Method for producing inorganic material, apparatus for producing inorganic material, and structure

The method of using a copper-based decomposition promoting component to thermally decompose organic materials at lower temperatures addresses the challenge of high-temperature processing in composite materials, preserving inorganic material properties and enabling effective recycling for weight reduction in structural applications.

WO2024247351A1PCT designated stage expired Publication Date: 2024-12-05HITACHI LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/000829
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-01-15
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current methods for thermally decomposing organic materials in composite materials require high temperatures, which can lead to deterioration of inorganic materials and make it difficult to recycle them effectively, especially in applications like aircraft and vehicle weight reduction where lower processing temperatures are needed.

Method used

A method involving a composite material with an organic component and an inorganic component, where the organic material is thermally decomposed in an oxidizing atmosphere using a decomposition promoting component with copper as the main transition metal element, reducing the decomposition temperature to 440°C or lower, thereby preserving the inorganic material's properties and facilitating recycling.

Benefits of technology

This approach allows for the thermal decomposition of organic materials at lower temperatures, preventing deterioration of inorganic materials and enabling the production of recycled composite materials with comparable physical properties to virgin materials, thus supporting weight reduction in structural applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024000829_05122024_PF_FP_ABST
    Figure JP2024000829_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing an inorganic material according to the present disclosure comprises a contact step (S1), an atmosphere control step (S2), and a heating step (S3). In the contact step (S1), a composite material (101) which comprises an organic material (106) that is composed of an organic material and an inorganic material (105) that is composed of an inorganic material is brought into contact with a decomposition promoting component (102) which promotes thermal decomposition of the organic material (106) and contains copper as a main component in terms of the mass ratio among the transition metal elements contained therein. In the atmosphere control step (S2), the atmosphere of a space in which a mixture (107) that contains the composite material (101) and the decomposition promoting component (102) is present is controlled to be a gas (103) that contains oxygen. In the heating step (S3), the composite material (101) and the decomposition promoting component (102) are heated in an oxidizing atmosphere in a state in which the composite material (101) and the decomposition promoting component (102) are in contact with each other.
Need to check novelty before this filing date? Find Prior Art

Description

Inorganic material manufacturing method, inorganic material manufacturing device, and structure

[0001] The present disclosure relates to a method for manufacturing an inorganic material, an apparatus for manufacturing an inorganic material, and a structure.

[0002] In response to environmental regulations and energy conservation efforts, efforts are being made to reduce the weight of aircraft, railway vehicles, automobiles, and other vehicles. In particular, composite materials, such as fiber-reinforced resins containing inorganic materials such as inorganic fibers and fillers, are being used in structural components to reduce weight and improve rigidity. However, composite materials contain multiple materials, and there is a need to separate the inorganic materials for recycling composite materials.

[0003] The abstract of Patent Document 1 states that "when producing fuel from a treatment object containing a polymeric organic substance, the method includes a step of contacting the treatment object with a catalyst containing an oxide semiconductor and a transition metal element, and a step of heating the treatment object that has been contacted with the catalyst containing the oxide semiconductor and the transition metal element in an atmosphere containing hydrogen and oxygen."

[0004] Japanese Patent Application Laid-Open No. 2022-55446

[0005] Paragraph 0033 of Patent Document 1 describes that combining an oxide semiconductor with a transition metal element promotes the oxidative decomposition reaction, thereby enabling a reduction in the treatment temperature. Details will be described later with reference to the Examples, but the inventors' investigations have revealed that when a decomposition-promoting component that promotes the thermal decomposition of an organic material contains copper as a main component by mass among the transition metal elements contained therein, the thermal decomposition temperature can be reduced compared to when other transition metal elements are used. The problem to be solved by the present disclosure is to provide a method for producing an inorganic material, an apparatus for producing an inorganic material, and a structure that can be thermally decomposed at lower temperatures than conventional methods.

[0006] The method for producing an inorganic material according to the present disclosure includes a heating step of heating in an oxidizing atmosphere a composite material containing an organic material composed of an organic substance and an inorganic material composed of an inorganic substance in contact with a decomposition-promoting component that promotes thermal decomposition of the organic material and contains copper as a main component by mass of the transition metal elements contained in the composite material. Other solutions will be described later in the description of the preferred embodiments of the present invention.

[0007] According to the present disclosure, it is possible to provide a method for producing an inorganic material that can be thermally decomposed at a lower temperature than conventional methods, an apparatus for producing an inorganic material, and a structure.

[0008] FIG. 1 is a flowchart showing a method for manufacturing an inorganic material according to the present disclosure. FIG. 2 is a flowchart showing a method for manufacturing an inorganic material according to another embodiment. FIG. 3 is a flowchart showing a method for manufacturing an inorganic material according to another embodiment. FIG. 4 is a perspective view showing a see-through inside of an apparatus for manufacturing an inorganic material according to the present disclosure. FIG. 5 is a perspective view showing a see-through inside of an apparatus for manufacturing an inorganic material according to another embodiment. FIG. 6 is a perspective view of a structure according to the present disclosure. FIG. 7 is a perspective view of a structure according to another embodiment. FIG. 8 is a graph showing the decomposition behavior of each decomposition-accelerating component. FIG. 9 is a graph showing the decomposition behavior of each decomposition-accelerating component according to another example.

[0009] Hereinafter, modes for carrying out the present disclosure (hereinafter referred to as "embodiments") will be described with reference to the drawings. In the following description of one embodiment, other embodiments applicable to the one embodiment will also be described as appropriate. The present disclosure is not limited to the one embodiment described below, and different embodiments can be combined with each other or modified as desired without significantly impairing the effects of the present disclosure. Furthermore, the same components will be given the same reference numerals, and duplicate descriptions will be omitted. Furthermore, components having the same functions will be given the same names. The contents shown are merely schematic, and for convenience of illustration, changes may be made from the actual configuration within the scope of not significantly impairing the effects of the present disclosure, and some components may be omitted or modified between drawings. Furthermore, the same embodiment does not necessarily have to include all of the configurations.

[0010] 1 is a flowchart showing a method for manufacturing an inorganic material 105 according to the present disclosure (hereinafter, simply referred to as the "manufacturing method according to the present disclosure" as appropriate). The manufacturing method shown in FIG. 1 can be performed, for example, by a manufacturing apparatus 200 shown in FIG. 4, which will be described later.

[0011] The manufacturing method of the present disclosure is a method for manufacturing an inorganic material 105 from a composite material 101 containing an inorganic material 105 and an organic material 106. As the composite material 101, for example, so-called "waste plastics" obtained from waste products such as home appliances (washing machines, dryers, refrigerators, vacuum cleaners, hot water heaters, etc.), aircraft, railway vehicles, automobiles, and industrial products can be used. Therefore, the manufacturing method of the present disclosure can also be said to be a method for recycling the composite material 101 and the inorganic material 105. The manufactured inorganic material 105 can be reused, for example, as a recycled material, as part of a new composite material 101.

[0012] The inorganic material 105 in the composite material 101 from which the inorganic material 105 is separated (recovered) may be a virgin material or a recycled material. The recycled material may be, for example, an inorganic material 105 manufactured by the manufacturing method of the present disclosure. Hereinafter, when simply referring to the "inorganic material 105," the inorganic material 105 may be either a virgin material or a recycled material unless otherwise specified.

[0013] In the manufacturing method of the present disclosure, the organic material 106 in the composite material 101 is thermally decomposed at a lower temperature than conventional methods (for example, 440°C or lower, preferably 400°C or lower). In the present disclosure, the thermal decomposition (thermal decomposition reaction) of the organic material 106 is carried out in an oxidizing atmosphere, and therefore can also be considered oxidative decomposition. By performing the thermal decomposition at a lower temperature than conventional methods, thermal degradation of the inorganic material 105 contained together with the organic material 106 can be suppressed, and changes in the physical properties of the inorganic material 105, such as a decrease in strength, can be suppressed. This makes it possible to produce a new composite material 101 whose physical properties are comparable to those of a composite material 101 using virgin inorganic material 105.

[0014] The inorganic material 105 contained in the composite material 101 is composed of an inorganic substance. Examples of inorganic substances include inorganic fibers, inorganic fillers, and metals. Examples of inorganic fibers include glass fibers, asbestos fibers, carbon fibers, silica fibers, silica-alumina fibers, alumina fibers, zirconia fibers, potassium titanate fibers, Tyranno fibers, silicon carbide fibers, and metal fibers. These fibers can be used alone or in combination of two or more. These fibers are used in the form of continuous fibers, long fibers, short fibers, chopped fibers, and the like, and in the form of unidirectional materials, plain weaves, nonwoven fabrics, and the like. However, the fiber shape or state is not limited to these fiber shapes or states.

[0015] Examples of inorganic fillers include powders of fused silica, crystalline silica, alumina, zircon, calcium silicate, calcium carbonate, potassium titanate, silicon carbide, aluminum nitride, boron nitride, beryllia, zircon, fosterite, stearite, spirel, mullite, titania, etc., as well as beads obtained by spheroidizing these. There are no limitations on the shape of the inorganic filler, and any shape, such as spherical or flaky, may be used.

[0016] Examples of metals contained in the inorganic material 105 include steel, aluminum, aluminum alloys, magnesium alloys, titanium alloys, etc. There is no limitation on the shape of the metal, and any shape such as plate, sphere, or flake may be used.

[0017] Of these, the inorganic material preferably includes at least one of carbon fiber and glass fiber. These are often used to improve the strength of the composite material 101, for example. For this reason, the composite material 101 has high strength, but due to this high strength, it is difficult to remove (separate) the inorganic material 105 from the composite material 101, for example, by crushing the composite material 101. However, according to the manufacturing method of the present disclosure, as described above, the thermal decomposition temperature of the organic material 106 can be lowered compared to conventional methods. Therefore, the organic material 106 can be easily thermally decomposed, and the inorganic material 105 can be removed (manufactured) from the composite material 101.

[0018] The organic material 106 is made of an organic substance, and the organic substance includes, for example, a resin such as a thermosetting resin or a thermoplastic resin. Examples of thermosetting resins include epoxy resin, phenolic resin, urea resin, melamine resin, unsaturated polyester resin, silicone resin, polyimide resin, bismaleimide resin, and thermosetting urethane resin. Examples of thermoplastic resins include polyethylene, polypropylene, polystyrene, acrylonitrile butadiene styrene, polyvinyl chloride, methacrylic resin, polyethylene terephthalate, polybutylene terephthalate, polyvinyl alcohol, polyamide, and polycarbonate. One type of resin may be used alone, or two or more types may be used in any desired ratio.

[0019] Among these, it is preferable that the organic material contains a thermosetting resin. Because a thermosetting resin hardens when heated, it is difficult to melt the organic material 106, and it is difficult to separate the inorganic material 105 contained together with the organic material 106 from the organic material 106. However, according to the manufacturing method of the present disclosure, the thermal decomposition temperature of the organic material 106 can be lowered compared to conventional methods, so that the organic material 106 can be easily thermally decomposed and the inorganic material 105 can be extracted (manufactured) from the composite material 101.

[0020] The composite material 101 may contain additives such as flame retardants, antioxidants, light stabilizers, dispersants, lubricants, plasticizers, antistatic agents, pigments, and dyes, as needed.

[0021] The manufacturing method of the present disclosure includes a contacting step S1, an atmosphere controlling step S2, and a heating step S3. The contacting step S1 is a step of contacting a composite material 101 with a decomposition-promoting component 102. In the present disclosure, mixing is exemplified as an example of contact. Accordingly, contact between the composite material 101 and the decomposition-promoting component 102 produces a mixture 107 containing the composite material 101 and the decomposition-promoting component 102. Note that "mixing" does not necessarily mean mixing to the extent that the composite material 101 and the decomposition-promoting component 102 are completely and uniformly mixed as a whole; for example, the composite material 101 and the decomposition-promoting component 102 may coexist in the same reaction vessel 1 ( FIG. 4 ).

[0022] The manner of contact is not particularly limited. For example, the composite material 101 crushed into rods having a length of approximately 1 mm to 10 mm can be mixed with the decomposition-promoting component 102 in powder form (for example, a particle size of 10 μm to 500 μm as determined by a laser diffraction scattering method). The mixing can be carried out, for example, by placing the composite material 101 and the decomposition-promoting component 102 in the reaction vessel 1 (FIG. 4; a container or the like). Alternatively, the decomposition-promoting component 102 may be attached to a structure such as the wall surface of the reaction vessel 1 or the stirring mechanism 5 (FIG. 4), and the composite material 101 may be brought into contact with the attached decomposition-promoting component 102.

[0023] The decomposition-promoting component 102 promotes the thermal decomposition of the organic material 106, and contains copper as the main component (preferably more than 50 mass%, more preferably 100 mass%) by mass ratio among the transition metal elements contained in the decomposition-promoting component 102. The decomposition-promoting component 102 includes components that do not change during the thermal decomposition of the organic material 106 (e.g., copper (II) oxide, etc.) and components that change during the thermal decomposition of the organic material 106 (e.g., copper (I) oxide, organic copper, etc.). Of these, the decomposition-promoting component 102 that does not change during the thermal decomposition can be referred to as, for example, a "catalyst."

[0024] The decomposition-promoting component 102 contains copper. The copper referred to here may be either elemental copper or a copper compound. When the decomposition-promoting component 102 contains copper, heating it in an oxidizing atmosphere oxidizes the copper in the decomposition-promoting component 102, generating copper (II) oxide. However, when the decomposition-promoting component 102 contains the above-described copper (II) oxide, the copper (II) oxide originally contained therein typically remains unchanged. Heating the copper (II) oxide causes thermal excitation within the copper (II) oxide, generating holes and electrons. The holes, due to their oxidizing power, steal electrons from organic matter surrounding the copper (II) oxide, thereby oxidizing and decomposing the organic matter. Additionally, the electrons generated by the thermal excitation transfer to oxygen in the atmosphere, generating active oxygen. Active oxygen promotes the oxidative decomposition of organic matter, which also contributes to the oxidative decomposition of the organic matter.

[0025] It has been found that by using a decomposition-promoting component 102 capable of producing primarily copper(II) oxide during thermal decomposition among various oxides, thermal decomposition can be carried out at low temperatures (for example, 440°C or less, preferably 400°C or less). Unlike other oxides, the mechanism by which copper(II) oxide can oxidatively decompose organic matter at low temperatures is not entirely clear. However, according to the inventor's investigations, this is thought to be due to the high activity (reactivity) of copper(II) oxide, the valence of copper contained in copper(II) oxide, the ease with which holes and electrons are generated in copper(II) oxide, and other factors. Note that this mechanism is merely speculative and is not limited to this content, and other reasons may also be possible.

[0026] As described above, the decomposition-accelerating component 102 contains copper as a main component. The term "main component" as used herein means that the component that is the largest in mass ratio among the transition metal elements contained in the decomposition-accelerating component 102 (for example, when there are two types of transition metal elements, copper is more than 50 mass%). The decomposition-accelerating component 102 preferably contains at least one of copper alone or a compound containing copper as a main component (hereinafter referred to as a copper compound). As the copper compound, for example, copper oxide, an organic copper compound, a copper alloy, etc. can be obtained. As the copper oxide, copper (I) oxide (Cu 2 Examples of the copper compound include copper(II) acetate (CuO), copper(II) oxide (CuO), and the like. Examples of the organic copper compound include copper(II) acetate and copper acetylacetonate(II). Only one copper compound may be used, or two or more copper compounds may be used in any desired ratio and proportion.

[0027] In particular, it is preferable that the decomposition-accelerating component 102 contains elemental copper. This allows the entire elemental copper to be oxidized to copper (II) oxide, thereby increasing the amount of copper (II) oxide involved in the thermal decomposition of the organic material 106. As a result, the amount of organic material 106 to be thermally decomposed can be increased, and the processing efficiency of the composite material 101 can be improved.

[0028] The decomposition-accelerating component 102 preferably contains at least one of copper (I) oxide and copper (II) oxide. Because copper is easily naturally oxidized by oxygen, even copper oxide that can be naturally oxidized, such as copper (II) oxide, can be used as the decomposition-accelerating component.

[0029] Furthermore, it is preferable that the decomposition-accelerating component 102 contains an organic copper compound. The organic copper compound has a carbon skeleton and therefore has excellent affinity with the organic material 106. Therefore, the organic copper compound can easily act on the organic material 106 and can easily accelerate the thermal decomposition of the organic material 106.

[0030] The decomposition-promoting component 102 preferably does not contain any oxide semiconductor (except copper oxide). Copper oxide here refers to copper (II) oxide and copper (I) oxide. Copper oxide is an oxide semiconductor, and by using copper oxide among oxide semiconductors, the organic material 106 can be thermally decomposed at a lower temperature than when other oxide semiconductors are used. Therefore, by not containing any oxide semiconductors other than copper oxide, the organic material 106 can be thermally decomposed at a lower temperature. However, although it is preferable not to contain any oxide semiconductors other than copper oxide, oxide semiconductors other than copper oxide may be contained as a supplementary component.

[0031] Specifically, the decomposition-promoting component 102 may supplementarily contain at least one of a compound that is a thermally stable oxide semiconductor and a compound that produces a thermally stable oxide semiconductor when heated with the organic material 106. Examples of such compounds include CaO, MnO, and ZrO. 2 , W.O. 2 , TiO 2 , V 2 O 5 , Cr 2 O 3 , NiO, Fe 2 O 3 , Fe 3 O 4 , ZnO, CoO, Co 3 O 4 At least one of the following may be mentioned.

[0032] It is preferable that the decomposition-promoting component 102 does not contain any transition metal elements (except copper). By using copper among the transition metals, copper oxide (II) can be generated when heated in an oxidizing atmosphere. As described above, copper oxide (II) allows the organic material 106 to be thermally decomposed at a lower temperature than when other transition metal elements are used. Therefore, by not including any transition metal elements other than copper, the organic material 106 can be thermally decomposed at a lower temperature. However, although it is preferable that the component does not contain any transition metal elements other than copper, it may contain transition metal elements other than copper as a supplementary component.

[0033] The content of decomposition-accelerating component 102 relative to organic material 106 is preferably 50% by mass or more. By using an amount of decomposition-accelerating component 102 within this range, organic material 106 can be thermally decomposed. However, the content of decomposition-accelerating component 102 can also be adjusted as appropriate depending on the shapes of organic material 106 and decomposition-accelerating component 102, etc. There is no particular upper limit to the content, and it may be determined as appropriate depending on the production cost of inorganic material 105, the internal volume of reaction tank 1 ( FIG. 4 ), etc.

[0034] The decomposition-accelerating component 102 preferably has a particulate shape (for example, powder shape). Such a shape increases the contact area with the organic material 106, and can accelerate the thermal decomposition of the organic material 106 that occurs at the contact area between the decomposition-accelerating component 102 and the organic material 106.

[0035] The atmosphere control step S2 ( FIG. 1 ) is a step of controlling the atmosphere at the contact portion where the composite material 101 and the decomposition-promoting component 102 are brought into contact. In the example of the present disclosure, for example, the atmosphere of the space in which the mixture 107 obtained in the contact step S1 exists (the atmosphere of the internal space of the reaction vessel 1 ( FIG. 4 )) is controlled. In the atmosphere control step S2, the atmosphere of the space in which the mixture 107 is placed is controlled to be a gas 103 containing oxygen. That is, the mixture 107 exists in the gas 103. The gas 103 is, for example, air, oxygen gas, etc.

[0036] Note that the atmosphere control step S2 does not have to be included when at least one of the composite material 101 and the decomposition-promoting component 102 contains a component that generates oxygen during the heating step S3. If the atmosphere control step S2 is not included, copper in the decomposition-promoting component 102 is oxidized by oxygen generated from at least one of the composite material 101 and the decomposition-promoting component 102 during the heating step S3. As a result, the heating step S3 is performed in which the composite material 101 and the decomposition-promoting component 102 are heated in an oxidizing atmosphere while in contact with each other.

[0037] The heating step S3 is a step of heating the composite material 101 and the decomposition-promoting component 102 in an oxidizing atmosphere while they are in contact with each other. In the example of the present disclosure, the heating step S3 is a step of heating the mixture 107 present in the gas 103.

[0038] The heating step S3 is performed by heating at a temperature that thermally decomposes the organic material 106. By heating at this temperature, the organic material 106 can be thermally decomposed.

[0039] However, the heating step S3 is preferably carried out by heating at a temperature that thermally decomposes the organic material 106, for example, 440° C. or lower, preferably 420° C. or lower, and more preferably 400° C. or lower. For example, heating at 440° C. or lower, preferably 420° C. or lower, and more preferably 400° C. or lower can suppress thermal degradation of the inorganic material 105, which has a significant impact when the recycled inorganic material 105 is reused. Furthermore, the heating step S3 is preferably carried out by heating at a temperature, for example, 200° C. or higher, preferably 250° C. or higher, more preferably 300° C. or higher, and particularly preferably 350° C. or higher.

[0040] The heating time in the heating step S3 is not particularly limited, but may be, for example, 5 minutes to 1 hour.

[0041] The solid organic material 106 is converted into exhaust gas 104 by thermal decomposition of the organic material 106. The exhaust gas 104 contains, for example, carbon dioxide and is appropriately discharged to the outside. Meanwhile, the inorganic material 105 contained in the composite material 101 remains in the reaction vessel 1 (FIG. 4). Therefore, the inorganic material 105 can be extracted from the reaction vessel 1.

[0042] The heating step S3 is preferably performed while the composite material 101 and the decomposition-promoting component 102 are in contact (e.g., mixed) with each other and while at least one of the composite material 101 and the decomposition-promoting component 102 is subjected to at least one of vibration and stirring. By performing the heating step S3 in this manner, the contact opportunity between the composite material 101 and the decomposition-promoting component 102 is increased, compared to when the heating step S3 is performed while the composite material 101 is left stationary, and the thermal decomposition of the organic material 106 can be promoted.

[0043] The heating step S3 is preferably carried out using the reaction vessel 1 (FIG. 4) used in the contacting step S1. By carrying out the contacting step S1 and the heating step S3 using the same reaction vessel 1, the thermal decomposition of the organic material 106 can be carried out continuously.

[0044] Fig. 2 is a flowchart showing a method for producing an inorganic material 105 according to another embodiment. In the embodiment shown in Fig. 2, unlike the embodiment shown in Fig. 1, the contacting step S1 is performed after the atmosphere controlling step S2. Specifically, for example, the atmosphere in the internal space of the reaction vessel 1 (Fig. 4) in which the decomposition-promoting component 102 is placed is composed of an oxygen-containing gas 103 (atmosphere controlling step S2). Therefore, the decomposition-promoting component 102 is present in the gas 103. Then, by further placing the composite material 101 in the reaction vessel 1 in this state, the atmosphere of the mixture 107 is composed of the gas 103 (contacting step S1).

[0045] The embodiment shown in FIG. 2 also makes it possible to oxidatively decompose the organic material 106 at a lower temperature than conventional methods.

[0046] FIG. 3 is a flowchart showing a method for producing an inorganic material 105 according to another embodiment. In the embodiment shown in FIG. 3, the heating step S3 in the embodiment shown in FIG. 2 includes a preheating step S31 and a main heating step S32. After the atmosphere control step S2, the preheating step S31, which is part of the heating step S3, is performed. The preheating step S31 is a step of raising the temperature of the decomposition-promoting component 102 to the heating temperature in the main heating step S32 described below. After the temperature of the decomposition-promoting component 102 is raised to the desired temperature, the composite material 101 is introduced into a reaction vessel, and a mixture 107 is produced (contact step S1). Then, the main heating step S32 is performed on the mixture 107. The main heating step S32 can be performed in the same manner as the heating step S3 described above with reference to FIG. 1, etc.

[0047] 3 also allows the organic material 106 to be oxidatively decomposed at a lower temperature than conventional methods. Furthermore, because the composite material 101 is brought into contact with the preheated decomposition-promoting component 102, it is possible to shorten the time required from bringing the composite material 101 into contact with the decomposition-promoting component 102 until the temperature reaches a temperature at which the composite material 101 can be thermally decomposed. This shortens the processing time for the composite material 101.

[0048] FIG. 4 is a perspective view showing the inside of a manufacturing apparatus 200 for the inorganic material 105 ( FIG. 1 ) of the present disclosure. The manufacturing apparatus 200 includes a reaction tank 1, a heating mechanism 2, an air inlet 3, an exhaust port 4, and a stirring mechanism 5. The reaction tank 1 contains a composite material 101 and a decomposition-promoting component 102. In the example shown in FIG. 4 , the composite material 101 broken (crushed) into elongated rod shapes is embedded in the powdered decomposition-promoting component 102. The reaction tank 1 is, for example, a hollow tank. The heating mechanism 2 heats the composite material 101 and the decomposition-promoting component 102 inside the reaction tank 1. The heating mechanism 2 is provided at the bottom of the reaction tank 1 and heats the composite material 101 and the decomposition-promoting component 102 from the bottom of the reaction tank 1. The heating mechanism 2 is, for example, an electric heating wire, a boiler, or the like.

[0049] The air supply port 3 (air supply pipe) supplies oxygen-containing gas 103 into the reaction tank 1. The exhaust port 4 (exhaust pipe) exhausts gas generated inside the reaction tank 1 from the reaction tank 1 as exhaust gas 104. The gas exhausted from the exhaust port 4 includes gas (e.g., carbon dioxide, water vapor, etc.) generated by thermal decomposition of the organic material 106. By exhausting the organic material 106 from the reaction tank 1 as a gas, the inorganic material 105 remains inside the reaction tank 1, making it easier to remove the inorganic material 105. The air supply port 3 and the exhaust port 4 are provided at the top of the reaction tank 1.

[0050] The stirring mechanism 5 stirs the composite material 101 and the decomposition-promoting component 102 inside the reaction tank 1. By providing the stirring mechanism 5, the composite material 101 and the decomposition-promoting component 102 come into contact with each other more frequently than when the reaction is allowed to proceed while stationary, and this can promote the thermal decomposition of the organic material 106 that occurs at the contact points between the composite material 101 and the decomposition-promoting component 102. The stirring mechanism 5 is, for example, a stirring blade, and in the illustrated example, the stirring blade is embedded in the powdered decomposition-promoting component 102.

[0051] As described above, the composite material 101 and the decomposition-promoting component 102 come into contact with each other inside the reaction vessel 1. Then, an oxygen-containing gas 103 is supplied into the reaction vessel 1 through the air supply port 3. Furthermore, the composite material 101 and the decomposition-promoting component 102 present inside the reaction vessel 1 are heated by the heating mechanism 2. This allows the manufacturing method of the present disclosure (e.g., FIG. 1 ) to be carried out. Furthermore, exhaust gas 104 generated by the decomposition reaction is exhausted from the reaction vessel 1 through the exhaust port 4. The inorganic material 105 remaining inside the reaction vessel 1 due to the thermal decomposition of the organic material 106 can be removed, for example, through an upper opening of the reaction vessel 1 using any jig (not shown). Removal can be performed, for example, after the supply of the gas 103 and the operation of the stirring mechanism 5 have been stopped.

[0052] Fig. 5 is a perspective view showing the inside of an apparatus 200 for producing an inorganic material 105 according to another embodiment. The apparatus 200 shown in Fig. 5 further includes a recovery mechanism 6 in addition to the components of the apparatus 200 shown in Fig. 4 above. The recovery mechanism 6 recovers the inorganic material 105 obtained by thermal decomposition of the organic material 106 in the composite material 101 from inside the reaction tank 1. The provision of the recovery mechanism 6 makes it easier to recover the inorganic material 105 from inside the reaction tank 1.

[0053] In the example of the present disclosure, the recovery mechanism 6 is an outlet (extraction pipe) provided on the lower side of the reaction vessel 1. The inorganic material 105 can be recovered by separating it from the decomposition-promoting component 102 by utilizing differences in specific gravity, shape, etc. The outlet is preferably provided in a portion close to the bottom of the reaction vessel 1.

[0054] The manufacturing method of the present disclosure using the manufacturing apparatus 200 shown in Fig. 5 can be continuously performed. Specifically, for example, by the manufacturing method of the present disclosure, an inorganic material 105 is produced by thermally decomposing an organic material 106 inside a reaction vessel 1. After production, the supply of gas 103 and the driving of the stirring mechanism 5 are stopped, and the recovery mechanism 6 recovers the inorganic material 105. After recovery, an optional transport mechanism (not shown) supplies the composite material 101 and the decomposition-promoting component 102 into the reaction vessel 1 through, for example, a raw material supply port (not shown) of the reaction vessel 1. Then, the manufacturing method of the present disclosure is performed again.

[0055] Fig. 6 is a perspective view of a structure 110 according to the present disclosure. Fig. 6 illustrates a member 112 provided in the structure 110, and in the example of Fig. 6, the member 112 is a plate material. The member 112 is made of a composite material 111. The composite material 111 is a newly manufactured composite material using an inorganic material 105 manufactured by the manufacturing method shown in Fig. 1 or the like, for example.

[0056] The structure 110 is any structure such as a railway vehicle, a ship, an aircraft, an automobile, a wind power generator, a modular bath, a septic tank, a printed circuit board, a playground equipment, or skis, and the member 112 can be any member that constitutes the structure 110. For example, the member 112 can be used as a blade in a wind power generator, an underframe or window frame for a railway vehicle, a portion from which a stator winding that constitutes a motor is taken out, a portion from which a permanent magnet that constitutes a rotor is taken out, or a component of an inverter.

[0057] The member 112 includes an inorganic material 105 ( FIG. 1 ) produced by at least a heating step S3 ( FIG. 1 ) in which the composite material 101 ( FIG. 1 ) and the decomposition-promoting component 102 ( FIG. 1 ) are heated in an oxidizing atmosphere while in contact with each other. The use of such a member 112 and a structure 110 including the member 112 can reduce the amount of inorganic material 105 that is discarded. Furthermore, the strength of the member 112 including the newly produced composite material 111 is reduced to a degree that does not significantly affect the use of the composite material 111, compared to the physical properties (e.g., strength) of the composite material 111 produced using the inorganic material 105, which is a virgin material. Therefore, a member 112 and a structure 110 having desired physical properties, such as strength, can be obtained.

[0058] It should be noted that the physical properties of the virgin inorganic material 105 do not strictly match those of the inorganic material 105 obtained by the manufacturing method of the present disclosure (i.e., obtained by recycling the composite material 101). Specifically, the physical properties of the inorganic material 105 change at least slightly due to heating for pyrolysis of the organic material 106. However, the degree of change varies depending on the heating conditions, such as the conditions during pyrolysis (e.g., heating temperature and heating time) and the shape of the composite material 101 during recycling. Therefore, it is impossible or impractical to quantitatively evaluate the physical properties of the inorganic material 105 obtained by recycling the composite material 101. Therefore, in the example of the present disclosure, the characteristics of the structure 110 are specified by the manufacturing method of the structure 110.

[0059] Furthermore, when looking at the structure 110, whether the structure 110 was manufactured using the inorganic material 105, which is a virgin material, or the inorganic material 105 obtained by recycling the composite material 101 can be determined by evaluating the physical properties (e.g., mechanical strength) of the inorganic material 105. That is, if the evaluated mechanical strength is the same (or approximately the same) as the mechanical strength of the virgin material, the structure 110 can be said to have been manufactured using the inorganic material 105, which is a virgin material. On the other hand, if the evaluated mechanical strength is lower than the mechanical strength of the virgin material, but does not have a significant impact on the use of the structure 110, the structure 110 can be said to have been manufactured using the inorganic material 105 obtained by recycling the composite material 101.

[0060] 7 is a perspective view of a structure 120 according to another embodiment. The structure 120 includes a member 122. The member 122 is configured from a composition 121 including the composite material 101 ( FIG. 1 ) and a decomposition-accelerating component 102 ( FIG. 1 ). The decomposition-accelerating component 102 is present, for example, in the organic material 106 in the composite material 101. Therefore, for example, the inorganic material 105 and the decomposition-accelerating component 102 are dispersed in the organic material 106.

[0061] 7, the inorganic material 105 can be separated by directly subjecting the used structure 120 to the heating step S3. This eliminates the need for the contact step S1 (FIG. 1), making it possible to easily recycle the structure 120.

[0062] The present disclosure will be described more specifically below with reference to examples.

[0063] Example 1 A glass fiber reinforced plastic (GFRP) was produced as composite material 101 (FIG. 1) using a bisphenol A diglycidyl ether type thermosetting epoxy resin as organic material 106 (FIG. 1) and glass fiber as inorganic material 105 (FIG. 1). The content of inorganic material 105 in composite material 101 was set to 50 mass%. Therefore, the content of organic material 106 in composite material 101 was also 50 mass%. Composite material 101 was broken into chips measuring approximately 5 mm in length, 2 mm in width, and 0.2 mm in thickness.

[0064] Copper (II) oxide (CuO) was prepared as the decomposition-promoting component 102 ( FIG. 1 ). The copper (II) oxide had an average particle size (D50) of 100 μm as measured by a laser diffraction particle size distribution analyzer. The chip-shaped composite material 101 and the decomposition-promoting component 102 were mixed (contact step S1) to obtain a mixture 107. The content of the decomposition-promoting component 102 in the mixture 107 was set to 50% by mass. Therefore, the content of the composite material 101 in the mixture 107 was also 50% by mass. Therefore, the content of the decomposition-promoting component 102 relative to the organic material 106 in the composite material 101 was 200% by mass.

[0065] The decomposition behavior of the organic material 106 was analyzed using the mixture 107. The analysis was performed using a thermal mass reduction device. The analysis conditions (decomposition conditions for the organic material 106) were that the temperature was increased from room temperature to 700°C at 10°C / min. Here, the temperature at which the mass of the organic material 106 was reduced to 5% (i.e., almost no organic material 106 remained) was defined as the decomposition temperature, and samples with a decomposition temperature of 440°C or less were evaluated as being capable of being decomposed at low temperatures. As a result of the analysis, the decomposition temperature was 362°C, confirming that the organic material 106 could be decomposed at 440°C or less.

[0066] Example 2: Copper (I) oxide (Cu) was used instead of copper (II) oxide. 2 The decomposition temperature was analyzed in the same manner as in Example 1 except that the decomposition temperature was 372°C.

[0067] Example 3 The decomposition temperature was analyzed in the same manner as in Example 1, except that copper (Cu) was used instead of copper (II) oxide. As a result, the decomposition temperature was 377°C.

[0068] Example 4: Copper (II) acetylacetonate (Cu(C) 5 H 7 O 2 ) 2 The decomposition temperature was analyzed in the same manner as in Example 1, except that the decomposition temperature was 392°C.

[0069] Example 5: Instead of copper (II) oxide, copper (II) oxide and titanium oxide (TiO 2 The decomposition temperature was analyzed in the same manner as in Example 1, except that a mixture of 1,000 sachets and 1,000 sachets in a mass ratio of 55:45 was used. The decomposition temperature was found to be 377°C.

[0070] Example 6 The decomposition temperature was analyzed in the same manner as in Example 5, except that the mass ratio of copper (II) oxide to titanium oxide was changed to 75:25. As a result, the decomposition temperature was 376°C.

[0071] Example 7 The decomposition temperature was analyzed in the same manner as in Example 5, except that cobalt oxide (CoO) was used instead of titanium oxide. As a result, the decomposition temperature was 363°C.

[0072] Example 8 The decomposition temperature was analyzed in the same manner as in Example 7, except that the mass ratio of copper (II) oxide to cobalt oxide was changed to 75:25. As a result, the decomposition temperature was 356°C.

[0073] Example 9 Except for using carbon fiber instead of glass fiber, the decomposition temperature was analyzed in the same manner as in Example 1. As a result, the decomposition temperature was 364°C.

[0074] Example 10 The decomposition temperature was analyzed in the same manner as in Example 1, except that an unsaturated polyester resin, which is a thermosetting resin, was used instead of the bisphenol A diglycidyl ether type epoxy resin. As a result, the decomposition temperature was 366°C.

[0075] Example 11 The decomposition temperature was analyzed in the same manner as in Example 1, except that the content of the decomposition-accelerating component 102 in the mixture 107 was changed from 50% by mass to 20% by mass. Therefore, the content of the decomposition-accelerating component 102 relative to the organic material 106 in the composite material 101 was 50% by mass. As a result, the decomposition temperature was 381°C.

[0076] Example 12 The decomposition temperature was analyzed in the same manner as in Example 1, except that the content of the decomposition-accelerating component 102 in the mixture 107 was changed from 50% by mass to 80% by mass. Therefore, the content of the decomposition-accelerating component 102 relative to the organic material 106 in the composite material 101 was 800% by mass. As a result, the decomposition temperature was 377°C.

[0077] Example 13 The decomposition temperature was analyzed in the same manner as in Example 1, except that the content of the decomposition-accelerating component 102 in the mixture 107 was changed from 50% by mass to 4.8% by mass. Therefore, the content of the decomposition-accelerating component 102 relative to the organic material 106 in the composite material 101 was 10% by mass. As a result, the decomposition temperature was 412°C.

[0078] In Example 13, the decomposition temperature exceeded 400°C, but this was lower than the decomposition temperatures in Comparative Examples 1 to 7, which illustrate the prior art described below. Therefore, by using the decomposition-promoting component 10, the decomposition temperature can be lowered compared to conventional methods. However, it was found that in order to further lower the decomposition temperature, the content of the decomposition-promoting component 102 relative to the organic material 106 in the composite material 101 is preferably 50% by mass or more (Examples 1 to 12).

[0079] Comparative Example 1 Except for using titanium oxide instead of copper (II) oxide, the decomposition temperature was analyzed in the same manner as in Example 1. As a result, the decomposition temperature was 505°C.

[0080] Comparative Example 2: Dichromate (Cr) was used instead of copper (II) oxide. 2 O 3 The decomposition temperature was analyzed in the same manner as in Example 1, except that the decomposition temperature was 495°C.

[0081] Comparative Example 3: Zinc oxide (ZnO) was used instead of copper (II) oxide. 2The decomposition temperature was analyzed in the same manner as in Example 1, except that the decomposition temperature was 492°C.

[0082] Comparative Example 4 The decomposition temperature was analyzed in the same manner as in Example 1, except that nickel oxide (NiO) was used instead of copper (II) oxide. As a result, the decomposition temperature was 514°C.

[0083] Comparative Example 5 The decomposition temperature was analyzed in the same manner as in Example 5, except that the mass ratio of copper (II) oxide to titanium oxide was changed to 25:75. As a result, the decomposition temperature was 445°C.

[0084] Comparative Example 6 The decomposition temperature was analyzed in the same manner as in Example 1, except that copper-supported titanium oxide was used instead of copper (II) oxide. In the copper-supported titanium oxide, the transition metal element that is the main component in terms of mass ratio among the transition metal elements contained therein is titanium. As a result of the analysis, the decomposition temperature was 456°C.

[0085] Comparative Example 7 The decomposition temperature was analyzed in the same manner as in Example 1, except that iron-supported titanium oxide was used instead of copper (II) oxide. In the iron-supported titanium oxide, the transition metal element that was the main component in terms of mass ratio among the transition metal elements contained therein was titanium. As a result of the analysis, the decomposition temperature was 500°C.

[0086] <Summary> From the above results, it was confirmed that according to the present disclosure, the decomposition temperature can be reduced to, for example, 440° C. or less, and the decomposition temperature can be particularly lowered compared to when a transition metal element other than copper is used as the main component.

[0087] <Difference in decomposition behavior due to difference in transition metal element> The same thermosetting resin was used except for various changes in the metal oxide, and the content of the thermosetting resin and the metal oxide was set to a mass ratio of 1:1, and the decomposition behavior was analyzed in the same manner as in Example 1.

[0088] FIG. 8 is a graph showing the decomposition behavior of each decomposition-promoting component 102. The graph in FIG. 8 illustrates the difference in decomposition temperature due to differences in the transition metal element of the main component contained in the decomposition-promoting component 102. The transition metal elements used were chromium (dotted line), nickel (dashed line), titanium (dashed line divided more finely than the dashed line representing nickel), zinc (dashed line), and copper (II) (dashed line). Of these, copper (II) is an example, while chromium, nickel, titanium, and zinc are all comparative examples. All transition metal elements are contained in the resin in the form of oxides. The vertical axis represents mass, and the horizontal axis represents temperature. The vertical axis represents a relative ratio, with the mass at the start of heating being 100%. FIG. 8 shows the change in mass loss when a sample is heated in the thermal mass reduction device used in Example 1. For reference, the "resin" indicated by the solid line is a reference example that does not contain the decomposition-promoting component 102. This point is also true for FIG. 9, which will be described later.

[0089] In all examples, a mass loss was observed as the sample was heated. This indicates that the organic material 106 was thermally decomposed as the sample was heated. In particular, for oxides other than copper (II) oxide (comparative examples), the mass decreased gradually as the temperature increased. When copper (II) oxide (example) was used, the mass rapidly decreased, reaching nearly 0%, when the sample was heated to approximately 350°C. This result indicates that the thermal decomposition of the organic material 106 rapidly progressed at a specific temperature (approximately 350°C). The reason for this is not necessarily clear and is not limited to this particular reason, but the inventors' investigations suggest that the thermal decomposition proceeded in a chain reaction. Therefore, it can be seen that the use of copper (II) oxide can accelerate the thermal decomposition of the organic material 106, resulting in thermal decomposition at a lower temperature than other metals.

[0090] FIG. 9 is a graph showing the decomposition behavior of each decomposition-promoting component 102 according to another example. The mass loss change was analyzed under the same conditions as in FIG. 8 , except that the decomposition-promoting component 102 was different. The decomposition-promoting components 102 were titanium oxide (thin dotted line), copper-supported titanium oxide (thick dashed line), iron-supported titanium oxide (dashed line), copper (thin dashed line), copper(I) oxide (thick dotted line), and copper(II) oxide (dash-dotted line). As described above, in both copper-supported titanium oxide and iron-supported titanium oxide, titanium is the predominant transition metal element by mass. Therefore, of these, copper (I) oxide and copper(II) oxide are examples, while titanium oxide, copper-supported titanium oxide, and iron-supported titanium oxide are comparative examples.

[0091] When the decomposition-promoting component 102 contains copper as the main component, i.e., copper elemental (thin dashed line), copper (I) oxide (thick dotted line), or copper (II) oxide (double-dashed line), the mass was nearly 0% at 400°C or below. In particular, when copper oxide, i.e., copper (I) oxide or copper (II) oxide, was used, the mass rapidly decreased at about 350°C, as described above in FIG. 8 . Some composites 101 may be used at relatively high temperatures. Therefore, by using a decomposition-promoting component 102 that undergoes a gradual change in mass until the temperature reaches a certain high temperature and then rapidly decreases in mass at a specific temperature, the degree of mass loss can be kept small even when the composite 101 is used at a relatively high temperature (but below the specific temperature).

[0092] REFERENCE SIGNS LIST 1 Reaction tank 101 Composite material 102 Decomposition-promoting component 103 Gas 104 Exhaust gas 105 Inorganic material 106 Organic material 107 Mixture 110 Structure 111 Composite material 112 Member 120 Structure 122 Member 2 Heating mechanism 200 Manufacturing apparatus 3 Air supply port 4 Exhaust port 5 Stirring mechanism 6 Recovery mechanism S1 Contact step S2 Atmosphere control step S3 Heating step S31 Preheating step S32 Main heating step

Claims

1. A method for producing an inorganic material, comprising: a heating step of heating in an oxidizing atmosphere a composite material containing an organic material composed of an organic substance and an inorganic material composed of an inorganic substance in contact with a decomposition-promoting component that promotes thermal decomposition of the organic material and contains copper as a main component by mass among the transition metal elements contained therein.

2. The method for producing an inorganic material according to claim 1, characterized in that the inorganic matter contains at least one of carbon fiber and glass fiber.

3. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component contains copper as an elemental element.

4. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component contains at least one of copper oxide (I) and copper oxide (II).

5. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component contains an organic copper compound.

6. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component has a particulate shape.

7. The method for producing an inorganic material according to claim 1, characterized in that the organic matter contains a thermosetting resin.

8. The method for producing an inorganic material according to claim 1, characterized in that the heating step is carried out by heating at a temperature at which the organic material is thermally decomposed.

9. The method for producing an inorganic material according to claim 8, characterized in that the heating step is carried out at a temperature of 400°C or less.

10. The method for producing an inorganic material as described in claim 1, characterized in that the heating step is carried out while the composite material and the decomposition-promoting component are in contact with each other and at least one of the composite material and the decomposition-promoting component is subjected to at least one of vibration and stirring.

11. The method for producing an inorganic material according to claim 1, characterized in that it includes a contacting step of contacting the composite material with the decomposition-promoting component, and the heating step is carried out using the reaction vessel used in the contacting step.

12. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component does not contain an oxide semiconductor (except for copper oxide).

13. The method for producing an inorganic material according to claim 1, characterized in that the decomposition-promoting component does not contain any transition metal elements (except copper).

14. The method for producing an inorganic material according to claim 1, characterized in that the content of the decomposition-promoting component relative to the organic material is 50 mass % or more.

15. An apparatus for manufacturing an inorganic material, comprising: a reaction vessel for accommodating a composite material comprising an organic material composed of an organic substance and an inorganic material composed of an inorganic substance; a decomposition-promoting component that promotes the thermal decomposition of the organic material and contains copper as a main component by mass among the transition metal elements contained therein; a heating mechanism for heating the composite material and the decomposition-promoting component inside the reaction vessel; an air supply port for supplying a gas containing oxygen into the inside of the reaction vessel; and an exhaust port for exhausting gas generated inside the reaction vessel from the reaction vessel.

16. The inorganic material manufacturing apparatus according to claim 15, further comprising a stirring mechanism for stirring the composite material and the decomposition-promoting component inside the reaction tank.

17. The inorganic material manufacturing apparatus according to claim 15, further comprising a recovery mechanism for recovering the inorganic material obtained by thermal decomposition of the organic material in the composite material from inside the reaction tank.

18. The inorganic material manufacturing apparatus according to claim 15, characterized in that the gas exhausted from the exhaust port includes a gas generated by thermal decomposition of the organic material.

19. A structure comprising a member containing the inorganic material manufactured by at least a heating process of heating the composite material in an oxidizing atmosphere while in contact with a decomposition-promoting component that promotes thermal decomposition of the organic material and contains copper as a main component by mass among the transition metal elements contained therein.

Citation Information

Patent Citations

  • Production of fine powdery copper oxide

    JP1990196021A

  • Method and equipment for obtaining hydrocarbon oil from waste plastic or rubber material

    JP1994228568A

  • Incineration method for suppressing production of dioxins and catalyst for incineration

    JP2003329223A

  • Etching treatment method for copper and wiring board and semiconductor package obtained by using the method

    JP2008088541A

  • Method of dispersing layered copper compound and dispersion liquid therewith

    JP2011144090A