safety, thereby improving the service life and safety of electronic devices using the battery.

[0034] A fourth aspect of the present application provides an energy storage system, comprising a power converter and the aforementioned battery pack. The power converter is configured to convert the voltage output by the battery pack into power, and / or the power converter is configured to convert the voltage output by an external power source into power before outputting it to the battery pack. Because the positive electrode in the aforementioned battery helps improve battery cycle stability, overall cycle life, voltage, and safety, it also helps improve the service life and safety of the energy storage system using the aforementioned battery pack. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] FIG1 is a schematic structural diagram of a positive electrode material provided in one embodiment of the present application.

[0036] FIG2 is a schematic structural diagram of a positive electrode plate provided in one embodiment of the present application.

[0037] FIG3 is a schematic structural diagram of a battery provided in an embodiment of the present application.

[0038] FIG4 is a schematic structural diagram of a battery pack provided in an embodiment of the present application.

[0039] FIG5 is a schematic structural diagram of an electronic device provided in an embodiment of the present application.

[0040] FIG6 is a graph showing the concentrations of Ni, Fe, and Mn in the core material of Example 1 as the distance from the center of the core material surface layer changes.

[0041] FIG7A is a cycle performance curve (positive electrode median voltage stability test) of a half-cell prepared using the positive electrode materials of Example 1 (after improvement) and Comparative Example 1 (before improvement).

[0042] FIG7B is a cycle performance curve (cycle stability test) of half-cells prepared using the positive electrode materials of Example 1 (after improvement) and Comparative Example 1 (before improvement).

[0043] FIG8 is a scanning electron microscope photograph of the positive electrode material of Comparative Example 1.

[0044] FIG9 is a scanning electron microscope photograph of the positive electrode material of Example 1 of the present application.

[0045] Description of main component symbols

[0046] Positive electrode 100

[0047] Current Collectors 101

[0048] Positive electrode active material layer 102

[0049] Positive electrode material 10

[0050] Core material 1

[0051] Coating material 2

[0052] Battery 200

[0053] Negative electrode 201

[0054] Diaphragm 202

[0055] Electrolyte 203

[0056] Battery Pack 300

[0057] Electronic equipment 400

[0058] Housing 401 DETAILED DESCRIPTION

[0059] The following specific embodiments illustrate the implementation of the present application. Those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with the embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide an in-depth understanding of the present application, the following description will contain many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other unless there is a conflict.

[0060] Hereinafter, if used, the terms "first," "second," etc., are used for descriptive purposes only and are not to be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature qualified as "first," "second," etc. may explicitly or implicitly include one or more of such features. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0061] The following describes the embodiments of the present application in conjunction with the accompanying drawings. Unless otherwise specified, the data range values ​​recorded in this application should include the end values.

[0062] Layered oxide sodium ion positive electrode materials have poor cycle stability, especially in high temperature environments where the cycle life is severely degraded; in addition, layered oxide materials also have problems with metal element dissolution and electrode degradation, and the dissolution of metal elements will pose a hidden danger to battery safety.

[0063] In view of this, an embodiment of the present application provides a battery, which includes a positive electrode sheet, a negative electrode sheet and a separator, the separator is arranged between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet includes a current collector and a positive electrode active material layer provided on the current collector, and the positive electrode active material layer includes a positive electrode material. After the positive electrode material is modified, the structural stability is stronger and the metal elements are not easily dissolved. The positive electrode material can be used as an active material of the positive electrode in sodium ion batteries or lithium ion batteries, but is not limited thereto. The battery using the positive electrode material has good cycle stability, long cycle life, high voltage, and high safety in use.

[0064] The positive electrode material provided in the embodiment of the present application includes a core material and a coating layer material coated on the surface of the core material, wherein the core material is a metal oxide and the core material is doped with a first inactive metal element; in addition, the coating layer material is a phosphate.

[0065] The core material is a layered metal oxide material containing an active metal element and a second inactive metal element. Specifically, the core material may be formulated as follows: ɑ X γ Y β O2, where ɑ ranges from 0.9 to 1.1, γ + β = 1, and in order to satisfy the algebraic sum of positive and negative valences in the above molecular formula to be zero, the values ​​of ɑ, γ, and β can satisfy A ɑ X γ Y β It has a valence of -4, A can be a sodium ion or a lithium ion, X is an active metal element, and Y is a second inactive metal element. Furthermore, the active metal element is selected from at least one of iron, cobalt, nickel, vanadium, copper and chromium, and these active metal elements exist in the core material in the form of ions; the second inactive metal element is selected from at least one of manganese (Mn) and niobium (Nb), and these inactive metal elements exist in the core material in the form of ions. For example, the general formula of the core material can be Na ɑ Ni x Fe y Mn β O2, ɑ range is 0.9~1.1, x+y+β=1. Among them, "active metal elements" refer to metal elements that participate in electrochemical reactions. Such metal elements will change their valence during the charge and discharge process. For example, the iron element in the core material is usually Fe 3+ , Fe 3+ It reacts with the electrolyte and is easily converted into Fe 4+, and then dissolve out of the core material; "inactive metal elements" refer to metal elements that do not participate in electrochemical reactions and whose valence state does not change during the charge and discharge process. Inactive metal elements mainly play a structural support role. In the core material, the aforementioned active metal elements can participate in electrochemical reactions, which can increase the specific capacity of the positive electrode material to meet the requirements of high energy density. The addition of the second inactive metal element can play a structural support role in the layered metal oxide, delaying or inhibiting the formation of phase transitions, and making the positive electrode material have higher safety and structural stability.

[0066] In some embodiments, the concentration of the active metal element gradually increases from the surface of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface of the core material to the core of the core material. Active metal elements (such as nickel and iron) are active and easily undergo valence changes when in contact with the electrolyte, causing the active metal elements to dissolve, resulting in reduced stability of the positive electrode material. The second inactive metal element (such as manganese) can play a role in structural support. The concentration of the active metal element is gradually increased from the surface of the core material to the core, and the concentration of the second inactive metal element is gradually reduced from the surface of the core material to the core, that is, the concentration of the active metal element on the surface of the core material is low, while the concentration of the second inactive metal element is high, which is conducive to further reducing the risk of active metal element dissolution and improving the stability of the positive electrode material.

[0067] In some embodiments, in the core material, the molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:4. For example, the molar ratio may be 9:1, 8:2, 7:3, or 6:4.

[0068] The core material is doped with a first inactive metal element, which does not participate in the charge-discharge reaction and does not undergo a change in valence during the charge-discharge process. The inclusion of the first non-metallic element in the core material provides effective structural support to stabilize the structure of the core material, thereby optimizing the layered structure of the positive electrode material and effectively suppressing harmful phase transitions of the positive electrode material during cycling (especially at high voltages), thereby improving the stability of the positive electrode material. Furthermore, doping the core material with the first inactive metal element can also reduce the problem of uneven stress within the core material during cycling, thereby reducing the formation of microcracks within the core material and further improving the stability of the positive electrode material. Therefore, doping the core material with the first inactive metal element is beneficial for improving the cycling stability, cycle life, and voltage of the positive electrode material.

[0069] In some embodiments, the content of the first inactive metal element in the core material can be uniformly distributed or non-uniformly distributed. Specifically, in the embodiment of the present application, the doping concentration of the first inactive metal element gradually decreases from the surface of the core material to the core of the core material to form a non-uniform gradient distribution morphology. And this non-uniform gradient distribution morphology mainly depends on the doping method of the first inactive metal element. In the embodiment of the present application, the first inactive metal element is directly mixed with the prepared core material. At this time, the first inactive metal element will be preferentially doped into the interlayer of the core material that has formed a fixed structure. Moreover, the usual layered metal oxide core material is a spherical particle with a certain particle size. The amount of the first inactive metal element doped into the positive electrode material will gradually decrease with the increase of the doping depth, thereby forming a non-uniform gradient distribution state. By designing the doping concentration of the doping element to gradually decrease from the surface of the core material to the core of the core material, the first inactive metal element is distributed in a non-uniform gradient state, which can ensure that the first inactive metal element optimizes the layered structure of the core material and improves the stability of the core material structure. At the same time, it can effectively reduce the doping amount of the first inactive metal element, improve the purity of the core material, and reduce the impact of the doping of the first inactive metal element on the electrochemical properties of the core material.

[0070] In some embodiments, the first inactive metal element to be doped may be selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + Among them, when the core material is a sodium oxide (that is, the battery is a sodium ion battery and the transported ions are sodium ions), the first inactive metal element is not Na + When the core material is a lithium oxide (ie the battery is a lithium ion battery and the transported ions are lithium ions), the first inactive metal element is not Li + By doping the core material with the first inactive metal element, the ion radius of this type of inactive metal element is closer to the transport ions in the core material (such as Li + Or Na + ) radius, such as the active metal elements listed above (such as Ni 2+ ) is more likely to occupy the position of transported ions, and the structural support is stronger, which is more conducive to limiting the transported ions in the core material (such as Li + Or Na + ) and active metal elements (such as Ni 2+) to improve the structural stability of the core material.

[0071] In some embodiments, a core material is first prepared, and then a first inactive metal element is doped into the core material by doping. The active metal element and the second inactive metal element are the main elements of the core material, and the amount of the doped first inactive metal element is much lower than that of the first inactive metal element. Specifically, in the core material, the molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04), further 1:(0.0001-0.01), further 1:(0.0001-0.005), and further 1:(0.0001-0.001). Exemplarily, the molar ratio of the core material to the first inactive metal element can be 1:0.001, 1:0.005, 1:0.01, etc. If the doping amount of the first inactive metal element is too low, it will not play a good structural support role and will have a weak effect on optimizing the layered structure of the core material. If the doping amount of the first inactive metal element is too high, the excessive amount of the first inactive metal element will reduce the purity of the core material, affect ion transport, and reduce the specific capacity of the positive electrode material. Therefore, how to reduce the doping amount of the first inactive metal element while ensuring that the core material has an excellent layered structure and improving the structural stability of the core material has become a research focus of the embodiments of this application. To this end, the embodiments of this application dope the first inactive metal element after the core material is synthesized and form a non-uniform gradient distribution state, thereby effectively reducing the doping amount of the first inactive metal element and controlling the molar ratio of the core material to the first inactive metal element within a low content range of 1: (0.0001-0.04), especially 1: (0.001-0.01). This can improve the purity of the core material while achieving improved structural stability of the core material, thereby reducing the impact of the doping of the first inactive metal element on the electrochemical performance of the positive electrode material.

[0072] In order to reduce the interfacial side reactions between the positive electrode sheet and the electrolyte, and further reduce the dissolution of metal elements on the surface of the core material, a phosphate coating material is used to coat the layered oxide core material. The coating layer material not only reduces the risk of contact between the metal elements in the core material and the electrolyte, reduces the dissolution of metal elements, and improves the safety of battery use, but also reduces the interfacial side reactions between the positive electrode sheet using this positive electrode material and the electrolyte, and reduces the risk of a passivation layer forming at the interface between the positive electrode sheet and the electrolyte, thereby ensuring smooth ion transmission, thereby improving the cycle stability and cycle life (especially the cycle life in high temperature environments) of the battery using this positive electrode material. In addition, phosphate contains PO bonds with strong bond energy, is not easy to lose oxygen atoms in the electrolyte, and has higher structural stability, which is conducive to further reducing interfacial side reactions.

[0073] In some embodiments, the phosphate contains at least two phosphate groups and / or at least one pyrophosphate group. Phosphates containing at least two phosphate groups and / or at least one pyrophosphate group have a high content of PO bonds, and the PO bonds have relatively strong bond energy and are less likely to lose oxygen atoms, thereby making the coating material more structurally stable and less likely to undergo side reactions with the electrolyte, thereby further improving the stability of the positive electrode material.

[0074] Specifically, the molecular formula of phosphate can be: x R y (PO4) a (P2O7) b , where A is a sodium ion or a lithium ion; R is selected from at least one of the elements Fe, V, Ti, Mn, and Co; and the values ​​of x, y, a, and b are such that the algebraic sum of the positive and negative valences in the general molecular formula of the phosphate is zero. Phosphates contain sodium or lithium, so the coating material can store sodium or lithium. Using this coating material to modify the surface of sodium oxide-containing or lithium oxide-containing positive electrode materials can reduce interfacial side reactions while maintaining the positive electrode material's capacity.

[0075] In some embodiments, when the core material is a sodium-containing oxide, the phosphate can be selected from at least one of Na2FeP2O7, Na3Fe2(PO4)P2O7, Na3V2Fe(PO4)3, Na3VMn2Fe(PO4)3, Na3VTiFe(PO4)3, Na3Fe2Fe(PO4)3, and Na3MnTiFe(PO4)3. The above phosphates have a large number of PO bonds and strong bond energy, which can make the phosphate coating more stable. Moreover, the coating layer material is a sodium storage material containing sodium ions. Modifying the surface of the sodium-containing cathode material is beneficial to reducing interfacial side reactions while not sacrificing the capacity of the cathode material.

[0076] In some embodiments, the average particle size of the coating material is 40 nm to 90 nm, and further 50 to 70 nm. For example, the average particle size of the coating material can be 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, or any two values ​​therebetween. Controlling the particle size of the phosphate facilitates forming a uniformly thick and evenly coated coating on the surface of the core material, thereby fully isolating the core material from the electrolyte.

[0077] In some embodiments, the mass ratio of the coating layer material to the positive electrode material is 1% to 40%, and further 5% to 20%. Exemplarily, the mass ratio of the coating layer material to the positive electrode material is 1%, 5%, 10%, 20%, 30% or 40%, etc. When the content of the coating layer material is too much, the thickness of the coating layer is too thick, which affects ion transmission. At the same time, it also reduces the proportion of the core material, reducing the capacity of the positive electrode material; when the content of the coating material is too little, a uniform and effective coating layer cannot be formed, and the effect of reducing the interface side reaction is not obvious. Therefore, the embodiment of the present application controls the content of the coating layer material in the positive electrode material within the above range. On the one hand, a positive electrode material with excellent surface morphology can be obtained after coating. The coating layer has a moderate thickness, which is conducive to reducing the interface side reaction while having a positive effect on the capacity and ion transmission of the positive electrode material.

[0078] In certain embodiments, the coating material is coated on the surface of the core material by solid phase grinding and microwave treatment after the core material is formed. The coating of the coating material on the surface of the core material can be made more uniform through solid phase grinding. Microwave treatment can also form chemical bonds (such as ionic bonds, covalent bonds, etc.) between the metal elements (such as manganese) in the core material and the oxygen elements in the coating material, such as Mn-O, thereby making the coating material and the core material have, in addition to hydrogen bonds and intermolecular forces, the above chemical bonds. The coating material has a stronger bonding force on the surface of the core material and is not easy to fall off into the electrolyte.

[0079] By creating a gradient distribution of active metal element concentrations within the core material, doping the core material with magnesium and calcium, and coating the core material with a phosphate coating, the positive electrode material achieves high structural stability, resulting in excellent cycling stability and a long cycle life. This reduces the dissolution of metal elements from the positive electrode material and increases the voltage of the positive electrode material. Batteries using this positive electrode material experience a cycle life increase of over 30% in high-temperature environments, effectively suppressing the dissolution of transition metal elements.

[0080] The following is an example of a nickel-iron-manganese ternary positive electrode material required for sodium ion batteries to specifically introduce a method for preparing the positive electrode material. The method comprises the following steps:

[0081] In the first step, nickel source, iron source and manganese source are co-precipitated to prepare a precursor with a concentration gradient.

[0082] The nickel source is nickel sulfate, the iron source is ferrous sulfate or hydrated ferrous sulfate, and the manganese source is manganese sulfate or hydrated manganese sulfate. The molar ratio of the nickel source, iron source, and manganese source is 1:1:1. Ni, Fe, and Mn have a concentration gradient from the surface of the material to the core of the grain.

[0083] In the second step, the precursor obtained in the first step is dried, and then a sodium source and a doping element are added, ball-milled and mixed evenly, and then solid-phase sintered into single crystal particles to obtain the core material.

[0084] After the precursor material is dried, the sodium source and the precursor are mixed in a molar ratio of (0.9-1.2):1, and then 1000-10000 ppm of doping elements are added. After ball milling and mixing, solid phase sintering is performed to form single crystal particles. The sodium source is sodium carbonate or hydrated sodium carbonate.

[0085] In the third step, phosphate is used as a coating layer, which is quickly ball-milled with the single crystal core material obtained in the second step and then subjected to microwave treatment to obtain a phosphate-coated single crystal layered oxide positive electrode material.

[0086] The ball milling parameters are: 1000-5000 r / min, ball milling 0.5-2 h, microwave heating parameters: temperature 150-500° C., heating time: 3-10 min.

[0087] Please refer to Figure 1, which is a schematic diagram of a positive electrode material provided in one embodiment of the present application. The positive electrode material 10 includes a core material 1 and a coating material 2 uniformly coated on the surface of the core material. The core material 1 is the aforementioned core material, and the coating material 2 is the aforementioned coating material.

[0088] Please refer to FIG. 2 , which is a schematic diagram of a positive electrode plate provided in an embodiment of the present application. The positive electrode plate 100 includes the positive electrode material as described above.

[0089] The positive electrode sheet 100 of the embodiment of the present application includes a current collector 101 and a positive electrode active material layer 102 disposed on the current collector 101 . The positive electrode active material layer 102 includes the aforementioned positive electrode material.

[0090] Please refer to Figure 3, which is a schematic diagram of a battery provided in one embodiment of the present application. The battery 200 includes a positive electrode sheet 100, a negative electrode sheet 201, a separator 202, and an electrolyte 203. The separator 202 is disposed between the positive electrode sheet 100 and the negative electrode sheet 201. The battery 200 can be a sodium-ion battery, and its form is not limited to cylindrical, pouch, or prismatic.

[0091] Based on the same technical concept, an embodiment of the present application also provides a battery pack comprising a plurality of the aforementioned batteries, wherein the plurality of batteries in the battery pack can be connected in series or in parallel.

[0092] Referring to FIG4 , the battery pack 300 includes a plurality of the aforementioned batteries 200 , with any two batteries 200 connected in series or in parallel. The battery pack 300 can be used in an energy storage system, which also includes a power converter. The power converter is electrically connected to the battery pack and is used to convert the voltage output by the battery pack into power and output it to the grid or load, and / or to convert the voltage output by an external power source into power and output it to the battery pack. The energy storage battery pack can be used in UPS backup power, site energy storage, smart photovoltaics, data center batteries, and power batteries, among other fields.

[0093] The use of the above-mentioned positive electrode materials is beneficial to improving the overall cycle stability, cycle life and voltage of the battery, while also improving the safety of the battery.

[0094] Based on the same technical concept, an embodiment of the present application further provides an electronic device comprising a housing and the aforementioned battery installed within the housing. The electronic device may be, for example, a consumer electronic product such as a mobile phone, tablet computer, power bank, portable computer, notebook computer, and other wearable or portable electronic devices, or may be a vehicle, energy storage device, base station, or other device, but is not limited thereto.

[0095] Please refer to FIG. 5 , which shows an electronic device 400 according to an embodiment of the present application. The electronic device 400 includes a housing 401 and the aforementioned battery 200 ( 300 ) installed in the housing 401 .

[0096] In this embodiment, the electronic device 400 may be a mobile phone. Using the aforementioned battery 200 can effectively increase the standby time and service life of this type of consumer electronic device 400 while improving its safety.

[0097] In other embodiments, the electronic device 400 may be an electric vehicle. Using the aforementioned battery 300 can effectively improve the range and service life of the electronic device 300 such as an electric vehicle, while also improving its safety.

[0098] The technical solutions of the embodiments of the present application are further described below through specific examples.

[0099] Example 1

[0100] Cathode material 1: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 doping elements are Ga and Zn, the coating layer material is Na3Fe2(PO4)P2O7, and the average particle size of the coating layer material is 50 nm.

[0101] As shown in FIG6 , in Example 1, Ni, Fe, and Mn have a concentration gradient from the surface to the core of the core material.

[0102] Example 2

[0103] Cathode material 2: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, doping elements are: Ti, Zn, coating layer material is: Na3V2Fe(PO4)3, and the average particle size of the coating layer material is: 40nm.

[0104] Example 3

[0105] Cathode material 3: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, doping elements are: Ga, Mg, Zn, coating material is: Na2FeP2O7, and the average particle size of the coating material is: 80nm.

[0106] Comparative Example 1

[0107] Cathode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, and no doping elements or coating materials.

[0108] Comparative Example 2

[0109] Cathode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, doping elements are: Ga, Mg, Zn, and there is no coating layer material.

[0110] Comparative Example 3

[0111] Cathode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, no doping elements, the coating material is Na3Fe2(PO4)P2O7, and the average particle size of the coating layer material is 50nm.

[0112] Preparation of half-cell:

[0113] The positive electrode material (active material) prepared in Example 1, carbon black (Super-P, conductive agent) and a binder (polyvinylidene fluoride and 1-methyl-2-pyrrolidone gel in a mass ratio of 1:9) were mixed, and then N-methylpyrrolidone was added and ball-milled to obtain a mixed slurry.

[0114] The mixed slurry is evenly coated on the carbon-coated aluminum foil using an automatic coating machine, the coated aluminum foil is placed in a blast drying oven for drying, and then transferred to a vacuum drying oven for vacuum drying and then taken out to obtain a positive electrode sheet.

[0115] The positive electrode sheet was rolled on a roller press and cut into 12mm diameter sheets for later use. The prepared positive electrode sheets were transferred to a glove box to prepare a half-cell. First, the positive electrode sheet was placed into a CR2025 button-type positive electrode casing, covered with a pre-cut Celgard separator, and a 2mm thick lithium sheet was added. Four to six drops of electrolyte were added, along with FEC as an additive. Finally, the negative electrode casing was attached and compacted to complete the half-cell.

[0116] The method for preparing half-cells using the positive electrode materials of Examples 2 to 3 and Comparative Examples 1 to 3 is the same as the above method and will not be described in detail here.

[0117] The obtained half-cell was subjected to cycle performance and metal element dissolution tests.

[0118] The cycle performance test conditions are: test temperature 25 ° C, current density 10 mA g -1 , the voltage range is 2 to 4 V. The test results are shown in FIG7A and FIG7B . The sodium ion battery positive electrode material prepared in Example 1 has better cycle stability and higher median voltage than that prepared in Comparative Example 1.

[0119] The metal element dissolution test conditions were as follows: scrape the disassembled negative electrode material, digest it with aqua regia, and then use an ICP instrument to test the metal element content. The test results are shown in Table 1.

[0120] Table 1

[0121] As can be seen from Table 1, the dissolution of metal elements in the positive electrode materials of Examples 1 to 3 of the present application is significantly reduced compared to that of Comparative Examples 1 to 3.

[0122] The positive electrode materials of Example 1 and Comparative Example 1 were subjected to scanning electron microscopy (SEM) testing, wherein FIG8 is an SEM image of the positive electrode material of Comparative Example 1, and FIG9 is an SEM image of the positive electrode material of Example 1; as can be seen from FIG8 and FIG9 , the surface of the positive electrode material of Example 1 is uniformly coated with phosphate.

[0123] It should be noted that the above are only specific embodiments of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any person skilled in the art within the technical scope disclosed in the present application should be included in the scope of protection of the present application; the embodiments of the present application and the features of the embodiments can be combined with each other unless there is a conflict. Therefore, the scope of protection of the present application shall be based on the scope of protection of the claims.

Claims

1. A battery, It is characterized in that It includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet includes a current collector and a positive electrode active material layer arranged on the current collector, and the positive electrode active material layer includes a positive electrode material; The positive electrode material comprises a core material and a coating layer material coated on the surface of the core material, the core material is a metal oxide, the coating layer material is a phosphate, and the core material is doped with a first inactive metal element; The core material contains an active metal element and a second inactive metal element, wherein the concentration of the active metal element gradually increases from the surface of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface of the core material to the core of the core material.

2. The battery according to claim 1, It is characterized in that The active metal element is selected from at least one of iron, cobalt, nickel, vanadium, copper and chromium; The second inactive metal element is selected from at least one of manganese and niobium.

3. The battery according to claim 1 or 2, It is characterized in that In the core material, a molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:

4.

4. The battery according to any one of claims 1 to 3, It is characterized in that The first inactive metal element is selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + At least one of; When the core material is a sodium-containing oxide, the first inactive metal element is not Na + ; When the core material is a lithium-containing oxide, the first inactive metal element is not Li + .

5. The battery according to any one of claims 1 to 4, It is characterized in that The doping concentration of the first inactive metal element gradually decreases from the surface layer of the core material to the core of the core material.

6. The battery according to any one of claims 1 to 5, It is characterized in that The molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04).

7. The battery according to any one of claims 1 to 6, It is characterized in that The phosphate contains at least two phosphate groups and / or at least one pyrophosphate group.

8. The battery according to claim 7, It is characterized in that The molecular formula of the phosphate is: x R y (PO 4 ) a (P 2 O 7 ) b , wherein A is a sodium ion or a lithium ion; R is selected from at least one of iron, vanadium, titanium, manganese and cobalt; The values ​​of x, y, a and b can satisfy that the algebraic sum of positive and negative valences in the molecular formula of the phosphate is zero.

9. The battery according to claim 8, It is characterized in that The core material is a sodium-containing oxide, and the phosphate is selected from Na 2 FeP 2 O 7 、Na 3 Fe 2 (PO 4 ) 2 O 7 、Na 3 V 2 Fe(PO 4 ) 3 、Na 3 V N 2 Fe(PO 4 ) 3 、Na 3 VTiFe(PO 4 ) 3 、Na 3 Fe 2 Fe(PO 4 ) 3 and Na 3 MnTiFe(PO 4 ) 3 At least one of .

10. The battery according to any one of claims 1 to 9, It is characterized in that The average particle size of the coating layer material is 40nm to 90nm.

11. The battery according to any one of claims 1 to 10, It is characterized in that The mass ratio of the coating layer material to the positive electrode material is 1% to 40%.

12. A battery pack, It is characterized in that The method comprises a plurality of batteries according to any one of claims 1 to 11, wherein the plurality of batteries are connected in series or in parallel.

13. An electronic device, It is characterized in that The invention comprises a housing and a battery according to any one of claims 1 to 11 located in the housing.

14. An energy storage system, It is characterized in that It comprises a battery pack and a power converter as described in claim 12, wherein the power converter is used to perform power conversion on the voltage output by the battery pack, and / or the power converter is used to perform power conversion on the voltage output by an external power source and output it to the battery pack.

Citation Information

Patent Citations

  • Anode active material, preparation method thereof and battery

    CN103050694A

  • Cathode active material for secondary battery, preparation method therefor, and secondary battery comprising same

    CN107408667A

  • Cathode active material for secondary battery, and secondary battery comprising same

    CN107636866A

  • Modified ultralow-temperature lithium iron phosphate composite material, positive electrode material and preparation method thereof

    CN113097456A

  • Positive electrode active material and lithium ion battery comprising same

    CN115036460A