Atomization core, atomizer and electronic atomization device

By using porous glass ceramic matrix and metal heating body, the problem of insufficient strength of the porous matrix of the electronic cigarette atomization core is solved, and a longer service life and better oil conduction effect are achieved, ensuring mechanical stability under high temperature conditions.

WO2024245035A1PCT designated stage expired Publication Date: 2024-12-05SMOORE INTERNATIONAL HOLDINGS LIMITED +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094269
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The porous matrix of existing electronic cigarette atomized cores has poor strength and insufficient thermal shock resistance, resulting in a short service life.

Method used

The porous glass ceramic matrix is ​​used as the porous matrix of the atomized core. By controlling the element content and pore size structure of the matrix, its strength and stability are improved, and combined with the metal heating element, atomized core with high compressive strength and uniform composition is prepared. .

Benefits of technology

It effectively extends the service life of the atomized core, improves the oil conduction effect and taste, and enhances the mechanical stability and reliability under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094269_05122024_PF_FP_ABST
    Figure CN2024094269_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An atomization core, an atomizer and an electronic atomization device. The atomization core comprises a porous matrix and a heating body, wherein the porous matrix is a porous glass ceramic matrix; any two measurement areas on the porous glass ceramic matrix are respectively denoted as a first measurement area and a second measurement area; in terms of atomic percentages, the content of a main element in the first measurement area is denoted as M at%, and the content of the corresponding main element in the second measurement area is denoted as N at%, with |M-N| / M being less than 10% and / or |M-N| / N being less than 10%; the length of the measurement areas is at least greater than 1 μm; and the main element is an element with an element content of more than 20 at% in the porous glass ceramic matrix. The strength of the porous matrix can be effectively improved, the stability of the matrix is better, and the service life thereof is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Atomizing core, atomizer and electronic atomizing device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to a Chinese patent application filed with the Patent Office of China on June 1, 2023, with application number 202310647629.4 and invention name “A kind of atomizing core, atomizer and electronic atomizing device”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the field of electronic atomization technology, and in particular to an atomization core, an atomizer, and an electronic atomization device. Background Art

[0004] As a promising alternative to traditional cigarettes, e-cigarettes offer the advantage of reducing harmful substances like tar and CO in smoke. Currently, commercially available e-cigarettes primarily utilize resistive heating for atomization, where the e-cigarette liquid is atomized by heat generated by the atomizer core. Existing atomizer cores typically consist of a porous matrix and a heating element. The porous matrix is ​​typically constructed from porous materials such as cotton wicks or porous ceramics to direct the atomized medium toward the heating element.

[0005] However, in the existing technology, ceramic materials are usually prepared using materials such as diatomaceous earth. The composition of traditional ceramic materials such as diatomaceous earth is complex, resulting in poor strength of the porous matrix of the electronic cigarette, poor thermal shock resistance, and easy local detachment and fracture, which in turn affects its service life.

[0006] Summary of the Invention

[0007] The purpose of this application is to overcome the defects of the prior art in that the porous matrix of the atomizer core has poor strength, which affects its service life, and further provide an atomizer core, an atomizer and an electronic atomization device.

[0008] To achieve the above objectives, this application adopts the following technical solutions:

[0009] The present application provides an atomizer core, which includes a porous substrate and a heating element;

[0010] The porous substrate is a porous glass-ceramic substrate, and any two measurement areas on the porous glass-ceramic substrate are respectively recorded as a first measurement area and a second measurement area. In terms of atomic percentage, the main element content in the first measurement area is recorded as Mat% and the corresponding main element content in the second measurement area is recorded as N at%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%;

[0011] The length of the measurement area is at least greater than 1 μm; the main element is an element with an element content greater than 20 at % in the porous glass-ceramic matrix.

[0012] Optionally, in atomic percentage, the main element content in the first measurement area is recorded as Mat%, and the corresponding main element content in the second measurement area is recorded as Nat%, where |MN| / M is less than 5% and / or |MN| / N is less than 5%.

[0013] Optionally, the main elements include a first main element and a second main element; in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64 at %; the content of the second main element is 20-36 at %.

[0014] Optionally, the first main element is oxygen, and the second main element is silicon;

[0015] Optionally, any two measurement areas on the porous glass-ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In terms of atomic percentage, the O element content in the first measurement area is recorded as Mat%, and the corresponding O element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the Si element content in the first measurement area is recorded as M'at%, and the corresponding Si element content in the second measurement area is recorded as N'at%, wherein |M'-N'| / M' is less than 10% and / or |M'-N'| / N' is less than 10%; the length of the measurement area is at least greater than 1 μm.

[0016] Optionally, the elements in the porous glass-ceramic matrix further include at least one element selected from the group consisting of sodium, magnesium, aluminum, and calcium.

[0017] Optionally, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

[0018] Optionally, the length of the measurement area is at least twice the average pore diameter.

[0019] Optionally, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa;

[0020] Optionally, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa.

[0021] Optionally, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase;

[0022] Optionally, the crystalline phase accounts for more than 50 wt%;

[0023] Optionally, the crystalline phase includes a quartz phase.

[0024] Optionally, the measurement area is at least one of circular, elliptical or rectangular.

[0025] Optionally, the heating element is a metal heating film.

[0026] The present application provides an atomizer, which includes the atomizer core described above.

[0027] The present application also provides an electronic atomization device, wherein the atomizer described above in the electronic atomization device further includes a battery assembly.

[0028] Beneficial effects of this application:

[0029] This application uses a porous glass-ceramic substrate as the porous substrate of the atomizer core, and simultaneously controls the main element content between any two measurement areas of the porous glass-ceramic substrate. Any two measurement areas on the porous glass-ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In atomic percentage, the main element content in the first measurement area is recorded as Mat%, and the corresponding main element content in the second measurement area is recorded as Nat%, where |MN| / M is less than 10% and / or |MN| / N is less than 10%. The length of the measurement area is at least greater than 1 μm. The main element is an element with an element content greater than 20 at% in the porous glass-ceramic substrate. The inventors have discovered that by controlling the above conditions, the strength of the porous substrate and the atomizer core can be effectively improved, the stability of the substrate is improved, and its service life is effectively extended. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the following is a brief introduction to the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0031] FIG1 is a physical picture of the atomizer core of Example 1 of the present application;

[0032] FIG2 is a physical picture of the porous substrate of the atomizer core of Example 1 of the present application;

[0033] FIG3 is an SEM image of the porous substrate of the atomizer core of Example 2 of the present application and the selected measurement area in Test Example 1;

[0034] FIG4 is a selected measurement area of ​​the porous substrate of Example 2 in Test Example 1 of this application;

[0035] FIG5 is a schematic structural diagram of the atomizer of the present application;

[0036] FIG6 is a schematic structural diagram of the electronic atomization device of the present application;

[0037] Reference numerals: 1-atomizer, 2-battery assembly. DETAILED DESCRIPTION

[0038] The following examples are provided to further better understand the present application, but are not limited to the best implementation mode described herein, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the scope of protection of the present application.

[0039] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0040] In the prior art, ceramic materials are usually prepared using materials such as diatomaceous earth. Traditional ceramic materials such as diatomaceous earth have complex compositions, and the porous matrix prepared therefrom has poor strength and poor thermal shock resistance, and is prone to detachment and breakage, thereby affecting its service life.

[0041] To this end, the present application provides an atomizer core, comprising a porous substrate and a heating element. The porous substrate is a porous glass-ceramic substrate. Any two measurement areas on the porous glass-ceramic substrate are respectively designated as a first measurement area and a second measurement area. In atomic percentage, the main element content in the first measurement area is designated as Mat% and the corresponding main element content in the second measurement area is designated as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%. The length of the measurement area is at least greater than 1 μm, and the main element is an element with a content greater than 20 at% in the porous glass-ceramic substrate. The inventors have discovered that by controlling the above conditions, the strength of the porous substrate and the atomizer core containing the substrate can be effectively improved, the stability of the substrate is improved, and its service life is effectively extended. In addition, the prepared porous substrate has uniform strength and composition throughout. Under thermal shock conditions during the atomization process, the porous substrate is also more stable and less prone to local cracks and damage due to different compositions. Moreover, its pore structure is easy to control, the oil conduction effect is good, and it is not easy to produce soot, which does not affect the taste. Therefore, the atomizer core prepared from the porous matrix has a longer service life, a better oil-conducting effect, and does not affect the taste.

[0042] In an optional embodiment, the first measurement region and the second measurement region may or may not intersect. Optionally, the first measurement region and the second measurement region do not intersect. In atomic percentage, the main element content of the first measurement region is recorded as Mat%, and the corresponding main element content of the second measurement region is recorded as Nat%, wherein |MN| / M and / or |MN| / N is less than 5%; for example, |MN| / M and / or |MN| / N can be 0.01%, 0.1%, 0.2%, 0.5%, 0.7%, 0.9%, 1%, 1.3%, 1.4%, 1.6%, 1.8%, 1.9%, 2%, 2.1%, 2.6%, 2.8%, 2.9%, 3%, 3.4%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.2%, 4.3%, 4.5%, 4.7%, 4.8%, 4.9%. The inventors found that by controlling |MN| / M and / or |MN| / N to be less than 5%, the strength uniformity of the porous matrix can be further improved, the stability of the matrix is ​​improved, and its service life is further effectively extended.

[0043] In an optional embodiment, the main elements include a first main element and a second main element; optionally, in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64at%; the content of the second main element is 20-36at%. For example, the content of the first main element can be 55at%, 57at%, 59at%, 60at%, 61at%, 63at%, or 64at%, and the content of the second main element can be 20at%, 21at%, 22at%, 24at%, 26at%, 27at%, 28at%, 29at%, 30at%, 31at%, 32at%, 33at%, 34at%, 35at%, or 36at%. Furthermore, the first main element is oxygen (O) and the second main element is silicon (Si).

[0044] In an optional embodiment, any two measurement areas on the porous glass-ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In terms of atomic percentage, the O element content in the first measurement area is recorded as Mat%, and the corresponding O element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the Si element content in the first measurement area is recorded as M'at%, and the corresponding Si element content in the second measurement area is recorded as N'at%, wherein |M'-N'| / M' is less than 10% and / or |M'-N'| / N' is less than 10%; the length of the measurement area is at least greater than 1 μm.

[0045] In an optional embodiment, the elements in the porous glass-ceramic matrix further include at least one element selected from the group consisting of sodium, magnesium, aluminum, and calcium. Alternatively, in atomic percentage, the elements in the porous glass-ceramic matrix further include at least one element selected from the group consisting of 2.4-6 at% sodium, 0.13-3.18 at% magnesium, 0.23-2.42 at% aluminum, and 1.35-6 at% calcium.

[0046] In an optional embodiment, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and the crystalline phase accounts for more than 50wt%. For example, it can be selected that the crystalline phase accounts for 50wt%, 55wt%, 60wt%, 65wt%, 66wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, and 95wt%. Furthermore, the crystalline phase includes a quartz phase. The matrix material of the porous glass-ceramic matrix prepared in this application is essentially glass-ceramic. Glass-ceramic has excellent mechanical and thermal properties such as corrosion resistance, high temperature resistance, thermal shock resistance, and adjustable thermal expansion. In particular, it is used in atomizer cores. Good corrosion resistance determines its good safety and is not easy to precipitate harmful components; good high temperature resistance and thermal shock resistance determine that it has good mechanical stability and reliability under repeated high temperature shocks.

[0047] In an optional embodiment, the average pore size of the porous glass-ceramic substrate is 15-45 μm. For example, the average pore size of the porous glass-ceramic substrate can be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, 40 μm, 41 μm, 42 μm, 43 μm, 44 μm, or 45 μm. The pore size range is moderate, achieving both liquid-guiding and liquid-locking effects. It should be noted that the pore size of the porous glass-ceramic matrix can also be controlled and adjusted by the selection of raw glass bubbles. By appropriate screening, raw glass bubbles of the required particle size can be obtained. Through suitable raw glass bubbles and preparation process, the pore structure of the porous glass-ceramic matrix can be controlled.

[0048] The D50 glass ceramic bubble diameter corresponds to the particle size at which the cumulative particle size distribution percentage of the glass ceramic bubbles reaches 50%. Its physical meaning is that 50% of the glass ceramic bubbles have a particle size larger than this, and 50% of the glass ceramic bubbles have a particle size smaller than this. D50 is also called the median diameter or median particle size. Similarly, the D50 pore size corresponds to the pore size at which the cumulative pore size distribution percentage of the porous glass ceramic matrix reaches 50%. Its physical meaning is that 50% of the pores have a pore size larger than this, and 50% of the pores have a pore size smaller than this.

[0049] In an optional embodiment, the length of the measuring area is at least twice the average pore size; for example, the length of the measuring area can be selected to be at least 2 times, 3 times, 5 times, 10 times, 20 times, 30 times, 50 times, 100 times, 150 times, or 200 times the average pore size. The aspect ratios of the selected measuring areas are all less than 2. The inventors have found that the measuring area selected within this range can effectively improve the strength of the matrix by controlling its main content components, while achieving uniform strength of the porous matrix. The present application adopts the method of glass bubble sintering to obtain the matrix material, and the composition of the porous matrix is ​​uniform within a specific range, which can make its structure controllable, and the strength, strength consistency and reliability of the finished product are higher.

[0050] In an optional embodiment, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa; further optionally, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa. For example, the compressive strength of the porous glass-ceramic matrix can be selected to be 6 MPa, 6.1 MPa, 6.3 MPa, 6.5 MPa, 6.6 MPa, 6.7 MPa, 6.8 MPa, 6.9 MPa, 7 MPa, 7.1 MPa, 7.3 MPa, 7.4 MPa, 7.5 MPa, 7.6 MPa, 7.8 MPa, 7.9 MPa, 8 MPa, 8.5 MPa, 9 MPa, 9.5 MPa, 10 MPa, 10.5 MPa, 11 MPa, 11.5 MPa, 12 MPa, 12.5 MPa, 13 MPa, 13.5 MPa, 14 MPa, 14.5 MPa, 15 MPa, 15.5 MPa, 16 MPa, 16.5 MPa, 17 MPa, 17.5 MPa, 18 MPa.

[0051] In an optional embodiment, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and the crystalline phase accounts for more than 50%. For example, the crystalline phase can account for 50%, 55%, 60%, 65%, 66%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, or 100%. Furthermore, the crystalline phase includes a quartz phase.

[0052] In an optional embodiment, the porosity in the porous glass-ceramic matrix is ​​50-90%; for example, the porosity in the porous glass-ceramic matrix can be 50%, 55%, 60%, 65%, 66%, 70%, 75%, 80%, 85%, or 90%.

[0053] The present application is further described below in conjunction with the preparation method.

[0054] In some optional embodiments, the method for preparing the atomizer core comprises the following steps:

[0055] 1) mixing glass raw materials with a binder, a slip agent, and water and extruding the mixture to obtain a green body;

[0056] 2) subjecting the green body in step 1) to a first sintering, a second sintering, and a third sintering to obtain a porous glass-ceramic substrate;

[0057] 3) The heating element raw material is prepared on the porous glass ceramic substrate in step 2) and sintered into shape.

[0058] In some optional embodiments, in step 1), the glass raw material may be selected from at least one of glass bubbles and glass powder; the binder may be an organic binder; specifically, the binder may be selected from at least one of methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose; the slip agent may be an aliphatic hydrocarbon slip agent, such as paraffin wax or metal stearate; specifically, the slip agent may be sodium stearate.

[0059] In some optional embodiments, the extrusion molding pressure in step 1) is 1-40 bar. Most of the glass bubbles do not break during the extrusion molding process, maintaining the complete spherical shape of the individual glass bubbles. Therefore, the extrusion molding pressure can be appropriately adjusted based on the compressive strength of the selected glass bubbles.

[0060] In some optional embodiments, the first temperature of the first sintering in step 2) is at least 200° C., for example, 300° C. to 400° C., and / or the first dwell time is at least 1 minute, for example, 1 to 10 hours. During the sintering process at this temperature, substances such as solvents and binders in the green body are removed.

[0061] In some optional embodiments, the second sintering temperature is greater than 400°C and less than the softening point of the glass in the glass bubbles; for example, 500°C, 600°C, or 700°C. The second dwell time is at least 1 minute, for example, 1 to 10 hours. The second temperature is greater than 400°C and less than the softening point of the glass in the glass bubbles / glass powder. This is intended to maintain the original morphology of the green body. At the same time, because the temperature is already above 400°C, the glass component in the glass bubbles / glass powder begins to undergo a phase transition. The disordered glass phase partially crystallizes into a crystalline phase within this temperature range, transforming the glass bubbles into glass-ceramic bubbles or increasing the proportion of the crystalline phase within the glass bubbles. Simultaneously, due to this transition, some glass bubbles begin to rupture, forming at least one opening. Therefore, the sintering time within this temperature range can be appropriately adjusted to adjust the crystallinity of the porous glass-ceramic. It is understood that the raw glass bubbles / glass powder may also contain a certain proportion of crystalline phase, which can shorten the sintering time during this process.

[0062] In some optional embodiments, the third temperature of the third sintering is greater than the softening point of the glass. Specifically, the softening point temperature of the glass is less than 900°C. The third residence time can be at least 1 minute, for example, 1 to 10 hours. At this temperature, the glass component has fluidity, so the adjacent glass-ceramic bubbles are directly bonded to each other, and the glass-ceramic bubbles are bonded to form a porous glass-ceramic matrix with an integrated structure; at the same time, because the glass-ceramic bubbles still have crystalline phase components, the crystalline phase components serve as a skeleton so that their morphology does not collapse and still maintains a basically complete morphology. In addition, the glass-ceramic bubbles further crack to form a large number of openings, which are interconnected to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0063] The third temperature is higher than the softening point of the glass of the glass bubbles. The glass-ceramic bubbles are heated to at least the softening temperature of the amorphous glass in the glass-ceramic bubbles, causing most of the glass-ceramic bubbles to open due to expansion of the gas within the bubbles. Simultaneously, the heating causes adjacent glass-ceramic bubbles to sinter together, forming a bond. Overall, the bonded open glass-ceramic bubbles form pores in a porous glass-ceramic matrix, effectively improving atomization efficiency and liquid conduction in atomizers and electronic atomization devices.

[0064] In some optional embodiments, the mass ratio of glass raw materials to binder, slip agent and water is (100-200): (10-50): (1-10): (50-150); optionally, the glass raw materials are selected from glass bubbles and glass powder; optionally, the mass ratio of glass bubbles to glass powder is (1-100): (0-100).

[0065] In some optional embodiments, in step 3): the raw material of the heating element can be at least one of electronic paste (metal paste), heating wire or heating mesh. The electronic paste can be directly applied to the surface of the porous glass-ceramic substrate in a preset shape by silk-screen printing, and sintered at a preset temperature. The sintering temperature can be adaptively adjusted according to the type of binding phase and metal component in the electronic paste, and the sintering temperature is usually 400-800°C. Optionally, in some other embodiments, the heating element can also be evaporated / deposited on the substrate by physical vapor deposition (PVD) or chemical vapor deposition (CVD). Alternatively, the metal wire or metal mesh is directly welded / attached to the surface of the substrate.

[0066] In some optional embodiments, the glass composition of the glass bulb can be soda-lime silicate glass, borosilicate glass, or other glass. Specifically, the glass composition may include: SiO2 74-85%, CaO 6.5-10%, B2O3 5-9%, Al2O3 0.4-2%, Fe2O3 0.01-1%, Na2O 1-3%, and K2O 0.1-0.5%.

[0067] In some optional embodiments, step 1) further includes adding a pore-forming agent. Optionally, the pore-forming agent is selected from at least one of starch, polymethyl methacrylate (PMMA), polystyrene (PS), and graphite. Optionally, the particle size of the pore-forming agent can range from 1 to 150 μm. It is understood that the addition of the pore-forming agent can further increase the porosity of the porous glass-ceramic matrix while maintaining the strength of the raw glass bubble.

[0068] In some optional embodiments, step 1) further includes a second inorganic material. The second inorganic material may be at least one of clay, talc, silica, and alumina. The melting point or softening point of the above-mentioned material is higher than the softening point of the glass in the glass bubbles. Optionally, the particle size of the pore-forming agent may range from 1 to 200 μm.

[0069] In some optional embodiments, the mass ratio of glass raw material to binder, slip agent, water, pore former and second inorganic material is (100-200): (10-50): (1-10): (50-150): (0-125): (0-9); optionally, the glass raw material is selected from glass bubbles and glass powder; optionally, the mass ratio of glass bubbles to glass powder is (1-100): (0-100).

[0070] As shown in FIG5 , the present application further provides an atomizer including the aforementioned atomizer core. The atomizer includes a housing, within which a liquid storage tank and an atomization chamber are formed. The liquid storage tank is used to store liquid atomization medium, and the atomization chamber is used to accommodate the aforementioned atomization core. The atomization core can atomize the liquid atomization medium.

[0071] As shown in FIG6 , the present application further provides an electronic atomization device, comprising the aforementioned atomizer 1 and a battery assembly 2. The battery assembly and the atomizer may be integral or detachable. The battery assembly is used to power the atomizer in a preset mode, causing the atomizer to atomize a liquid atomizing medium in accordance with the preset mode.

[0072] The present application is further described in detail below with reference to specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in this application.

[0073] The glass bubbles of this application are made of soda-lime silicate glass. The following examples all use glass bubbles made of the same composition. The raw material parameters are shown in Table 1. The specific implementation is described below.

[0074] Example 1

[0075] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0076] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, and 50 g of water and extruded to obtain a green body at a molding pressure of 7 bar;

[0077] 2) subjecting the green body in step 1) to a first sintering, a second sintering, and a third sintering to obtain a porous glass-ceramic substrate, wherein the first sintering temperature is 230° C. and the first sintering time is 1 hour, the second sintering temperature is 650° C. and the second sintering time is 2 hours; and the third sintering temperature is 1050° C. and the third sintering time is 1 hour; finally, the green body is naturally cooled in the furnace to obtain a porous glass-ceramic substrate;

[0078] 3) Printing the heating element slurry on the porous glass ceramic substrate prepared in step 2) and sintering the slurry at a temperature of 620° C. for 1 hour to obtain the atomizing core. The heating element slurry is made of stainless steel.

[0079] As shown in FIG1 , the prepared atomizer core has a porous matrix which is a porous glass-ceramic matrix (as shown in FIG2 ), and the porous matrix has a pore structure which is interconnected.

[0080] Example 2

[0081] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0082] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 25 g of a pore-forming agent, and 67 g of water, and the mixture was extruded to obtain a green body at a molding pressure of 14 bar.

[0083] 2) subjecting the green body in step 1) to a first sintering, a second sintering, and a third sintering to obtain a porous glass-ceramic substrate, wherein the first sintering temperature is 230° C. and the first sintering time is 1 hour, the second sintering temperature is 650° C. and the second sintering time is 2 hours, and the third sintering temperature is 1210° C. and the third sintering time is 1 hour; finally, the green body is naturally cooled in the furnace to obtain a porous glass-ceramic substrate;

[0084] Step 3) is the same as in Example 1.

[0085] Example 3

[0086] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0087] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, and 75 g of water and extruded to obtain a green body at a molding pressure of 24 bar.

[0088] Step 2) and step 3) are the same as in Example 1.

[0089] Example 4

[0090] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0091] 1) 20 g of glass bubbles were mixed with 80 g of glass powder, 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 50 g of a pore-forming agent, and 75 g of water, and extruded to form a green body at a molding pressure of 13 bar. The pore-forming agent was polymethyl methacrylate (PMMA). The glass powder had no internal cavities and was made of the same glass type as the glass bubbles. The particle size of the glass powder was 1-20 μm.

[0092] Step 2) and step 3) are the same as in Example 1.

[0093] Example 5

[0094] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0095] 1) 20 g of glass bubbles were mixed with 80 g of glass powder, 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 50 g of a pore-forming agent, and 75 g of water, and extruded to form a green body at a molding pressure of 24 bar. The pore-forming agent was polymethyl methacrylate (PMMA). The glass powder had no internal cavities and was made of the same glass type as the glass bubbles. The particle size of the glass powder was 1-20 μm.

[0096] Step 2) and step 3) are the same as in Example 1.

[0097] Table 1 Parameters of raw glass bubbles in the examples

[0098] Test Example 1

[0099] The porous glass-ceramic substrate of the atomizer core of the present embodiment was scanned by SEM and its element content was measured. The element content was measured using an energy dispersive spectrometer (EDS). The pore size was measured using mercury intrusion porosimetry (using a mercury intrusion porosimeter).

[0100] Figures 3 and 4 are respectively the SEM images of Example 2 and the EDS analysis of different measurement areas and different range sizes. As shown in Figure 3, two different measurement areas are selected, and the aspect ratios of the selected measurement areas are all less than 2. They are marked as Area 1 (or marked as M) and Area 2 (or marked as N), and the element contents of each measurement area are detected as shown in Table 2. Among them, the detection area is a rectangle, and the length of the detection area is 151.17μm; the D50 of the raw material particles is 41μm, and the average pore size of the finished porous glass-ceramic matrix is ​​23.07μm. Obviously, the difference in the main elements of Area 1 (or marked as M) and Area 2 (or marked as N) is 1% (oxygen element) and 0% (silicon element), respectively. Similarly, the results shown in Table 2 are obtained by measuring other embodiments.

[0101] Table 2 Element contents of examples

[0102] As shown in Figure 4, measurements were performed on different regions of the porous glass-ceramic substrate obtained in Example 2. The test results are shown in Table 3.

[0103] Table 3 Element contents in different regions of Example 2

[0104] As shown in Table 3, the measurement region length of Region 1 is approximately 5 μm and its width is approximately 3 μm. Its main component, oxygen, differs by 8% from that of Region 2, and its main component, silicon, differs by 28%. Similarly, the difference between Region 2 and Region 3 is also significant. These compositional differences are significantly greater than the compositional differences seen in the various embodiments in Table 1. The inventors of the present application believe that due to the phase transitions that occur during the sintering process of the glass bubbles or glass powders of the present application, compositional segregation occurs, but this segregation occurs only within a very small range, typically not exceeding the size of a single glass bubble. Therefore, when the lengths / ranges of the different measurement regions are greater than the length / range of a single glass bubble, the compositional differences are minimal, indicating a uniform and consistent composition. Similarly, when the lengths / ranges of the different measurement regions are less than the length / range of a single glass bubble, the compositional differences are significant, indicating an uneven and inconsistent composition. This is because these smaller regions may actually correspond to different compositions, such as crystalline or glassy phases, within the matrix material, with significantly different compositions. Typically, the grain size in glass ceramics is less than 1 μm; therefore, when the measurement area length / range is greater than 1 μm, several crystalline phase regions and amorphous phase regions can be included in equal proportions within the measurement area, so that the test results of the composition tend to be consistent; that is, the composition of different measurement areas is uniform and consistent. Furthermore, since a completely molten liquid environment is not formed in this application, the flow of the liquid phase usually only occurs in a small range between adjacent / adjacent monomer glass bubbles. Therefore, when the measurement area length / range is greater than 2 times the matrix pore diameter, at least several sub-regions with different compositions can be included in equal proportions, and the composition results of different measurement areas tend to be uniform and consistent. For the sake of simplicity, the average pore diameter is used as the length / range standard of the glass ceramic bubbles in the matrix in this application. The average pore diameter of the matrix in this application is approximately 15-45 μm, and the corresponding measurement area length / range is greater than 30-90 μm. It should be noted that when the measurement area is elliptical, the length of the measurement area is its major axis; similarly, when the measurement area is circular, the length of the measurement area is its diameter. At the same time, the aspect ratio of the measurement area should not be too large. Usually, a ratio less than 2 can more accurately reflect the composition of the measurement area.

[0105] As shown in region 1 in FIG4 , its microstructure is significantly different from the surrounding tissue, indicating that the porous glass-ceramic matrix includes a crystalline phase, and further, the crystalline phase includes a quartz phase.

[0106] Test Example 2

[0107] The compressive strength test of the porous glass-ceramic matrix in the above embodiment was carried out. Five parallel samples of the same embodiment were tested separately. The test method was based on GB / T 4740-1999 "Test Method for Compressive Strength of Ceramic Materials". The pore size and porosity of the porous glass-ceramic matrix and other related parameters were measured by mercury intrusion (the test instrument was a mercury intrusion instrument). The atomizer core in the above embodiment was tested for failure during the preset number of puffs (the preset number of puffs in this application was 500 puffs). The lifespan was statistically recorded. The failure conditions mainly include: 1. The resistance of the atomizer core changed significantly abnormally (such as: the resistance increased significantly due to the breakage or detachment of the heating element); 2. The atomization volume was less than half of the initial atomization volume. The above test conditions were 6.5W power, bare chip (not assembled into an atomizer), and each puff process (i.e., each puff) included: puffing for 3s and then pausing for 8s. The test results are shown in Table 4.

[0108] Table 4

[0109] As shown in Table 4, the inventors' analysis indicates that the porous glass-ceramic matrix exhibits excellent overall compressive strength, with all matrices exhibiting a compressive strength exceeding 1.5 MPa. For example, Example 2 exhibits a porosity of 77.80%, a high porosity approaching 80%, while still maintaining high compressive strength. In some embodiments, compressive strengths exceed 6 MPa, corresponding to porosities exceeding 60%. The inventors' analysis indicates that compositional uniformity is extremely high above the range of a single glass bubble or glass powder. This improves the overall compressive strength of the matrix while also ensuring uniform strength across all locations, without significant localized strength defects. This enhances the strength uniformity of the porous matrix. Furthermore, due to this uniform composition, the porous matrix is ​​more stable under thermal shock during the atomization process, making it less susceptible to localized cracking and damage due to compositional variations. Furthermore, the composition is free of harmful substances such as heavy metals that can leach out. Consequently, the atomizer core has a longer service life and is safer and more reliable.

[0110] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications derived therefrom remain within the scope of protection of this application.

Claims

1. An atomizer core, characterized in that: The atomizing core comprises a porous matrix and a heating element; The porous substrate is a porous glass ceramic substrate, and any two measurement areas on the porous glass ceramic substrate are respectively recorded as a first measurement area and a second measurement area, and in terms of atomic percentage, the main element content of the first measurement area is recorded as Mat% and the corresponding main element content of the second measurement area is recorded as N at%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; The length of the measuring area is at least greater than 1 μm; the main element is an element with an element content greater than 20 at % in the porous glass-ceramic matrix.

2. The atomizer core according to claim 1, characterized in that: In terms of atomic percentage, the main element content in the first measurement area is recorded as Mat%, and the corresponding main element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 5% and / or |MN| / N is less than 5%.

3. The atomizer core according to claim 1 or 2, characterized in that: The main elements include a first main element and a second main element; in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64 at%; the content of the second main element is 20-36 at%; Preferably, the first main element is oxygen, and the second main element is silicon; Preferably, the elements in the porous glass-ceramic matrix further include at least one element of sodium, magnesium, aluminum and calcium.

4. The atomizer core according to any one of claims 1 to 3, characterized in that: The average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

5. The atomizer core according to claim 4, characterized in that: The length of the measurement area is at least twice the average pore diameter.

6. The atomizer core according to any one of claims 1 to 5, characterized in that: The compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa; Preferably, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa.

7. The atomizer core according to any one of claims 1 to 6, characterized in that: The porous glass-ceramic matrix includes a crystalline phase and an amorphous phase; Preferably, the proportion of the crystalline phase is greater than 50wt%; Preferably, the crystalline phase includes a quartz phase.

8. The atomizer core according to any one of claims 1 to 7, characterized in that: The measurement area is at least one of a circle, an ellipse or a rectangle.

9. The atomizer core according to any one of claims 1 to 8, characterized in that: The heating element is a metal heating film.

10. An atomizer (1), characterized in that: The atomizer (1) comprises the atomizer core according to any one of claims 1 to 9.

11. An electronic atomization device, characterized in that: The electronic atomization device comprises the atomizer (1) according to claim 10, and also comprises a battery assembly (2).

Citation Information

Patent Citations

  • Electronic atomization device, and atomizer and heating assembly thereof

    CN110384258A

  • Composition and ceramic atomizing core thereof

    CN113636857A

  • Hierarchical pore glass ceramic and preparation method thereof

    CN114620938A

  • Heating assembly, atomizer and electronic atomization device

    CN114794574A

  • Compositions and methods for making glass ceramic porous structures

    CN116063092A