Resin composition, optical fiber, optical fiber manufacturing method, optical fiber ribbon, and optical fiber cable

The resin composition using plant-derived photopolymerizable urethane (meth)acrylate and specific monomers addresses the challenge of maintaining low-temperature characteristics and trauma resistance in optical fibers, achieving high biomass and performance equivalence to conventional fibers, thus supporting carbon neutrality.

WO2024247601A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016810
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2024-05-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current resin compositions for optical fiber secondary coating using plant-derived materials face challenges in maintaining the optical fiber's performance, particularly low-temperature characteristics and trauma resistance, while aiming for a high degree of biomass and carbon neutrality.

Method used

A resin composition incorporating photopolymerizable urethane (meth)acrylate derived from plant components, combined with a photopolymerization initiator, is used for the secondary coating of optical fibers, which enhances low-temperature characteristics and trauma resistance, with a biomass degree of 20% or more and 70% or less, and specific monomers like normal octyl (meth)acrylate and lauryl (meth)acrylate to improve toughness.

Benefits of technology

The solution provides optical fibers with excellent low-temperature characteristics and trauma resistance, contributing to carbon neutrality by increasing the biomass content and improving the mechanical properties of the resin layer, while maintaining performance equivalent to or exceeding conventional optical fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016810_05122024_PF_FP_ABST
    Figure JP2024016810_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This resin composition for a secondary coating of an optical fiber comprises a photoinitiator and a photopolymerizable compound containing a urethane (meth)acrylate derived from a plant component. An optical fiber according to the present disclosure comprises a glass fiber that includes a core and a cladding, a primary resin layer that is in contact with the glass fiber and covers the glass fiber, and a secondary resin layer that covers the primary resin layer, wherein the secondary resin layer contains a cured product of the abovementioned resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, optical fiber, optical fiber manufacturing method, optical fiber ribbon, and optical fiber cable

[0001] The present disclosure relates to a resin composition for a secondary coating of an optical fiber, an optical fiber, a method for manufacturing an optical fiber, an optical fiber ribbon, and an optical fiber cable. This application claims priority to Japanese Application No. 2023-090940, filed on June 1, 2023, and incorporates by reference all of the contents of said Japanese application.

[0002] Generally, optical fibers are provided with a coating resin layer for protecting the glass fiber, which is an optical transmission medium. The coating resin layer is composed of, for example, two layers: a primary resin layer in contact with the glass fiber and a secondary resin layer formed on the outer surface of the primary resin layer. For example, Patent Documents 1 to 5 describe resin compositions for secondary coatings that contain a photopolymerizable compound such as urethane (meth)acrylate.

[0003] Japanese Patent Application Laid-Open No. 2012-57124 Japanese Patent Application Laid-Open No. 2005-255955 Japanese Patent Application Laid-Open No. 2004-161991 Special Publication No. 2010-510332 Special Publication No. 2005-89586

[0004] A resin composition for a secondary coating of an optical fiber according to one embodiment of the present disclosure contains a photopolymerizable compound including a urethane (meth)acrylate derived from a plant component, and a photopolymerization initiator.

[0005] Fig. 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. Fig. 2 is a schematic cross-sectional view showing an optical fiber ribbon according to an embodiment. Fig. 3 is a schematic cross-sectional view showing an optical fiber ribbon according to an embodiment. Fig. 4 is a plan view showing the appearance of an optical fiber ribbon according to an embodiment. Fig. 5 is a schematic cross-sectional view showing an optical fiber cable according to an embodiment. Fig. 6 is a schematic cross-sectional view showing an optical fiber cable according to an embodiment.

[0006] [Problem to be Solved by the Present Disclosure] In recent years, various industries have placed importance on activities aimed at achieving the Sustainable Development Goals (SDGs). One such activity calls for contributing to a recycling-oriented society by utilizing renewable resources. One example of such renewable resources is biomass resources processed from plant-derived raw materials. Since the utilization of biomass resources is considered important from the perspective of carbon neutrality, there is also a demand in the field of optical fibers for forming a coating resin layer using a resin composition with a high biomass content. However, simply forming a coating resin layer using plant-derived raw materials makes it difficult to maintain the performance of the optical fiber, such as its low-temperature characteristics and external damage resistance.

[0007] The present disclosure aims to provide a resin composition that has a high biomass content and can form a resin layer suitable for a secondary coating of an optical fiber, as well as an optical fiber that has excellent low-temperature properties and external damage resistance.

[0008] [Effects of the Present Disclosure] According to the present disclosure, it is possible to provide a resin composition that has a high biomass content and is capable of forming a resin layer suitable for a secondary coating of an optical fiber, as well as an optical fiber that has excellent low-temperature properties and external damage resistance.

[0009] [Description of Embodiments of the Present Disclosure] First, the contents of the embodiments of the present disclosure will be listed and described.

[0010] (1) A resin composition for a secondary coating of an optical fiber according to one aspect of the present disclosure includes a photopolymerizable compound including a plant-derived urethane (meth)acrylate and a photopolymerization initiator. Such a resin composition has a high biomass content, can form a resin layer suitable for a secondary coating of an optical fiber, and can improve the low-temperature properties and external damage resistance of the optical fiber.

[0011] (2) In the above (1), from the viewpoint of further improving the low-temperature characteristics of the optical fiber, the biomass ratio of the urethane (meth)acrylate may be 20% or more and 70% or less.

[0012] (3) In the above (1) or (2), from the viewpoint of further improving the low-temperature characteristics of the optical fiber, the content of the urethane (meth)acrylate may be 10 parts by mass or more and 80 parts by mass or less based on 100 parts by mass of the total amount of the resin composition.

[0013] (4) In any of the above (1) to (3), the photopolymerizable compound may further contain a monomer derived from a plant component, in order to further increase the biomass content.

[0014] (5) In the above (4), from the viewpoint of imparting appropriate toughness to the secondary resin layer, the monomer derived from a plant component may be at least one selected from the group consisting of normal octyl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycerin di(meth)acrylate, decanediol di(meth)acrylate, glycerin propylene oxide-modified tri(meth)acrylate, and glycerin tri(meth)acrylate.

[0015] (6) In any of the above (1) to (5), the resin composition may have a biomass ratio of 10% or more and 50% or less, from the viewpoint of further improving the low-temperature characteristics and external damage resistance of the optical fiber.

[0016] (7) In any of the above (1) to (6), from the viewpoint of further improving the low-temperature characteristics of the optical fiber, the resin composition according to the present embodiment is applied to an optical fiber having an integrated light amount of 100 mJ / cm. 2 and an illumination intensity of 100 mW / cm 2 The glass transition temperature of the resin film when cured with ultraviolet light under the above conditions may be 60°C or higher and 100°C or lower.

[0017] (8) In the above (7), from the viewpoint of improving the lateral pressure resistance and external damage resistance of the optical fiber, the resin film may have a Young's modulus of 600 MPa or more and 2000 MPa or less at 23°C.

[0018] (9) An optical fiber according to one aspect of the present disclosure includes a glass fiber including a core and a cladding, a primary resin layer that contacts the glass fiber and coats the glass fiber, and a secondary resin layer that coats the primary resin layer, wherein the secondary resin layer contains a cured product of the resin composition described in any one of (1) to (8). Such an optical fiber can contribute to carbon neutrality while having low-temperature properties and external damage resistance equal to or better than those of conventional optical fibers.

[0019] (10) A method for producing an optical fiber according to one aspect of the present disclosure includes a coating step of coating the resin composition according to any one of (1) to (8) above on the outer periphery of a glass fiber including a core and a cladding, and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step. This makes it possible to produce an optical fiber with excellent low-temperature properties and external damage resistance.

[0020] (11) An optical fiber ribbon according to one aspect of the present disclosure includes a plurality of optical fibers as described in (9) arranged in parallel and coated with a ribbon resin. Such an optical fiber ribbon has excellent low-temperature properties and can be packed densely in an optical fiber cable.

[0021] (12) An optical fiber cable according to an aspect of the present disclosure includes the optical fiber ribbon according to (11) above housed within the cable. The optical fiber cable including such an optical fiber ribbon has excellent low-temperature characteristics.

[0022] (13) An optical fiber cable according to an aspect of the present disclosure includes a plurality of optical fibers according to the above (9) housed within the cable. Such an optical fiber cable has excellent low-temperature characteristics.

[0023] [Details of the Embodiments of the Present Disclosure] Specific examples of the resin composition and optical fiber according to the present embodiment will be described with reference to the drawings as necessary. The present disclosure is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims. In the following description, the same elements in the drawings will be denoted by the same reference numerals, and redundant explanations will be omitted. In this specification, (meth)acrylate means acrylate or the corresponding methacrylate, and the same applies to other similar expressions such as (meth)acryloyl. Furthermore, PO-modified means propylene oxide-modified, and EO-modified means ethylene oxide-modified. In this specification, ppm indicates mass ratio.

[0024] In this specification, the term "biomass degree" refers to the mass percentage of plant-derived components (biomass-derived components) in a resin composition or raw material. For example, if raw material A has a molecular weight of 100, and the plant-derived molecular weight is 70 and the petroleum-derived molecular weight is 30, the biomass degree of raw material A is 70%. Furthermore, the biomass degree of a resin composition containing 60 g of raw material B with a biomass degree of 30% and 40 g of raw material C with a biomass degree of 50% is (60 g × 30% + 40 g × 50%) / (60 g + 40 g) = 38%.

[0025] (Resin Composition) The resin composition for the secondary coating of an optical fiber according to this embodiment contains a photopolymerizable compound containing a plant-derived urethane (meth)acrylate and a photopolymerization initiator. The plant-derived urethane (meth)acrylate (hereinafter referred to as "urethane (meth)acrylate (A)") is a urethane (meth)acrylate synthesized using plant-derived raw materials. The use of urethane (meth)acrylate (A) allows the formation of a resin layer with a high biomass content, thereby improving the low-temperature properties and external damage resistance of the optical fiber.

[0026] The biomass ratio of the resin composition according to this embodiment may be 10% or more and 50% or less, 15% or more and 50% or less, 20% or more and 50% or less, or 25% or more and 50% or less, from the viewpoint of further improving the low-temperature characteristics and external damage resistance of the optical fiber.

[0027] From the viewpoint of further increasing the biomass degree of the resin composition, the biomass degree of the urethane (meth)acrylate (A) may be 20% or more and 70% or less, 25% or more and 65% or less, 30% or more and 60% or less, 35% or more and 55% or less, or 40% or more and 50% or less.

[0028] Generally, urethane (meth)acrylates can be obtained by reacting a polyol, a polyisocyanate, and a hydroxyl group-containing (meth)acrylate (or an isocyanate group-containing (meth)acrylate). The polyols include plant-derived polyols and petroleum-derived polyols, and the polyisocyanates include plant-derived polyisocyanates and petroleum-derived polyisocyanates.

[0029] The urethane (meth)acrylate (A) can be synthesized by using at least one of a plant-derived polyol and a plant-derived polyisocyanate as a raw material. When synthesizing the urethane (meth)acrylate (A), a plant-derived polyol and a petroleum-derived polyol may be used in combination, or a plant-derived polyisocyanate and a petroleum-derived polyisocyanate may be used in combination.

[0030] Examples of plant-derived polyols include plant-derived polyester polyols, plant-derived polyether polyols, plant-derived polycarbonate polyols, soybean oil-modified polyols, castor oil-modified polyols, algae-derived polyols, and cardanol polyols.

[0031] Examples of plant-derived polyester polyols include polyester polyols having a structure derived from dimer acid, polyester polyols having a structure derived from 1,3-propanediol, and polyester polyols using sebacic acid derived from castor oil.

[0032] Examples of plant-derived polyether polyols include polyether polyols obtained by ring-opening polymerization of tetrahydrofuran, polyether polyols obtained by copolymerization of tetrahydrofuran and 2-methyltetrahydrofuran, and polyether polyols obtained by polymerizing 1,3-propanediol.

[0033] Examples of plant-derived polycarbonate polyols include isosorbide-derived polycarbonate polyols and polycarbonate polyols having a structure derived from 1,10-decanediol.

[0034] Examples of petroleum-derived polyols include polyethylene glycol (PEG), polypropylene glycol (PPG), PEG-PPG-PEG block copolymers, polycarbonate diol, polybutadiene diol, and bisphenol A-ethylene oxide adduct diol.

[0035] Examples of plant-derived polyisocyanates include 1,5-pentamethylene diisocyanate, dimer acid diisocyanate, lysine diisocyanate, lysine triisocyanate, octamethylene diisocyanate, and decamethylene diisocyanate.

[0036] Examples of petroleum-derived polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, 1,5-naphthalene diisocyanate, norbornene diisocyanate, tetramethylxylylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0037] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, caprolactone (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, 2-hydroxy-o-phenylphenolpropyl (meth)acrylate, 2-hydroxy-3-methacrylpropyl acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol tri(meth)acrylate.

[0038] The urethane (meth)acrylate (A) may have two or more, three or more, or four or more (meth)acryloyl groups, which are photopolymerizable functional groups. The number of functional groups in the urethane (meth)acrylate (A) may be two or three.

[0039] The number average molecular weight (Mn) of the urethane (meth)acrylate (A) may be 500 or more and 10,000 or less, 1,000 or more and 9,000 or less, 1,500 or more and 8,000 or less, 2,000 or more and 7,000 or less, or 2,500 or more and 5,000 or less. The weight average molecular weight (Mw) of the urethane (meth)acrylate (A) may be 1,000 or more and 20,000 or less, 1,500 or more and 10,000 or less, 2,000 or more and 8,000 or less, 2,500 or more and 7,000 or less, or 3,000 or more and 6,000 or less.

[0040] The glass transition temperature (Tg) of the homopolymer of the urethane (meth)acrylate (A) may be 0° C. or higher, 20° C. or higher, or 40° C. or higher, and may be 100° C. or lower, 80° C. or lower, or 70° C. or lower. Tg can be measured by a dynamic viscoelasticity test of the homopolymer.

[0041] Commercially available urethane (meth)acrylate (A) products include, for example, SARBIO 7300NS, SARBIO 7302NS, SARBIO 7403NS, SARBIO 7404NS, SARBIO 7405NS, and SARBIO 7406NS manufactured by Arkema, UFB-C01 and UFB-0146 manufactured by Kyoeisha Chemical Co., Ltd., UT-8166, UT-8200, UT-7792, and UT-7999 manufactured by Mitsubishi Chemical Corporation, and 8UX-2017A manufactured by Taisei Fine Chemical Co., Ltd.

[0042] From the viewpoint of further improving the low-temperature characteristics of the optical fiber, the content of the urethane (meth)acrylate (A) may be 10 parts by mass or more and 80 parts by mass or less, 10 parts by mass or more and 75 parts by mass or less, 15 parts by mass or more and 70 parts by mass or less, or 20 parts by mass or more and 60 parts by mass or less, based on 100 parts by mass of the total amount of the resin composition.

[0043] The resin composition according to this embodiment may further contain a petroleum-derived urethane (meth)acrylate (hereinafter referred to as "urethane (meth)acrylate (B)"). The urethane (meth)acrylate (B) is a urethane (meth)acrylate that does not use plant-derived raw materials. As the urethane (meth)acrylate (B), for example, a reaction product of a petroleum-derived polyol, a petroleum-derived polyisocyanate, and a hydroxyl group-containing (meth)acrylate can be used.

[0044] From the viewpoint of obtaining a Young's modulus suitable for the secondary resin layer, the number average molecular weight (Mn) of the petroleum-derived polyol used in synthesizing the urethane (meth)acrylate (B) may be 300 or more and 2500 or less, 500 or more and 2000 or less, or 800 or more and 1500 or less.

[0045] From the viewpoint of obtaining a Young's modulus suitable for the secondary resin layer, the Mn of the urethane (meth)acrylate (B) may be 500 or more and 10,000 or less, 1,000 or more and 9,000 or less, 1,500 or more and 8,000 or less, or 2,000 or more and 7,000 or less. The Mw of the urethane (meth)acrylate (B) may be 1,000 or more and 20,000 or less, 1,500 or more and 10,000 or less, 2,000 or more and 8,000 or less, or 2,500 or more and 7,000 or less.

[0046] The Mn and Mw of the urethane (meth)acrylate (A) and the urethane (meth)acrylate (B) can be measured by gel permeation chromatography (GPC).

[0047] As a catalyst for synthesizing the urethane (meth)acrylate (A) and the urethane (meth)acrylate (B), for example, an organotin compound is used. Examples of the organotin compound include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexyl mercaptoacetate), dibutyltin bis(isooctyl mercaptoacetate), and dibutyltin oxide.

[0048] When synthesizing the urethane (meth)acrylate (A) and the urethane (meth)acrylate (B), 4-methoxyphenol or 2,6-di-tert-butyl-p-cresol may be added as a polymerization inhibitor.

[0049] The resin composition according to this embodiment may further include, as the photopolymerizable compound, a photopolymerizable compound (hereinafter referred to as a "monomer") other than the urethane (meth)acrylate (A) and the urethane (meth)acrylate (B). The monomer can be distinguished from the urethane (meth)acrylate in that it does not have a urethane bond. Examples of the monomer include (meth)acrylic acid esters, N-vinyl compounds, (meth)acrylamide compounds, and epoxy (meth)acrylates. The monomer may be a monofunctional monomer having one photopolymerizable ethylenically unsaturated group, or a polyfunctional monomer having two or more ethylenically unsaturated groups.

[0050] Examples of monofunctional (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, cyclic trimethylolpropane formal acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, nonylphenolpolyethylene glycol (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, m-phenoxybenzyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl acrylate, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and ω-carboxy-polycaprolactone (meth)acrylate.

[0051] Examples of polyfunctional (meth)acrylic acid esters include ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate. , bifunctional monomers such as 1,12-dodecanediol di(meth)acrylate, 1,14-tetradecanediol di(meth)acrylate, 1,16-hexadecanediol di(meth)acrylate, 1,20-eicosanediol di(meth)acrylate, isopentyldiol di(meth)acrylate, 3-ethyl-1,8-octanediol di(meth)acrylate, tricyclodecanol di(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, bisphenol F epoxy di(meth)acrylate, EO adduct di(meth)acrylate of bisphenol A, EO adduct di(meth)acrylate of bisphenol F, PO adduct di(meth)acrylate of bisphenol A, and PO adduct di(meth)acrylate of bisphenol F;Trimethylolpropane tri(meth)acrylate, trimethyloloctane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, trimethylolpropane polypropoxy tri(meth)acrylate, trimethylolpropane polyethoxypolypropoxy tri(meth)acrylate, tris[(meth)acryloyloxyethyl]isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol polyethoxytetra(meth)acrylate trifunctional or higher functional monomers such as tris[(meth)acryloyloxyethyl]isocyanurate, ...

[0052] Examples of the (meth)acrylamide compound include dimethyl(meth)acrylamide, diethyl(meth)acrylamide, (meth)acryloylmorpholine, hydroxymethyl(meth)acrylamide, hydroxyethyl(meth)acrylamide, isopropyl(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, dimethylaminopropylacrylamide methyl chloride, diacetone acrylamide, (meth)acryloylpiperidine, (meth)acryloylpyrrolidine, (meth)acrylamide, N-hexyl(meth)acrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide.

[0053] Examples of N-vinyl compounds include N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylmethyloxazolidinone, N-vinylimidazole, and N-vinyl-N-methylacetamide.

[0054] As the epoxy (meth)acrylate, for example, a reaction product of a diglycidyl ether compound having a bisphenol skeleton and a compound having a (meth)acryloyl group, such as (meth)acrylic acid, can be used.

[0055] In order to further increase the biomass ratio of the resin composition, a monomer derived from a plant component may be used as the monomer. From the viewpoint of further increasing the biomass ratio of the resin composition, the biomass ratio of the monomer derived from a plant component may be 15% or more and 75% or less, 18% or more and 72% or less, or 20% or more and 70% or less.

[0056] Examples of monomers derived from plant components include normal octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isoamyl (meth)acrylate, glycerin carbonate (meth)acrylate, glycerin di(meth)acrylate, decanediol di(meth)acrylate, glycerin tri(meth)acrylate, glycerin PO-modified tri(meth)acrylate, diglycerin EO-modified tetra(meth)acrylate, polyglycerin hexa(meth)acrylate, and sorbitol EO-modified hexa(meth)acrylate.

[0057] In view of ease of adjusting the Young's modulus and Tg of the resin layer, at least one monomer selected from the group consisting of normal octyl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycerin di(meth)acrylate, decanediol di(meth)acrylate, glycerin PO-modified tri(meth)acrylate, and glycerin tri(meth)acrylate may be used as the plant-derived monomer.

[0058] The content of the monomer derived from plant components may be 10 parts by mass or more and 60 parts by mass or less, 10 parts by mass or more and 55 parts by mass or less, or 15 parts by mass or more and 50 parts by mass or less, based on 100 parts by mass of the total amount of the resin composition.

[0059] The photopolymerization initiator can be appropriately selected from known radical photopolymerization initiators. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184, manufactured by IGM Resins), 2,2-dimethoxy-2-phenylacetophenone (Omnirad 651, manufactured by IGM Resins), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Omnirad TPO, manufactured by IGM Resins), ethyl (2,4,6-trimethylbenzoyl)-phenylphosphinate (Omnirad TPO-L, manufactured by IGM Resins), and 2-benzyl-2-dimethylamino-4'-morpholinobutyrophenone (Omnirad 369, manufactured by IGM Resins). Examples of suitable amines include 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad 379, IGM Resins), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, IGM Resins), and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Omnirad 907, IGM Resins).

[0060] The photopolymerization initiator may be a mixture of two or more types. The photopolymerization initiator may contain 2,4,6-trimethylbenzoyldiphenylphosphine oxide, as this provides an excellent rapid curing property of the resin composition.

[0061] The content of the photopolymerization initiator may be 0.1 parts by mass or more and 5 parts by mass or less, 0.3 parts by mass or more and 4 parts by mass or less, or 0.4 parts by mass or more and 3 parts by mass or less, based on 100 parts by mass of the total amount of the resin composition.

[0062] The resin composition according to this embodiment may further contain a sensitizer, a photoacid generator, a leveling agent, an antifoaming agent, an antioxidant, an ultraviolet absorber, and the like.

[0063] Examples of the sensitizer include anthracene compounds such as 9,10-dibutoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene; thioxanthone compounds such as 2,4-diethylthioxanthone, 2,4-diethylthioxanthen-9-one, 2-isopropylthioxanthone, and 4-isopropylthioxanthone; amine compounds such as triethanolamine, methyldiethanolamine, and triisopropanolamine; benzoin compounds, anthraquinone compounds, ketal compounds, and benzophenone compounds.

[0064] The photoacid generator includes A + B - Examples of the photoacid generator include sulfonium salts such as CPI-100P, 101A, 110P, 200K, 210S, 310B, and 410S (manufactured by San-Apro Ltd.) and Omnicat 270 and 290 (manufactured by IGM Resins), and iodonium salts such as CPI-IK-1 (manufactured by San-Apro Ltd.), Omnicat 250 (manufactured by IGM Resins), and WPI-113, 116, 124, 169, and 170 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).

[0065] From the viewpoint of coatability, the viscosity of the resin composition according to this embodiment at 25°C may be 0.5 Pa·s or more and 20 Pa·s or less, 0.8 Pa·s or more and 18 Pa·s or less, or 1 Pa·s or more and 10 Pa·s or less. The viscosity of the resin composition at 25°C is measured using a rheometer ("MCR-102" manufactured by Anton Paar) with a cone plate CP25-2 and a shear rate of 10 s -1 The measurement can be performed under the following conditions.

[0066] From the viewpoint of improving the low-temperature characteristics of the optical fiber, the resin composition is applied to an optical fiber with an integrated light amount of 100 mJ / cm 2 and an illumination intensity of 100 mW / cm 2 The Tg of the resin film when cured with ultraviolet light under the above conditions may be 60°C or more and 100°C or less, 65°C or more and 99°C or less, 68°C or more and 98°C or less, or 70°C or more and 98°C or less.

[0067] From the viewpoint of improving the lateral pressure resistance and external damage resistance of the optical fiber, the resin composition is applied to the optical fiber with an integrated light dose of 100 mJ / cm 2 and an illumination intensity of 100 mW / cm 2 The Young's modulus of the resin film when cured with ultraviolet light under the above conditions may be 600 MPa or more and 3000 MPa or less, 650 MPa or more and 2000 MPa or less, or 700 MPa or more and 1300 MPa or less at 23°C.

[0068] 1 is a schematic cross-sectional view showing an example of an optical fiber according to the present embodiment. The optical fiber 10 includes a glass fiber 13 including a core 11 and a cladding 12, and a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15 provided around the glass fiber 13.

[0069] The cladding 12 surrounds the core 11. The core 11 and the cladding 12 mainly contain glass such as silica glass, and for example, the core 11 can be made of silica glass doped with germanium or pure silica glass, and the cladding 12 can be made of pure silica glass or silica glass doped with fluorine.

[0070] 1 , for example, the outer diameter (D2) of the glass fiber 13 is approximately 100 μm to 125 μm, and the diameter (D1) of the core 11 constituting the glass fiber 13 is approximately 7 μm to 15 μm. The thickness of the coating resin layer 16 is typically approximately 22 μm to 70 μm. The thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be approximately 5 μm to 50 μm.

[0071] When the outer diameter of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 60 μm to 70 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 10 μm to 50 μm, for example, the thickness of the primary resin layer 14 may be 35 μm and the thickness of the secondary resin layer 15 may be 25 μm. The outer diameter of the optical fiber 10 may be about 245 μm to 265 μm.

[0072] When the outer diameter of the glass fiber 13 is about 125 μm and the thickness of the coating resin layer 16 is 20 μm or more and 48 μm or less, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 8 μm to 38 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 165 μm to 221 μm.

[0073] When the outer diameter of the glass fiber 13 is about 100 μm and the thickness of the coating resin layer 16 is 22 μm to 37 μm, the thickness of each of the primary resin layer 14 and the secondary resin layer 15 may be about 5 μm to 32 μm, for example, the thickness of the primary resin layer 14 may be 25 μm and the thickness of the secondary resin layer 15 may be 10 μm. The outer diameter of the optical fiber 10 may be about 144 μm to 174 μm.

[0074] By applying the resin composition according to this embodiment to the secondary resin layer, an optical fiber having excellent low-temperature characteristics while increasing the biomass content can be produced.

[0075] The method for manufacturing an optical fiber according to this embodiment includes a coating step of coating the resin composition on the outer periphery of a glass fiber including a core and a cladding, and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step.

[0076] The primary resin layer 14 can be formed by curing a resin composition containing, for example, a photopolymerizable compound including urethane (meth)acrylate, a photopolymerization initiator, a silane coupling agent, etc. The resin composition forming the primary resin layer has a different composition from the resin composition for the secondary coating. The resin composition for the primary coating can be prepared using a conventionally known technique.

[0077] From the viewpoint of improving the microbending resistance of the optical fiber, the Young's modulus of the primary resin layer may be 0.80 MPa or less, 0.70 MPa or less, 0.60 MPa or less, or 0.50 MPa or less at 23°C ± 2°C. If the Young's modulus of the primary resin layer exceeds 0.80 MPa, external forces may be more easily transmitted to the glass fiber, and the increase in transmission loss due to microbending may be significant. From the viewpoint of improving the low-temperature properties of the optical fiber, the Young's modulus of the primary resin layer may be 0.10 MPa or more, 0.15 MPa or more, or 0.20 MPa or more at 23°C ± 2°C.

[0078] The Young's modulus of the primary resin layer can be measured by the Pullout Modulus (POM) method at 23°C. Two locations of the optical fiber are fixed with two chuck devices, and the portion of the coating resin layer (primary resin layer and secondary resin layer) between the two chuck devices is removed. Next, one chuck device is fixed, and the other chuck device is slowly moved in the opposite direction of the fixed chuck device. When the length of the portion of the optical fiber sandwiched between the moving chuck devices is L, the amount of chuck movement is Z, the outer diameter of the primary resin layer is Dp, the outer diameter of the glass fiber is Df, the Poisson's ratio of the primary resin layer is n, and the load during movement of the chuck device is W, the Young's modulus of the primary resin layer can be calculated using the following formula: Young's modulus (MPa) = ((1 + n)W / πLZ) × ln(Dp / Df)

[0079] From the viewpoint of improving the microbending resistance of the optical fiber, the Young's modulus of the secondary resin layer may be 600 MPa or more, 700 MPa or more, or 800 MPa or more at 23° C.±2° C. The upper limit of the Young's modulus of the secondary resin layer is not particularly limited, but from the viewpoint of imparting appropriate toughness to the secondary resin layer, it may be 3000 MPa or less, 2500 MPa or less, or 2000 MPa or less at 23° C.±2° C.

[0080] The Young's modulus of the secondary resin layer can be measured by the following method. First, the optical fiber is immersed in a mixed solvent of acetone and ethanol, and only the coating resin layer is extracted into a cylindrical shape. At this time, the primary resin layer and the secondary resin layer are integrated, but the Young's modulus of the primary resin layer is 1 / 10,000 to 1 / 1,000 of that of the secondary resin layer, so the Young's modulus of the primary resin layer can be ignored. Next, the solvent is removed from the coating resin layer by vacuum drying, and then a tensile test (tensile speed: 1 mm / min) is performed at 23°C, and the Young's modulus can be determined using the secant equation with 2.5% strain.

[0081] The method for manufacturing an optical fiber according to this embodiment uses the resin composition according to this embodiment as the resin composition for the secondary coating, thereby making it possible to manufacture an optical fiber with a high biomass content and excellent low-temperature properties.

[0082] (Optical Fiber Ribbon) The optical fibers according to this embodiment can be used to fabricate an optical fiber ribbon, which is formed by arranging a plurality of the optical fibers in parallel and coating them with a ribbon resin.

[0083] 2 is a schematic cross-sectional view showing an optical fiber ribbon according to one embodiment. The optical fiber ribbon 100 includes a plurality of optical fibers 10 and a connecting resin layer 40 in which the optical fibers 10 are (integrally) coated with a ribbon resin and connected. While FIG. 2 shows four optical fibers 10 as an example, the number is not particularly limited.

[0084] The optical fibers 10 may be integrated in a state where they are in contact with each other and arranged in parallel, or some or all of the optical fibers 10 may be integrated in a state where they are arranged in parallel with a fixed interval between them. The center-to-center distance F between adjacent optical fibers 10 may be 220 μm or more and 280 μm or less. When the center-to-center distance is 220 μm or more and 280 μm or less, the optical fibers can be easily placed in existing V-grooves, and an optical fiber ribbon with excellent bulk fusion splicing properties can be obtained. The thickness T of the optical fiber ribbon 100 may be 164 μm or more and 285 μm or less, depending on the outer diameter of the optical fibers 10.

[0085] 3 is a schematic cross-sectional view showing an example of an optical fiber ribbon in which optical fibers are integrated in a state in which they are arranged in parallel at a fixed interval. The optical fiber ribbon 100A shown in FIG. 3 is formed by connecting 12 optical fibers 10, each of which has two optical fibers 10, at a fixed interval with a ribbon resin. The ribbon resin forms a connecting resin layer 40.

[0086] The ribbon resin may be a resin material generally known as a ribbon material. From the viewpoint of preventing damage to the optical fiber 10 and facilitating its severability, the ribbon resin may contain a thermosetting resin such as a silicone resin, an epoxy resin, or a urethane resin, or an ultraviolet-curing resin such as an epoxy acrylate, a urethane acrylate, or a polyester acrylate.

[0087] When the optical fibers 10 are arranged in parallel at regular intervals, i.e., when adjacent optical fibers 10 are joined via ribbon resin without touching each other, the thickness of the connecting portion at the center of the optical fibers 10 may be 150 μm or more and 220 μm or less. Because the optical fiber ribbon is prone to deformation when being stored in a cable, the optical fiber ribbon may have a recess at the connecting portion of the optical fibers. The recess may be formed in a triangular shape with a narrowing angle on one side of the connecting portion.

[0088] The optical fiber ribbon according to this embodiment may have connecting portions and non-connecting portions intermittently in the longitudinal and width directions. FIG. 4 is a plan view showing the appearance of an optical fiber ribbon according to one embodiment. The optical fiber ribbon 100B has a plurality of optical fibers, a plurality of connecting portions 20, and non-connecting portions (separated portions) 21. The non-connecting portions 21 are formed intermittently in the longitudinal direction of the optical fiber ribbon. The optical fiber ribbon 100B is an intermittently connected optical fiber ribbon in which connecting portions 20 and non-connecting portions 21 are provided intermittently in the longitudinal direction for every two optical fibers 10A. A "connecting portion" refers to a portion where adjacent optical fibers are integrated via a connecting resin layer, and a "non-connecting portion" refers to a portion where adjacent optical fibers are not integrated via a connecting resin layer and there is a gap between the optical fibers.

[0089] In the optical fiber ribbon having the above configuration, the non-connecting portions 21 are intermittently provided at the connecting portions 20 provided every two fibers, making the optical fiber ribbon easily deformable. Therefore, when mounting the optical fiber ribbon in an optical fiber cable, the optical fiber ribbon can be easily rolled up and mounted, making it suitable for high-density mounting. Furthermore, the connecting portions 20 can be easily torn starting from the non-connecting portions 21, making it easy to separate the optical fibers 10 from the optical fiber ribbon into individual fibers.

[0090] The optical fiber ribbon according to this embodiment uses the above optical fiber, and therefore has a high biomass content, excellent low-temperature properties, and can be packed densely into an optical fiber cable.

[0091] (Optical fiber cable) In the optical fiber cable according to the present embodiment, the optical fiber ribbon is housed within the cable. Examples of the optical fiber cable include a slotted optical fiber cable having a plurality of slots (grooves). The optical fiber ribbons can be mounted within the slots so that the mounting density in each slot is approximately 25% to 65%. Mounting density refers to the ratio of the cross-sectional area of ​​the optical fiber ribbon mounted within the slot to the cross-sectional area of ​​the slot. The optical fiber cable according to the present embodiment may also be configured such that the plurality of optical fibers are housed within the cable without being coated with a ribbon resin.

[0092] An example of an optical fiber cable according to this embodiment will be described with reference to Figures 5 and 6. In Figures 5 and 6, an intermittently connected optical fiber ribbon is housed, but a bundle of optical fibers that are not coated with a ribbon resin may also be housed.

[0093] FIG. 5 is a schematic cross-sectional view of a slotless optical fiber cable 60 using the intermittently connected optical fiber ribbons 100B described above. The optical fiber cable 60 includes a cylindrical tube 61 and multiple optical fiber ribbons 100B. The multiple optical fiber ribbons 100B may be bundled together using fillers 62 such as aramid fibers. Each of the multiple optical fiber ribbons 100B may have different markings. The optical fiber cable 60 is formed by twisting multiple bundled optical fiber ribbons 100B together, extruding a resin to form a tube 61 around the bundle, and then covering the tube with a tension member 63 and an outer jacket 64. If waterproofing is required, a water-absorbing yarn may be inserted inside the tube 61. The tube 61 may be formed using a resin such as polybutylene terephthalate or high-density polyethylene. A tear cord 65 may be provided on the outside of the tube 61.

[0094] FIG. 6 is a schematic cross-sectional view of a slotted optical fiber cable 70 using the intermittently connected optical fiber ribbons 100B described above. The optical fiber cable 70 includes a slotted rod 72 having a plurality of slots 71 and a plurality of optical fiber ribbons 100B. The optical fiber cable 70 is configured such that a plurality of slots 71 are radially formed in a slotted rod 72 having a central tension member 73. The slots 71 may be twisted in a spiral or SZ configuration along the length of the optical fiber cable 70. Each slot 71 accommodates a plurality of optical fiber ribbons 100B that have been unwound from a parallel state and placed in a densely packed state. Each optical fiber ribbon 100B may be bundled with an identification bundling material. A holding winding tape 74 is wound around the slotted rod 72, and an outer jacket 75 is formed around the holding winding tape 74. The outer jackets 64 and 75 may be formed using a resin such as polyvinyl chloride or polyethylene.

[0095] An optical fiber cable including the optical fiber or optical fiber ribbon according to this embodiment has a high biomass content and excellent low-temperature properties.

[0096] The present disclosure will be described in more detail below by showing the results of evaluation tests using examples and comparative examples according to the present disclosure. Note that the present disclosure is not limited to these examples.

[0097] [Synthesis of Urethane Acrylate] (B-1) Polypropylene glycol with an Mn of 1000 (trade name "Sannyx PP-1000" manufactured by Sanyo Chemical Industries, Ltd.) and 2,4-tolylene diisocyanate (TDI) were charged into a reaction vessel so that the molar ratio of NCO to OH (NCO / OH) was 2.0. Subsequently, 200 ppm of dibutyltin dilaurate was added as a catalyst relative to the final total amount charged, and 500 ppm of 2,6-di-tert-butyl-p-cresol (BHT) was added as a polymerization inhibitor relative to the final total amount charged. Thereafter, the mixture was reacted at 60°C for 1 hour to prepare an NCO-terminated prepolymer. Next, 2-hydroxyethyl acrylate (HEA) was added so that the molar ratio of OH of HEA to NCO of the NCO-terminated prepolymer was 1.05, and the mixture was reacted at 60°C for 1 hour to obtain urethane acrylate (B-1). The urethane acrylate (B-1) had an Mn of 3,200 and an Mw of 3,800.

[0098] (Z-1) An NCO-terminated prepolymer was prepared by reacting polypropylene glycol (trade name "PP-3000" manufactured by Sanyo Chemical Industries, Ltd.) with TDI so that the NCO / OH ratio was 1.5. As a catalyst, 200 ppm of dibutyltin dilaurate was added relative to the final total amount charged, and 500 ppm of BHT was added relative to the final total amount charged as a polymerization inhibitor. Next, methanol was added so that the molar ratio of methanol to OH (MeOH / NCO) of the NCO-terminated prepolymer was 0.2, and HEA was added so that the molar ratio of OH in HEA was 0.85. The mixture was allowed to react at 60°C for 1 hour to obtain urethane acrylate (Z-1). The urethane acrylate (Z-1) had an Mn of 13,100 and an Mw of 17,700.

[0099] The Mn of polypropylene glycol is a value calculated from the hydroxyl value. The Mn and Mw of urethane acrylate were measured using a Waters ACQUITY APC RI system under the following conditions: sample concentration: 0.2 mass% THF solution, injection volume: 20 μL, sample temperature: 15 ° C, mobile phase: THF, XT column for organic solvents: particle diameter 2.5 μm, pore size 450 Å, column inner diameter 4.6 × column length 150 mm + particle diameter 2.5 μm, pore size 125 Å, column inner diameter 4.6 × column length 150 mm + particle diameter 1.7 μm, pore size 45 Å, column inner diameter 4.6 × column length 150 mm, column temperature: 40 ° C, flow rate: 0.8 mL / min.

[0100] The following urethane acrylates were prepared as urethane acrylate (A): Urethane acrylate (A-1): SARBIO 7302NS manufactured by Arkema (biomass ratio: 44%, Mn: 3100, Mw: 5000, Tg: 68°C, number of functional groups: 3) Urethane acrylate (A-2): UFB-0146 manufactured by Kyoeisha Chemical Co., Ltd. (biomass ratio: 47%, Mn: 4100, Mw: 5400, Tg: 54°C, number of functional groups: 2)

[0101] The following monomers were prepared as plant-derived monomers. LA: Lauryl acrylate (biomass degree: 70%) IBXA: Isobornyl acrylate (biomass degree: 66%) NOAA: Normal octyl acrylate (biomass degree: 61%) THFA: Tetrahydrofurfuryl acrylate (biomass degree: 54%) DDA: Decanediol diacrylate (manufactured by Arkema, trade name "SARBIO 5201NS", biomass degree: 50%) GLDA: Glycerin diacrylate (manufactured by Toagosei Co., Ltd., trade name "Aronix M-920", biomass degree: 45%) GLTA: Glycerin triacrylate (manufactured by Toagosei Co., Ltd., trade name "Aronix M-930", biomass degree: 37%) GLPOTA: Glycerin PO-modified triacrylate (manufactured by Arkema, trade name "SARBIO 5300NS, biomass content: 21%)

[0102] Phenoxyethyl acrylate (PEA), tripropylene glycol diacrylate (TPGDA), and bisphenol A epoxy di(meth)acrylate (BisAEA) (manufactured by Osaka Organic Chemical Industry Co., Ltd., product name "Viscoat #540") were prepared as petroleum-derived monomers. Omnirad TPO and Omnirad 184 were prepared as photopolymerization initiators.

[0103] [Resin composition for secondary coating] A resin composition for secondary coating for each test example was prepared by mixing urethane acrylate, monomer, and photopolymerization initiator in the amounts (parts by mass) shown in Table 1. The biomass degree of the resin composition was calculated from the biomass degree of each raw material. Test Examples 1 to 11 correspond to working examples, and Test Examples 12 to 14 correspond to comparative examples.

[0104] [Resin Film] After applying the resin composition onto a polyethylene terephthalate (PET) film using a spin coater, the resin composition was applied to the film at 100 mJ / cm using an electrodeless UV lamp system (D bulb, manufactured by Heraeus). 2 and 100 mW / cm 2 The resin film was peeled off from the PET film to obtain a resin film.

[0105] (Young's Modulus) A resin film was punched into a dumbbell shape according to JIS K 7127 Type 5, and pulled using a tensile tester at 23±2°C, 50±10% RH, at a pulling rate of 1 mm / min, with a gauge length of 25 mm, to obtain a stress-strain curve. The Young's modulus of the resin film was calculated by dividing the stress obtained by the secant equation at 2.5% strain by the cross-sectional area of ​​the resin film.

[0106] (Glass Transition Temperature) The resin film was punched into a strip shape with a width of 6 mm, and the dynamic viscoelasticity was measured using an "RSA-G2" manufactured by TA Instruments under the conditions of a tensile mode (gauge length: 25 mm), a frequency of 11 Hz, a temperature rise rate of 5°C / min, and a temperature range of 25°C to 150°C, and the peak top temperature of tan δ was determined as Tg.

[0107] [Resin composition for primary coating] A resin composition for primary coating was obtained by mixing 75 parts by mass of urethane acrylate (Z-1), 18 parts by mass of nonylphenol polyethylene glycol acrylate (manufactured by Miwon, trade name "Miramer M164"), 5 parts by mass of N-vinyl caprolactam, 1 part by mass of Omnirad TPO, and 1 part by mass of 3-acryloxypropyltrimethoxysilane.

[0108] [Optical Fiber] A resin composition for a primary coating and a resin composition for a secondary coating were each applied to the outer peripheral surface of a glass fiber 13 having a diameter of 125 μm. Next, each resin composition was cured by irradiating with ultraviolet light to form a coating resin layer 16 including a primary resin layer 14 and a secondary resin layer 15, thereby producing an optical fiber 10. The thickness of the primary resin layer 14 was 35 μm, and the thickness of the secondary resin layer 15 was 25 μm, and an optical fiber having an outer diameter of 245 μm was obtained.

[0109] (Low-temperature characteristics) An optical fiber was wound in one layer around a glass bobbin with a tension of 50 g, and the transmission characteristics of signal light with a wavelength of 1550 nm were measured to determine the transmission loss under the temperature conditions of 23° C. and −40° C. If the difference in transmission loss, obtained by subtracting the transmission loss at 23° C. from the transmission loss at −40° C., was 0.01 dB or less, it was evaluated as “A,” and if it exceeded 0.01 dB / km, it was evaluated as “B.”

[0110] (Appearance after screening test) After applying a screening tension of 1.5 kg to a 1000 km optical fiber and rewinding it, the presence or absence of deposits originating from the secondary resin layer on the belt of the production line was checked. Cases without deposits were evaluated as "A", and cases with deposits were evaluated as "B".

[0111]

[0112] DESCRIPTION OF SYMBOLS 10, 10A...Optical fiber 11...Core 12...Cladding 13...Glass fiber 14...Primary resin layer 15...Secondary resin layer 16...Coating resin layer 20...Connecting portion 21...Non-connecting portion 40...Connecting resin layer 60, 70...Optical fiber cable 61...Tube 62...Interposition 63, 73...Tension member 64, 75...Outer jacket 65...Tear cord 71...Slot 72...Slot rod 74...Press-winding tape 100, 100A, 100B...Optical fiber ribbon D1...Diameter D2...Outer diameter F...Center-to-center distance T...Thickness

Claims

1. A resin composition for secondary coating of optical fiber, comprising a photopolymerizable compound including a urethane (meth)acrylate derived from a plant component, and a photopolymerization initiator.

2. The resin composition according to claim 1, wherein the urethane (meth)acrylate has a biomass content of 20% or more and 70% or less.

3. A resin composition according to claim 1 or claim 2, wherein the content of the urethane (meth)acrylate is 10 parts by mass or more and 80 parts by mass or less based on 100 parts by mass of the total amount of the resin composition.

4. A resin composition according to any one of claims 1 to 3, wherein the photopolymerizable compound further contains a monomer derived from a plant component.

5. The resin composition described in claim 4, wherein the monomer derived from a plant component is at least one selected from the group consisting of normal octyl (meth)acrylate, lauryl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, glycerin di(meth)acrylate, decanediol di(meth)acrylate, glycerin propylene oxide modified tri(meth)acrylate, and glycerin tri(meth)acrylate.

6. A resin composition according to any one of claims 1 to 5, wherein the biomass ratio of the resin composition is 10% or more and 50% or less.

7. The resin composition is irradiated with an integrated light dose of 100 mJ / cm 2 and illuminance 100 mW / cm 2 The resin composition according to claim 1 , wherein the resin film has a glass transition temperature of 60° C. or higher and 100° C. or lower when cured with ultraviolet light under the above conditions.

8. The resin composition according to claim 7, wherein the Young's modulus of the resin film is 600 MPa or more and 2000 MPa or less at 23°C.

9. An optical fiber comprising: a glass fiber including a core and a cladding; a primary resin layer in contact with and covering said glass fiber; and a secondary resin layer covering said primary resin layer, wherein said secondary resin layer comprises a cured product of a resin composition according to any one of claims 1 to 8.

10. A method for manufacturing an optical fiber, comprising: a coating step of coating the resin composition according to any one of claims 1 to 8 onto the outer periphery of a glass fiber including a core and a cladding; and a curing step of curing the resin composition by irradiating it with ultraviolet light after the coating step.

11. An optical fiber ribbon comprising a plurality of optical fibers according to claim 9 arranged in parallel and coated with a ribbon resin.

12. An optical fiber cable, comprising the optical fiber ribbon according to claim 11 housed within the cable.

13. An optical fiber cable comprising a plurality of optical fibers according to claim 9 housed within the cable.

Citation Information

Patent Citations

  • Photocurable resin composition

    JP2000026555A

  • Radiation curable coating composition

    JP2003511531A

  • LED curing of radiation-curable optical fiber coating compositions

    JP2013512856A

  • Biomaterial-based UV coating compositions

    JP2020516726A