Method for stabilizing carbon content of molten steel in a refining furnace
Patent Information
- Application Number
- PCT/CN2024/096528
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
Smart Images

Figure CN2024096528_05122024_PF_FP_ABST
Abstract
Description
METHOD FOR STABILIZING CARBON CONTENT OF MOLTEN STEEL IN A REFINING FURNACETECHNICAL FIELD
[0001] The present invention belongs to the technical field of steel production, and in particular the invention relates to a method for stabilizing carbon content of molten steel to minimize carbon pickup in molten steel in a refining furnace.BACKGROUND
[0002] After tapping molten steel from a primary steelmaking furnace such as basic oxygen furnace (BOF) , electric arc furnace (EAF) , induction furnace (IF) , or energy optimization furnace (EOF) , the molten steel is often subjected to further refining (referred to as “treatment” herein) in a number of alternative processes collectively known as “ladle metallurgy” . The following references to a “refining furnace” are understood to be references to a furnace for carrying out “ladle metallurgy” processes.
[0003] The precise role of the ladle metallurgy processes varies depending on the configuration and the product range of the steel plant. Typically, control of key process parameters is achieved through control of three main variables namely (i) addition of chemical reagents and fluxes, (ii) heating through electrically-powered electrodes, and (iii) stirring molten steel by the injection of an inert gas, typically argon.
[0004] Typically, graphite electrodes are used for heating molten steel in a refining furnace for producing steel that is suitable for use in a twin roll thin strip casting process to raise the temperature of molten steel to a casting temperature. However, because graphite is a main component of the electrodes, and because molten steel is vigorously stirred during heating resulting in significant contact between the molten steel and the electrodes over a prolonged time period, it is easy to cause carbon pickup in the molten steel in a refining furnace by loss of carbon from the electrodes into molten steel. This in turn can lead to an unstable twin roll thin strip casting process. In addition, because of the increased carbon content in cast thin steel strip, the mechanical properties of strip can be affected, leading to problems such as cracking in the finished products after bending and deformation.
[0005] Therefore, an important issue for a twin roll thin strip casting process and for thin steel strip quality produced in the process is how to effectively ensure the stability of carbon content in molten steel in a refining furnace that operates with electrically-powered electrodes, i.e., by minimizing carbon pickup in molten steel from electrodes in the refining furnace.SUMMARY
[0006] In order to solve the above technical problem, the present invention provides a method for stabilizing carbon content of molten steel in a ladle in a refining furnace that treats molten steel in a “ladle metallurgy” process, the method characterized in comprising any one or more than one of the following steps:
[0007] (1) melting solid slag (if any) before heating molten steel using electrically-powered electrodes in the refining furnace:
[0008] for molten steel that is transferred to the refining furnace after vacuum treatment in a vacuum furnace, carrying out argon blowing and heating and melting solid slag (if any) before heating molten steel in the ladle using electrically-powered electrodes;
[0009] (2) applying an electric arc between electrically-powered electrodes and molten steel and supplying a small flow rate of argon while heating the molten steel via the electrodes,
[0010] (2.1) controlling the flow rate of argon into a bottom section of the ladle to a target flow rate of argon of 100-200 L / min while the molten steel is being heated using electrically-powered electrodes to reduce scouring, i.e., abrading, of electrodes by flow of the molten steel and foamed slag past the electrodes,
[0011] (3) adding lime in batches to molten steel in the refining furnace:
[0012] (3.1) adding a first batch of lime when the electrically-powered electrodes are not in contact with the molten steel;
[0013] (3.2) adding at least two batches of lime to the molten steel, each comprising 30%-50%by weight of the first batch of lime added to the ladle.
[0014] The method for stabilizing carbon content of molten steel in the refining furnace may further comprise the following step:
[0015] (4) blowing argon before the end of treatment in the refining furnace.
[0016] stopping heating using electrically-powered electrodes before the end of treatment of the molten steel, and then blowing argon into the ladle at a target flow rate of 600 L / min and stirring molten steel in the ladle for 4-5 minutes.
[0017] The method for stabilizing carbon content of molten steel in the refining furnace may further comprise:
[0018] (5) controlling the residence time of molten steel in the ladle,
[0019] carrying out the following four-step molten steel treatment method when the residence time of the molten steel in the ladle exceeds 5 hours,
[0020] vacuum tank degasser (VTD) → refining furnace (LMF –also known as a ladle metallurgical furnace) → vacuum tank degasser (VTD) → refining furnace (LMF) .
[0021] The method for stabilizing carbon content of molten steel in the ladle may further comprise following step:
[0022] (6) controlling heating time using electrically-powered electrodes in the refining furnace,
[0023] controlling a single period of heating using electrically-powered electrodes in the refining furnace to be not more than 10 minutes.
[0024] Beneficial technical effects
[0025] The method for stabilizing carbon content of molten steel in a refining furnace using electrically-powered electrodes for heating molten steel in a ladle in the furnace according to the present invention is characterized by one or more than one of the following steps for the treatment of molten steel in the refining furnace: using a small flow rate of argon , adding lime in batches, carrying out solid slag (if any) melting and argon blowing in a bottom section of the ladle in the refining furnace in the treatment process. The selection of one or more than one of these steps make it possible to limit carbon pickup in the refining process to a very low level, which makes it possible to ensure the stability of carbon content in the molten steel and the final quality of twin roll cast thin steel strip.BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to illustrate the technical solutions of the embodiments of the present disclosure more clearly, the accompanying drawings of the embodiments of the present disclosure will be briefly introduced hereinafter. Obviously, the drawings in the following description are only related to some embodiments of the present disclosure, and do not limit the present disclosure.
[0027] Fig. 1 schematically shows an embodiment of smelting process for producing molten steel for producing ultra-thin strip in a twin roll strip casting process; and
[0028] Fig. 2 is a comparison of carbon content in the refining furnace before and after adjustment according to the stabilization method of the present invention.DETAILED DESCRIPTION OF EMBODIMENTS
[0029] In order to make the purpose, technical solutions, and advantages of the present disclosure clearer, the technical solutions of an embodiment of the present disclosure is described below.
[0030] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure shall have their ordinary meanings as understood by those of ordinary skills in the field to which this disclosure belongs.
[0031] Below is an embodiment of the present invention, and the embodiment is only one of a number of embodiments of the present invention. Based on the embodiment of the present disclosure, all other embodiments obtained by those of ordinary skill in the art without creative labor are within the protection scope of the present disclosure.
[0032] According to the present invention, selectively adjusting the treatment process of molten steel in a ladle in a refining furnace that operates with electrically-powered electrodes for heating molten steel in the ladle can limit carbon pickup to a very low level, with downstream benefits in a twin roll strip casting process. Adjustment options include include melting solid slag (if any) before heating molten steel using electrically-powered electrodes in the refining furnace, controlling the flow rate of argon into a bottom section of the ladle to a target flow rate of argon of 100-200 L / min while the molten steel is being heated using electrically-powered electrodes in the refining furnace to reduce scouring, i.e., abrading, of electrodes by flow of the molten steel and foamed slag past the electrodes, and adding lime in batches to molten steel.
[0033] Carbon pickup in a refining furnace –general comments: the temperature of molten steel that is decarburized in a vacuum in a vacuum furnace is low, and it is necessary to heat molten steel in a refining furnace to a target temperature using electrically-powered electrodes. Heating is also necessary for slagging operations. Because a main component of electrically-powered electrodes in a refining furnace is carbon (graphite) , and because molten steel is vigorously stirred during heating in a refining furnace, which results in significant contact between the molten steel and the electrodes for a long time, it is easy to cause carbon pickup of the molten steel in the refining furnace, which results in an increased final carbon content of the molten steel and downstream consequences in downstream twin roll strip casting processes.
[0034] According to an embodiment of the present invention, the following technical means are adopted.
[0035] 1. Process flow for ultra-thin strip:
[0036] Fig. 1 shows the process flow for ultra-thin strip, in which EAF refers to an electric arc furnace, VTD refers to a vacuum tank degasser, LMF refers to a refining furnace (also called a ladle metallurgy furnace) and CCM refers to a twin roll ultra-thin strip casting machine.
[0037] In a process for preparing steel for casting, as shown diagrammatically in FIG. 1, typically molten steel smelted in an electric arc furnace (EAF) is transferred to a ladle (typically a 100 tonnes capacity ladle and noting that ladle sizes can vary in steelmaking plants and be larger than 100 tonnes) and transported in the ladle to a vacuum tank degasser (VTD) and is treated in the VTD. The molten steel is then transported in the ladle to a refining furnace (LMF –also known as a ladle metallurgical furnace) and is treated further in the ladle in the LMF. Finally, the treated steel is cast into thin strip in a twin roll ultra-thin strip casting machine (CCM) .
[0038] The steel grades produced by the embodiment typically have carbon less than about 0.05%by weight. The steel grade also typically has low nitrogen less than about 0.005%by weight and low sulfur less than about 0.003%by weight, or less than about 0.0015%by weight.
[0039] The twin roll ultra-thin strip casting machine (CCM) and the process for operating the machine is well known and disclosed in a number of patents and patent applications in the names of the applicant.
[0040] 2. Four-step ladle treatment for ultra-thin strip:
[0041] A four-step method for treating molten steel for casting ultra-thin strip comprises:
[0042] EAF → VTD → LMF → VTD → LMF → CCM
[0043] A two-step method for treating molten steel for casting ultra-thin strip comprises:
[0044] EAF → VTD → LMF → CCM
[0045] When the ultra-thin strip is produced by the four-step method, i.e., VTD → LMF → VTD → LMF, slagging and alloying of the molten steel are carried out in the second VTD treatment; When the two-step method is adopted, decarbonization, alloying, slagging, desulfurization and degassing of molten steel are completed in the VTD.
[0046] 3. Comparison of carbon contents in the refining furnace before and after adjustment:
[0047] Fig. 2 is a comparison of carbon contents of molten steel in a refining furnace before and after treatment in the refining furnace operating with electrically-powered electrodes for heating molten steel according to an embodiment of the stabilization method of the present invention.
[0048] The method steps for stabilizing carbon content of molten steel in the refining furnace according to the embodiment are as follows:
[0049] (1) Melting solid slag (if any) after vacuum treatment of molten steel in the vacuum tank degasser and before heating molten steel in the refining furnace via electrically-powered electrodes, for example by carrying out argon blowing with a large argon gas flow rate (typically > 200 L / min) to assist slag melting;
[0050] (2) Heating molten steel in the refining furnace using electrically-powered electrodes with a small flow rate of argon. For example, controlling the flow rate of argon in a bottom section of the ladle during heating molten steel using electrically-powered electrodes or reducing the flow rate of argon in an early stage of heating molten steel using electrically-powered electrodes, and reducing scouring, i.e., abrading, of electrodes from flow of molten steel and foaming slag past the electrodes, which can effectively avoid carbon pickup of the molten steel. The target flow rate of argon is at 100-200 L / min.
[0051] (3) Adding lime in batches and reducing the heating times in the treatment process, adding the first batch of lime when the electrodes are just above the molten steel, and then, according to submerged arc conditions, adding lime to the molten steel several times with a weight of 30%-50%of the first batch of lime, which effectively reduces the chance of increasing the carbon content during the treatment process. Preferably, lime is added to the molten steel with a weight of 50%of the first batch of lime.
[0052] (4) Blowing argon with a large flow rate before the end of treatment in the refining furnace. Stopping heating using electrically-powered electrodes before end of treatment and blowing argon with a large flow rate and stirring for 4-5 minutes, with a target flow rate of argon of 600 L / min, conducting temperature measurements and sampling until the temperatures are uniform, and concluding treatment after all the requirements are met.
[0053] (5) Controlling treatment time of the molten steel strictly. If the residence time of the molten steel in the ladle is completed is expected to exceed 5 hours, the "four-step method” is adopted, that is, vacuum tank degasser (VTD) → refining furnace (LMF) → vacuum tank degasser → refining furnace.
[0054] In addition, control of the quality of the electrodes in the refining furnace and control of the ladle refractories will also have an impact on the stability of the carbon content, as follows:
[0055] (a) It is preferred to use electrodes with good quality, mainly having regard to the proportion of large particles and the thermal shock capacity at high temperatures, so as to reduce the cracking and chipping of electrodes. The reaction between the electrodes and the metal oxide entering slag, which results in carbide entering molten steel to directly increase carbon, is reduced.
[0056] (b) Magnesia-carbon bricks in the refining furnace lining, especially at the slag line, are subject to corrosion. A temperature increase with a large amplitude in the refining furnace should be avoided as much as possible, and the duration for single heating period should not exceed 10 minutes, so as to avoid carbon pickup caused by overheating of the molten steel surface due to long time of heating by electrically-powered electrodes and by excessive corrosion of magnesia-carbon bricks at the slag line.
[0057] What have been described above are only specific embodiments of the present invention. It should be pointed out that for those of ordinary skills in the art, without departing from the principle of the present disclosure, several improvements and embellishments can be made, and these improvements and embellishments should also be regarded as the scope of protection of the present disclosure.
Claims
1.A method for stabilizing carbon content of molten steel in a ladle in a refining furnace that treats molten steel in a “ladle metallurgy” process, the method characterized in comprising the following steps:(1) melting solid slag (if any) before heating molten steel using electrically-powered electrodes in the refining furnace:for molten steel that is transferred to the refining furnace after vacuum treatment in a vacuum furnace, carrying out argon blowing and heating and melting solid slag (if any) before heating molten steel in the ladle using electrically-powered electrodes;(2) applying an electric arc between electrically-powered electrodes and molten steel and supplying a small flow rate of argon while heating the molten steel via the electrodes:(2.1) controlling the flow rate of argon into a bottom section of the ladle to a target flow rate of argon of 100-200 L / min while the molten steel is being heated using electrically-powered electrodes to reduce scouring, i. e., abrading, of electrodes by flow of the molten steel and foamed slag past the electrodes,(3) adding lime in batches to molten steel:(3.1) adding a first batch of lime when the electrically-powered electrodes are not in contact with the molten steel;(3.2) adding at least two batches of lime to the molten steel, each batch of lime comprising 30%-50%by weight of the first batch of lime added to the ladle.2.The method for stabilizing carbon content of molten steel in the refining furnace defined in claim 1 further comprising the following step:(4) blowing argon before the end of treatment in the refining furnace:stopping heating using electrically-powered electrodes before the end of treatment of the molten steel, and then blowing argon into the ladle at a target flow rate of 600 L / min and stirring molten steel in the ladle for 4-5 minutes.3.The method for stabilizing carbon content of molten steel in the refining furnace defined in claim 2 further comprising the following step:(5) controlling the residence time of molten steel in the ladle,carrying out the following four-step molten steel treatment method when the residence time of the molten steel in the ladle exceeds 5 hours,vacuum tank degasser (VTD) → refining furnace (LMF -also known as a ladle metallurgical furnace) → vacuum tank degasser (VTD) → refining furnace (LMF) .4.The method for stabilizing carbon content of molten steel in the refining furnace defined in claim 3 further comprises the following step:(6) controlling heating time using electrically-powered electrodes in the refining furnace:controlling a single period of heating using electrically-powered electrodes in the refining furnace to be not more than 10 minutes.
Citation Information
Patent Citations
Method of smelting ultra-low carbon steel in LF (Ladle Furnace)
CN103160648A
Method for melting ultra-low carbon steel in LF (ladle furnace)
CN103469076A
Improved manufacture of low carbon steel
CN111194357A
Method for stabilizing carbon content of molten steel in refining furnace
CN116694868A
Method of promoting the decarburization reaction in a vacuum refining furnace
US5110351A
Cited By
Full-process intelligent refining system applied to RH furnace