Micron-sized monodisperse lithium-rich manganese-based positive electrode material having twin boundary, and preparation therefor

The micron-scale monodispersed lithium-rich manganese-based positive electrode material rich in twin boundaries is constructed through high-temperature ion exchange method, which solves the problems of poor capacity attenuation, voltage attenuation and rate performance of existing materials, and achieves high rate performance and long cycle stability micron-level lithium-rich cathode material.

WO2024244545A1PCT designated stage expired Publication Date: 2024-12-05PEKING UNIV

Patent Information

Application Number
PCT/CN2024/077713
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-02-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing lithium-rich manganese-based positive electrode materials have problems of poor capacity attenuation, voltage attenuation and rate performance, and the synthesis of micron-level monodispersed lithium-rich materials is difficult, which leads to difficulties in commercial applications.

Method used

The high-temperature ion exchange method is used to construct a layered micron-scale monodispersed lithium-rich manganese-based positive electrode material with rich twin boundaries. The Li[LixMnyNizCo1-x-y-z]O2 structure is prepared through liquid phase co-precipitation and high-temperature sintering steps to realize the Li layer and transition metal The alternating arrangement of layers forms a twin interface in which the local oxygen atom stacking method is ABCACB.

Benefits of technology

The lithium ion migration speed is significantly improved, the phase transition is suppressed, the rate performance and cycle stability of the cathode material are improved, and the micron-level lithium-rich cathode material with high energy density and long cycle life is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024077713_05122024_PF_FP_ABST
    Figure CN2024077713_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A micron-sized monodisperse lithium-rich manganese-based positive electrode material having rich twin boundaries, the chemical formula thereof being Li[LixMnyNizCo1-x-y-z]O2, wherein Li layers and transition metal layers are alternately arranged, 0.1<x≤0.25, 0.45≤y≤0.6, and 0≤z≤0.15. Different from oxygen atoms of a common lithium-rich positive electrode material in a face-centered cubic packing mode ABCABC, according to the present invention, a lithium-rich manganese-based positive electrode material with some oxygen atoms in a face-centered cubic packing mode ABCACB is constructed by means of a unique high-temperature ion exchange mode. The positive electrode material has advantages of good primary particle dispersity, uniform particles, and improvement of the rate capability of the material by introducing rich twin boundaries. Moreover, micron-sized boundary-free particles effectively reduce the specific surface area, attenuate surface side reaction, inhibit anisotropic volume change, mitigate particle crushing, and improve cycle performance. In addition, according to the present invention, the synthesis method for the lithium-rich manganese-based positive electrode material is simple and easy to implement, and facilitates industrial mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Micron-scale monodispersed lithium-rich manganese-based cathode materials with twin boundaries and their preparation Technical Field

[0001] The present invention belongs to the field of lithium-ion battery materials and electrochemistry, and relates to a micron-sized monodispersed lithium-rich manganese-based positive electrode material with abundant twin boundaries, a preparation method thereof, and a battery. Background Art

[0002] Since their commercialization in 1991, lithium-ion batteries have been used in a wide range of fields, including consumer electronics, electric vehicles, and artificial intelligence. The rapid development of society, particularly the increasing popularity of new energy vehicles and the rapid development of large-scale energy storage grids, has placed higher demands on the energy density and safety of battery systems. The energy density and cost of lithium-ion batteries are primarily limited by the cathode material. Therefore, improving the performance of cathode materials is currently a key focus of lithium battery research.

[0003] The specific capacities of lithium cobalt oxide, lithium iron phosphate, and lithium manganese oxide cathodes are all below 200 mAh / g. Traditional layered cathode materials based on transition metal ion redox reactions have low specific capacities and high costs, hindering the development of lightweight and long-range electric vehicles.

[0004] Developing high-energy-density, low-cost cathode materials is a key area of ​​lithium battery research. Lithium-rich manganese-based cathode materials possess multiple redox centers. In addition to cation valence changes, lattice oxygen also participates in charge compensation, being oxidized during charging and partially reduced during discharge. This results in a specific capacity exceeding 300 mAh / g, a high operating voltage of 3.5V, and a relatively high energy density. However, lithium-rich materials face challenges such as capacity fading, voltage decay, and poor rate performance, which severely hinder their commercialization. Suppressing surface oxygen release and surface structural degradation while leveraging the reversibility of bulk oxygen is key to achieving the stability of lithium-rich manganese-based cathode materials. Researchers have conducted extensive research to stabilize the surface, inhibit oxygen release, and surface reconstruction. However, obtaining a high-quality coating on polycrystalline lithium-rich materials is currently difficult. The oxygen release and voltage decay issues have only been partially addressed. Furthermore, phase transitions and cracking remain unavoidable after long cycles.

[0005] Compared with secondary spherical particles, micron-scale monodisperse lithium-rich cathode materials have the following advantages: (1) They have a smaller specific surface area, which inhibits surface oxygen release; (2) They reduce the contact area with the electrolyte and reduce side reactions; (3) They eliminate the influence of grain boundaries, avoid large stress at the grain boundaries, eliminate intergranular cracking, and improve cycle stability; (4) Monodisperse materials have high mechanical strength and do not produce anisotropic stress changes during compaction, so they are not easy to break, which can increase the compaction density and meet industrial needs; (5) Materials with specific orientations can be synthesized and are easy to surface modify.

[0006] Currently, there are few reports on micron-scale monodisperse lithium-rich materials. It can be said that truly monodisperse micron-scale lithium-rich materials have yet to be synthesized. Because of their monodispersity, grain-boundary-free morphologies are difficult to synthesize. Even in the more mature ternary and high-nickel systems, their micron-scale primary particles often have grain boundaries. Their electrochemical performance lacks significant advantages over current polycrystalline materials, and their poor rate performance hinders the further development of micron-scale lithium-rich materials. Currently, there are no reports of micron-scale lithium-rich cathode materials with high-rate performance. Summary of the Invention

[0007] The present invention addresses the shortcomings of the existing technology and provides a method for preparing a micron-sized, monodisperse, lithium-rich manganese-based cathode material, thereby obtaining a micron-sized, monodisperse cathode material with abundant twin boundaries and a corresponding lithium-ion battery. On the one hand, lithium ion migration near the twin boundaries is faster, resolving the problem of slow lithium ion diffusion in micron-sized cathode materials. On the other hand, transition metal migration near the twin boundaries is suppressed, effectively inhibiting phase transitions and improving cycle stability. This invention, for the first time, achieves both high-rate performance and long-cycle stability for lithium-rich manganese-based cathode materials on micron-sized particles.

[0008] The present invention adopts the following technical solutions:

[0009] A layered micron-scale monodispersed lithium-rich manganese-based cathode material with abundant twin boundaries, the chemical formula of which is Li[Li x Mn y Ni z Co 1-x-y-z ]O2, Li layer and transition metal layer [Li x Mn y Ni z Co 1-x-y-z ] are arranged alternately, where 0.1 <x≤0.25,0.45≤y≤0.6,0≤z≤0.15。

[0010] The structure of the layered micron-scale monodispersed lithium-rich manganese-based positive electrode material belongs to Space group or C2 / m space group or both, where the Li layer and transition metal layer [Li x Mn y Ni z Co 1-x-y-z ] are arranged alternately.

[0011] Different from the conventional lithium-rich positive electrode material in which oxygen atoms are stacked in a face-centered cubic manner (ABCABC), the present invention constructs a lithium-rich manganese-based positive electrode material with abundant twin boundaries through a unique high-temperature ion exchange method. The local oxygen atom stacking manner is ABCACB, producing abundant twin interfaces.

[0012] The preparation method of the layered micron-sized lithium-rich manganese-based positive electrode material with abundant twin boundaries of the present invention comprises the following steps:

[0013] 1) Preparation of nickel-cobalt-manganese hydroxide precursor material by liquid phase coprecipitation method;

[0014] 2) The precursor material prepared in step 1) is fully ground and mixed with lithium source and sodium source, and sintered at high temperature to obtain sodium salt intermediate Na a [Li x Mn y Ni z Co 1-x-y-z ]O2, of which 0.1 <x≤0.25,0.45≤y≤0.6,0≤z≤0.15,0.6≤a≤1;

[0015] 3) The sodium salt intermediate prepared in step 2) is mixed with a lithium source, sintered at a high temperature, and then washed, filtered, and dried to obtain the target product.

[0016] Specifically, the above step 1) is based on the transition metal layer [Li x Mn y Ni z Co 1-x-y-z ] One or more compounds containing nickel, cobalt and manganese elements are prepared into a solution of a certain concentration in the stoichiometric ratio shown in FIG. ], and a certain amount of surfactant used as a dispersant is dissolved therein, which is recorded as solution A; a precipitant and a complexing agent are prepared into a mixed solution, which is recorded as solution B, and then it is dropped into a co-precipitation reactor at the same time as solution A to react to obtain a precursor material.

[0017] Among them, the precipitant is preferably one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and sodium oxalate; the complexing agent is preferably one or more of ammonia water, ethylenediamine, ammonium bicarbonate, and ammonium pyrophosphate; and the selected surfactant is preferably one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl lactam, polystyrene sulfonate, and sodium polyacrylate.

[0018] The compound containing nickel, cobalt, and manganese elements can be selected from one or more of their sulfates, acetates, and nitrates, and is prepared into a salt solution with a total transition metal concentration of 1 to 5 mol / L, and the amount of surfactant used is 0.02 to 2 wt % to obtain solution A.

[0019] The concentration of the precipitant is 2~10 mol / L, and the concentration of ammonia water as the complexing agent is 0.1~3 mol / L.

[0020] Preferably, step 1) solution A and solution B are simultaneously added dropwise to the reactor using a peristaltic pump. During the reaction, the flow rate of solution A is controlled at 0.8-1 mL / min and is uniformly added dropwise to the reactor containing deionized water as the base liquid. Solution B is injected into the reactor through the pH self-feedback control system by frequency conversion. The pH of the reaction system is controlled to be stable at a certain value, the temperature is controlled between 50-55°C, the stirring speed is controlled at 900-1100 r / min, the reaction time is 4-8 h, and an inert gas (such as argon) is passed throughout the process for protection; after the addition is completed, the mixture is aged at 50-55°C and stirred at 600-700 r / min for 8-16 h, the precipitate is filtered and washed 4-8 times, and dried in a vacuum oven for 12-24 h.

[0021] In step 2) above, a micron-sized sodium salt intermediate is obtained, achieving a micron-sized morphology. The sodium salt intermediate includes one or more of the P2, P3, and O3 configurations. In step 3) above, the sodium salt intermediate with the micron-sized morphology is mixed with a lithium source and sintered at high temperature to simultaneously achieve morphology inheritance, lithium-sodium exchange, and the formation of twin boundary stacking faults, thereby preparing a micron-sized, monodisperse, lithium-rich cathode material with abundant twin boundaries.

[0022] Step 2) According to the chemical formula Na a [Li x Mn y Ni z Co 1-x-y-z ]O2 shows a stoichiometric ratio or lithium and sodium have an excess of 1% to 10%. The precursor material is fully ground and mixed with a lithium source and a sodium source, and sintered at a high temperature to obtain a micron-sized sodium salt intermediate. The compound used as the sodium source is selected from one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium acetate, sodium nitrate, sodium oxalate, and sodium oxide. The compound used as the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, lithium acetate, lithium oxalate, lithium nitrate, lithium oxide, and lithium peroxide. During the sintering process, lithium and sodium are preferably in excess of 1% to 10%. Preferably, pre-calcination is performed at 200 to 600°C for 2 to 6 hours, and then the temperature is raised to 600 to 850°C and calcined for 10 to 20 hours.

[0023] The compound used as the lithium source in step 3) is selected from one or more of lithium chloride, lithium hydroxide, lithium carbonate, lithium acetate, lithium oxalate, lithium nitrate, lithium oxide, and lithium peroxide. In laboratory studies, lithium nitrate and lithium chloride are preferred lithium sources, but in industrial large-scale production, other lithium sources besides lithium nitrate and lithium chloride can be used. Preferably, the sodium salt intermediate Na a [Li x Mn y Ni z Co 1-x-y-z]O2 is subjected to an ion exchange reaction with 5-10 times the molar amount of a lithium source at 600-750°C for 6-12 hours. The resulting product is washed, filtered, and dried to obtain a micron-sized, monodisperse, lithium-rich manganese-based cathode material with abundant twin boundaries. In some embodiments of the present invention, the ion exchange reaction product is washed with water and ethanol, filtered, and dried at 100-300°C to obtain the micron-sized, monodisperse, lithium-rich manganese-based cathode material.

[0024] In some embodiments of the present invention, after the precursor material is uniformly mixed with the lithium source and the sodium source, the temperature is raised to 200-600°C at a heating rate of 2-10°C / min in a tube furnace under air atmosphere, and pre-sintered at 200-600°C for 2-6 hours. Then, the temperature is raised to 600-850°C at a heating rate of 1-10°C / min, and the sintering temperature is controlled at 600-850°C for 10-20 hours. The temperature is then lowered to 300°C at a rate of 1-5°C / min, and then naturally cooled to room temperature to obtain a sodium salt intermediate. Then, after the sodium salt intermediate is uniformly mixed with the lithium source, the temperature is raised to 600-750°C at a heating rate of 2-10°C / min, and the sintering temperature is controlled at 600-750°C for 6-12 hours. After washing, filtration, and drying, the target positive electrode material is obtained.

[0025] The lithium-rich manganese-based positive electrode material prepared by the present invention has uniform particle size, primary particle size at the micron level, good dispersibility, and abundant twin boundaries.

[0026] The lithium-rich manganese-based positive electrode material of the present invention can be used to prepare a positive electrode plate, which can be used together with a negative electrode plate, a separator, an electrolyte, etc. to form a lithium-ion battery.

[0027] This invention proposes a method for synthesizing micron-sized, monodisperse lithium-rich manganese-based cathode materials. Unlike conventional lithium-rich cathode materials with a face-centered cubic (ABCABC) stacking pattern of oxygen atoms, this method utilizes a unique high-temperature ion exchange process to construct a localized oxygen stacking pattern of ABCACB. By introducing abundant twin boundaries into the micron-sized particles, the energy barrier for lithium ion migration is significantly reduced, thereby improving rate performance. This method effectively addresses the problem of large particle size leading to low specific capacity and poor rate performance in lithium-rich manganese-based cathode materials. The primary particles of the cathode material prepared by this invention exhibit excellent dispersibility and uniformity (monodisperse particles of approximately 1-2 microns), achieving for the first time the exceptional rate performance of large-particle cathode materials. The introduction of twin boundaries into lithium-rich manganese-based cathode materials demonstrates significant potential for improving performance by utilizing surface defects. Furthermore, the micron-sized, boundary-free particles effectively reduce specific surface area, mitigate surface side reactions, inhibit anisotropic volume changes, slow particle breakage, and improve cycle performance. Furthermore, the synthesis method of this invention is simple and easy to implement, making it suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1. SEM electron microscope image of the lithium-rich manganese-based positive electrode material prepared in Example 1 of the present invention.

[0029] Figure 2. XRD pattern of the lithium-rich manganese-based positive electrode material prepared in Example 1 of the present invention.

[0030] Figure 3. Spherical aberration electron microscopy images of the lithium-rich manganese-based cathode material prepared in Example 1 of the present invention, including the high-angle annular dark-field phase (a) and the annular bright-field phase (b), and a schematic diagram of the atomic arrangement near the twin boundary (c).

[0031] Figure 4. Spherical aberration electron microscopy image of the lithium-rich manganese-based cathode material prepared in Example 1 of the present invention, high-angle annular dark field phase (a), and its inverse Fourier transform spectrum (b) and Fourier transform spectrum (c).

[0032] Figure 5. Performance diagram of the lithium-rich manganese-based cathode material prepared in Example 1 of the present invention, where a is the 0.1C charge-discharge curve and b is the rate performance diagram.

[0033] Figure 6. Lithium-rich manganese-based cathode material prepared in Example 1 of the present invention in the voltage range of 2.1-4.6 V and the current density of 200 mA g -1 Cycle performance diagram of 200 cycles. DETAILED DESCRIPTION

[0034] The present invention will be further supplemented below with reference to the accompanying drawings through embodiments, but the scope of the present invention is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the scope of protection of the present invention.

[0035] Example 1: Hydroxide co-precipitation + solid phase method (P2 type intermediate) + molten salt exchange method to synthesize micron-scale monodispersed lithium-rich manganese-based cathode material Li with O3 configuration and twin boundaries 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.

[0036] Step 1: Dissolve appropriate amounts of nickel sulfate, cobalt sulfate, and manganese sulfate in 0.5 L of deionized water at a ratio of 1:1:4, with a total ion concentration of 2 mol / L. Dissolve 1 g of polyvinylpyrrolidone in the solution to obtain Solution A. Sodium hydroxide was used as the precipitant, and ammonia was used as the complexing agent. A mixed alkali solution (0.5 L) with a concentration of 4 mol / L sodium hydroxide and 1 mol / L ammonia was prepared. Prior to the reaction, 750 mL of deionized water was added to a 3 L reactor as the base solution, and a small amount of ammonia was added to adjust the pH to approximately 10.0. The reactor was then sealed and purged with argon for half an hour to expel all air. Solution A was then pumped into the reactor at a constant rate, while the mixed alkali solution was pumped into the reactor using a pH self-feedback control system. The reactor temperature was maintained at 55°C. The reaction pH was maintained at 10.0, and stirring was performed at 1000 rpm to synthesize the hydroxide precursor. The precursor material synthesized by the liquid phase method was repeatedly filtered and washed five times with deionized water, dried in a vacuum oven at 100°C for 12 h, and the target precursor was obtained after being taken out and stored in a glove box.

[0037] Step 2: Sodium carbonate, lithium carbonate, and the precursor obtained in Step 1 above were weighed separately at a Na:Li:M ratio of 5:1:4 (M represents the transition metal elements Ni, Co, and Mn), thoroughly ground, and mixed and sintered. The sintering process involved heating to 450°C at a rate of 5°C / min for 4 h, then heating to 850°C at a rate of 5°C / min for 10 h, then cooling to 300°C at a rate of 2°C / min, and then cooling to room temperature in the furnace to obtain a P2 intermediate.

[0038] Step 3: Lithium chloride and the P2 intermediate obtained in Step 2 were weighed in a molar ratio of 5:1 and mixed and sintered. The sintering process was to increase the temperature to 650°C at a rate of 5°C / min and sinter for 6 hours, followed by furnace cooling to room temperature. After the lithium chloride exchange, the cooled molten salt became agglomerated and adhered to the porcelain boat. The lithium salt needed to be dissolved with water and then rinsed off gradually. Finally, the mixture was repeatedly washed and filtered three times with deionized water. The mixture was then dried in a forced air oven at 100°C for 12 hours to obtain the target cathode material.

[0039] Step 4: Mix the target cathode material with carbon black and PVDF in a mass ratio of 8:1:1, using N-methylpyrrolidone as the solvent. The mixture is then coated onto aluminum foil and dried in a forced-air oven at 100°C for 2 hours. After removal, the foil is rolled on a roller press and cut into electrode discs with a diameter of 14 mm. This serves as the positive electrode, the lithium sheet as the negative electrode, and Celgard 2400 as the separator. The electrolyte is a high-voltage electrolyte from Dongguan Shanshan. CR2032 coin cells are assembled in a glove box and tested on a Newway battery test system at 30°C.

[0040] The synthesized positive electrode material has good dispersibility and is monodisperse, with a particle size of 1-2 μm, as shown in Figure 1.

[0041] The synthesized cathode material has the standard X-ray diffraction pattern of lithium-rich manganese-based cathode materials, as shown in Figure 2, and the space group is , there is a weak superlattice peak at 20~25°, indicating that the transition metal layer Li and transition metal ions are arranged in an orderly manner.

[0042] In the synthesized positive electrode material, the local oxygen atom stacking pattern is ABCACB, as shown in Figure 3.

[0043] Through Fourier transform and inverse Fourier transform, it can be observed that the synthesized positive electrode material has abundant twin boundaries, as shown in Figure 4.

[0044] The synthesized cathode material exhibits excellent electrochemical cycling stability and rate performance: at 20 mA g -1 At a current density of 1.5 volts, it is gradually activated in the voltage ranges of 2.0-4.5 V, 2.0-4.6 V, and 2.0-4.8 V. The discharge capacity in the voltage range of 2.0-4.8 V is 300 mAh g -1 , see Figure 5a; at 200 mA g -1 , 400 mA g -1 , 1000 mA g -1 At the current density, the discharge specific capacity is 253, 230, and 186 mAh g, respectively. -1 , showing excellent electrochemical performance, as shown in Figure 5b. At 200 mA g -1 At the charge and discharge current density, 240 mAh g -1 The discharge specific capacity of the battery can be maintained at over 85% after 200 cycles, showing good cycle performance, as shown in Figure 6.

[0045] Example 2: Hydroxide co-precipitation + solid phase method (P2 type intermediate) + solid phase method synthesis of micron-scale monodisperse lithium-rich manganese-based positive electrode material Li with O3 configuration and twin boundaries 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.

[0046] The difference from step 3 in Example 1 is that the lithium source used in the reaction is changed to lithium hydroxide, and the remaining steps are the same. The specific steps are: lithium hydroxide and the P2-type intermediate obtained in step 2 are weighed in a molar ratio of 1.02:1 and mixed and sintered. The sintering process is to heat the temperature to 650°C at a heating rate of 5°C / min and sinter for 6 hours, and then cool to room temperature with the furnace. Finally, it is repeatedly washed and filtered three times with deionized water, and dried in a 100°C forced air oven for 12 hours to obtain the target positive electrode material. Lithium hydroxide is used as the lithium source, and it is still in powder form after the reaction. It can be poured directly from the porcelain boat, which simplifies the water washing process and has greater industrial application value.

Claims

1. A micron-scale monodisperse lithium-rich manganese-based cathode material, which has a layered structure, a local oxygen atom stacking pattern of ABCACB, and abundant twin interfaces; its chemical formula is Li[Li x Mn y Ni z Co 1-x-y-z ]O2, where the Li layer and transition metal layer [Li x Mn y Ni z Co 1-x-y-z ] Alternate arrangement, 0.1 <x≤0.25,0.45≤y≤0.6,0≤z≤0.15。 2. The micron-sized monodispersed lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The structure of the lithium-rich manganese-based positive electrode material belongs to The space group is either C2 / m or a combination of both.

3. The method for preparing the micron-sized monodispersed lithium-rich manganese-based positive electrode material according to claim 1 or 2 comprises the following steps: 1) Preparation of nickel-cobalt-manganese hydroxide precursor material by liquid phase co-precipitation method; 2) The precursor material prepared in step 1) is fully ground and mixed with the lithium source and the sodium source, and sintered at high temperature to obtain the sodium salt intermediate Na a [Li x Mn y Ni z Co 1-x-y-z ]O2, of which 0.1 <x≤0.25,0.45≤y≤0.6,0≤z≤0.15,0.6≤a≤1; 3) The sodium salt intermediate prepared in step 2) is mixed with a lithium source, sintered at a high temperature, and then washed, filtered, and dried to obtain a micron-sized monodispersed lithium-rich manganese-based positive electrode material.

4. The preparation method according to claim 3, characterized in that: Step 1) Press the transition metal layer [Li x Mn y Ni z Co 1-x-y-z ] A compound containing nickel, cobalt and manganese elements is prepared into a solution in the stoichiometric ratio shown in FIG. 1 , and a surfactant used as a dispersant is dissolved therein, which is recorded as solution A; a precipitant and a complexing agent are prepared into a mixed solution, which is recorded as solution B, and then it is dripped into a co-precipitation reactor together with solution A to react to obtain a precursor material.

5. The preparation method according to claim 4, characterized in that: The compound containing nickel, cobalt and manganese elements in step 1) is selected from one or more of their sulfates, acetates and nitrates; the precipitant is selected from one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate and sodium oxalate; the complexing agent is selected from one or more of ammonia water, ethylenediamine, ammonium bicarbonate and ammonium pyrophosphate; the selected surfactant is selected from one or more of polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl lactam, polystyrene sulfonate and sodium polyacrylate.

6. The preparation method according to claim 5, characterized in that: In step 1), a compound containing nickel, cobalt and manganese elements is prepared into a salt solution with a total transition metal concentration of 1-5 mol / L, and a surfactant is added in an amount of 0.02-2 wt % to obtain solution A; the concentration of the precipitant in the solution B is 2-10 mol / L, and when ammonia water is used as a complexing agent, its concentration is 0.1-3 mol / L.

7. The preparation method according to claim 4, characterized in that: Step 1) Solution A and Solution B are simultaneously added dropwise to the reactor using a peristaltic pump. During the reaction, the flow rate of Solution A is controlled at 0.8-1 mL / min, and the solution is uniformly added dropwise to the reactor containing deionized water as the base liquid. Solution B is injected into the reactor through a pH self-feedback adjustment system to control the pH of the reaction system to be stable at a certain value, the temperature is controlled between 50-55°C, the stirring speed is controlled at 900-1100 r / min, the reaction time is 4-8 h, and an inert gas is provided throughout the process. After the addition is completed, the solution is aged at 50-55°C and stirred at 600-700 r / min for 8-16 h, the precipitate is filtered and washed 4-8 times, and dried in a vacuum oven for 12-24 h.

8. The preparation method according to claim 3, characterized in that: Step 2) According to the chemical formula Na a [Li x Mn y Ni z Co 1-x-y-z ]O2 as shown in the stoichiometric ratio or lithium and sodium in excess of 1% to 10%. The precursor material is fully ground and mixed with the lithium source and the sodium source, first pre-fired at 200 to 600°C for 2 to 6 hours, and then heated to 600 to 850°C and calcined for 10 to 20 hours to obtain a micron-sized sodium salt intermediate; wherein the compound serving as the sodium source is selected from one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, sodium acetate, sodium nitrate, sodium oxalate, and sodium oxide; the compound serving as the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, lithium acetate, lithium oxalate, lithium nitrate, lithium oxide, and lithium peroxide.

9. The preparation method according to claim 3, characterized in that: Step 3) The sodium salt intermediate is subjected to an ion exchange reaction with 5 to 10 times the molar amount of a lithium source at 600 to 750° C. for 6 to 12 hours, and the obtained product is washed, filtered, and dried to obtain the micron-sized monodispersed lithium-rich manganese-based positive electrode material, wherein the compound serving as the lithium source is selected from one or more of lithium chloride, lithium hydroxide, lithium carbonate, lithium acetate, lithium oxalate, lithium nitrate, lithium oxide, and lithium peroxide.

10. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The positive electrode plate comprises the micron-sized monodispersed lithium-rich manganese-based positive electrode material according to claim 1 or 2.

Citation Information

Patent Citations

  • Synthesis method of low-voltage hysteresis O2 type lithium-rich manganese-based positive electrode material

    CN114695874A

  • Method for regulating and preparing high-nickel layered oxide microcell structure

    CN115215385A

  • Micron-sized monodisperse lithium-rich manganese-based positive electrode material with twin boundaries and preparation thereof

    CN117038953A

Cited By

  • Manganous oxide nanodot / carbon material as well as preparation method and application thereof

    CN119297259A

  • Micro-nano magnesium-doped indium-coated lithium-rich manganese-based positive electrode material and precursor and preparation method thereof

    CN119349666A

  • Lithium-rich manganese positive electrode material as well as surface modification method and application thereof

    CN119797445A

  • Lithium-rich manganese oxide material subjected to surface modification treatment as well as preparation method and application of lithium-rich manganese oxide material

    CN119833605A

  • Preparation method of quintuple twin crystal gold nanoparticles

    CN119973130A