Method for producing a composite material

The method employs magnesium silicate binders from ultramafic rocks to create a composite material with a controlled pH, addressing environmental concerns and material durability by enabling the use of diverse reinforcements in reinforced concrete.

WO2024245559A1PCT designated stage expired Publication Date: 2024-12-05OLIMENT GMBH +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2023/064681
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional cement production for reinforced concrete generates high environmental impacts and new binders with lower pH values are not suitable for corrosion protection of steel reinforcement, while alternative reinforcing materials like carbon and glass fibers face durability issues due to high pH values in standard cements.

Method used

A method using magnesium silicate binders derived from ultramafic rocks and industrial waste, treated hydro-thermally to produce magnesium hydroxide and silicate hydrates, which are then dewatered and used to create a composite material with a lower pH pore solution, allowing for the use of carbon, glass, or steel reinforcements without corrosion.

Benefits of technology

This method reduces environmental impact, enables the use of various reinforcing materials by maintaining a stable pH, and produces a composite material with high performance and durability, avoiding the corrosion issues associated with high pH values.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2023064681_05122024_PF_FP_ABST
    Figure EP2023064681_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a composite material from cement stone, aggregate and reinforcing means. Cement stone is produced by providing a starting product comprising at least 20% by weight of one or more of the following constituents: ultramafic rock, weathering products of ultramafic rock, olivine and / or industrial waste; homogenising the starting product and hydrothermally treating the homogenised starting product in a thermal treatment apparatus at a temperature of above 100°C for at least 12 hours. Furthermore, the converted starting product is dewatered to remove bound water by thermal treatment and / or reactive grinding. Then, the converted, dewatered starting product is used as a binder, and for hardening, setting water is added, the water / binder ratio being 1:2 or less. Before, after and / or at the same time as the setting water is added, an aggregate and reinforcing means are added to the converted, dewatered starting product in order to increase the load-carrying capacity, the reinforcing means being resistant to pH values of below 11 and / or having protection against pH values of below 11. In addition or as an alternative, means for raising the pH value of the porous solution of the cement stone can be added to the starting product of the cement stone.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD FOR PRODUCING A COMPOSITE MATERIAL

[0002] The invention relates to methods for producing a composite material from cement stone, aggregate and reinforcing materials.

[0003] The use of reinforced concrete is indispensable for the construction industry in its current form. In reinforced concrete, the concrete absorbs compressive stresses, while the steel reinforcement inserts are responsible for dissipating tensile forces. At the same time, the concrete protects the steel from corrosion. This corrosion protection is based on a very high pH value in the pore solution of the concrete. At a pH value of around 11, normal reinforcing steel no longer rusts because very thin passivation layers form on the surface, sealing the steel surface against the ingress of oxygen and water, thus preventing corrosion. The pore solution of concrete produced with cements according to DIN EN 197 has pH values ​​above 12, and the use of these cements therefore provides effective corrosion protection for steel reinforcement.Reinforced concrete, a composite material, offers high performance and durability at low cost, making it widely used for these reasons. However, the production of conventional cements is associated with significant environmental impacts. Novel binders have been proposed as substitutes for cement, particularly to reduce carbon dioxide emissions from concrete. However, these binders sometimes exhibit pH values ​​below 11.5 after hardening and are therefore unsuitable for the production of reinforced concrete, as the reinforcing steel is no longer protected from corrosion.

[0004] Various alternative materials have also been proposed to replace steel reinforcement. These include, in particular, carbon and glass fibers. Both materials exhibit very high tensile strengths and can also be used to dissipate tensile forces in reinforced concrete. Another advantage is the corrosion resistance of both fiber types. Neither carbon nor glass fibers normally react with water and / or oxygen. However, high pH values ​​can be detrimental to the bond strength and durability of carbon and / or glass fibers. For this reason, their use in standard cements according to DIN EN 197 can be problematic, as these cements have high pH values ​​in the pore solution. In glass fibers, such high pH values ​​can dissolve the fibers and thus weaken them.For this reason, glass types with higher chemical resistance to alkalis must be used for reinforcement in concrete construction, or the glass must be protected with a protective layer to prevent direct contact with the pore solution of the cement paste. In the case of carbon fibers, the plastics used to bond the individual carbon fibers together can be compromised. High pH values ​​can therefore lead to damage in both types of reinforcement.

[0005] DE 2409231 A1 discloses the use of mineral fibers with an inorganic binder such as cement. To prevent the problems described above, it is proposed to lower the pH value by additional treatment with CO2.

[0006] Furthermore, US Pat. No. 5,002,610 discloses a binder based on magnesium oxide and aluminum phosphate that hardens very quickly. However, the manufacturing process is extremely complicated and requires repeated drying, grinding, and remixing of various components.

[0007] The invention is therefore based on the object of specifying a method for producing a composite material from cement stone, aggregate and reinforcing materials, which can have carbon, glass fibers or even steel reinforcements as reinforcing materials.

[0008] This object is achieved according to the invention by a method having the features of claim 1.

[0009] Further advantageous embodiments are specified in the dependent claims, the further description, and the exemplary embodiments. According to claim 1, at least cement paste, aggregate, and reinforcing material are used to produce the composite material according to the invention, similar to conventional concrete.

[0010] For the purposes of the invention, the term "hardened cement paste" is also used for a hardened binder, which, according to the invention, differs from classic hardened cement paste with a high proportion of hardened Portland cement. The invention primarily relates to the use of binders based on magnesium silicate, which do not need to contain Portland cement clinker. Although these binders do not comply with DIN EN 197, the terms "hardened cement paste" and "concrete" are used for the products made from them for the purposes of the invention.

[0011] According to the invention, for producing a cement stone, a starting product is provided which contains at least 20 mass%, preferably at least 40 mass%, more preferably at least 60 mass%, and even more preferably at least 80 mass% of one or more of the following components. These components can be ultramafic rocks, such as dunite, weathering products of ultramafic rocks, such as serpentinite, olivine, or industrial waste materials. It is essential that all of these raw materials each have a Mg concentration or a Mg content of at least 5 mass%, preferably 10 mass%, and more preferably over 20 mass%, and ideally over 30 mass%. The data refer to the proportion of the element magnesium in the total sample, whereby the element magnesium can be present in various phases such as olivine, enstatite, serpentinite, or other compounds.The stated concentrations therefore do not refer to the proportion of the MgO (periclase) phase in the starting product. The starting product preferably contains no free MgO (periclase), but rather the stated magnesium concentrations. This starting product is milled with a fineness corresponding to a BET surface area of ​​0.1 m. 2 / g or finer. A BET surface area of ​​0.5 m 2 / g, more preferably a BET surface area of ​​1.0 m 2 / g, in particular a BET surface area of ​​3.0 m 2 / g or even finer.

[0012] An important mineral in ultramafic rocks is olivine. It is a solid solution series between fayalite (Fe2SiO4), forsterite (Mg2SiO4), tephroite (Mn2SiO4), and other minerals of the form A2[SiO4], where various divalent ions can occur for A, as well as a combination of the various cations. Natural olivine deposits have been documented, and the olivine is often a magnesium-rich material with iron components.

[0013] Serpentinite is a metamorphic rock that forms through the weathering of ultramafic rocks and can contain mineral phases such as lizardite, antigorite, talc, and other crystalline and amorphous compounds.

[0014] Examples of industrial waste materials that can be used in the context of the invention are foundry sand or refractory materials.

[0015] After the raw material has been prepared, it is homogenized, if necessary. The listed possible components of the raw material are often natural rocks or materials from natural deposits. Experience has shown that these are neither pure nor homogenized. Homogenization can be performed, for example, with a mixer or simultaneously with grinding to the desired fineness.

[0016] Following homogenization, the thus prepared starting product is subjected to hydrothermal treatment. This takes place in a heat treatment facility at a temperature above 100°C for at least 12 hours, preferably at least 24 hours. The heat treatment facility can be, for example, a heat tunnel or an autoclave. An autoclave is usually understood to be a gas-tight, sealable pressure vessel that can be used for the thermal treatment of substances in the overpressure range. It is preferred if the heat treatment facility is understood to be a vessel, a combination of devices such as an oven and a sealed mold, or a device for enclosing a volume. The treatment preferably takes place at temperatures above 100°C, in particular above 150°C, even better above 200°C, and even more preferably above 250°C.For successful implementation, it is advantageous if the treatment is carried out for longer than 36 hours, even more preferably longer than 48 hours. However, particularly good results can be achieved if the treatment is carried out for even longer, for example, over several days, for example, 4, preferably 7 days or longer. Furthermore, water can be added to the homogenized starting product by directly adding it before, after, and / or simultaneously with homogenization in the preceding step, and by mixing the water with the starting product. Alternatively or additionally, steam can also be introduced into the heat treatment device.

[0017] During the hydro-thermal treatment of the homogenized starting product, this is at least partially transformed into magnesium hydroxide (Mg(OH)2) and magnesium silicate hydrates due to the presence of H2O

[0018] (Mg3Si2O5(OH)4,Mg3Si4Oio(OH)2). The underlying reactions are as follows, which are simplified here starting with forsterite (Mg2SiO4):

[0019] (1 ) 2 Mg2SiO4+ 3 H2O Mg3Si2O5(OH)4+ Mg(OH)2

[0020] (2) 3 Mg2SiO4 + 5 SiO2 + 2 H2O ^2 Mg3Si4Oio(OH)2, where reaction (1) primarily occurs. This is also preferred within the scope of the invention, since Mg3Si2O5(OH)4 is better suited for subsequent hardening than Mg3Si4Oio(OH)2. Furthermore, it should be noted that the amount of the respective products and their ratio depend, among other things, on the exact composition of the starting product.

[0021] The magnesium hydroxide (Mg(OH)2) can be present as brucite. The magnesium silicate hydrate (Mg3Si2Os(OH)4, MgsSi4Os(OH)2) can be present in the form of lizardite, antigorite, talc, and other minerals. It should be noted that the stoichiometric water content is sometimes lower—in the range of 13 mass% for antigorite—than that determined by experiments—in the range of 16 to 20 mass%. This can be explained by the fact that some of the materials are so fine that water can adhere to their surfaces.

[0022] Similarly, such deviations from stoichiometry also apply to the ratio between Mg and Si. Furthermore, foreign ions, such as Fe, can also be incorporated into the reaction products. However, other reaction products such as hydromagnesite, hematite, magnetite, or gibbsite can also be formed. This depends on the exact composition of the starting product. All or some of the reaction products may contain iron, carbonate, alkalis, or other foreign ions.

[0023] During the treatment, magnesium silicates such as olivine or enstatite contained in the starting material are not broken down into oxides. In particular, no unbound SiO2 is formed, either in crystalline or amorphous form. SiO2 is also not formed from magnesium silicate in the subsequent treatment steps.

[0024] Subsequently, the converted starting product is at least partially dewatered of bound water by thermal treatment and / or reaction milling. Bound water is sometimes also referred to as crystal water. It must be distinguished from unbound water, which can be considered free H2O. Complete dewatering can be achieved with considerable effort. According to the invention, the water content of bound water should be reduced by at least 60%, preferably by at least 80%.

[0025] For thermal treatment, the converted starting product can be heated to a temperature between 180 °C and 1000 °C. Depending on the fineness, heating for just a few minutes is sufficient. The thermal treatment should not last longer than one hour. Temperatures between 300 °C and 800 °C are preferred, and between 500 °C and 700 °C are even more advantageous. Alternatively or additionally, the converted starting product can also be subjected to reaction milling to rearrange the crystal structures. In so-called reaction milling, crystalline water can also be removed from the converted starting product by rearranging the crystal structures. For this purpose, auxiliary materials such as quartz can be added to the grinding process.

[0026] During this dehydration step, any magnesium hydroxide (Mg(OH)2) present in the converted starting product is at least partially converted into magnesium oxide (MgO, periclase), and any magnesium silicate hydrate (Mg3Si2O5(OH)4, Mg3Si4Qio(OH)2) present is at least partially converted into dehydrated magnesium silicate hydrate, which can be simplified as xMgOSiO2 yH2O. Dehydration refers to the reduction of the crystalline water or water of crystallization in the converted starting product. The underlying chemical processes are, again simplified, as follows:

[0027] (3) Mg(OH)2-> MgO + H20

[0028] (4) Mg3Si2O5(OH)4->2 xMgO SiO2yH2O + z H20

[0029] (5) Mg3Si4Oio(OH)2->4 aMgO SiO2bH2O + cH2O, where (4) produces a largely amorphous reaction product with a Mg to Si ratio of 1.5 to 2 and a residual water content of approximately 3%. The reaction product formed in equation (5) has a lower Mg to Si ratio. Hence the variables a, b, c, x, y, and z. This depends on the exact composition of the starting product and the treatment parameters.

[0030] After dewatering, the water content of the bound water in the converted, dewatered starting product is preferably below 10 mass%, advantageously below 5 mass%, more preferably below 3.5 mass%, even more preferably below 2.5 mass%.

[0031] The transformed and dehydrated starting product is thus present as a multiphase product. Other possible secondary phases include hematite, magnetite, enstatite, feldspars, pyroxenes, quartz, and amorphous phases.

[0032] The at least partially converted and dewatered starting product is used as a binder. For hardening, aggregate and setting water are added to the converted, dewatered starting product, with the water to binder ratio being, in particular, 1:2 or less. In other words, the converted and dewatered starting product is used as a complete or partial cement substitute for hardened cement. The water to binder ratio is preferably in the range of 1:2 or less. This means that the ratio is 1:2.22, preferably 1:2.5, and ideally 1:2.86, and even better 1:3.33 or less. It has been found that a higher ratio, i.e. a higher water content, prolongs hardening and reduces strength. The concrete produced in this way binds CO2 from the ambient air even at room air and room temperature.The CO2 partial pressure should not exceed 1000 ppm, as otherwise increased shrinkage may occur. During curing, no thermal treatment to increase the reaction temperature, especially no heat treatment, should be performed.

[0033] After mixing with water, a chemical reaction occurs between the converted, dehydrated starting material and the mixing water. The phases formed in the previous firing process, such as MgO, xMgO, SiC, yFW, aMgO, SiCh, bkhO, react with water to form hydrous compounds such as Mg(OH)2, Mg3Si2Os(OH)4, Mg3Si4Oio(OH)2, and other compounds. This corresponds to equations (3) to (5) with the reaction arrow reversed. The temporal course of the hydration reaction can be monitored by calorimetry (see Fig. 1). The rate of heat release depends on several factors.

[0034] If a starting product is provided that already contains at least 20 mass% magnesium silicate hydrate, preferably at least 40 mass%, more preferably at least 60 mass%, and even more preferably at least 80 mass%, as is the case with serpentinite, for example, the steps of water addition and hydrothermal treatment can be omitted. In other words, this starting product can be processed with only the grinding and dewatering steps, and the conversion steps are not necessary. Serpentinite is a metamorphic rock that forms through natural transformation, particularly weathering, of ultramafic rocks.

[0035] To produce the composite material according to the invention, an aggregate such as sand or gravel is added to the converted, dewatered starting material before, after, and / or simultaneously with the addition of the setting water. For the sake of simplicity, reference is made to the converted starting material within the scope of the invention; this also includes serpentinite as a starting material, which strictly speaking does not need to be converted.

[0036] In construction, aggregates generally refer to natural and artificial rock particles. These can originate from natural deposits, for example, or arise from the recycling of building materials or as an industrial by-product. Alternative, outdated but roughly synonymous terms in the construction industry are concrete aggregate, mineral mixture, mineral blend, or mineral. Furthermore, reinforcing agents are added to the possibly converted, dewatered starting product before, after, and / or simultaneously with the addition of the setting water to increase its load-bearing capacity.In this case, reinforcing agents are selected which are resistant to pH values ​​below 11, reinforcing agents which are provided with protection against pH values ​​below 11 and / or agents are added to the starting product, in particular the converted, dewatered starting product, to raise the pH value of the pore solution of the cement stone to a pH value above 11.0.

[0037] According to the invention, it was recognized, on the one hand, that by combining a hydrothermal treatment and the expulsion of crystal water from natural materials, such as ultramafic rocks, an intermediate material can be produced which is suitable for binding with water and solidifying.

[0038] Olivine-rich rocks that can be used according to the invention include dunite, wehrlite, and habsburgite. These rocks often have a low degree of weathering. However, weathered rocks with a similar chemical composition but a higher water content can also be used. Examples of weathered rocks include serpentinite.

[0039] A further basic idea of ​​the invention can be seen in the use of the intermediate material to deviate from known Portland cement-based cements, which have a relatively high pH value. According to the invention, it was recognized that the pore solution of a cement paste made from the converted, dewatered starting product, as understood according to the invention, usually has pH values ​​below 11. This allows the use of reinforcement made of glass fibers or carbon fibers, or combinations of both, which are not stable against media with pH values ​​above 11 without further treatment.

[0040] If other reinforcing agents such as steel reinforcement are to be used, the invention provides protection against pH values ​​below 11 present in the pore solution of the cement paste according to the invention. Alternatively or additionally, depending on the reinforcing agent used, other agents can be added to the serpentinite- and / or olivine-based binder to raise the pH of the pore solution to a pH above 11.0. For this purpose, slaked lime, quicklime, alkalis such as sodium hydroxide or potassium hydroxide, and CKD (cement kiln dust, kiln dust from cement production) can be added.

[0041] At least when using tempered serpentinite in the starting product, but preferably also when using a natural or artificial olivine source, the starting product should be free of alite and belite, as these can cause hardening problems.

[0042] It is advantageous if the pore solution of the cement paste has a pH of 11 or lower. This is particularly the case if the cement paste according to the invention consists essentially of the converted, dewatered starting product. This eliminates the need for any further adjustments to the starting material of the cement paste for use with glass fiber and / or carbon fiber reinforcement.

[0043] In principle, any reinforcement can be used according to the invention. However, it is particularly advantageous to select reinforcements containing carbon, mineral, especially basalt, and / or glass fibers. These fibers have the advantage over conventional steel reinforcements of being lighter and producing significantly less CO2 during production.

[0044] According to one design, reinforcements can be selected that are designed to withstand pH values ​​below 11 without a protective layer. This is particularly possible with reinforcements made of carbon and / or glass fiber. However, a protective layer against such low pH values ​​can also be applied, particularly with steel reinforcement.

[0045] It is further advantageous to select reinforcements that contain carbon, mineral, particularly basalt, and / or glass fibers in the form of fiber reinforcement, mesh reinforcement, bar reinforcement, and / or other reinforcement forms. The advantage of using carbon, mineral, particularly basalt, and / or glass fibers is that they can be formed into any desired shape and subsequently used to manufacture the composite material. This allows for an optimal reinforcement shape to be provided depending on the expected load.

[0046] In a further embodiment, steel reinforcements can also be used alternatively or additionally in the composite material according to the invention. If these are used, it is preferred to add Portland cement clinker, in particular, to the cement paste in addition to the converted, dewatered starting product. This is particularly suitable for increasing the pH value, thus preventing corrosion of steel reinforcement due to the low pH value. In addition, compared to other substances that influence the pH value, Portland cement clinker offers the advantage of making its own separate contribution to strength.

[0047] In addition, the reinforcements may be provided with at least one protective layer to protect against alkaline environments with a pH value below 11. This protective layer can be applied, for example, by applying paint and / or varnish. The protective layer can be plastic-based. Another option is to apply hot-dip galvanizing to steel reinforcements.

[0048] The hydrothermal treatment of the homogenized starting product for at least partial conversion into magnesium hydroxide and / or magnesium silicate hydrate is one of the process steps that, according to the invention, takes the longest. Therefore, it is preferred if one or more treatments to accelerate the ongoing reactions are carried out during the hydrothermal treatment. Various treatment methods are suitable for this purpose, which can be carried out individually or in combination with one another. These are explained in more detail below. All or just a few selected treatment methods can be combined.

[0049] One possibility is to continuously or discontinuously crush or break up, in particular to finely grind, the homogenised starting product during the hydrothermal treatment or between several hydrothermal treatments in the heat treatment facility in order to accelerate the conversion.

[0050] Continuous or discontinuous comminution can prevent or reduce clumping or intergrowth of the materials present during hydrothermal treatment. This ensures that a sufficiently large surface area remains for the processes described above to take place. Several options are available for the precise implementation.

[0051] On the one hand, it is possible to stop the hydrothermal treatment, remove the material from the heat treatment facility, crush it or break it up, for example by grinding it, and then feed it back into the heat treatment facility.

[0052] On the other hand, it is also possible to provide a corresponding comminution system in the heat treatment facility, which carries out comminution continuously or discontinuously during the hydrothermal treatment.

[0053] Another possibility is to operate a heat treatment facility, particularly continuously, and to discharge a portion of the material from the heat treatment facility during the hydrothermal treatment, to crush it, and then to return it to the facility. This is particularly useful if the starting product is present in a suspension in the heat treatment facility or at least in a pumpable form. In this case, for example, a line from an autoclave can be provided that leads to a crushing device such as a mill and back into the autoclave, which is an example of a heat treatment facility within the meaning of the invention. This can be referred to as a continuous circulation process.

[0054] An additional possibility for accelerating the reaction is if, for the hydrothermal treatment of the homogenized starting product in the heat treatment facility, the homogenized starting product is present in a suspension which is stirred continuously or discontinuously during the hydrothermal treatment. For example, an agitator can be provided to ensure movement of the suspension. In this context, grinding can also be provided alternatively or additionally - as described above. Wet grinding is particularly suitable for this purpose, as part of the suspension can be transported out of the heat treatment facility, wet-ground and then added back to it. However, wet grinding can also take place directly in the heat treatment facility.

[0055] It may be advantageous to dry the homogenized and converted starting product to remove unbound water prior to the dewatering step, i.e., the removal of bound water. This is particularly advisable and useful if the hydrothermal treatment of the starting product was carried out in an aqueous suspension.

[0056] The dried starting product can then be fed to the dewatering step. The proposed thermal treatment can also be referred to as tempering or calcining. It can be carried out in a thermal treatment unit such as a rotary kiln or using a circulating fluidized bed of hot gases. When using a fluidized bed, dewatering occurs within a few seconds. Alternatively, the necessary energy can also be generated electrically, for example, in a muffle furnace. This requires times of approximately 5 to 10 minutes. Systems without direct contact of the material with a flame are generally preferable, as it is easier to precisely maintain the firing temperature. Furthermore, open systems are preferred to remove the resulting water vapor, which accelerates the reaction.

[0057] It is advantageous if the thermal treatment unit has an essentially homogeneous temperature distribution. This allows for good dewatering without the formation of unwanted by-products. Therefore, in order to maintain the desired dewatering temperature in the furnace as precisely as possible and over a large part of the material's residence time, it is advantageous if the furnace is not heated directly with a flame. In this case, the material would be temporarily exposed to very high temperatures, which would lead to olivine formation. For example, the temperature distribution in a directly heated rotary kiln is too uneven. Therefore, it is advantageous to use a rotary kiln as the thermal treatment unit, in particular an indirectly heated rotary kiln without any open flames in the reaction chamber.The temperature during thermal treatment, which can also be referred to as firing temperature, can be controlled particularly precisely in electrically heated kilns. Electric heating should be used in particular to precisely maintain the target temperature in the kiln chamber. It is advantageous to heat the kiln with electrical energy from renewable energy sources, as this does not produce any CO2 emissions or exhaust gases and no fuel is consumed. In contrast, preheating is also possible using other heat sources, in particular a heat exchanger, which extracts some of the heat from the dehydrated starting product, such as the fired serpentinite, and thereby cools it, while simultaneously transferring this heat to unfired serpentinite. The use of flue gas from combustion processes should also be avoided if possible, as this can lead to, for example, uncontrolled binding of CO2.

[0058] To achieve a sufficient residence time at the target temperature, rotary kilns are preferred because of their large volume and thus high throughput. Furthermore, rotary kilns are characterized by good thermal efficiency.

[0059] Another alternative is ultrasonic treatment of the homogenized starting product. Similar to grinding, this ensures that substances formed on the starting product, such as magnesium hydroxide and / or magnesium silicate hydrate, separate from the remaining substances in the starting product, thus creating a sufficiently large surface area to allow the reaction to proceed smoothly. This can be achieved, for example, using an ultrasonic horn or similar device.

[0060] Another option is to add nucleating agents, pH-raising agents, foreign ions, and / or other additives to the starting product at the beginning, before or during homogenization, after homogenization, or even in the heat treatment facility to accelerate the reaction. Examples of nucleating agents that can be added include brucite, lizardite, antigorite, prehydrated olivine-bearing rock, or mixtures of these substances. The addition of at least 2% by mass of nucleating agents is preferred.

[0061] As agents for raising the pH value, which thus modify a solution in which the reaction takes place, substances can be added which release NaOH, KOH, NaCl, KCl, Na2SO4, MgSO4, K2SO4, Na2CO3, Ca(OH)2 and / or K2CO3 after their addition, thereby increasing the pH value in the solution so that the reaction proceeds more quickly.

[0062] Other additives that also accelerate the reaction include dolomite, feldspars, pyroxenes, and mixtures thereof. The addition of these substances can lead to the formation of new reaction products. Examples of foreign ions are aluminum, sulfate, or alkalis. These can also lead to the formation of new reaction products. It is preferable to avoid additives containing magnesite, hydromagnesite, and / or nesquehonite, as these can potentially slow down the reactions.

[0063] In principle, the reaction can also be initiated in the autoclave simply by increasing the temperature. Temperatures above 150 °C, preferably above 200 °C, and even more preferably above 250 °C are possible.

[0064] To provide the starting product with a fineness corresponding to a BET surface area of ​​0.1 m 2 / g or finer, it is preferred if the starting product is subjected to grinding, in particular wet grinding. The starting product is usually not of a higher fineness - even if it is already very fine, partly due to natural weathering. This fineness can easily be increased by grinding. Wet grinding is also preferred here, as it is often more energy-efficient than dry grinding. Since the starting product is subsequently subjected to a hydrothermal treatment in which it comes into contact with water, the advantage of wet grinding can already be utilized in this step, particularly since the ground material does not need to be dried.

[0065] The starting products provided according to the invention are usually not pure substances, so that impurities are present to a high degree. However, it is advantageous if at least the molar ratio of Mg to Ca is 10:1 or greater and / or the molar ratio of Si to Al is also 10:1 or greater. It has been shown that the presence of calcium and aluminum in relation to magnesium or silicon slows down the reactions or sometimes stops them completely. It is therefore not insignificant to shift the corresponding molar ratios significantly towards magnesium or silicon. Preferably, the molar ratio of Mg to Ca is at least 20:1 and / or the molar ratio of Si to Al is at least 20:1.

[0066] The invention is explained in more detail below using exemplary embodiments with reference to the single figure. This figure shows:

[0067] Fig. 1 shows a hydration profile of a product produced by the process according to the invention.

[0068] To verify the invention, the following tests were conducted, among others. Pure forsterite was used in the first test and natural olivine in the second. Serpentinite was also used in the fourth test.

[0069] Pure Forsterite

[0070] For the first investigation, pure forsterite (Mg2SiO4) was used, which was produced by firing a mixture of magnesium hydroxide carbonate and amorphous SiO2 in a laboratory furnace. After firing, the starting material was ground in a vibrating disc mill. The specific surface area according to the BET method was 1 m 2 / G.

[0071] A mixture of forsterite and 1 molar NaOH solution in a ratio of 1:2.2 was prepared and treated in an autoclave at a temperature of 200°C. The reaction was interrupted for a while, and the material was dried and ground. After a treatment period of 4 weeks, no forsterite was detectable in the treated and washed material by X-ray phase analysis. The loss on ignition after completion of the autoclave treatment was 19.3 mass%. 3.0 g of each of the dried and ground material was fired in a platinum crucible at temperatures of 450°C, 600°C, or 750°C for one hour each in a muffle furnace. The fired samples exhibited a loss on ignition of 13.5% (450°C), 2.8% (600°C), and 0.52% (750°C).

[0072] The reactivity of the material as a binder was investigated by determining water binding after 7 days of hydration. For this purpose, the materials fired at different temperatures were ground in a hand mortar and mixed with water using a water-to-binder ratio of 0.40 (1:2.5). The mixture was then stored in sealed containers at 22°C for 7 days. Hydration of the samples was then stopped by drying at 60°C, and the ignition losses were determined by thermal analysis.

[0073] The resulting ignition losses were 20.5% (450°C), 25.3% (600°C), and 7.1% (750°C), respectively. Accordingly, all three binders hydrated and bound water.

[0074] The hydration process of the sample fired at 600°C was investigated by calorimetry (DCA) at 25°C. This showed a very rapid reaction, with a maximum of the main hydration phase after about 2 hours, and the reaction was completed in less than 24 hours. A total heat release of approximately 450 J / g was shown in Fig. 1.

[0075] As a result, the binder reacts faster than most conventional cements. An examination of the hydrated and dried sample after DCA analysis using 29 Si MAS NMR spectroscopy showed that all silicon was present as magnesium silicate hydrate.

[0076] Natural olivine

[0077] For the second study, natural olivine from a locality in Norway was used. Its chemical analysis revealed the following composition: 41.9% SiO2, 49.9% MgO, 6.9% Fe2O3, 0.6% Al2O3, 0.1% CaO, and 0.5% loss on ignition.

[0078] The material was ball milled to a fineness of 7300 cm 2 / g Blaine was ground and mixed with 1 molar NaOH solution in a ratio of 1:2. The material was autoclaved at 200°C for 22 days, interrupted once for grinding.

[0079] After autoclaving, the intermediate product was dried, ground and the loss on ignition was analyzed (16.3%).

[0080] Individual batches of the intermediate product were fired at various temperatures, and water binding by hydration was investigated for 7 days at 22°C. Before hydration, the ignition losses (6.8% after 550°C, 3.1% after 600°C, 2.2% after 650°C, 1.7% after 700°C) were lower than after reaction with water and subsequent drying at 60°C (20.1% after 550°C, 23.7% after 600°C, 24.7% after 650°C, 22.8% after 700°C).

[0081] Consequently, natural materials such as olivine can also be used for binder production, with hydration being demonstrated after the described pretreatment. pH value

[0082] Furthermore, the pH of the cement paste according to the invention was analyzed. For this purpose, a binder made of pure synthetic forsterite without foreign ions was analyzed.

[0083] After half a year of hydration, the pH value of the sample was 9.5.

[0084] In a further study, the pH value in the pore solution of the binder according to the invention was measured. For this purpose, serpentinite was ground to a specific surface area of ​​0.55 m 2 / g and 1 kg of the ground material were fired for 1 hour at 700°C. Deagglomeration then occurred by grinding in a ball mill for 5 minutes. The resulting binder was mixed with water, with a water / binder ratio of 0.40. The binder paste was allowed to harden for 2 days at room temperature, and then the pore solution was pressed out using a high-pressure press (testing machine) and a pressing die. The pH value of the solution was determined and found to be 10.3. A comparison sample was also prepared to which 1.6% NaOH (based on the binder) was added. When the alkaline pore solution was pressed out after hardening, a pH value of 12.4 was measured. Consequently, the addition of alkaline compounds can increase the pH and prevent corrosion of the steel reinforcement.

[0085] The use of forsterite, which belongs to the olivine group, makes it possible to produce a binder for a composite material with a very low pH value compared to cement paste made from traditional Portland cement clinker. This low pH value allows the use of glass and / or carbon fiber reinforcements for the first time without any further pretreatment.

Claims

PATENT CLAIMS 1 Process for producing a composite material from cement stone, aggregate and reinforcing agents, wherein for producing a cement stone a) a starting product is provided which contains at least 20 mass% of one or more of the following components: • ultramafic rocks, especially dunite, • Weathering products of ultramafic rocks, especially serpentinite, • Olivine, • industrial waste materials with a Mg concentration of at least 5 mass% and with a fineness corresponding to a BET surface area of ​​0.1 m 2 / g or finer, b) the starting product is homogenised, c) the homogenised starting product is subjected to a hydro-thermal treatment in a heat treatment facility at a temperature above 100°C for at least 12 hours, d) water is added to the homogenised starting product by: • direct addition of water before, after and / or simultaneously with the homogenization in step b) and the mixing of the starting product with the water and / or • Introducing steam into the heat treatment facility, wherein after step c) the starting product has been at least partially converted into magnesium hydroxide Mg(OH)2 and / or magnesium silicate hydrate in the presence of H2O, e) the converted starting product is at least partially dewatered of bound water by means of thermal treatment and / or reaction milling, • during thermal treatment, the converted starting product is treated at a temperature between 180°C and 1000°C, • wherein during reaction milling a rearrangement of the crystal structures in the converted starting product occurs, wherein after step e) in the converted, dehydrated starting product present magnesium hydroxide is at least partially dehydrated into magnesium oxide and present magnesium silicate hydrate is at least partially dehydrated and can thereby be converted into dehydrated magnesium silicate hydrate, f) the converted, dehydrated starting product is used as a binder and setting water is added to the converted, dehydrated starting product for hardening, wherein the water-binder ratio is in particular 1:2 or less, wherein when providing a starting product which already has at least 20 mass% magnesium silicate hydrate, for example serpentinite, steps c) and d) can be dispensed with, wherein an aggregate is added to the converted, dehydrated starting product before, after and / or simultaneously with the addition of the setting water,such as sand or gravel, is added, whereby reinforcing agents are added to the converted, dewatered starting product before, after and / or simultaneously with the addition of the setting water to increase the load-bearing capacity, whereby, - reinforcement materials are selected that are resistant to pH values ​​below 11, - reinforcements are provided with protection against pH values ​​below 11 and / or - agents are added to the starting product to raise the pH value of the pore solution of the cement stone to a pH value of or above 11.

2. Process according to claim 1, characterized in that the pore solution of the cement stone has a pH value of 11 or lower.

3. Method according to claim 1 or 2, characterized in that reinforcements are selected which are designed without a protective layer to resist pH values ​​below 11.

4. Method according to one of claims 1 to 3, characterized in that reinforcements comprising carbon, mineral, in particular basalt, and / or glass fibers are selected as reinforcements.

5. Method according to claim 3 or 4, characterized in that reinforcement means are selected in which the carbon, mineral, in particular basalt and / or glass fibers are in the form of fiber reinforcement, mat reinforcement, rod reinforcement and / or other forms of reinforcement.

6. Method according to one of claims 1 to 5, characterized in that reinforcement means comprising steel reinforcements are selected as reinforcement means.

7. Method according to one of claims 1 to 6, characterized in that that the reinforcements are provided with a protective layer to protect against an alkaline environment with a pH value below 11.

8. The method according to any one of claims 1 to 7, characterized in that the reinforcements are hot-dip galvanized and / or coated with a paint or varnish layer, particularly made of plastic, to protect them against an alkaline environment with a pH value below 11. The method according to any one of claims 1 to 8, characterized in that, for at least partially converting the starting product in step c), one or more treatments are carried out to accelerate the reactions occurring during the hydrothermal treatment. 10 Process according to one of claims 1 to 9, characterized in that before, during the hydrothermal treatment or between several hydrothermal treatments in the heat treatment device in step c), the homogenized starting product is continuously or discontinuously comminuted, in particular finely ground, to accelerate the conversion. 11 Method according to one of claims 1 to 10, characterized in that for the hydrothermal treatment of the homogenized starting product in the heat treatment device, the homogenized starting product is present in a suspension which is stirred continuously and / or discontinuously during the hydrothermal treatment. 12 Method according to one of claims 1 to 11, characterized in that in step c) an ultrasonic treatment of the homogenized starting product is carried out. 13 Method according to one of claims 1 to 12, characterized in that to provide the starting product with a fineness corresponding to a BET surface area of ​​0.1 m 2 / g or finer, the starting product is subjected to grinding, in particular wet grinding.

14. Process according to one of claims 1 to 13, characterized in that the starting product has a molar ratio of Mg to Ca of 10:1 or greater and / or a molar ratio of Si to Al of 10:1 or greater.

Citation Information

Patent Citations

  • Structural bodies based on inorganic binders - reinforced with inorganic fibre mats

    DE2409231A1

  • Process for making reinforced magnesium phosphate fast-setting cements

    US5002610A

  • Hydrated calcium silicate and hydrated magnesium silicate cementing material for mine filling and preparation method of hydrated calcium silicate and hydrated magnesium silicate cementing material

    CN115057638A

  • Magnesia based binder composition

    EP2508496A1

  • Integrated chemical process

    WO2008061305A1