The combination of a porous carbon heating element and a porous ceramic body in a laminated sheet form addresses inefficiencies in conventional heaters by enhancing heat transfer and temperature regulation, enabling efficient and rapid temperature changes with improved structural integrity and oxidation resistance.

WO2024247423A1PCT designated stage expired Publication Date: 2024-12-05TOMOEGAWA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008310
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-03-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional heaters face inefficiencies in temperature regulation and heat transfer, particularly in sheet-like designs where heat transfer becomes anisotropic, and materials like carbon fibers and stainless steel fibers have low heat generation efficiency.

Method used

A heater comprising a porous carbon heating element and a porous ceramic body, both in sheet form, where the porous carbon element is primarily made of carbon with a high organic binder content and the ceramic body is mainly ceramic with an inorganic binder, allowing for efficient heat generation and transfer by laminating these elements to enhance thermal conductivity and resistance.

Benefits of technology

The solution enables efficient heating and cooling of gases passing through, allowing for quick temperature changes and reduced load on the heating element, while maintaining structural integrity and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008310_05122024_PF_FP_ABST
    Figure JP2024008310_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The objective of the present invention is to provide a heater capable of efficiently raising and lowering the temperature. This heater achieves the objective by comprising: a porous heating element mainly composed of carbon and having a structure in which an organic binder connects a particle portion H and another particle portion H through at least a part of the space therebetween; and a porous ceramic body mainly composed of a ceramic and having a structure in which an inorganic binder connects at least one pairing selected from the group consisting of a particle portion C and another particle portion C, a fiber portion c and another fiber portion c, and the particle portion C and the fiber portion c, through at least a part of the space therebetween.
Need to check novelty before this filing date? Find Prior Art

Description

heater

[0001] The present invention relates to a heater.

[0002] Several heaters have been proposed in the past.

[0003] Patent Document 1 describes an air-permeable and liquid-permeable heater having an electrically conductive fiber sheet and an insulating heat-resistant fiber sheet attached to at least one main surface of the electrically conductive fiber sheet, wherein the electrically conductive fiber sheet and the insulating heat-resistant fiber sheet are bound together by a heat-resistant binder having a higher resistance than the electrically conductive fiber sheet.

[0004] Patent Document 2 describes a heater comprising a porous carbon body formed by carbonizing a plastic foam body, a terminal connected to external power, and an electrical path electrically connecting the porous carbon body and the terminal, and characterized in that the heater heats a substance to be heated by heat generated by passing electricity through the porous carbon body.

[0005] JP 2021-048000 A JP 3-127479 A

[0006] The present invention provides a heater that can efficiently raise and lower the temperature.

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. The present invention comprises the following (1) to (7): (1) a heater comprising: a porous heating element mainly made of carbon, having a structure in which at least a portion of the spaces between particle portions H and another particle portion H are bound by an organic binder; and a porous ceramic body mainly made of ceramic, having a structure in which at least a portion of the spaces between at least one selected from the group consisting of particle portions C and another particle portion C, fiber portions c and another fiber portion c, and the particle portions C and the fiber portions c are bound by an inorganic binder. (2) A sheet-like heater according to (1) above, in which the porous heating element and the porous ceramic body are sheet-like, and the sheet-like porous heating element and the sheet-like porous ceramic body are laminated. (3) The heater according to (1) or (2) above, wherein in the porous heating element, the particle portion H having a particle diameter of 1 to 100 μm accounts for 40% by volume or more, and in the porous ceramic body, the particle portion C having a particle diameter of 1 to 50 μm and the fiber portion c having a fiber length of 20 to 1000 μm and a fiber diameter of 1 to 20 μm account for 70% by mass or more in total. (4) The heater according to any of (1) to (3) above, wherein the organic binder is a carbonized thermosetting resin. (5) The heater according to any of (1) to (4) above, wherein at least a portion of the porous heating element has a coating made of a non-oxide ceramic or an oxide ceramic on its surface, thereby providing oxidation resistance. (6) The heater according to any one of (1) to (5) above, wherein the porous heating element contains 5 to 50 volume % of fiber portion h, and the organic binder connects at least a portion between the particle portion H and the fiber portion h. (7) A method for manufacturing a heater, which can obtain the heater according to any one of (1) to (6) above, comprising the steps of: mixing carbon particles and a component that will become the organic binder in a solvent to obtain a slurry, applying the slurry to the surface of a substrate, drying the slurry, and firing the slurry in an inert gas atmosphere to form the porous heating element; and mixing ceramic particles and / or ceramic fibers and a component that will become the inorganic binder in a solvent to obtain a slurry, applying the slurry to the surface of a substrate, drying the slurry, and firing the slurry to form the porous ceramic body.(8) The method for manufacturing a heater according to (7) above, further comprising a step of laminating the porous heating element and the porous ceramic body.

[0008] According to the present invention, it is possible to provide a heater that can efficiently raise and lower the temperature.

[0009] Fig. 1 is a diagram showing a state in which particle portions H, which are components of a porous heating element, are connected by an organic binder. Fig. 2(a) is a conceptual diagram showing a state in which components 7 that become organic binders connect the surfaces of carbon particles 5 together during the manufacturing process, and Fig. 2(b) is a conceptual diagram showing a state in which organic binders 9 connect the surfaces of carbon particles 5 together. These are SEM images of the surface of a sheet-like porous heating element obtained in the examples, observed with a scanning electron microscope; Fig. 3(a) is an SEM image at 200x magnification, and Fig. 3(b) is an SEM image at 1000x magnification. These are schematic diagrams for explaining the apparatus used to evaluate the sheet-like heaters obtained in the examples.

[0010] The present invention will be described. The present invention is a heater comprising a porous heating element mainly made of carbon and having a structure in which at least a portion of the gap between particle portions H and another particle portion H is bound by an organic binder, and a porous ceramic body mainly made of ceramic and having a structure in which at least a portion of the gap between at least one portion selected from the group consisting of particle portions C and another particle portion C, fiber portions c and another fiber portion c, and the particle portions C and the fiber portions c is bound by an inorganic binder. Such a heater will be referred to hereinafter as the "heater of the present invention."

[0011] In the heater of the present invention, it is preferable that the porous heating element and the porous ceramic body are in a sheet shape, and that the sheet-shaped porous heating element and the sheet-shaped porous ceramic body are laminated together. In this case, the heater of the present invention is also in a sheet shape.

[0012] The heater of the present invention can be preferably used as a ventilation heater. That is, a gas is passed through a porous heating element that has been energized to generate heat, and the heated gas is then discharged from the heater of the present invention, allowing the heated gas to heat an object to be heated. Specifically, for example, the heater of the present invention is installed at the outlet tip of a tube, and after energizing the porous heating element of the heater of the present invention, a gas such as air or nitrogen is supplied to the porous heating element through the tube. The gas is heated as it passes through the porous heating element, and the heated gas can heat an object to be heated. In this way, it can be used as a ventilation heater. If the porous heating element is energized using a pulse power source, it can also be used as a ventilation heater capable of pulse heating. It is preferable to configure the gas that has passed through the porous ceramic body to pass through the heated porous heating element. In this case, heat generated from the porous heating element is less likely to transfer to the porous ceramic body, thereby increasing heater efficiency. Furthermore, the gas velocity is relatively reduced by passing through the porous ceramic body, thereby reducing impact and load on the porous heating element.

[0013] In the heater of the present invention, the contact area between the particles of the porous heating element is small, so grain boundary resistance occurs at the contact interface, resulting in a high electrical resistance. Therefore, the porous heating element as an electrical flow path can achieve the desired resistance even if the flow path length is shortened. In other words, the ratio of the length to the width of the flow path (length / width) can be reduced. Therefore, the porous heating element does not need to have a complex shape (pattern) to lengthen the electrical flow path.

[0014] The inventors also believe that heat transfer in the porous heating element of the heater of the present invention is isotropic. Therefore, when the heater of the present invention is used as a ventilation heater, i.e., when gas is passed through the heater of the present invention, the passing gas can be efficiently heated or cooled. Therefore, the heater of the present invention quickly switches between heating and cooling. In contrast, the inventors believe that heat transfer is anisotropic in the case of a sheet-like heater, such as that described in Patent Document 1, which generates heat by passing electricity through an electrically conductive fiber sheet. That is, the thermal conductivity in the direction parallel to the principal surface of the sheet-like heater is thought to be higher than the thermal conductivity in the thickness direction. In this case, differences in heat transfer occur between the direction parallel to the principal surface and the thickness direction. Furthermore, in such sheet-like heaters, the fibers are less likely to tangle in the thickness direction than in the direction parallel to the principal surface, resulting in differences in the likelihood of heat retention. Furthermore, carbon fiber and stainless steel fiber have low volume resistivities, so their heating efficiency is not sufficiently high.

[0015] <Porous Heating Element> The porous heating element will now be described. The porous heating element is mainly made of carbon. Here, "mainly" means that the content is 70% by mass or more. That is, the porous heating element contains 70% by mass or more of carbon, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0016] The carbon content in the porous heating element is measured using organic elemental analysis (EA) and an inductively coupled plasma (ICP) optical emission spectrometer. Specifically, the contents of H, C, O, N, S, F, Cl, and rare gas elements are measured using organic elemental analysis (EA), and other elements are measured using an inductively coupled plasma (ICP) optical emission spectrometer, and the carbon content in the porous heating element is measured based on the results of these measurements.

[0017] Components other than carbon that may be contained in the porous heating element include elements such as nitrogen and sulfur derived from trace amounts of residual organic matter such as phenolic resin and polyimide resin, as well as metal elements such as iron and nickel contained in carbon fibers, which will be described later.

[0018] The porous heating element has a structure in which particle portions H and other particle portions H are bound by an organic binder. The porous heating element may include a component other than particle portions H. For example, it may include fiber portions h made of carbon fibers such as carbon nanotubes and carbon microfibers as one of its components. In this case, it is preferable that the porous heating element has a structure in which the particle portions H and other particle portions H are bound by an organic binder, and further the particle portions H and fiber portions h are bound by an organic binder.

[0019] Here, the particle portion H and the fiber portion h will be explained. First, the major axis of 200 randomly selected parts (including particle portion H, fiber portion h, or others, but excluding organic binders) is measured in an SEM image of the porous heating element obtained by magnifying it 1000 times using a scanning electron microscope. The major axis refers to the longest diameter of the part in the SEM image. Next, a point that bisects the major axis is determined, and two points where a line perpendicular to this line intersects with the outer edge of the part are found. The distance between these two points is measured and used as the minor axis. The major axis and minor axis are determined in this way, and if the ratio (major axis / minor axis) is 0.5 to 2.0, the part is determined to be particle portion H. If the ratio is 5 or more, the part is determined to be fiber portion h. Parts that do not fall into either category are classified as other.

[0020] Next, the area of ​​each of the 200 parts selected in the SEM image is measured using an image analyzer or the like. The total area of ​​the particle portion H, the total area of ​​the fiber portion h, and the total area of ​​other parts are then calculated. Note that in an SEM image obtained at 1000x magnification, it is possible that the entire fiber portion h does not fit within a single SEM image. In this case, multiple SEM images are obtained to confirm the overall shape of the fiber portion h. Next, the total area of ​​each part is raised to the power of 2 / 3 to calculate the volumetric ratio (volume %) of each part. Here, the total of the volumetric ratio (volume %) of the particle portion H, the volumetric ratio (volume %) of the fiber portion h, and the volumetric ratio (volume %) of other parts is assumed to be 100 volume %. In reality, the porous heating element contains organic binders, but as described below, the amount (area or volume) of these binders that can be confirmed in the SEM image is small.

[0021] The content ratio of the particle portion H thus determined in the porous heating element is preferably 40% by volume or more, more preferably 50% by volume or more, even more preferably 60% by volume or more, still more preferably 70% by volume or more, still more preferably 80% by volume or more, and even more preferably 90% by volume or more. Also, it is preferably 95% by volume or less.

[0022] Furthermore, it is preferable that the abundance ratio of the fiber part h determined in this manner is 50 volume % or less in the porous heating element, preferably 5 to 50 volume %, more preferably 5 to 35 volume %, and even more preferably 10 to 25 volume %.

[0023] For parts determined to be particle portions H because the ratio of major axis to minor axis falls within a specific range as described above, the simple average of the major axis and minor axis is calculated, and this value is designated as the particle diameter of the particle portions H. When the abundance ratio (volume %) of particle portions H having a diameter (particle diameter) of 1 to 100 μm (preferably 3 to 50 μm, more preferably 6 to 20 μm) thus calculated is calculated in the same manner as described above, the abundance ratio of particle portions H having a diameter (particle diameter) of 1 to 100 μm (preferably 3 to 50 μm, more preferably 6 to 20 μm) in the porous heating element is preferably 40 vol% or more, more preferably 50 vol% or more, more preferably 60 vol% or more, more preferably 70 vol% or more, more preferably 80 vol% or more, and even more preferably 90 vol% or more. Also, it is preferably 95 vol% or less.

[0024] Furthermore, for each part determined to be fiber portion h because the ratio of major axis to minor axis falls within a specific range as described above, the fiber length and fiber diameter are determined. The fiber diameter is determined by randomly selecting 10 locations in the part (fiber portion), measuring the fiber diameters at those locations, and taking the simple average of the measured fiber diameters as the fiber diameter of that part (fiber portion h). When the abundance ratio (volume %) of fibers having a fiber length of 10 to 10,000 μm (preferably 10 to 1,000 μm) and a fiber diameter of 0.001 to 50 μm (preferably 0.1 to 10 μm) is determined in the same manner as described above, the abundance ratio of fibers having a fiber length of 10 to 10,000 μm (preferably 10 to 1,000 μm) and a fiber diameter of 0.001 to 50 μm (preferably 0.1 to 10 μm) in the porous heating element is preferably 50 vol% or less, more preferably 5 to 35 vol%, and even more preferably 10 to 25 vol%.

[0025] The shape of the particle portion H, which is one of the components of the porous heating element, is not particularly limited, and may be spherical or crushed. The circularity of the particle portion H in the porous heating element is preferably 0.5 to 1.0, more preferably 0.5 to 0.8, and even more preferably 0.7 to 0.8. When the circularity of the particle portion H in the porous heating element is within this range, the organic binder is easily bonded to the particle portion, and the strength of the porous heating element tends to be increased.

[0026] The circularity of the particle part H, which is one of the components of the porous heating element, means a value obtained by measuring as follows. First, as described above, for 200 parts in the SEM image that are judged to be particle part H because the ratio of the major axis to the minor axis falls within a specific range, the area (S) and the length of the outer edge (L) of each part are measured using an image analyzer or the like. Then, 4πS / L 2 The obtained value is taken as the circularity.

[0027] The porous heating element has a structure in which particle portions H and other particle portions H are connected by an organic binder. Furthermore, when the porous heating element includes fiber portions h, it is preferable that the particle portions H and the fiber portions h also have a structure in which the organic binder connects them. A typical example is where the particle portions are bonded by the organic binder at their contact points.

[0028] The organic binder may be an organic resin, preferably an organic resin with a heating history, and more preferably a thermosetting resin that has been carbonized by heating. Examples of thermosetting resins include polyimide resin, phenolic resin, epoxy resin, melamine resin, and polyurethane resin. Such thermosetting resins are preferably heated to a residual carbon content of 20 to 60% (preferably 40 to 60%) to form an organic binder. The residual carbon content is determined by thermogravimetry in an inert gas atmosphere such as argon, helium, or nitrogen, where the temperature is increased from room temperature to 1000°C at a rate of 10°C / min.

[0029] The content of organic binders in the porous heating element will now be described. As shown in Fig. 3(b) below, an SEM image of the surface of the porous heating element observed at 1000x magnification using a scanning electron microscope confirms that multiple particles are connected to each other by organic binders. A conceptual diagram of a portion of the porous heating element (i.e., showing a portion of the porous heating element) is shown in Fig. 1.

[0030] Here, the particle portion H(1) located in the center of FIG. 1 is connected to three adjacent particle portions via organic binders. As can be seen from FIG. 3(b), the size of the organic binders present in the connected portions is very small in the SEM image. Focusing on the particle portion H(1) located in the center of FIG. 1, the outer edge of the particle portion H(1) consists of a portion connected to the three adjacent particle portions (shown by dotted lines in FIG. 1) and the other portion (shown by solid lines in FIG. 1). Here, the major axis and minor axis of a particle having an outer edge consisting of the portion (dotted lines) on the outer edge of the particle portion H(1) that is in contact with the three adjacent particle portions and the portion (solid lines) on the outer edge of the particle portion H(1) that is not in contact with the three adjacent particle portions are determined, and the average is taken as the diameter of the particle. Then, using the diameter value, 4π(diameter / 2) 3 Next, the lengths (α, β, γ) of the points (dotted lines) on the outer edge of the particle part H(1) that are in contact with the three adjacent particle parts H are added together (α + β + γ in the case of Figure 1), and this is divided by 2π ((α + β + γ) / 2π in the case of Figure 1), and this value is set as r (r = (α + β + γ) / 2π), and the resulting value is 4πr 3 / 3 = V2 is calculated. Next, a value is calculated from V2 / (V1 + V2) × 100. This value is measured for 100 particle portions H(1) in an SEM image of the porous heating element obtained by magnifying it 1000 times using a scanning electron microscope, and a simple average value of these values ​​is calculated. The calculated value is then defined as the content of organic binders in the porous heating element.

[0031] The content of organic binders thus determined is preferably 5 to 50%, more preferably 7 to 30%, and even more preferably 10 to 15%.

[0032] In addition, the porous heating element may be composed only of particle parts H other than the organic binder, or may have fiber parts h in addition to particle parts H. In this case, the organic binder may connect between the particle parts H and fiber parts h, and / or between the fiber parts h and other fiber parts h. However, it is extremely difficult to specify the amount of organic binder present between particle parts h and fiber parts h, or between fiber parts h and other fiber parts h. Therefore, the content of organic binder in the porous heating element is defined as above, assuming that the value measured as above represents the amount of organic binder present between particle parts H and other particle parts H.

[0033] As mentioned above, the porous heating element is preferably in a sheet form. The thickness of the sheet-like porous heating element is preferably 20 to 2000 μm, more preferably 50 to 1000 μm, and even more preferably 100 to 300 μm. In the cross section of the sheet-like porous heating element or the sheet-like heater of the present invention, taken in a direction parallel to the perpendicular to its main surface, the thickness of the porous heating element is measured using a micrometer at 10 generally uniform locations from one end face to the other end face, and the measured thickness values ​​at the 10 locations are simply averaged to determine the thickness of the porous heating element.

[0034] The porous heating element preferably has a volume resistivity of 0.01 to 1.00 Ω cm, more preferably 0.02 to 0.50 Ω cm, and even more preferably 0.05 to 0.15 Ω cm. After connecting electrodes to the ends of the porous heating element and connecting tester terminals to the electrodes to measure the actual resistance [Ω] using the two-terminal method, the volume resistivity is calculated from the aspect ratio (length / width) and thickness values, which are the dimensions of the porous heating element.

[0035] The porosity of the porous heating element is preferably 20 to 90%, more preferably 35 to 75%, and even more preferably 50 to 60%. Here, the porosity of the porous heating element is a value determined by measurement using the Archimedes method. The Archimedes method is as follows: The weight W of the porous heating element in waterAq [g], saturated weight W a+w [g], dry weight W Air This method measures the mass [g] and can be calculated using the following formula: o = (W a+w -W Air ) / (W a+w -W Aq ) Note that porosity = P o × 100 (%).

[0036] The thermal conductivity of the porous heating element is preferably 0.1 to 10.0 W / (m·K), more preferably 0.6 to 5.0 W / (m·K), and even more preferably 0.30 to 2.0 W / (m·K). The thermal conductivity of the porous heating element is determined by the following measurement: The thermal diffusivity α [m 2 / s] was measured, and the specific heat capacity Cp [J / (kg / K)] and the density ρ [kg / m 3 ], the thermal conductivity λ [W / (m K)] is calculated. Here, the density ρ [kg / m 3 ] is calculated by measuring the weight of the porous heating element cut into a shape such as a cube whose volume can be easily determined. The calculation formula is as follows: λ = α × Cp × ρ

[0037] The porous heating element preferably has a Gurley air permeability of 0.1 to 20 s / 100 mL when 150 μm thick, more preferably 0.5 to 15 s / 100 mL, and even more preferably 1 to 10 s / 100 mL. The Gurley air permeability of the porous heating element is determined by measuring the time required for 100 mL of air to pass through the porous heating element three or more times using the Gurley tester method (JIS P8117:2009), and averaging the measured values ​​to determine the Gurley air permeability of the porous heating element.

[0038] It is preferable that at least a portion of the porous heating element has a non-oxide ceramic coating such as silicon carbide or an oxide ceramic coating such as metal on its surface. In this case, the porous heating element has oxidation resistance. That is, it is preferable that at least a portion of the surface of the particle portion H, fiber portion h, other components, and organic binder that form the porous heating element has a non-oxide ceramic coating containing a silicide such as silicon carbide (SiC) or an oxide ceramic coating such as metal formed thereon. In this case, the porous heating element is less likely to deteriorate even if the temperature of the gas supplied to the porous heating element is increased or oxygen is added to the gas.

[0039] Here, the non-oxide ceramic coating includes, in addition to silicon carbide (SiC), specifically, boron nitride (BN), titanium nitride (TiN), silicon nitride (Si3N4), gallium nitride (GaN), aluminum nitride (AlN), carbon nitride (CN x ), Sialon (Si3N4-AlN-Al2O3 solid solution), tungsten carbide (WC), chromium carbide (CrC), vanadium carbide (VC), niobium carbide (NbC), molybdenum carbide (MoC), tantalum carbide (TaC), titanium carbide (TiC), zirconium carbide (ZrC), hafnium carbide (HfC), boron carbide (B4C), molybdenum boride (MoB), chromium boride (CrB2), hafnium boride The coating may be a coating made of hafnium (HfB), zirconium boride (ZrB), tantalum boride (TaB), titanium boride (TiB), zirconium oxide silicate, hafnium oxide silicate, titanium oxide silicate, lanthanum oxide silicate, yttrium oxide silicate, titanium oxide silicate, tantalum oxide silicate, tantalum oxynitride silicate hydroxyapatite, calcium phosphate, or the like.

[0040] The oxide ceramic coating of metals and the like specifically includes alumina (aluminum oxide, Al2O3), zirconia (zirconium oxide, ZrO2), yttria (yttrium oxide, Y2O3), talc (hydrated magnesium silicate, Mg3Si4O 10 (OH) 10), Hematite (Iron (III) oxide, Fe2O3), Chromia (Chromium (III) oxide, Cr2O3), Titania (Titanium (IV) oxide, Ti2O), Magnesia (Magnesium oxide, MgO), Silica (Silicon dioxide, SiO2), Calcia (Calcium oxide, CaO), Ceria (Cerium (IV) oxide, CeO2), Tin oxide (SnO2), Zinc oxide (ZnO), Steatite (Magnesium metasilicate, MgO.SiO2), Copper oxide The coating may be made of ferrite (2MgO.2Al2O3.5SiO2), mullite (3Al2O3.2SiO2), ferrite (MnFe2O4), spinel (MgAl2O4), zircon (ZrSiO4), barium titanate (BaTiO3), lead titanate (PbTiO3), forsterite (Mg2SiO4), phosphorus-doped tin oxide (PTO), antimony-doped tin oxide (ATO), tin-doped indium oxide (ITO), or the like.

[0041] The thickness of the non-oxide ceramic coating and the oxide ceramic coating of a metal or the like is not particularly limited, but is preferably 0.01 to 10 μm, and more preferably 0.1 to 1 μm. The distribution of metal elements is observed using an SEM-EDS analyzer for the surface area of ​​a cross section of the porous heating element cut in a direction perpendicular to the main surface of the non-oxide ceramic coating or the oxide ceramic coating, and the thickness is measured at 10 or more locations based on the distribution. The thickness of the non-oxide ceramic coating or the oxide ceramic coating is determined by averaging the measured values. When measuring the thickness of a non-oxide ceramic coating, it is preferable to embed the porous heating element having a non-oxide ceramic coating on its surface in resin, and then measure the thickness of the porous heating element cut in a direction perpendicular to the main surface of the non-oxide ceramic coating using an SEM-EDS analyzer in the same manner as described above for the surface area of ​​the cross section.

[0042] Methods for forming a non-oxide ceramic coating or an oxide ceramic coating of metal or the like on at least a portion of the surface of a porous heating element are as follows. As an example of a non-oxide ceramic coating, a silicon carbide (SiC) coating can be formed on at least a portion of the surface of the porous heating element by impregnating the porous heating element with a polycarbosilane solution and then heating it in an inert atmosphere. As an example of an oxide ceramic coating, a metal oxide coating can be formed on at least a portion of the surface of the porous heating element by impregnating the porous heating element with an organic compound solution of an alkoxide or acetonate of a desired metal and then hydrolyzing or pyrolyzing it.

[0043] <Porous ceramic body> The porous ceramic body will now be described. The porous ceramic body is mainly composed of ceramic. Here, "mainly" means that the content is 70% by mass or more. That is, the porous ceramic body contains 70% by mass or more of ceramic, preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.

[0044] The ceramic content in the porous ceramic body is a value obtained by the following measurement. First, the content of each element contained in the porous ceramic body is measured using an ICP optical emission spectrometer. Next, the form of the compound contained in the porous ceramic body is identified using a powder X-ray diffractometer (XRD), and if necessary, the abundance ratio of each component is determined from the intensity appearing in the X-ray diffraction pattern. From this information, the ceramic content in the porous ceramic body is determined.

[0045] The ceramic contained in the porous ceramic body may be an oxide ceramic or a non-oxide ceramic. Examples of oxide ceramic include alumina (aluminum oxide, AlO), zirconia (zirconium oxide, ZrO), yttria (yttrium oxide, YO), and talc (hydrated magnesium silicate, MgSiO). 10 (OH) 10), Hematite (Iron oxide (III), Fe2O3), Chromia (Chromium oxide (III), Cr2O3), Titania (Titanium oxide (IV), Ti2O), Magnesia (Magnesium oxide, MgO), Silica (Silicon dioxide, SiO2), Calcia (Calcium oxide, CaO), Ceria (Cerium oxide (IV), CeO2), Tin oxide (SnO2), Zinc oxide (ZnO), Steatite (Magnesium metasilicate, MgO.SiO2), Co Examples of suitable tantalum oxides include dierite (2MgO.2Al2O3.5SiO2), mullite (3Al2O3.2SiO2), ferrite (MnFe2O4), spinel (MgAl2O4), zircon (ZrSiO4), barium titanate (BaTiO3), lead titanate (PbTiO3), forsterite (Mg2SiO4), phosphorus-doped tin oxide (PTO), antimony-doped tin oxide (ATO), and tin-doped indium oxide (ITO).

[0046] Examples of non-oxide ceramics include silicon carbide (SiC), boron nitride (BN), titanium nitride (TiN), silicon nitride (Si3N4), gallium nitride (GaN), aluminum nitride (AlN), and carbon nitride (CN x ), Sialon (Si3N4-AlN-Al2O3 solid solution), tungsten carbide (WC), chromium carbide (CrC), vanadium carbide (VC), niobium carbide (NbC), molybdenum carbide (MoC), tantalum carbide (TaC), titanium carbide (TiC), zirconium carbide (ZrC), hafnium carbide (HfC), boron carbide (B4C), molybdenum boride (MoB), chromium boride (CrB2), Examples of the inorganic oxide include hafnium boride (HfB2), zirconium boride (ZrB2), tantalum boride (TaB2), titanium boride (TiB2), zirconium oxide silicate, hafnium oxide silicate, titanium oxide silicate, lanthanum oxide silicate, yttrium oxide silicate, titanium oxide silicate, tantalum oxide silicate, tantalum oxynitride silicate, hydroxyapatite, and calcium phosphate.

[0047] Components other than ceramic that may be contained in the porous ceramic body include a small amount of an organic binder such as an acrylic binder.

[0048] The porous ceramic body has a structure in which an inorganic binder connects at least a portion of at least one portion selected from the group consisting of a particle portion C and another particle portion C, a fiber portion c and another fiber portion c, and the particle portion C and the fiber portion c. That is, the porous ceramic body may have only a structure in which an inorganic binder connects a particle portion C and another particle portion C. The porous ceramic body may also have only a structure in which an inorganic binder connects a fiber portion c and another fiber portion c. The porous ceramic body may also have a structure in which an inorganic binder connects a particle portion C and a fiber portion c. Furthermore, the porous ceramic body may contain other components that do not fall under the category of particle portion C and fiber portion c. The inorganic binder may also form a coating that covers at least a portion of the surface of the particle portion C and / or fiber portion c.

[0049] Here, the particle portion C, fiber portion C, and inorganic binders will be described. First, the major axis of 200 randomly selected parts (including particle portion C, fiber portion C, and others, but excluding inorganic binders) was measured in an SEM image of the porous ceramic body obtained by magnifying it 1000 times using an SEM-EDS analyzer. The major axis refers to the longest diameter of the part in the SEM image. Next, a point that bisects the major axis is determined, and two points where a line perpendicular to this line intersects with the outer edge of the part are found. The distance between these two points is measured and used as the minor axis. The major axis and minor axis are determined in this way, and if the ratio (major axis / minor axis) is 0.5 to 2.0, the part is determined to be particle portion C. If the ratio is 5 or more, the part is determined to be fiber portion C. Parts that do not fall into either category are considered to be other.

[0050] Next, EDS analysis is performed on each of the 200 parts and inorganic binders selected from the SEM image to identify the elements that make them up. Next, the porous ceramic body is powdered and analyzed using a powder X-ray diffractometer (XRD) to identify the form of the compounds contained in the porous ceramic body, and if necessary, the abundance ratio of each component is determined from the intensity displayed in the X-ray diffraction pattern. Then, based on this information and the content of each element contained in the porous ceramic body measured using an ICP optical emission spectrometer when determining the ceramic content of the porous ceramic body, the constituent components of the particle portion, fiber portion, other components, and inorganic binder that make up the porous ceramic body are identified, and their specific gravity is determined. Furthermore, for each of the 200 parts and inorganic binders selected from the SEM image, the area within the SEM image is measured using an image processing device or the like. Then, the total area of ​​the particle portion C, the total area of ​​the fiber portion C, the total area of ​​the other components, and the total area of ​​the inorganic binder are determined. In addition, in an SEM image obtained at 1000x magnification, it is possible that the entirety of one fiber portion c does not fit in one SEM image. In this case, multiple SEM images are obtained so that the overall shape of the fiber portion c can be confirmed. Next, the total area of ​​each is raised to the power of 2 / 3 to determine the abundance ratio of each as a volume ratio (volume %), and then, from the specific gravity of each, the content (%), which is the mass ratio of each of the particle portion, fiber portion, other components, and inorganic binder that make up the porous ceramic body, is determined.

[0051] The total abundance ratio of the particle portion C and the fiber portion c thus determined in the porous ceramic heating element is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 85% by mass or more, still more preferably 90% by mass or more, and even more preferably 95% by mass or more. Also, it is preferably 98% by mass or less.

[0052] As described above, the major axis / minor axis ratio of each of 200 parts selected from the SEM image was measured, and for parts determined to be particle portions C because the ratio was within a specific range, the simple average of the major axis and minor axis was calculated, and this value was designated as the particle diameter of the particle portions C. The particle portions C having a diameter (particle diameter) of 1 to 50 μm (preferably 3 to 35 μm, more preferably 5 to 20 μm) thus determined were distinguished from particle portions C having diameters other than those determined, and the total area of ​​each in the SEM image was measured using an image analyzer or the like. The volume was then determined by raising each total area to the power of 2 / 3, and the value obtained was further converted into a mass proportion using the specific gravity of the material constituting each particle portion C. The abundance ratio of particle portions C having a diameter (particle diameter) of 1 to 50 μm (preferably 3 to 35 μm, more preferably 5 to 20 μm) in the porous ceramic body thus determined is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. It is also preferably 98% by mass or less.

[0053] Furthermore, as described above, the major axis / minor axis ratio of each of 200 parts selected in the SEM image was measured, and for parts determined to be fiber part c because the ratio was within a specific range, the fiber length and fiber diameter were determined for each part. The fiber diameter was determined by randomly selecting 10 locations in the part (fiber part), measuring the fiber diameter at those locations, and taking the simple average of the measured fiber diameters as the fiber diameter of that part (fiber part). Fiber parts c having the fiber length thus determined of 20 to 1,000 μm (preferably 50 to 500 μm, more preferably 100 to 250 μm) and the fiber diameter of 1 to 20 μm (preferably 2 to 10 μm, more preferably 3 to 5 μm) were distinguished from other fiber parts c, and the total area of ​​each in the SEM image was measured using an image analyzer or the like. The volume was then determined by raising each total area to the power of 2 / 3, and further converted to a mass ratio using the specific gravity of the material that constitutes each part. The abundance ratio of the fibrous portion c having a fiber length of 20 to 1000 μm (preferably 50 to 500 μm, more preferably 100 to 250 μm) and a fiber diameter of 1 to 20 μm (preferably 2 to 10 μm, more preferably 3 to 5 μm) determined in this manner is preferably 70 mass % or more, more preferably 80 mass % or more, even more preferably 90 mass % or more, and even more preferably 95 mass % or more in the porous ceramic body. Also, it is preferably 98 mass % or less.

[0054] Furthermore, the sum of the abundance ratio of particle portions C having a diameter (particle diameter) of 1 to 50 μm (preferably 3 to 35 μm, more preferably 5 to 20 μm) and the abundance ratio (volume %) of fiber portions c having a fiber length of 20 to 1000 μm (preferably 50 to 500 μm, more preferably 100 to 250 μm) and a fiber diameter of 1 to 20 μm (preferably 2 to 10 μm, more preferably 3 to 5 μm) in the porous ceramic body, determined as described above, is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and even more preferably 95 mass% or more. Also, it is preferably 98 mass% or less.

[0055] In the porous ceramic body, an inorganic binder bonds at least a portion of the spaces between at least one selected from the group consisting of the spaces between the ceramic particles, the spaces between the ceramic fibers, and the spaces between the ceramic particles and the ceramic fibers.

[0056] Examples of inorganic binders include silicate-based binders such as lithium silicate, sodium silicate, and potassium silicate. Other examples include phosphate-based binders such as aluminum phosphate and magnesium phosphate. Other examples include cement-based binders such as Portland cement and alumina cement. Among these, silicate-based binders are preferred.

[0057] The content of the inorganic binder in the porous ceramic body is preferably 0.5 to 30 mass %, more preferably 1 to 15 mass %, and even more preferably 2 to 5 mass %. The content of the inorganic binder in the porous ceramic body is a value determined by the measurement as described above.

[0058] As described above, the porous ceramic body is preferably in a sheet form. The thickness of the sheet-like porous ceramic body is preferably 50 to 20 mm. When the porous ceramic body is made of ceramic particles having a particle diameter of 1 to 50 μm and an inorganic binder, the thickness of the sheet-like porous ceramic body is preferably 50 μm to 1 mm. When the porous ceramic body is made of ceramic fibers having a fiber diameter of 1 to 20 μm and a fiber length of 20 to 1000 μm and an inorganic binder, the thickness of the sheet-like porous ceramic body is preferably 1 mm to 20 mm.

[0059] The thickness of the porous ceramic body is determined by measuring it in the same manner as the thickness of the sheet-like porous heating element described above.

[0060] The porous ceramic body preferably has a porosity of 20 to 98%, more preferably 30 to 96%, and even more preferably 40 to 95%. The porosity of the porous ceramic body is a value determined by measurement using the Archimedes method, similar to the method for measuring the porosity of the porous heating element described above.

[0061] The thermal conductivity of the porous ceramic body is preferably 0.1 to 20.0 W / (m K), more preferably 0.5 to 15 W / (m K), and even more preferably 1.00 to 10 W / (m K). The thermal conductivity of the porous ceramic body is a value determined by measurement using a laser flash method, similar to the method for measuring the thermal conductivity of the porous heating element described above.

[0062] The porous ceramic body preferably has a Gurley air permeability of 0.1 to 20 s / 100 mL when it is 500 μm to 5 mm thick, more preferably 0.2 to 15 s / 100 mL, and even more preferably 0.3 to 10 s / 100 mL. The Gurley air permeability of the porous ceramic body is a value determined by measurement using a Gurley tester, similar to the method for measuring the Gurley air permeability of the porous heating element described above.

[0063] <Heater of the Present Invention> The heater of the present invention comprises a porous heating element and a porous ceramic body as described above. In the heater of the present invention, the porous heating element and the porous ceramic body are preferably arranged adjacent to each other. When the heater of the present invention is in sheet form, the sheet-shaped porous heating element and the sheet-shaped porous ceramic body are preferably laminated by partially adhering their main surfaces to each other. In this case, compared to when the porous heating element is fully adhered, damage to one of the porous heating element and the porous ceramic body due to the difference in thermal expansion between the porous heating element and the porous ceramic body can be avoided when the porous heating element is heated. The method for adhering the main surfaces to each other is not particularly limited, and for example, these main surfaces can be attached using a conventionally known adhesive. Alternatively, for example, two punched metal sheets formed by forming a plurality of holes in a metal plate may be prepared, and a laminate consisting of the porous heating element and the porous ceramic body may be sandwiched between them, and the punched metal sheets may be connected to each other to fix the porous heating element and the porous ceramic body in the laminate.

[0064] The heater of the present invention may include a plurality of porous heating elements or a plurality of porous ceramic bodies. For example, a sheet-shaped porous heating element may be sandwiched between two sheet-shaped porous ceramic bodies.

[0065] <Manufacturing Method> The manufacturing method of the heater of the present invention is not particularly limited. The heater of the present invention is preferably manufactured by a manufacturing method including the steps of: mixing carbon particles, a component that will become the organic binder, and, if necessary, carbon fibers in a solvent to obtain a slurry; applying the slurry to the surface of a substrate, drying the slurry, and firing the slurry in an inert gas atmosphere to form the porous heating element; and mixing ceramic particles and / or ceramic fibers and a component that will become the inorganic binder in a solvent to obtain a slurry; applying the slurry to the surface of a substrate, drying the slurry, and firing the slurry to form the porous ceramic body. Hereinafter, such a manufacturing method will also be referred to as the "manufacturing method of the present invention."

[0066] The manufacturing method of the present invention preferably further comprises a step of laminating the porous heating element and the porous ceramic body.The manufacturing method of the present invention preferably further comprises a step of laminating the sheet-shaped porous heating element and the sheet-shaped porous ceramic body.

[0067] The manufacturing method of the present invention will be described.

[0068] A method for forming the porous heating element will now be described. First, carbon particles, a component that will become an organic binder, and, if necessary, carbon fibers are added to a solvent and mixed to form a slurry.

[0069] Here, the particle diameter of the carbon particles is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 6 to 20 μm. The average particle diameter of the carbon particles is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 6 to 20 μm. The carbon particles are scattered on a plate, and the major and minor axes are measured using a scanning electron microscope (SEM) or an optical microscope. The simple average value of these is taken as the particle diameter of the carbon particles. The average particle diameter of the carbon particles is the median diameter determined by a laser diffraction scattering method using a dispersion in which carbon particles are dispersed in a dispersion medium (water, toluene, etc.) to a concentration of 100 ppm to 1% by mass.

[0070] The component that becomes the organic binder may be an organic resin, preferably a thermosetting resin, more preferably a polyimide resin, a phenol resin, an epoxy resin, a melamine resin, a polyurethane resin, or the like.

[0071] Examples of carbon fibers include carbon nanotubes and carbon microfibers.

[0072] The blending amounts of the carbon particles, the components that become the organic binder, and, if necessary, the carbon fibers are not particularly limited. The organic binder is preferably 5 to 50 parts by mass, more preferably 7 to 35 parts by mass, and even more preferably 10 to 15 parts by mass, relative to 100 parts by mass of the total amount of the carbon particles and the carbon fibers. The carbon fibers are preferably 0 to 50 parts by mass, more preferably 5 to 35 parts by mass, and even more preferably 10 to 25 parts by mass, relative to 100 parts by mass of the carbon particles.

[0073] The solvent is preferably an organic solvent, such as cyclohexanone, methanol, ethanol, isopropanol, or toluene.

[0074] The solid content of the slurry is preferably 15 to 50% by mass, and more preferably 25 to 35% by mass.

[0075] Next, a substrate (film) made of, for example, polyester is prepared, and the slurry is applied to the surface of this substrate by a conventionally known method. Here, it is preferable that the thickness of the slurry applied to the surface of the substrate is 200 to 600 μm.

[0076] Next, the substrate with the slurry applied to its surface is placed in a dryer or the like to remove at least a portion of the solvent from the slurry, thereby solidifying the slurry to obtain a solid material. As a result, it is believed that the carbon particles 5 are bound together by components 7 that serve as organic binders, as shown in Figure 2(a) for example.

[0077] The solidified slurry is then peeled off from the substrate and fired in an inert gas atmosphere. Examples of inert gas include nitrogen, helium, and argon. The firing temperature is preferably 800 to 1500°C. The firing time is preferably 1 to 24 hours.

[0078] 2(b), the carbon particles 5 are believed to be bound together by the organic binder 9. The present inventors presume that at least a portion of the carbon particles 5 and the organic binder 9 are bound or adhered together by an anchor effect or an intermolecular force.

[0079] By carrying out such a process, a porous heating element can be formed.

[0080] The method for forming the porous ceramic body will be described below. First, ceramic particles and / or ceramic fibers, a component to be used as an inorganic binder, and other components, if necessary, are added to a solvent in a predetermined blending ratio and mixed to form a slurry.

[0081] Here, the particle size of the ceramic particles is preferably 1 to 50 μm, more preferably 3 to 35 μm, and even more preferably 5 to 20 μm. The average particle size of the ceramic particles is preferably 1 to 50 μm, more preferably 3 to 35 μm, and even more preferably 5 to 20 μm. Here, the particle size and average particle size of the ceramic particles refer to values ​​obtained by measurement using the same method as for the carbon particles.

[0082] The fiber length of the ceramic fibers is preferably 20 to 1000 μm, more preferably 50 to 500 μm, and even more preferably 100 to 250 μm. The fiber diameter of the ceramic fibers is preferably 1 to 20 μm, more preferably 2 to 10 μm, and even more preferably 3 to 5 μm. Here, the fiber length and fiber diameter of the ceramic fibers refer to values ​​obtained by measurement using the following method. First, the raw ceramic fibers are scattered on a plate, and approximately 100 fibers are randomly selected and their fiber length and fiber diameter are measured using an SEM or optical microscope. Here, the fiber diameter is the average value of fiber diameters measured at 10 randomly selected locations on each ceramic fiber.

[0083] The blending amounts of ceramic particles, ceramic fibers, and components that form the inorganic binder are not particularly limited. The inorganic binder is preferably 0.5 to 30 parts by mass, more preferably 1 to 15 parts by mass, and even more preferably 2 to 5 parts by mass, per 100 parts by mass of the total amount of ceramic particles and ceramic fibers. The ceramic fibers are preferably 0 to 100 parts by mass, more preferably 0 to 50 parts by mass, and even more preferably 0 to 25 parts by mass, per 100 parts by mass of ceramic particles. Furthermore, the ceramic particles are preferably 0 to 100 parts by mass, more preferably 0 to 50 parts by mass, and even more preferably 0 to 25 parts by mass, per 100 parts by mass of ceramic fibers.

[0084] It is preferable to add a weak acid such as acetic acid, phosphoric acid, oxalic acid, succinic acid, malonic acid, citric acid, malic acid, or lactic acid, or a strong acid such as diluted hydrochloric acid, nitric acid, or sulfuric acid to the solvent. These solvents promote the hardening of the inorganic binder. If the solvent is a strong acid, the hardening of the inorganic binder tends to proceed too quickly, making it difficult to apply the binder in subsequent steps.

[0085] The component that serves as the inorganic binder is preferably a silicate binder.

[0086] Ceramic particles and / or ceramic fibers may be added to a solution in which an inorganic binder has been dissolved in a predetermined blending ratio, and mixed to form a slurry.

[0087] The solvent is preferably water, methanol, ethanol, isopropanol, toluene, or the like.

[0088] The solid content of the slurry is preferably 40 to 70% by mass, and more preferably 50 to 65% by mass.

[0089] Next, a substrate (film) made of, for example, polyester is prepared, and the slurry is applied to the surface of this substrate by a conventionally known method. Here, it is preferable that the thickness of the slurry applied to the surface of the substrate is 1 to 10 mm.

[0090] Next, the substrate with the slurry applied to its surface is placed in a dryer, for example, to remove at least a portion (preferably all) of the solvent from the slurry, thereby solidifying the slurry and obtaining a solid material. If the slurry contains unnecessary components, these are removed by washing with water. For example, if a silicate-based binder is used as the inorganic binder component, the slurry is further hardened under a carbon dioxide atmosphere and then dried, and the separated salt and the unreacted remaining silicate-based binder are removed by washing with water.

[0091] Thereafter, the solidified slurry is peeled off from the substrate and fired at a temperature of preferably 500 to 1600° C. The firing time is preferably 1 to 24 hours.

[0092] It is believed that such treatment results in the ceramic particles being bonded to each other, the ceramic fibers being bonded to each other, and the ceramic particles and ceramic fibers being bonded to each other by the inorganic binder. The inventors presume that at least a portion of the ceramic particles and the inorganic binder are chemically bonded, and similarly, at least a portion of the ceramic fibers and the inorganic binder are chemically bonded.

[0093] By carrying out such a treatment, a porous ceramic body can be formed.

[0094] The method for attaching the porous heating element obtained as described above to the porous ceramic body is not particularly limited, and for example, they can be attached using a conventionally known adhesive. In this case, it is preferable that the porous heating element and the porous ceramic body are partially in close contact with each other. Alternatively, for example, the porous heating element and the porous ceramic body in the laminate can be attached by sandwiching a laminate formed by stacking a sheet-shaped porous heating element and a sheet-shaped porous ceramic body between two sheets of punched metal made of metal plates with multiple holes formed therein and connecting the punched metals together.

[0095] Example 1 Preparation of a Sheet-Like Porous Heating Element 20 g of sintered carbon particles with a particle size of 6 μm and 16 g of a 30% by weight cyclohexanone solution of polyimide resin were prepared and added to cyclohexanone and mixed to prepare a slurry. This slurry was then applied to the treated surface of a release PET film using a film applicator to a thickness of 300 μm. The coating was then dried to evaporate the solvent, and then baked at 1000°C for 1 hour in a nitrogen atmosphere to obtain a sheet-like porous heating element with a thickness of 150 μm. The porosity of this porous heating element was measured using the Archimedes method and found to be 55%.

[0096] The surface of the obtained sheet-like porous heating element was then observed with a scanning electron microscope to obtain SEM images. The obtained SEM images are shown in Figure 3. Figure 3(a) is an SEM image at 200x magnification, and Figure 3(b) is an SEM image at 1000x magnification. From Figure 3, it was confirmed that the polyimide had been carbonized and that point bonding had occurred between the baked carbon particles.

[0097] <Preparation of a Sheet-Like Porous Ceramic Body> 50 g of alumina particles with a particle size of 20 μm, 8.3 g of a 30% by weight potassium silicate aqueous solution, and 1.6 g of a 6% by weight acetic acid aqueous solution were prepared and added to water and mixed to prepare a slurry. Next, this slurry was applied to the surface of a PET film to a thickness of 1 mm using a film applicator. After drying to evaporate the water, the film was left in a carbon dioxide atmosphere at room temperature and atmospheric pressure for 24 hours to convert the potassium silicate to silicic acid. The film was then washed with water to remove residual potassium silicate. This was then fired at 1000°C for 1 hour to obtain a sheet-like porous ceramic body (A) with a thickness of 500 μm. The porosity of this sheet-like porous ceramic body (A) was measured using the Archimedes method and found to be 40%.

[0098] The surface of the obtained sheet-like porous ceramic body (A) was observed with a scanning electron microscope to obtain an SEM image, which confirmed that the silicic acid had polymerized and the alumina particles had bonded together.

[0099] <Heater> A potassium silicate aqueous solution was applied as an inorganic adhesive in the form of dots at regular intervals on the main surface of the porous ceramic body (A), and the main surface of a sheet-like porous heating element was adhered thereto to produce a sheet-like heater (A).

[0100] <Evaluation> A test piece measuring 10 mm x 20 mm was cut from the sheet heater (A) obtained as described above. Next, as shown in FIG. 4, the test piece was placed in a sealed container 20 capable of circulating nitrogen at 6 L / min. An external power source was connected to the sheet-like porous heating element 10. Electrodes 22, 24, covering the entire end face of the test piece, including the 10 mm side, were connected to each end face. A thermocouple 26 was installed on the main surface of the sheet-like porous heating element 10 to measure the surface temperature of the porous heating element over time. A voltage of 55 V was applied, and the time required for the temperature to rise from room temperature to 800°C, the maximum temperature at the applied voltage, was confirmed. After reaching 800°C, the current was stopped, and the time required for the temperature to fall to 100°C was confirmed. As a result, it was confirmed that the temperature reached 800°C in 50 seconds after voltage application, and that the temperature fell to 100°C in 90 seconds after current application was stopped. In other words, it was confirmed that the sheet heater (A) produced here can be efficiently heated and cooled.

[0101] Example 2 <Preparation of a sheet-shaped porous heating element> The same sheet-shaped porous heating element as used in Example 1 was prepared.

[0102] <Preparation of a Sheet-Like Porous Ceramic Body> A block of alumina fibers with a fiber diameter of 1 to 20 μm and a fiber length of 20 to 1000 μm was impregnated under reduced pressure at 0.1 atmosphere with a 30% by mass aqueous potassium silicate solution. The block was then dried to evaporate the water and left in a carbon dioxide atmosphere at room temperature and atmospheric pressure for 24 hours to convert the potassium silicate to silicic acid. The block was then washed with water to remove residual potassium silicate. The block was then fired at 1000°C for 1 hour to combust traces of organic components contained in the alumina fiber block. This block was then machined to obtain a 5 mm-thick sheet-like porous ceramic body (B). The porosity of this sheet-like porous ceramic body (B) was measured using the Archimedes method and found to be 95%.

[0103] The surface of the obtained sheet-like porous ceramic body (B) was observed with a scanning electron microscope to obtain an SEM image, which confirmed that the silicic acid had polymerized and the alumina particles had bonded together.

[0104] <Heater> A potassium silicate aqueous solution was applied as an inorganic adhesive in the form of dots at regular intervals to the main surface of the porous ceramic body (B), and the main surface of a sheet-like porous heating element was adhered thereto to produce a sheet-like heater (B).

[0105] <Evaluation> A test piece measuring 10 mm x 20 mm was cut out from the sheet-like heater (B) obtained as described above. Then, as in Example 1, a voltage of 55 V was applied to the test piece, and the time required for the temperature to rise from room temperature to 800°C, the maximum temperature at the applied voltage, was confirmed. After the temperature reached 800°C, the current was stopped, and the time required for the temperature to fall to 100°C was confirmed. As a result, as in Example 1, it was confirmed that the temperature reached 800°C in 47 seconds after the voltage application, and that the temperature fell to 100°C in 83 seconds after the current was stopped. In other words, it was confirmed that the heater (B) produced here could efficiently raise and lower its temperature.

[0106] This application claims priority based on Japanese Patent Application No. 2023-86588, filed May 26, 2023, the disclosure of which is incorporated herein in its entirety by reference.

[0107] REFERENCE SIGNS LIST 1 particle part H 5 carbon particles 7 component to be organic binder 9 organic binder 10 porous heating element 12 porous ceramic body 20 sealed container 22, 24 electrodes 26 thermocouple 28 inorganic adhesive

Claims

1. A heater comprising: a porous heating element mainly made of carbon, with a structure in which at least a portion of the spaces between particle portions H and other particle portions H are connected by an organic binder; and a porous ceramic body mainly made of ceramic, with a structure in which at least a portion of the spaces between at least one portion selected from the group consisting of particle portions C and other particle portions C, fiber portions c and other fiber portions c, and the particle portions C and the fiber portions c are connected by an inorganic binder.

2. The heater according to claim 1, in which the porous heating element and the porous ceramic body are in sheet form, and the sheet-shaped porous heating element and the sheet-shaped porous ceramic body are laminated.

3. A heater as described in claim 1 or 2, wherein in said porous heating element, the particle portion H having a particle diameter of 1 to 100 μm accounts for 40 volume % or more, and in said porous ceramic body, the total presence ratio of said particle portion C having a particle diameter of 1 to 50 μm and said fiber portion c having a fiber length of 20 to 1000 μm and a fiber diameter of 1 to 20 μm is 70 mass % or more.

4. A heater according to any one of claims 1 to 3, wherein the organic binder is a carbonized thermosetting resin.

5. A heater according to any one of claims 1 to 4, wherein at least a portion of the porous heating element has a coating made of a non-oxide ceramic or an oxide ceramic on its surface, thereby providing oxidation resistance.

6. A heater according to any one of claims 1 to 5, wherein the porous heating element contains 5 to 50 volume percent fibrous portion h, and at least a portion of the space between the particle portion H and the fibrous portion h is connected by the organic binder.

7. A method for manufacturing a heater, which provides the heater according to any one of claims 1 to 6, comprising the steps of: mixing carbon particles and a component that will become the organic binder in a solvent to obtain a slurry, applying the slurry to the surface of a substrate, drying, and firing in an inert gas atmosphere to form the porous heating element; and mixing ceramic particles and / or ceramic fibers and a component that will become the inorganic binder in a solvent to obtain a slurry, applying the slurry to the surface of a substrate, drying, and firing to form the porous ceramic body.

8. The method for manufacturing a heater according to claim 7, further comprising a step of laminating said porous heating element and said porous ceramic body.

Citation Information

Patent Citations

  • heater

    JP1991127479A

  • Conductive sheet and its manufacture

    JP1999026140A

  • Planar heating element using carbon microfiber and manufacturing method thereof

    JP2009543288A

  • Ventilation / liquid-permeable heater and manufacturing method thereof