Masterbatch and foam molded body

The masterbatch with a specific antioxidant content in thermally foamable microspheres and a base resin addresses the shrinkage issues in plastic foam molded products, enhancing their stability and smoothness by maintaining effective shrinkage resistance at high temperatures.

WO2024247567A1PCT designated stage expired Publication Date: 2024-12-05KUREHA CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016087
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-04-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional plastic foam molded products experience sagging and surface roughness due to shrinkage issues when thermally foamable microspheres expand and contract, leading to impaired smoothness and increased roughness, necessitating a solution for enhanced shrinkage resistance.

Method used

A masterbatch comprising thermally foamable microspheres, a base resin, and an antioxidant with a specific content range, where the antioxidant content is 0.2 to 4 parts by mass, and preferably 0.4 to 3 parts by mass, is used to achieve improved shrinkage resistance, with phenol or phosphite compounds being preferred for effective performance.

Benefits of technology

The masterbatch exhibits excellent shrinkage resistance, maintaining stability and smoothness at elevated temperatures, as measured by thermomechanical analysis, with a shrinkage resistance index of 4.0 minutes or more at 250°C and 22 minutes or more at 230°C, significantly reducing surface imperfections in foamed molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016087_05122024_PF_FP_ABST
    Figure JP2024016087_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a masterbatch from which a foam molded body excellent in shrinkage resistance can be obtained; and a foam molded body of the masterbatch. The present invention uses the masterbatch, which contains thermally-foamable microspheres (A), a base resin (B), and an antioxidant (C). The content of the antioxidant (C) is 0.2-4 parts by mass with respect to a total of 100 parts by mass of the thermally-foamable microspheres (A) and the base resin (B). The base resin (B) is preferably a polyethylene resin. The antioxidant (C) is preferably a phenolic compound containing a hindered phenol compound or a phosphite compound.
Need to check novelty before this filing date? Find Prior Art

Description

Masterbatches and foam moldings

[0001] The present invention relates to a masterbatch and a foam-molded article made from the masterbatch.

[0002] Conventionally, plastic foam molded articles have been used in a variety of applications because they can exhibit heat insulation properties, heat insulation properties, sound insulation properties, sound absorption properties, vibration damping properties, weight reduction, etc., depending on the material of the molded article and the state of the formed bubbles. Examples of methods for producing such plastic foam molded articles include a method in which a masterbatch containing thermally foamable microspheres is heated with a resin to foam and then molded.

[0003] Here, thermally foamable microspheres, also known as thermally foamable microcapsules, are microencapsulated volatile foaming agents in a shell resin. Thermally foamable microspheres have the property of rapidly expanding when heated above the foaming initiation temperature.

[0004] As the masterbatch, for example, a masterbatch containing thermally expandable microspheres and using a polyethylene resin and a polyethylene wax in combination has been proposed (Patent Document 1).

[0005] JP 2009-144122 A

[0006] When thermally foamable microspheres are heated above the foaming initiation temperature, they expand themselves to form foam particles (closed-cell bodies). However, when heated further, the thickness of the outer shell becomes thinner, allowing the volatile foaming agent to permeate through the outer shell, resulting in a decrease in internal pressure and shrinkage of the thermally foamable microspheres. When thermally foamable microspheres shrink, the appearance of the foamed molded article becomes saggy and gas flow marks become a problem. When the foamed molded article sags, the surface smoothness of the foamed molded article is impaired and roughness occurs. The masterbatch disclosed in Patent Document 1 also has the problem that the foamed molded article is prone to shrinkage. For this reason, foamed molded articles with excellent shrinkage resistance are desired.

[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a masterbatch that can give a foamed molded article having excellent shrinkage resistance, and a foamed molded article made from the masterbatch.

[0008] Generally, additives such as antioxidants are added to commercially available synthetic resins such as polyethylene and polypropylene, but the amount added is generally 0.1 wt %. After extensive research, the inventors discovered that the amount of antioxidant contained in commercially available synthetic resins alone is not effective in suppressing shrinkage resistance during foaming, and that adding an additional antioxidant can impart shrinkage resistance, leading to the completion of the present invention.

[0009] An embodiment of the present invention relates to the following masterbatch and foamed molded article.

[0010] [1] A masterbatch comprising thermally foamable microspheres (A), a base resin (B), and an antioxidant (C), wherein the content of the antioxidant (C) is 0.2 parts by mass or more and 4 parts by mass or less per 100 parts by mass of the total of the thermally foamable microspheres (A) and the base resin (B). [2] The masterbatch according to [1], wherein the shrinkage resistance (250°C) measured by the following measurement method is 4.0 minutes or more. Shrinkage resistance (250°C) = 1 / 2Tb - 1 / 2Ta (A container containing the masterbatch was used as a measurement sample and placed in the heating furnace of a thermomechanical analyzer (TMA), and the temperature inside the heating furnace was raised from 30°C to 190°C over a set time of 2 minutes, and then raised from 190°C to 250°C over a set time of 0 minutes. When the masterbatch was heated at 250°C for a total heating time of 20 minutes from the point at 30°C, the minimum height of the masterbatch was 0% and the maximum foam height was 100%, and the short-term time at which the height displacement was 50% was defined as 1 / 2Ta and the long-term time as 1 / 2Tb.) [3] The masterbatch according to [1], whose shrinkage resistance (230°C) measured by the following measurement method is 22 minutes or more. Shrinkage resistance (230°C) = 1 / 2Tb - 1 / 2Ta (A container containing the masterbatch was used as a measurement sample and placed in the heating furnace of a thermomechanical analyzer (TMA). The temperature inside the heating furnace was raised from 30°C to 170°C over a set time of 2 minutes, and then raised from 170°C to 230°C over a set time of 0 minutes. The masterbatch was heated at 230°C for a total heating time of 30 minutes from the 30°C point, and the minimum height of the masterbatch was set to 0% and the maximum foam height was set to 100%, whereby 1 / 2Ta is the short-term time at which the height displacement was 50%, and 1 / 2Tb is the long-term time.) [4] The masterbatch according to any of [1] to [3], wherein the base resin (B) is a polyethylene-based resin. [5] The masterbatch according to any of [1] to [4], wherein the antioxidant (C) contains a phenol-based compound including a hindered phenol-based compound, or a phosphite-based compound. [6] The masterbatch according to any one of [1] to [5], wherein the content of the antioxidant (C) is 0.4 parts by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the total of the thermally foamable microspheres (A) and the base resin (B).[7] A foam-molded product of the masterbatch according to any one of [1] to [6].

[0011] According to the present invention, it is possible to provide a masterbatch that can give a foamed molded article having excellent shrinkage resistance, and a foamed molded article made from the masterbatch.

[0012] FIG. 1 is a schematic diagram showing the relationship between the displacement of the masterbatch at each time and time when the masterbatch of the present embodiment is heated at a predetermined temperature (foaming temperature) for a predetermined time using a thermomechanical analysis (TMA) device and the foaming temperature is maintained for a predetermined time.

[0013] <Masterbatch> The masterbatch of this embodiment contains thermally foamable microspheres (A), a base resin (B), and an antioxidant (C). The content of the antioxidant (C) is 0.2 parts by mass or more and 4 parts by mass or less, relative to 100 parts by mass of the total of the thermally foamable microspheres (A) and the base resin (B). Since the masterbatch of this embodiment contains a specific amount of antioxidant (C), a foam molded article having excellent shrinkage resistance can be obtained.

[0014] The essential and optional components contained in the masterbatch will be described below.

[0015] <Thermal Foamable Microspheres (A)> The thermal foamable microspheres (A) have a structure in which a foaming agent is encapsulated in an outer shell formed from a polymer.

[0016] (Polymer) From the viewpoint of excellent gas barrier properties and heat resistance, the polymer forming the outer shell is preferably, for example, a homopolymer or copolymer having structural units derived from one or more monomers selected from the group consisting of (meth)acrylonitrile, (meth)acrylic acid esters, (meth)acrylic acid, vinyl chloride, vinylidene chloride, and styrene. Among these, copolymers having structural units derived from (meth)acrylonitrile, (meth)acrylic acid, and (meth)acrylic acid esters are preferred. In this specification, "(meth)acrylonitrile" means both "acrylonitrile" and "methacrylonitrile," and "(meth)acrylic" means both "acrylic" and "methacrylic."

[0017] The polymer may be crosslinked with a crosslinkable monomer. Examples of the crosslinkable monomer include bifunctional crosslinkable monomers such as aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene, and derivatives thereof; diethylenically unsaturated carboxylic acid esters such as ethylene glycol diacrylate, diethylene glycol diacrylate, ethylene glycol dimethacrylate, and diethylene glycol dimethacrylate; polyethylenically unsaturated carboxylic acid esters such as triethylene glycol diacrylate and triethylene glycol dimethacrylate; acrylates or methacrylates derived from aliphatic alcohols at both ends such as 1,4-butanediol and 1,9-nonanediol; and divinyl compounds such as N,N-divinylaniline and divinyl ether.

[0018] (Blowing Agent) The blowing agent is a substance that turns into a gas when heated. As the blowing agent, a hydrocarbon having a boiling point corresponding to the foaming initiation temperature can be used, and examples thereof include hydrocarbons such as ethane, ethylene, propane, propene, n-butane, isobutane, butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, heptane, n-octane, isooctane, isododecane, petroleum ether, and isoparaffin mixtures, as well as isomer mixtures thereof; CCl 3 F, CCl 2 F 2 , CClF 3 , CClF 2 -CClF 2 and tetraalkylsilanes such as tetramethylsilane, trimethylethylsilane, trimethylisopropylsilane, trimethyl-n-propylsilane, etc. These may be used either alone or in combination of two or more.

[0019] Among these, isobutane, n-butane, n-pentane, isopentane, n-hexane, isohexane, heptane, 2,2,4-trimethylpentane, isooctane, isododecane, and mixtures of their isomers, petroleum ether, and mixtures of two or more of these are preferred. If desired, compounds that are thermally decomposed to gaseous form by heating may also be used.

[0020] The content of the foaming agent is preferably 5 parts by mass or more and 70 parts by mass or less, more preferably 10 parts by mass or more and 60 parts by mass or less, and even more preferably 15 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the polymer.

[0021] The thermally expandable microspheres (A) preferably have an average particle size of 5 μm or more and 100 μm or less. The thermally expandable microspheres (A) preferably have an expansion initiation temperature of 140° C. or more and 250° C. or less and a maximum expansion temperature of 180° C. or more and 300° C. or less.

[0022] Such thermally expandable microspheres (A) can be produced by suspension polymerization of the above-mentioned monomer and, if necessary, the above-mentioned crosslinkable monomer together with the above-mentioned blowing agent in an aqueous dispersion medium containing a dispersion stabilizer. As such thermally expandable microspheres (A), for example, trade names "S2640" (manufactured by Kureha Co., Ltd.) and trade name "S2340" (manufactured by Kureha Co., Ltd.) are preferably used.

[0023] <Base Resin (B)> The base resin (B) may be a known thermoplastic resin or thermoplastic elastomer, and is not particularly limited. Examples of thermoplastic resins used for the base resin (B) include polyvinyl chloride, polystyrene, polypropylene-based resins, polypropylene oxide, polyethylene-based resins, and acrylic-based resins. Examples of thermoplastic elastomers used for the base resin (B) include ethylene-based, vinyl chloride-based, olefin-based, urethane-based, and ester-based elastomers. Among these, polyethylene-based resins are preferred from the viewpoint of blendability with the thermally expandable microspheres. Examples of polyethylene-based resins include low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. Examples of linear low-density polyethylenes that are suitable for use include those under the trade names "Novatec" (manufactured by Mitsubishi Chemical Corporation), "Nipolon" (manufactured by Tosoh Corporation), "Ultra-Zex" (manufactured by Prime Polymer Co., Ltd.), and "Excellent" (manufactured by Sumitomo Chemical Co., Ltd.).

[0024] These thermoplastic resins or thermoplastic elastomers may be used alone or in combination of two or more.

[0025] The mass content ratio of the thermally foamable microspheres (A) to the base resin (B), where the sum of A and B is 100, is preferably A:B=20-80:80-20, more preferably A:B=30-70:70-30, and even more preferably A:B=40-60:60-40.

[0026] <Antioxidant (C)> Examples of the antioxidant (C) include tocopherol-based compounds, phenol-based compounds, hindered amine-based compounds, phosphite-based compounds, sulfur-based compounds, benzotriazole-based compounds, benzophenone-based compounds, hydroxylamine-based compounds, salicylic acid ester-based compounds, and triazine-based compounds. These can be used alone or in combination of two or more. Among these, phenol-based compounds and phosphite-based compounds are preferred from the viewpoint of obtaining foamed molded articles having excellent shrinkage resistance.

[0027] Phenolic compounds include hindered phenolic compounds and phenolic compounds other than hindered phenolic compounds (hereinafter also referred to as "other phenolic compounds"). In this specification, "hindered phenolic compounds" refers to compounds that are used as antioxidants and that contain a structure in which tert-butyl groups are bonded to the two ortho-positions of a phenolic hydroxyl group. In this specification, "other phenolic compounds" refers to compounds that are used as antioxidants and that contain phenolic hydroxyl groups but do not fall under the category of the above-mentioned hindered phenolic compounds.

[0028] Examples of the hindered phenol compounds include pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]: trade name "Irganox 1010" (manufactured by BASF Corporation), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene: trade name "Irganox 1330" (manufactured by BASF Corporation), and tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate: trade name "Irganox 3114" (manufactured by BASF Corporation). 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate: trade name "Irganox 1076" (manufactured by BASF), 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]: trade name "Irganox 1035" (manufactured by BASF), N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide]: trade name "Irganox 1098" (manufactured by BASF), 1,6-hexanediol bis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] trade name "Irganox 259" (manufactured by BASF Corporation), 4-[[4,6-bis(octylthio)-1,3,5-triazin-2-yl]amino]-2,6-di-tert-butylphenol: trade name "Irganox 565" (manufactured by BASF Corporation), 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenylmethyl)-2,4,6-trimethylbenzene: trade name "ADK STAB AO-330" (manufactured by ADEKA Corporation), 1,3,5-tris(3, Examples of suitable esters include (5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (trade name "ADK STAB AO-20") (manufactured by ADEKA Corporation), octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name "ADK STAB AO-50") (manufactured by ADEKA Corporation), and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name "ADK STAB AO-60") (manufactured by ADEKA Corporation).Among these, the trade names "Irganox 1076" (manufactured by BASF), "Irganox 245" (manufactured by BASF), "Irganox 1010" (manufactured by BASF), and "ADK STAB AO-330" (manufactured by ADEKA) are preferably used.

[0029] Other phenolic compounds include, for example, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylenebis(oxyethylene)]: trade name "Irganox 245" (manufactured by BASF), 4,4',4''-(1-methylpropanyl-3-ylidene)tris[6-tert-butyl-m-cresol]: trade name "ADEKA STAB AO-30" (manufactured by ADEKA), 6,6' -di-tert-butyl-4,4'-butylidenedi-m-cresol: trade name "ADK STAB AO-40" (manufactured by ADEKA Corporation), 3,9-bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane: trade name "ADK STAB AO-80" (manufactured by ADEKA Corporation), and the like.

[0030] Examples of phosphite compounds include 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, trade name "ADK STAB PEP-36" (manufactured by ADEKA Corporation), 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, trade name "ADK STAB PEP-8" (manufactured by ADEKA Corporation), 2,2'-methylenebis(4,6-di-tert-butylphenyl)2-ethylhexyl phosphite, trade name "ADK STAB HP-10" (manufactured by ADEKA Corporation), and tris(2,4-di-tert-butylphenyl) phosphite, trade name "ADEKA STAB HP-10" (manufactured by ADEKA Corporation). Examples of suitable phosphates include "ADEKA STAB 2112" (manufactured by ADEKA Corporation), tris(nonylphenyl)phosphite (trade name "ADEKA STAB 1178" (manufactured by ADEKA Corporation), tetra-C12-15-alkyl(propane-2,2-diylbis(4,1-phenylene))bis(phosphite) (trade name "ADEKA STAB 1500" (manufactured by ADEKA Corporation), 2-ethylhexyldiphenylphosphite (trade name "ADEKA STAB C" (manufactured by ADEKA Corporation), isodecyldiphenylphosphite (trade name "ADEKA STAB 135A" (manufactured by ADEKA Corporation), triisodecylphosphite (trade name "ADEKA STAB 3010" (manufactured by ADEKA Corporation), and triphenylphosphite (trade name "ADEKA STAB TPP" (manufactured by ADEKA Corporation). Among these, "ADEKA STAB PEP-36" (manufactured by ADEKA Corporation) is preferred. Among these, the trade name "ADK STAB PEP-36" (manufactured by ADEKA Corporation) is preferably used. Among these, the trade name "ADK STAB PEP-36" (manufactured by ADEKA Corporation) is preferably used.

[0031] From the viewpoint of obtaining a foamed molded article having excellent shrinkage resistance, the content of the antioxidant (C) is preferably 0.4 to 3 parts by mass, more preferably 0.5 to 2 parts by mass, per 100 parts by mass of the combined total of the thermally foamable microspheres (A) and the base resin (B). When a commercially available product is used as the base resin (B), if an antioxidant is blended in the base resin (B), the antioxidant (hereinafter also referred to as "pre-added antioxidant") is also considered to be the antioxidant (C). In this case, the content of the antioxidant (C) is the total amount of the pre-added antioxidant and the antioxidant blended during the preparation of the masterbatch.

[0032] (Other Components) The masterbatch may contain components (hereinafter also referred to as "other components") other than the thermally expandable microspheres (A), the base resin (B), and the antioxidant (C) as long as the effects of the present invention are not impaired. Examples of other components include lubricants, plasticizers, stabilizers, fillers, and dispersibility improvers.

[0033] The masterbatch is obtained by melt-kneading the thermally expandable microspheres (A), the base resin (B), the antioxidant (C), and, if necessary, other components. The masterbatch may be in the form of, for example, powder, flakes, or pellets.

[0034] The expansion density of the masterbatch is preferably 0.005 g / ml or more and 1 g / ml or less, and more preferably 0.01 g / ml or more and 0.8 g / ml or less. The volume expansion ratio of the masterbatch is preferably 2.5 times or more and 150 times or less, and more preferably 2.5 times or more and 120 times or less.

[0035] (Shrinkage Resistance) The shrinkage resistance of the masterbatch is evaluated using a thermomechanical analyzer (TMA). Specifically, a container containing the masterbatch is used as a measurement sample and placed in the heating furnace of the thermomechanical analyzer (TMA). The temperature inside the heating furnace is raised to the foaming temperature, and the foaming temperature is maintained for a predetermined time. The height displacement of the masterbatch at each time point from the start of heating is measured, thereby evaluating the shrinkage resistance of the masterbatch. Specifically, as shown in FIG. 1 , when the minimum displacement of the masterbatch is 0% and the maximum displacement is 100%, the elapsed heat treatment times at which the displacement during expansion and contraction is 50% are calculated as 1 / 2Ta and 1 / 2Tb, respectively, and 1 / 2Tb - 1 / 2Ta is used as an index of shrinkage resistance.

[0036] In the above measurement, it is preferable to carry out the measurement in a state where an aluminum lid is placed on the top of the measurement sample and a force of 0.1 N is applied from above using a pressure pin. Note that the "displacement" refers to the amount of displacement of the pressure pin in the vertical direction when measuring with a thermomechanical analysis (TMA) device.

[0037] In the measurement sample, the amount of masterbatch used is preferably about 2.0 to 3.0 mg. The measurement container is preferably an SUS container with a diameter of 7 mm and a height of 2 mm.

[0038] The foaming temperature is preferably any one of 230° C., 240° C., and 250° C., and the total heating time from the start of heating is preferably any one of 20 minutes and 30 minutes.

[0039] When the foaming temperature of the masterbatch is 230°C, it is preferable to increase the temperature inside the heating furnace from 30°C to 170°C in 2 minutes, then increase the temperature from 170°C to 230°C in 0 minutes, and measure the height displacement of the masterbatch at each time from the start of heating at 230°C for a total heating time of 30 minutes from the point at 30°C. Under the above measurement conditions, 1 / 2Tb-1 / 2Ta is preferably 22 minutes or more, more preferably 25 minutes or more, and even more preferably 27 minutes or more.

[0040] When the foaming temperature of the masterbatch is 250°C, it is preferable to increase the temperature inside the heating furnace from 30°C to 190°C in 2 minutes, then increase the temperature from 190°C to 250°C in 0 minutes, and measure the height displacement of the masterbatch at each time from the start of heating at 250°C for a total heating time of 20 minutes from the point at 30°C. Under the above measurement conditions, 1 / 2Tb-1 / 2Ta is preferably 4.0 minutes or more, more preferably 6 minutes or more, and even more preferably 7 minutes or more.

[0041] <<Foam Molded Article>> A foam molded article can be obtained by adding the masterbatch of this embodiment to a thermoplastic resin and foam molding it. Examples of thermoplastic resins include polyethylene, polypropylene, polystyrene, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyvinyl chloride, acrylonitrile-styrene copolymer, acrylonitrile-butadiene-styrene copolymer, polyacetal, polyethylene terephthalate, polybutylene terephthalate, methacrylic, polycarbonate, polyamide, polyurethane, ionomer, and various thermoplastic elastomers (TPE, TPO, TPS, TPU, TPV, etc.). The content of the masterbatch varies depending on the expansion ratio of the final product, but is generally 0.1 to 20 parts by mass per 100 parts by mass of the thermoplastic resin. The molding method may be a conventional method such as injection molding.

[0042] The foamed molded articles are useful as injection molded articles, blow molded articles, calendar molded articles, and extrusion molded articles, for example, films, sheets, building materials (flooring materials, wall materials, embedded panel materials, etc.), automotive molded articles (sealing materials, interior molding materials such as door trims and instrument panels, body materials such as bumpers), shoe soles, etc.

[0043] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0044] <<Preparation and Evaluation of Masterbatches>> <Examples 1 to 12 and Comparative Examples 1 to 4> In the examples and comparative examples, first, the following masterbatch precursors MP1 and MP2 were prepared according to the method described below, and each of the obtained masterbatch precursors was mixed with antioxidant (C) to prepare each of the masterbatches of the following Examples 1 to 12 and Comparative Examples 1 to 4 according to the method described below. The maximum foaming temperature of the obtained masterbatch precursors, as well as the foaming density, volume foaming ratio, and shrinkage resistance of the obtained masterbatches were measured and evaluated according to the methods described below.

[0045] [Preparation of Masterbatch] (Materials Used) In the Examples and Comparative Examples, the following A1 to A2 were used as the thermally expandable microspheres (A): A1: S2640 (manufactured by Kureha Corporation, average particle size: 20.5 μm, foaming initiation temperature: 194° C., maximum foaming temperature: 265° C.) A2: S2340 (manufactured by Kureha Corporation, average particle size: 21.7 μm, foaming initiation temperature: 182° C., maximum foaming temperature: 242° C.)

[0046] In the examples and comparative examples, the following B1 was used as the base resin (B): B1: Excellen FX551 (linear low-density polyethylene, manufactured by Sumitomo Chemical Co., Ltd.) Note that no antioxidant was blended in the base resin B1.

[0047] In the examples and comparative examples, the following C1 to C5 were used as the antioxidant (C): C1: Irganox 1076 (manufactured by BASF Japan Ltd.) C2: Irganox 245 (manufactured by BASF Japan Ltd.) C3: Irganox 1010 (manufactured by BASF Japan Ltd.) C4: Adekastab PEP-36 (manufactured by ADEKA Corporation) C5: Adekastab AO-330 (manufactured by ADEKA Corporation)

[0048] (Preparation of Masterbatch Precursor) The thermally expandable microspheres (A) and the base resin (B) were mixed to the contents shown in Table 1 below to obtain each masterbatch precursor.

[0049]

[0050] (Preparation of Masterbatches) The masterbatch precursor obtained was mixed with the antioxidant (C) so as to have the contents shown in Tables 2 and 3 below, thereby obtaining the masterbatches of Examples 1 to 12 and Comparative Examples 1 to 4.

[0051]

[0052]

[0053] [Evaluation of Masterbatch Precursor] (Maximum Foaming Temperature) TMA measurement was carried out using a Mettler Toledo TMA / SDTA840. Using 2.0 to 3.0 mg of sample, the temperature was raised at a rate of 5°C / min, and the foaming behavior was observed. More specifically, the sample (masterbatch precursor) was placed in a container, and a load of 0.1 N was applied, and the temperature was raised at a rate of 5°C / min, and the height change was continuously measured. The temperature at which the height of the sample in the container reached its maximum was determined as the maximum foaming temperature (T max )

[0054] [Masterbatch Evaluation] (Foam Density) The masterbatches of the Examples and Comparative Examples were foamed, and the foam density was measured. Specifically, 0.2 to 0.3 g of the masterbatch was weighed into an aluminum cup, heated and foamed in an oven at a predetermined temperature (foaming temperature) for a predetermined time, removed, and placed in a 100 ml measuring flask. The volume was filled up with isopropanol, and the true density of the foamed masterbatch was determined from the sample weight and the weight after filling up (Archimedes method). For the masterbatches of Examples 1 to 5, 11 to 12, and Comparative Examples 1 to 3, the foam density was measured for those heat-treated at 240°C for 3 minutes and those heat-treated at 250°C for 3 minutes. For the masterbatches of Examples 6 to 10 and Comparative Example 4, the foam density was measured for those heat-treated at 230°C for 3 minutes and those heat-treated at 240°C for 3 minutes.

[0055] (Volume Expansion Ratio) The volume expansion ratio was calculated using the expansion ratio. Specifically, the following formula was used: Volume expansion ratio of masterbatch = true specific gravity of masterbatch before heating / true specific gravity of masterbatch after heat-foaming The true specific gravity of the masterbatch before heating was measured in the same manner as in measuring the foam density.

[0056] (Shrinkage Resistance) The masterbatches of the Examples and Comparative Examples were foamed, and their shrinkage resistance was measured. Specifically, approximately 2.0 to 3.0 mg of the masterbatch was placed in a measurement container (a stainless steel container with a diameter of 7 mm and a height of 2 mm), an aluminum lid was placed on top, and a force of 0.1 N was applied to the top using a pressure probe. The container was then placed in the heating furnace of a thermomechanical analysis (TMA) device. The furnace temperature was then heated for a predetermined time to foam the masterbatch, and the heating furnace temperature (foaming temperature) was maintained for a predetermined time, and the height displacement of the masterbatch was measured at each time point from the start of heating. When the minimum height was defined as 0% and the maximum foam height was defined as 100%, the elapsed time for heat treatment at which a displacement of 50% was reached during expansion and contraction was calculated as ½Ta (short-term side) and ½Tb (long-term side), respectively, and ½Tb - ½Ta was used as an index of shrinkage resistance. For the masterbatches of Examples 1 to 5, 11 to 12 and Comparative Examples 1 to 3, the temperature inside the heating furnace was raised from 30°C to 180°C over a set time of 2 minutes, then raised from 180°C to 240°C over a set time of 0 minutes, and heat-treated at 240°C for a total heating time of 20 minutes from the 30°C point; and the temperature inside the heating furnace was raised from 30°C to 190°C over a set time of 2 minutes, then raised from 190°C to 250°C over a set time of 0 minutes, and heat-treated at 250°C for a total heating time of 20 minutes from the 30°C point. ½Ta and ½Tb were measured for these masterbatches. For the masterbatches of Examples 6 to 10 and Comparative Example 4, the temperature inside the heating furnace was raised from 30°C to 170°C over a set time of 2 minutes, then raised from 170°C to 230°C over a set time of 0 minutes, and heat-treated at 230°C for a total heating time of 30 minutes from the 30°C point. Similarly, the temperature inside the heating furnace was raised from 30°C to 170°C over a set time of 2 minutes, then raised from 170°C to 250°C over a set time of 0 minutes, and heat-treated at 250°C for a total heating time of 20 minutes from the 30°C point. ½Ta and ½Tb were measured for these masterbatches.

[0057] From Tables 2 and 3, it can be seen that the masterbatches of Comparative Examples 1 to 4, which did not contain antioxidant (C), all had poor shrinkage resistance, with ½Tb−½Ta being less than 4.0 minutes when held at 250° C. On the other hand, the masterbatches of Examples 1 to 12, which contained antioxidant (C), all had ½Tb−½Ta being 4.0 minutes or more when held at 250° C., and were therefore excellent in shrinkage resistance.

Claims

1. A master batch comprising thermally foamable microspheres (A), a base resin (B), and an antioxidant (C), wherein the content of the antioxidant (C) is 0.2 parts by mass or more and 4 parts by mass or less per 100 parts by mass of the total of the thermally foamable microspheres (A) and the base resin (B).

2. The masterbatch according to claim 1, having a shrinkage resistance (250°C) of 4.0 minutes or more, as measured by the following measurement method: Shrinkage resistance (250°C) = 1 / 2Tb - 1 / 2Ta (a container containing the masterbatch is used as a measurement sample and placed in the heating furnace of a thermomechanical analyzer (TMA), the temperature inside the heating furnace is raised from 30°C to 190°C in a setting of 2 minutes, and then the temperature is raised from 190°C to 250°C in a setting of 0 minutes, and the masterbatch is heated at 250°C for a total heating time of 20 minutes from the point of 30°C. When the minimum height of the masterbatch is 0% and the maximum foaming height is 100%, the time on the short-term side when the height displacement is 50% is 1 / 2Ta and the time on the long-term side is 1 / 2Tb.) 3. The masterbatch according to claim 1, having a shrinkage resistance (230°C) of 22 minutes or more, as measured by the following measurement method: Shrinkage resistance (230°C) = 1 / 2Tb - 1 / 2Ta (a container containing the masterbatch is used as a measurement sample and placed in the heating furnace of a thermomechanical analyzer (TMA), the temperature inside the heating furnace is raised from 30°C to 170°C in a setting of 2 minutes, and then the temperature is raised from 170°C to 230°C in a setting of 0 minutes, and the masterbatch is heated at 230°C for a total heating time of 30 minutes from the point of 30°C. When the minimum height of the masterbatch is 0% and the maximum foaming height is 100%, the time on the short-term side at which the height displacement is 50% is 1 / 2Ta and the time on the long-term side is 1 / 2Tb.) 4. The masterbatch according to claim 2 or 3, wherein the base resin (B) is a polyethylene-based resin.

5. The masterbatch according to claim 2 or 3, wherein the antioxidant (C) comprises a phenolic compound including a hindered phenolic compound, or a phosphite compound.

6. The master batch according to claim 2 or 3, wherein the content of the antioxidant (C) is 0.4 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the total of the thermally foamable microspheres (A) and the base resin (B).

7. A foamed molded product made from the masterbatch according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Foamable resin composition and application of the same

    JP2012140608A

  • Resin composition for foaming resin sheet and foaming resin sheet

    JP2016160414A

  • Masterbatch of thermally expandable microcapsules

    JP2019108507A

  • Nucleating Agent for Foamed Cable Insulation

    JP2019529625A

  • Method for manufacturing thermoplastic resin composition pellet

    JP2023066410A