Metal paste and metal particle aggregate
A metal paste with specific components forms strong and conductive metal particle aggregates, addressing the challenges of oxidation, corrosion, and void generation in electrically conductive bonding, achieving robust and efficient bonding processes.
Patent Information
- Application Number
- PCT/JP2024/017003
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-07
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for electrically conductive bonding, such as those using copper sintered bodies or conductive pastes, face challenges like oxidation, corrosion, and insufficient strength due to void generation and complex processing steps, particularly in forming metal particle aggregates with suitable strength and conductivity.
A metal paste containing metal particles, a reducing organic substance, a basic compound, a coordinating organic compound, and a resin, with a specific molar ratio and composition, is used to form metal particle aggregates that suppress void generation and enhance sintering, allowing for strong and conductive bonding without the need for removing surface oxides or using reducing atmospheres.
The metal paste effectively forms metal particle aggregates with excellent strength and conductivity, reducing processing complexity and void formation, enabling reliable electrically conductive bonding with improved bondability and strength.
Smart Images

Figure JP2024017003_05122024_PF_FP_ABST
Abstract
Description
Metal paste and metal particle aggregates
[0001] The present disclosure relates to a metal paste and a metal particle aggregate. This application claims priority from Japanese Patent Application No. 2023-087440, filed May 29, 2023, the contents of which are incorporated herein by reference.
[0002] Conventionally, as a method for electrically conductively joining, for example, a base material and a material to be joined are bonded together via a sheet for sinter bonding, and then heated to form a sintered bond.
[0003] For example, Patent Document 1 discloses a bonding method using a copper sintered body, in which copper nanoparticles are formed into a sheet shape, sintered, laminated with an object to be bonded, and then bonded by pressure and heat to form a laminate.
[0004] As a sinter-bonding sheet, for example, Patent Document 2 discloses a plate- or sheet-shaped composite material containing copper fine particles having an average particle size of 300 nm or less, copper coarse particles having an average particle size of 3 μm to 11 μm, and a reducing agent. Patent Document 3 also discloses a sinter-bonding sheet containing conductive metal-containing sinterable particles and a binder component, and having a specific area ratio that can be transferred to a silver surface by pressure treatment under specified conditions.
[0005] Another method for achieving conductive bonding is to bond a base material and a material to be bonded together via a metal paste, followed by heating and firing the bond.
[0006] For example, Patent Document 4 discloses a conductive paste used to form a metal sintered body, which contains a mixture of formic acid and a basic compound combined at a specific molar ratio as a dispersion medium, thereby generating formic acid gas, enabling good firing even without a reducing atmosphere, and capable of suppressing corrosion of metal particles by formic acid.
[0007] JP 2022-029194 A JP 2021-116450 A JP 2020-150189 A JP 2020-025765 A
[0008] However, in the bonding method using the copper sintered body of Patent Document 1, the copper sintered body obtained by sintering a sintering precursor (copper nanoparticle aggregate) in a reducing atmosphere must be subjected to firing immediately after removal to prevent re-oxidation before bonding to the object to be bonded. In addition, when a surface oxide film is removed using a reducing agent (formic acid) or an etching solution (aqueous sulfuric acid solution) after sintering, it is necessary to remove these before bonding to avoid corrosion, and there were problems with the operation being complicated.
[0009] Furthermore, the plate- or sheet-like composite materials of Patent Documents 2 and 3 are formed by compressing powder, and therefore have problems in that the strength is insufficient in the state of a sintered precursor (metal particle aggregate), and it is difficult to control the sintered state to obtain a strength suitable for application to a joining process. Furthermore, when the conductive paste of Patent Document 4 is used, the sintered precursor (metal particle aggregate) can be sintered without removing the dispersion medium containing formic acid, but when the metal particle aggregate is formed and heated, the generation of voids due to decomposition gas of formic acid is not sufficiently suppressed, and there are cases in which the joinability is reduced.
[0010] Therefore, an object of the present disclosure is to provide a metal paste that can suppress the occurrence of voids and more easily form metal particle aggregates with excellent strength, and a metal particle aggregate that is a formed product of the metal paste.
[0011] As a result of intensive research to solve the above-mentioned problems, the inventors have found that by using a metal paste containing metal particles, a reducing organic substance, a basic compound, a coordinating organic compound other than the basic compound, and a resin, the generation of voids due to decomposition gas of the reducing organic substance is suppressed without removing the reducing organic substance such as formic acid, and the metal oxide film on the surface of the metal particles dissolves and precipitates as small-diameter metal particles, thereby easily producing a metal particle aggregate (semi-sintered body) in which the aggregation state is controlled to have a strength suitable for application to a joining process and which results in a sintered body with excellent conductivity. The invention disclosed herein was completed based on these findings.
[0012] That is, the present disclosure provides a metal paste containing metal particles, a reducing organic substance, a basic compound, a coordinating organic compound excluding compounds that fall under the basic compound, and a resin, wherein the molar ratio of basic groups of the basic compound to acidic groups of the reducing organic substance (basic groups / acidic groups) is 0.4 or more.
[0013] The metal particles preferably contain copper.
[0014] The reducing organic substance preferably contains formic acid.
[0015] The content of the reducing organic substance is preferably 5% by mass or less.
[0016] The basic compound is represented by the following formula (1): (In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c are not simultaneously hydrogen atoms. A double line including a dashed line represents a single bond or a double bond. When it is a double bond, R c does not exist. a ~R c any two of which may be bonded to each other to form a ring together with the adjacent nitrogen atom) is preferably a nitrogen-containing compound represented by the following formula:
[0017] The coordinating organic compound is preferably a compound having a carboxy group.
[0018] The resin is preferably a thermoplastic resin.
[0019] The thermoplastic resin is preferably polyvinyl butyral.
[0020] The content of the resin is preferably 1.0% by mass or less.
[0021] The present disclosure also provides a metal paste containing metal particles, wherein the metal paste is heated in a nitrogen atmosphere from room temperature to 200°C at a heating rate of 20°C / min, and when the metal paste is heated and molded for 5 minutes after reaching 200°C, metal particles are generated on the surfaces of the metal particles, and the particle diameter of the generated metal particles is smaller than the number average particle diameter of the metal particles in the metal paste.
[0022] The present disclosure also provides a metal particle aggregate, which is a molded product of the metal paste.
[0023] The present disclosure also provides a method for producing a metal particle aggregate, in which the metal paste is molded and heated to obtain the metal particle aggregate.
[0024] The present disclosure also provides a method for producing a sintered body, which comprises firing the metal particle aggregate to obtain a sintered body.
[0025] The present disclosure also provides a method for producing a bonded body, in which a substrate and an object to be bonded are brought into contact with each other via the metal particle aggregate, and then fired.
[0026] The present disclosure also provides an electronic device comprising a substrate, a workpiece, and a sintered body that is a sintered product of the metal particle aggregate that contacts the substrate and the workpiece and bonds the substrate and the workpiece.
[0027] By using the metal paste of the present disclosure, the generation of voids is suppressed and metal particle aggregates with excellent strength can be easily formed.
[0028] FIG. 1 shows a top view of a state in which a metal particle aggregate is formed on an oxygen-free copper foil in an example. FIG. 1 shows SEM images of the metal particle aggregate and sintered body of Example 1. FIG. 1 shows SEM images of the metal particle aggregate and sintered body of Example 5. FIG. 1 shows SEM images of the metal particle aggregate and sintered body of Example 7. FIG. 1 shows SEM images of the metal particle aggregate and sintered body of Example 10. FIG. 1 shows SEM images of the metal particle aggregate and sintered body of Example 12. FIG. 1 shows a top view (left) of a joining test using the metal paste of Example 7 showing an SEM image of the metal particle aggregate of Comparative Example 1, and an SAT image (right) obtained by ultrasonic video inspection. FIG. 1 shows a cross-sectional SEM image of a joined body obtained in a joining test using the metal paste of Example 8. FIG. 1 shows a cross-sectional SEM image of a joined body obtained in a joining test using the metal paste of Example 9. FIG. 1 shows an SAT image obtained by ultrasonic video inspection in a joining test using the metal paste of Example 10. FIG. 1 shows a cross-sectional SEM image of a joined body obtained in a joining test using the metal paste of Comparative Example 3.
[0029] [Metal Paste] The metal paste of the present disclosure contains at least metal particles, a reducing organic substance, a basic compound, a coordinating organic compound excluding compounds that fall under the basic compound, and a resin.
[0030] Since the metal paste of the present disclosure contains a reducing organic substance, the process of activating the metal particle surfaces is not required when firing a metal particle aggregate (semi-sintered body), which is a molded product of the metal paste, to obtain a sintered body.
[0031] Furthermore, since the metal paste of the present disclosure contains a basic compound, it can effectively remove metal oxide films from the surfaces of metal particles when obtaining a sintered body and when forming metal particle aggregates, and it can also suppress corrosion of the surfaces of metal particles caused by reducing organic substances.
[0032] Furthermore, since the metal paste of the present disclosure contains a coordinating organic compound, it is believed that the metal particle surfaces are likely to dissolve and form metal complexes when forming metal particle aggregates. The formed metal complexes are likely to undergo thermal or reductive decomposition and precipitate as small metal particles on the metal particle surfaces. The presence of small metal particles on the metal particle surfaces increases the influence of surface diffusion, making the metal particle aggregate (semi-sintered body) more likely to sinter even at lower temperatures. In other words, the small metal particles are partially sintered by heating when forming the metal particle aggregate, acting as bonds between the metal particles, resulting in the metal particle aggregate (semi-sintered body) having excellent strength. Furthermore, the coordinating organic compound coordinates to the activated metal surface after the metal oxide film has been removed, suppressing decomposition of the reducing organic compound due to contact with the metal surface. This eliminates the need to remove the reducing organic compound before forming, and easily suppresses the generation of voids when forming the metal particle aggregate.
[0033] Furthermore, since the metal paste of the present disclosure contains a resin, it has an appropriate viscosity, which makes it easy to form metal particle aggregates, and also provides strength to the metal particle aggregates.
[0034] Viscosity of the metal paste of the present disclosure (25°C, shear rate 10 s -1 The viscosity of the paste is preferably 1 to 1,000 Pa·s, more preferably 5 to 800 Pa·s, and even more preferably 10 to 500 Pa·s, from the viewpoints of suppressing sagging or flow of the metal paste, improving application accuracy, and stably maintaining a uniform dispersion state of the metal particles. The viscosity can be measured using a rheometer (MCR302, manufactured by Anton Paar) with a measuring jig of PP25 and a gap of 0.5 mm.
[0035] The TI value (JIS Z3248-3) at 25° C. is, for example, preferably 0.1 to 1.5, more preferably 0.2 to 1.2, even more preferably 0.3 to 1.0, and particularly preferably 0.5 to 0.8.
[0036] <Metal Particles> The metal contained in the metal particles contained in the metal paste of the present disclosure may be any metal that has electrical conductivity after sintering, and examples thereof include gold, silver, copper, nickel, palladium, tin, aluminum, or alloys thereof, or oxides thereof (copper oxide (CuO, CuO)), silver oxide, etc.). Among these, at least one selected from copper, silver, and oxides thereof is preferred, with copper and / or silver being more preferred, and copper being even more preferred, in terms of obtaining a sintered body with high electrical conductivity. These may be used alone or in combination of two or more types.
[0037] The metal particles may have various shapes such as spherical, ellipsoidal flake (flat), fibrous, or amorphous, but are preferably spherical or flake in shape from the viewpoint of the coatability and storage stability of the conductive paste. These may be used alone or in combination of two or more types.
[0038] The volume average particle diameter (median diameter, D 50 ) is preferably 100 nm to 100 μm, more preferably 200 nm to 20 μm, and even more preferably 500 nm to 10 μm.
[0039] Examples of the metal particles include nano-sized particles (having a volume average particle diameter of, for example, 1 nm or more and less than 300 nm, preferably 1 to 200 nm, and more preferably 1 to 150 nm), sub-micro-sized particles (having a volume average particle diameter of, for example, 0.10 μm or more and less than 1.00 μm, preferably 0.15 to 0.95 μm, and more preferably 0.20 to 0.90 μm), and micro-sized particles (having a volume average particle diameter of, for example, 1.0 to 100 μm, preferably 1.0 to 30 μm, more preferably 1.0 to 20 μm, even more preferably 1.0 to 10 μm, and particularly preferably 1.0 to 5.0 μm). The metal particles may be a combination of two or more types of metal particles having different volume average particle diameters. Among these, the metal particles preferably include the sub-micro-sized particles, and the micro-sized particles may be used together with the sub-micro-sized particles. In particular, from the viewpoint of increasing the strength of the metal particle aggregate, the metal particles preferably contain submicron-sized particles (A) having a volume average particle diameter of 100 to 400 nm (preferably 120 to 300 nm), and more preferably contain submicron-sized particles (B) having a volume average particle diameter larger than that of the submicron-sized particles (A) (for example, a volume average particle diameter of more than 400 nm but less than 1.0 μm, preferably 450 to 800 nm) together with the submicron-sized particles (A). The volume average particle diameter of the metal particles can be measured, for example, using a commercially available laser particle size distribution analyzer (for example, SALD-7000 manufactured by Shimadzu Corporation). In addition, when two or more types of metal particles having different volume average particle diameters are contained, the respective volume average particle diameters can be confirmed as the particle diameter of the maximum value detected in particle size distribution measurement.
[0040] The mass ratio of the submicron-sized particles to the total metal particles (submicron-sized particles / total metal particles) is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.4 or more, and particularly preferably 0.6 or more. The mass ratio may be 1.0 or less, or 0.9 or less.
[0041] When the metal particles include the micro-sized particles, the mass ratio of the micro-sized particles to the total metal particles (micro-sized particles / total metal particles) is preferably 0.9 or less, more preferably 0.8 or less, even more preferably 0.6 or less, and particularly preferably 0.4 or less. The mass ratio may be greater than 0 and may be 0.1 or more.
[0042] The mass ratio of copper particles to all metal particles (copper particles / all metal particles) is preferably greater than 0.5, more preferably 0.7 or more, even more preferably 0.8 or more, and particularly preferably 0.9 or more.
[0043] The total amount of the metal particles in the metal paste of the present disclosure is preferably 70 to 99 mass%, more preferably 72 to 95 mass%, and even more preferably 75 to 93 mass%, relative to the total amount of the metal paste (100 mass%).
[0044] <Reducing Organic Substance> Examples of reducing organic substances contained in the metal paste of the present disclosure include alcohols (lower alcohols such as ethanol, higher alcohols such as palmitol), aldehydes (formaldehyde, acetaldehyde, cyclic trimers and tetramers of these aldehydes), amino acids, organic acids (carboxylic acids, etc.), aromatic compounds (polyphenols, phenolic acid compounds, etc.). Among these, organic acids (carboxylic acids, etc.) and aromatic compounds are preferred because they exhibit acidity, and carboxylic acids are more preferred because they are easy to handle at room temperature and not highly toxic. These may be used alone or in combination of two or more types.
[0045] Examples of the carboxylic acid include formic acid, acetic acid, lactic acid, propionic acid, acrylic acid, malic acid, n-hexanoic acid, succinic acid, n-octanoic acid, tartaric acid, and oxalic acid. Among these, formic acid and oxalic acid are preferred because they are excellent in reducing properties and can easily produce a sintered body having excellent electrical conductivity.
[0046] The reducing organic substance preferably contains formic acid from the viewpoint of excellent reducibility and void suppression, and further preferably contains a compound having a boiling point higher than that of formic acid (particularly a compound having a boiling point higher than that of the coordinating organic compound) together with formic acid from the viewpoint of being able to exhibit reducing properties over a wide temperature range.
[0047] When formic acid is contained as the reducing organic substance, the content of formic acid is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more, relative to the total amount (100% by mass) of the reducing organic substances. When another reducing organic substance other than formic acid (e.g., a compound having a boiling point higher than that of formic acid) is contained together with formic acid, the content of the other reducing organic substance is preferably 0.1 molar parts or less, more preferably 0.05 molar parts or less, relative to 1 molar part of formic acid.
[0048] The content of the reducing organic substance is preferably 5% by mass or less (for example, 0.1 to 5% by mass) relative to the total amount (100% by mass) of the metal paste, more preferably 0.1 to 4.0% by mass, even more preferably 0.2 to 3.7% by mass, and particularly preferably 0.3 to 3.5% by mass.
[0049] <Basic Compound> The basic compound contained in the metal paste of the present disclosure is not particularly limited as long as it acts as a base and achieves the effects of the present disclosure, but specific examples include nitrogen-containing compounds such as ammonia, amine compounds, and phosphorus-containing compounds such as phosphines and phosphate esters. Among these, nitrogen-containing compounds represented by the following formula (1) are preferred because they make it easier to obtain a sintered body with excellent electrical conductivity. In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and is at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c are not hydrogen atoms at the same time. A double line including a dashed line represents a single bond or a double bond. In the case of a double bond, R cdoes not exist. a ~R c Any two of may be bonded to each other to form a ring together with the adjacent nitrogen atom.
[0050] R a ~R c Examples of the hydrocarbon group include an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Among these, an aliphatic hydrocarbon group and an alicyclic hydrocarbon group are preferred, and an aliphatic hydrocarbon group is more preferred.
[0051] Examples of the aliphatic hydrocarbon group include a linear or branched alkyl group, a linear or branched alkenyl group, a linear or branched alkynyl group, and a linear or branched alkylidene group, and among these, a linear or branched alkyl group is preferred.
[0052] The linear or branched alkyl group is preferably a linear alkyl group having 1 to 20 carbon atoms, more preferably 1 to 15 carbon atoms, or a branched alkyl group having preferably 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a decyl group, a dodecyl group, a tetradecyl group, an octadecyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a 2-ethylhexyl group.
[0053] The linear or branched alkenyl group is preferably a linear alkenyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkenyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples thereof include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 3-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 3-pentenyl group, a 4-pentenyl group, a 1-hexenyl group, a 3-hexenyl group, a 5-hexenyl group, a 1-heptenyl group, a 1-octenyl group, a 1-nonenyl group, a 1-decenyl group, an isopropenyl group, a 2-methyl-1-propenyl group, a methallyl group, a 3-methyl-2-butenyl group, and a 4-methyl-3-pentenyl group.
[0054] The linear or branched alkynyl group is preferably a linear alkynyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkynyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, a 2-pentynyl group, a 3-pentynyl group, a 4-pentynyl group, a 1-hexynyl group, a 2-hexynyl group, a 3-hexynyl group, a 4-hexynyl group, a 5-hexynyl group, a 1-heptynyl group, a 1-octynyl group, a 1-nonynyl group, a 1-decynyl group, a trimethylsilylethynyl group, and a triethylsilylethynyl group.
[0055] The linear or branched alkylidene group is preferably a linear alkylidene group having 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkylidene group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkylidene group include a methylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a sec-butylidene group, a pentylidene group, an isopentylidene group, an octylidene group, and an isooctylidene group.
[0056] Examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkenyl group.
[0057] The cycloalkyl group is preferably a cycloalkyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group.
[0058] The cycloalkenyl group is preferably a cycloalkenyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopentenyl group and a cyclohexenyl group.
[0059] The aromatic hydrocarbon group is preferably an aryl group having 6 to 18 carbon atoms, more preferably 6 to 18 carbon atoms, and even more preferably 6 to 10 carbon atoms, and examples thereof include a phenyl group and a naphthyl group.
[0060] In formula (1), the double line including the dashed line represents a single bond or a double bond. When the double line including the dashed line is a double bond, R c does not exist, and R in formula (1) a and R b The nitrogen atom to which is bonded represents an imino group or an N-substituted imino group.
[0061] R a ~R c The total number of amino groups, N-substituted amino groups and N,N-substituted amino groups that may be contained in the alkyl group is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2.
[0062] R a ~R c The total number of imino groups and N-substituted imino groups that may be contained in the alkyl group is preferably 0 to 4, more preferably 1 to 3, and even more preferably 1 or 2.
[0063] R a ~R c The total number of hydroxyl groups that may be possessed by is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2.
[0064] The substituents of the N-substituted amino group, N,N-substituted amino group, and N-substituted imino group are the same as those of the above R a ~R c The hydrocarbon groups are the same as those described above.
[0065] R a ~R c Any two of these may be bonded to each other to form a ring together with the adjacent nitrogen atom. Examples of the ring formed include a pyrrolidine ring, a pyrroline ring, a piperidine ring, a pyrrole ring, an imidazolidine ring, an imidazole ring, a piperazine ring, an imidazolidine ring, a pyridine ring, a diazine ring, and a triazine ring.
[0066] R a ~R cThe hydrocarbon group in the formula (I) may have a substituent other than an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, or a hydroxyl group. Examples of such a substituent include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an oxo group, a substituted oxy group (an alkoxy group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyloxy group having 7 to 16 carbon atoms, an acyloxy group having 1 to 4 carbon atoms, etc.), a carboxy group, a substituted oxycarbonyl group (an alkoxycarbonyl group having 1 to 4 carbon atoms, an aryloxycarbonyl group having 6 to 10 carbon atoms, an aralkyloxycarbonyl group having 7 to 16 carbon atoms, etc.), a cyano group, a nitro group, a sulfo group, a mercapto group, and a heterocyclic group.
[0067] Specific examples of the basic compound represented by formula (1) include, for example, R a ~R c an alkylamine in which at least one of R in formula (1) is a linear or branched alkyl group; a , R b are independently a hydrogen atom or a linear or branched alkyl group, and R c is a linear or branched alkyl group having one hydroxyl group; a is a hydrogen atom or a linear or branched alkyl group, and R b and R c are the same or different and are linear or branched alkyl groups each having one hydroxyl group; a ~R c are the same or different and are a linear or branched alkyl group having one hydroxyl group; a , R b are the same or different and are a hydrogen atom or a linear or branched alkyl group, and R c an aminoalkanediol in which R in formula (1) is a linear or branched alkyl group having two hydroxyl groups; a ~R c a diamine having a total of one amino group; a ~R ca triamine having a total of two amino groups; R in formula (1) a ~R c a diaminoalkanol having a total of one amino group and a total of one hydroxyl group; R in formula (1) a ~R c an imidazole compound in which a ring is formed by incorporating nitrogen atoms of the imino groups, the total number of which is 1; a , R b is bonded to an imino group, and a ring is formed containing the imino group (such as a pyridine-based compound, a diazine-based compound, or a triazine-based compound).
[0068] Examples of the alkylamine include methylamine, ethylamine, propylamine, butylamine, pentylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, piperidine, trimethylamine, triethylamine, dimethyldecylamine, dimethyldodecylamine, 4-dimethylaminopyridine, 2-aminopyrazine, 2-aminopyrimidine, 3-aminopyridazine, 2-aminotriazine, diazabicyclononene, and diazabicycloundecene.
[0069] Examples of the monoalkanolamine include 2-aminoethanol, 3-aminopropanol, 1-amino-2-propanol, 1-amino-2-methyl-2-propanol, 2-amino-2-methyl-1-propanol, 4-amino-1-butanol, 6-amino-1-hexanol, 10-amino-1-decanol, 12-amino-1-dodecanol, N-methyl-2-aminoethanol, N-ethyl-2-aminoethanol, N-propyl-2-aminoethanol, 2-dimethylaminoethanol, 6-diethylaminohexanol, 1-(2-hydroxyethyl)pyrrolidine, 2-(hydroxymethyl)pyrrolidine, 2-(2-hydroxyethyl)-1-methylpyrrolidine, 1-piperidineethanol, and 1-ethanol-4-propanolpiperidine.
[0070] Examples of the dialkanolamine include diethanolamine, di-n-propanolamine, diisopropanolamine, di-n-butanolamine, diisobutanolamine, and N-methyldiethanolamine.
[0071] Examples of the trialkanolamine include triethanolamine, tri-n-propanolamine, triisopropanolamine, tri-n-butanolamine, and triisobutanolamine.
[0072] Examples of the aminoalkanediol include 1-amino-2,3-propanediol, 4-amino-1,2-butanediol, 4-amino-1,3-butanediol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 1-methylamino-2,3-propanediol, 1-ethylamino-2,3-propanediol, 1-propylamino-2,3-propanediol, 1-butylamino-2,3-propanediol, 3-dimethylamino-1,2-propanediol, and 2-diethylamino-1,3-propanediol.
[0073] Examples of the diamine include 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,5-diamino-2-methylpentane, N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyl-1,3-propanediamine, N,N'-diethyl-1,3-propanediamine, N,N'-dimethyl-1,4-butanediamine, and N,N'-diethyl-1,4-butanediamine. Examples thereof include hexanediamine, N,N'-dimethyl-1,6-hexanediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dimethyl-1,3-propanediamine, N,N-diethyl-1,3-propanediamine, N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dimethyl-1,6-hexanediamine, 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, piperazine, N-methylpiperazine, N-ethylpiperazine, N,N'-dimethylpiperazine, and homopiperazine.
[0074] Examples of the triamine include diethylenetriamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 3,3'-diaminodipropylamine, N-(3-aminopropyl)-N-methyl-1,3-propanediamine, N'-[3-(dimethylamino)propyl]-N,N-dimethyl-1,3-propanediamine, 2,6,10-trimethyl-2,6,10-triazaundecane, N-(2-aminoethyl)piperazine, 1,4,7-triazacyclononane, N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 1-(2-aminoethyl)-4-methylpiperazine, and 1-(2-dimethylaminoethyl)-4-methylpiperazine.
[0075] Examples of the diaminoalkanol include 1,3-diaminopropan-2-ol, 2-(2-aminoethylamino)ethanol, 2-(2-aminopropylamino)ethanol, 2-(2-aminoethylmethylamino)ethanol, 1-(2-hydroxyethyl)piperazine, 4-methylpiperazine-1-ethanol, and 1,4-bis(2-hydroxyethyl)piperazine.
[0076] Examples of the imidazole compound include imidazole, 2-methylimidazole, 2-propylimidazole, N-methylimidazole, N-propylimidazole, N-butylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-acetylimidazole, and 2-hydroxybenzimidazole.
[0077] Examples of the nitrogen-containing aromatic compound include pyridine, α-picoline, β-picoline, γ-picoline, 2,6-lutidine, 2,3-lutidine, pyrazine, 2-hydroxypyrazine, pyrimidine, 2-hydroxypyrimidine, 4-hydroxypyrimidine, pyridazine, 3-hydroxypyridazine, 4-hydroxypyridazine, triazine, and 2-hydroxytriazine.
[0078] The basic compound contained in the metal paste of the present disclosure is preferably a chelating basic compound having an ethylenediamine structure or an ethanolamine structure in its molecular structure, since this facilitates stabilization of metal ions dissolved in metal oxides on the surfaces of metal particles by chelating coordination. The amino group in the above structure may be any of primary, secondary, and tertiary amino groups, but is preferably a tertiary amino group from the viewpoint of suppressing side reactions between the basic compound and reducing organic substances.
[0079] The basic compound preferably contains an alkylamine having at least one linear alkyl group having 1 to 20 carbon atoms (preferably 1 to 15 carbon atoms) in addition to the chelating basic compound.
[0080] The basic compounds may be used alone or in combination of two or more.
[0081] In the metal paste of the present disclosure, the molar ratio of the basic groups of the basic compound to the acidic groups of the reducing organic substance (basic groups / acidic groups) is 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, even more preferably 1.0 or more, and particularly preferably 1.6 or more. If the molar ratio is less than 0.4, the reaction between the acidic groups of the reducing organic substance and the metal may progress, causing the metal paste to become an aggregated solid and unable to maintain its paste state. The molar ratio is preferably 2.0 or less, more preferably 1.8 or less, and even more preferably 1.7 or less. If the molar ratio is 2.0 or less, the surface of the metal particles is easily reduced, resulting in excellent conductivity of the sintered body. The number of moles of acidic groups contained in the reducing organic substance is calculated by multiplying the number of moles of the reducing organic substance by the number of acidic groups contained in the reducing organic substance, and the number of moles of basic groups contained in the basic compound is calculated by multiplying the number of moles of the basic compound by the number of basic groups contained in the basic compound. The acidic group refers to a functional group exhibiting acidity. The number of moles of the acidic group is preferably the number of moles of one or more groups selected from the group consisting of a carboxy group and a phenolic hydroxyl group, and is particularly preferably the number of moles of a carboxy group. The basic group refers to a functional group that exhibits basicity. The number of moles of the basic group is preferably the number of moles of an amino group.
[0082] The content of the basic compound in the metal paste of the present disclosure is preferably 0.1 to 10 mass%, more preferably 0.3 to 9 mass%, and even more preferably 0.5 to 8 mass%, relative to the total amount (100 mass%) of the metal paste.
[0083] <Coordinating Organic Compound> The coordinating organic compound contained in the metal paste of the present disclosure is a compound that coordinates to the metal surface of the metal particles, and is a compound excluding compounds that fall under the category of the basic compounds. The coordinating organic compound preferably has a boiling point higher than that of at least one of the reducing organic compounds. In this case, the coordinating organic compound remains more than the reducing organic compound during firing, making it easier to suppress contact between the reducing organic compound and the active metal surface, thereby suppressing decomposition of the reducing organic compound.
[0084] Examples of the coordinating organic compound include at least one compound selected from the group consisting of compounds having a carboxy group, compounds having a ketone group (e.g., diketones such as acetylacetone, β-ketoesters, etc.), compounds having a hydroxyl group, compounds having a sulfo group, and compounds having a thiol group. Among these, compounds having a carboxy group are preferred because they facilitate the precipitation of dissolved metal oxides as small metal particles.
[0085] The compound having a carboxy group is preferably a monovalent or divalent carboxylic acid, and more preferably a monovalent carboxylic acid, in that the metal particle aggregates can be easily sintered in a subsequent step.
[0086] The carboxylic acid may be the same as the carboxylic acid described above for the reducing organic substance. Furthermore, because of their easy availability, low toxicity, and low odor, they may be carboxylic acids having 2 to 15 carbon atoms (preferably 5 to 12, and more preferably 8 to 10). Specific examples include acetic acid (boiling point 118°C), lactic acid (boiling point 122°C), propionic acid (boiling point 141°C), acrylic acid (boiling point 141°C), malic acid (boiling point 167°C), pentanoic acid (boiling point 186°C), n-hexanoic acid (boiling point 205°C), heptanoic acid (boiling point 223°C), 2-ethylhexanoic acid (boiling point 228°C), succinic acid (boiling point 235°C), n-octanoic acid (boiling point 237°C), nonanoic acid (boiling point 254°C), decanoic acid (boiling point 269°C), dodecanoic acid (boiling point 299°C), tartaric acid (boiling point 275°C), and oxalic acid (boiling point 365°C). Since carboxylic acids function as both reducing organic substances and coordinating organic compounds, when using carboxylic acids as coordinating organic compounds, one carboxylic acid having the lowest boiling point may be used in combination with another carboxylic acid having a higher boiling point than the one carboxylic acid. In this case, the carboxylic acid with the relatively high boiling point acts primarily as a protecting agent, and the carboxylic acid with the relatively low boiling point acts as a reducing agent.
[0087] The boiling point of the carboxylic acid at normal pressure is preferably above 110°C, more preferably 150°C or higher, and even more preferably 200°C or higher, because the carboxylic acid is less likely to volatilize than formic acid (boiling point 101°C).
[0088] In the metal paste of the present disclosure, the ratio of the number of moles of the coordinating functional groups contained in the coordinating organic compound to the number of moles of the acidic groups contained in the reducing organic compound (coordinating functional groups / acidic groups) is preferably 0.05 to 1.20, more preferably 0.40 to 1.10, and even more preferably 0.50 to 0.70. A molar ratio of 0.05 or higher facilitates the precipitation of small-diameter metal particles, while a molar ratio of 1.20 or lower reduces the likelihood of the coordinating organic compound remaining after firing. The coordinating functional group is a functional group capable of coordinating to a metal element. The number of moles of the coordinating functional group is preferably the number of moles of one or more groups selected from the group consisting of ketone groups and carboxy groups, and is particularly preferably the number of moles of carboxy groups.
[0089] In the metal paste of the present disclosure, the molar ratio of the number of moles of the coordinating functional group contained in the coordinating organic compound to the basic group of the basic compound (coordinating functional group / basic compound) is preferably 0.10 to 1.00, more preferably 0.15 to 0.75, and even more preferably 0.20 to 0.60. When the molar ratio is 0.10 or more, precipitation of small-diameter metal particles is easily obtained, and when it is 1.00 or less, the coordinating organic compound is less likely to remain after firing.
[0090] The content of the coordinating organic compound in the metal paste of the present disclosure is preferably 0.1 to 10 mass %, more preferably 0.2 to 9 mass %, and even more preferably 0.3 to 8 mass %, relative to the total amount (100 mass %) of the metal paste.
[0091] <Resin> Examples of resins contained in the metal paste of the present disclosure include thermoplastic resins (polyester-based resins, polyamide-based resins, polyurethane-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic resins, styrene-based resins, halogen-containing vinyl-based resins, polyvinyl acetal-based resins, cellulose-based resins (ethyl cellulose resins, alkyl cellulose resins, etc.), thermoplastic silicone resins, etc.), thermosetting resins (epoxy resins, unsaturated polyester resins, diallyl phthalate resins, silicone resins, etc.), etc. Among these, thermoplastic resins are preferred from the viewpoint of their ability to relieve internal stress during heating, and (meth)acrylic resins and polyvinyl acetal resins are preferred from the viewpoint of the adhesion and strength of the metal particle aggregate to the substrate.
[0092] Examples of the polyvinyl acetal resin include polyvinyl butyral.
[0093] The content of the resin in the metal paste of the present disclosure is preferably 1.0 mass% or less, more preferably 0.05 to 1.0 mass%, and even more preferably 0.1 to 0.9 mass%, relative to the total amount (100 mass%) of the metal paste.
[0094] <Solvent> The metal paste of the present disclosure may contain a solvent such as water or an organic solvent in addition to the above-described reducing organic substance, basic compound, and coordinating organic compound in order to adjust the fluidity (viscosity) and operability. Examples of the organic solvent include alcohol-based solvents (e.g., monoalcohols such as 3-methoxybutanol, glycols such as ethylene glycol), ester-based solvents (e.g., acetate esters such as 3-methoxybutyl acetate, and ester oils such as butyl stearate, hexyl laurate, and triethyl citrate), ketone-based solvents (e.g., ketones such as cyclohexanone), ether-based solvents (e.g., ethers such as 1,4-dioxane, ethylene glycol ethers such as diethylene glycol monomethyl ether, and propylene glycol ethers such as dipropylene glycol n-propyl ether), hydrocarbon-based solvents (e.g., alkanes such as tetradecane, and petroleum hydrocarbons such as mineral spirits), aromatic solvents (e.g., aromatic hydrocarbons such as xylene, and aromatic ethers such as diphenyl ether), other aprotic polar solvents (amide-based solvents such as dimethylformamide, and urea-based solvents such as 1,3-dimethylimidazolidinone), and terpenes (limonene, terpineol, and esters thereof) commonly used in metal pastes and paints. These may be used alone or in combination of two or more.
[0095] The content of the solvent is preferably 100 parts by mass or less, and more preferably 50 parts by mass or less, per 100 parts by mass of the total of the metal particles, reducing organic substance, basic compound, coordinating organic compound, and resin.
[0096] The metal paste of the present disclosure may contain, for example, additives (surface conditioners, leveling agents, antifoaming agents, dispersants, thixotropy-imparting agents, etc.) within a range that does not impair the effects of the present disclosure. The content of the additives in the metal paste is, for example, 1 mass % or less (preferably 0.5 mass % or less).
[0097] The metal paste of the present disclosure can be produced through a process of mixing the above-mentioned metal particles, reducing organic substance, basic compound, coordinating organic compound, and resin, as well as any solvent and additives.
[0098] The temperature during mixing preferably does not exceed 100°C.
[0099] The mixture may be cooled to room temperature (for example, 25° C.) or below after mixing, and may be gradually cooled to room temperature or rapidly cooled by ice cooling or the like.
[0100] [Metal Particle Aggregate] The metal particle aggregate of the present disclosure is a molded product obtained by heating and molding the metal paste (e.g., by increasing the temperature from room temperature to 200°C at a heating rate of 20°C / min in a nitrogen atmosphere and then heating for 5 minutes after reaching 200°C), and is a semi-sintered body in which sintering has progressed partially due to small-diameter metal particles precipitated on the surfaces of the metal particles contained in the metal paste. The particle diameter of the small-diameter metal particles is smaller than the number-average particle diameter of the metal particles in the metal paste. The small-diameter metal particles are preferably metal nanoparticles. The particle diameter of the small-diameter metal particles is preferably less than 600 nm, more preferably 1 nm or more and less than 600 nm, even more preferably 5 nm or more and less than 100 nm, and particularly preferably 10 nm or more and less than 60 nm. The small-diameter metal particles are formed by dissolving at least a portion of the surface of the metal particles, and the metal complex is then precipitated by thermal decomposition and / or reductive decomposition. The thermal decomposition and / or reductive decomposition proceeds by heating in the presence of the reducing organic substance.
[0101] The metal paste can be formed, for example, by applying the metal paste to the surface of a substrate by a known, commonly used printing method, such as inkjet printing, spray printing, screen printing, dispenser printing, relief printing (flexographic printing), dye-sublimation printing, offset printing, intaglio printing (gravure printing), contact printing, or microcontact printing, or by using a screen mask or metal mask as appropriate.
[0102] The molded metal paste can be heated at a temperature ranging from 50 to 250°C, preferably from 80 to 220°C, and more preferably from 100 to 200°C. The heating time is, for example, from 1 minute to 1 hour (2 to 30 minutes, or 3 to 15 minutes). The heating may be performed in an inert atmosphere (such as a nitrogen, helium, or argon atmosphere) or in a reducing atmosphere (such as a formic acid gas or hydrogen gas atmosphere).
[0103] A sintered body (metal particle sintered body) can be obtained by firing the metal particle aggregate, and a bonded body can be obtained by bringing a substrate and a workpiece into contact with each other via the metal particle aggregate and firing the resulting bonded body. The bonded body thus obtained comprises a substrate, a workpiece, and a sintered body that is a sintered product of the metal particle aggregate that bonds the substrate and the workpiece. The sintered body is in contact with the substrate and the workpiece.
[0104] The metal particle aggregate can be fired at a temperature ranging from 120 to 300°C, preferably from 150 to 250°C, and more preferably from 180 to 220°C. The heating time is, for example, from 10 minutes to 3 hours (15 minutes to 2 hours, or from 20 minutes to 1 hour). Furthermore, the bonded body (laminate) may be pressurized against the bonding surfaces at a pressure of, for example, 20 MPa or less. Since the reducible organic substance remains, the firing may be carried out in an inert atmosphere (such as a nitrogen, helium, or argon atmosphere). Furthermore, to obtain a more reduced state, firing may be carried out in an inert atmosphere together with an additional reducing agent, or in a reducing atmosphere (such as a formic acid gas or hydrogen gas atmosphere).
[0105] Examples of the substrate include substrates formed from metals (including alloys), ceramics (metal oxides, metal nitrides, silicon, silicon nitride, aluminum nitride, etc.), glass, polymeric materials, etc., substrates obtained by surface-treating the above materials with metal plating, and multilayer boards made from a combination of the above materials.
[0106] The object to be joined is not particularly limited as long as it can be joined by the metal particle aggregate layer, and examples thereof include semiconductor chips (discrete semiconductors such as capacitors, transistors, diodes (power diodes), MOS FETs, IGBTs, and integrated circuits such as ICs and LSIs), heat sinks, and other electric and electronic components, as well as bus bars, connectors, and harnesses for in-vehicle components.
[0107] The metal particle aggregate can be used for semiconductor bonding, wire bonding, clip bonding, forming wiring on wiring boards, forming multilayer printed wiring boards, forming bumps, bonding between bumps, etc., and can be suitably used in the manufacture of electronic devices (printed electronic devices (printed wiring boards, capacitors, inductors, varistors, thermistors, transistors, speakers, actuators, antennas, solid oxide fuel cells, hybrid ICs, etc.)), rotating electric machines, etc. In particular, the metal particle aggregate can be suitably used in the manufacture of semiconductor devices and rotating electric machines that require excellent bonding properties over a large area, and bonding between substrates and heat sinks, for example, bonding between an insulating substrate and a heat sink of a power semiconductor, because the generation of voids due to decomposition gases is suppressed and the metal particle aggregate has suitable strength.
[0108] [Metal particle sintered body] The above-mentioned metal particle sintered body preferably has a volume resistivity of 120 mΩ cm or less, more preferably 100 mΩ cm or less, even more preferably 90 mΩ cm or less, even more preferably 80 mΩ cm or less, still more preferably 50 mΩ cm or less, and particularly preferably 30 mΩ cm or less.
[0109] The configurations and combinations thereof in the above-described embodiments are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited to the embodiments, but is limited only by the claims.
[0110] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to these examples in any way.
[0111] The metal particles, reducing organic substance, basic compound, coordinating organic compound, solvent, and resin used are as follows.
[0112] <Metal Particles> TNCu: Copper particles, granular, average particle diameter 110 nm, trade name "TNCu", manufactured by Taiyo Nippon Sanso Co., Ltd. CH0200L1: Copper particles, granular, average particle diameter 200 nm, trade name "CH-0200L1", manufactured by Mitsui Mining & Smelting Co., Ltd. CT0500: Copper particles, granular, average particle diameter 500 nm, trade name "CT-0500", manufactured by Mitsui Mining & Smelting Co., Ltd. HWQ: Copper particles, granular, average particle diameter 10 μm, trade name "HWQ-10 μm", manufactured by Fukuda Metal Foil & Powder Co., Ltd. 1200YP: Copper particles, flake-shaped, average particle diameter 3.1 μm, trade name "1200YP", manufactured by Mitsui Mining & Smelting Co., Ltd.
[0113] <Reducing organic substances> ・Formic acid: Reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. ・Oxalic acid: Reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0114] <Basic compounds> MDETA: N-methyldiethanolamine, a reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. PMDTA: pentamethyldiethylenetriamine, a reagent manufactured by Tokyo Chemical Industry Co., Ltd. DMDA: N,N-dimethyldecylamine, a reagent manufactured by Tokyo Chemical Industry Co., Ltd. TEA: triethanolamine, a reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0115] <Coordinating organic compounds> nOcA: n-octanoic acid, a reagent manufactured by Tokyo Chemical Industry Co., Ltd. nHxA: n-hexanoic acid, a reagent manufactured by Tokyo Chemical Industry Co., Ltd.
[0116] <Resin> PVB: Polyvinyl butyral, trade name "S-LEC BL-1", manufactured by Sekisui Chemical Co., Ltd. EC: Ethyl cellulose, trade name "ETHOCEL STD 300 cps", manufactured by Nisshin Seiki Co., Ltd.
[0117] <Solvents> DMI: 1,3-dimethyl-2-imidazolidinone, a reagent manufactured by Tokyo Chemical Industry Co., Ltd. MMPG: propylene glycol monomethyl ether, manufactured by Daicel Corporation TECit: triethyl citrate, a reagent manufactured by Tokyo Chemical Industry Co., Ltd.
[0118] <Additives> BYK-348: Surface conditioner, manufactured by BYK Japan Co., Ltd.
[0119] The equipment used for drying the metal paste and for sintering and bonding is as follows: Sintering furnace: Product name "VS-320", manufactured by Budatec Pressurizing device: Product name "SP-60", manufactured by Budatec
[0120] Examples 1 to 11 and Comparative Examples 1 to 4 [Preparation of Metal Paste] A reducing organic substance, a basic compound, a coordinating organic compound, and a solvent were weighed into a screw tube so as to have the respective blending ratios shown in Table 1. A thermoplastic resin was weighed into this screw tube so as to have the blending ratios shown in Table 1, and then heated at 50°C while stirring with a stirrer to obtain various mixed solutions in which the thermoplastic resin had been dissolved. Various copper powders were weighed into 100 mL plastic containers so as to have a total of 20 g (100 parts by mass) of copper powder in the copper powder blending ratios shown in Table 1. The mixed solutions in which the thermoplastic resin had been dissolved were blended into these containers, and the mixtures were stirred for 2 minutes at 2000 rpm using a planetary centrifugal mixer (trade name "Awatori Rentaro", manufactured by Thinky Corporation) in stirring mode to prepare metal pastes.
[0121]
[0122] [Measurement of Viscosity] Using a rheometer (trade name "MCR302", manufactured by Anton Paar), the viscosity was measured at 25°C, a shear rate of 10 s, a measuring jig of PP25, and a gap of 0.5 mm. -1 The shear viscosity after rotating the plate for 10 minutes under the above conditions was taken as the viscosity value of the metal paste.
[0123] [Measurement of TI value] Under the same equipment conditions as viscosity measurement, a shear rate of 0.01 s -1 Shear rate from 1000 s -1 Measurements were carried out while changing the shear rate under logarithmic conditions up to 5 s -1 Viscosity (η1) at (D1) and shear rate 20 s -1 The TI value [Log(η1 / η2) / Log(D2 / D1)] was calculated from the viscosity (η2) at (D2).
[0124] (Viscosity in Examples) In Example 1, the molar ratio of the basic group of the basic compound to the acidic group of the reducing organic compound (basic group / acidic group) was 1.4, and the viscosity was measured at a shear rate of 10 s-1 In Examples 2 and 3, the molar ratio of the basic group of the basic compound to the acidic group of the reducing organic compound (basic group / acidic group) was 1.4, and the solid content was reduced by using a common organic solvent such as DMI or MMPG, resulting in a metal paste with a viscosity of 300 Pa·s and a TI value of 0.7. -1 A soft metal paste with a viscosity of 20 to 30 Pa·s and a TI value of 0.5 to 0.7 was obtained under the conditions. In Examples 4 to 6, the molar ratio of the basic group of the basic compound to the acidic group of the reducing organic compound (basic group / acidic group) was 1.0 to 1.4, and by mixing micro-sized copper particles with a large particle size, a soft metal paste with a viscosity of 20 to 30 Pa·s and a TI value of 0.5 to 0.7 was obtained under the conditions. -1 Under these conditions, a nearly liquid metal paste was obtained with a viscosity of approximately 10 Pa·s and a TI value of approximately 0.1. In Example 10, the molar ratio of the basic groups of the basic compound to the acidic groups of the reducing organic substance (basic groups / acidic groups) was 1.1, and by adding ethyl cellulose as a resin, a highly thixotropic metal paste with a TI value of 0.8 was obtained. In all Examples, by setting the molar ratio of the basic groups to the acidic groups within an appropriate range, metal pastes could be produced stably.
[0125] In Comparative Example 2, the molar ratio of the basic groups of the basic compound to the acidic groups of the reducing organic compound (basic groups / acidic groups) was 0.3. The metal paste of Comparative Example 2 generated heat when the solvent and metal powder were mixed, and after stirring, the metal paste became an aggregated solid, making it impossible to measure viscosity. This is thought to be because the ratio of the basic groups of the basic compound to the acidic groups of the reducing organic compound was low, so the acidic groups of the reducing organic compound did not have the effect of inhibiting the reaction with copper.
[0126] [Preparation of Metal Particle Aggregates] Using a metal mask having a 4 mm long, 4 mm wide, and 100 μm thick opening pattern with 8 openings vertically and 8 openings horizontally arranged at 2 mm intervals (64 openings in total), a metal paste was printed in the center of an oxygen-free copper foil measuring 260 mm long, 200 mm wide, and 100 μm thick, as shown in Figure 1. The copper foil on which the metal paste was printed was heated from room temperature to 200°C at a heating rate of 20°C / min in a nitrogen atmosphere, and then heated for 5 minutes after reaching 200°C, thereby preparing a metal particle aggregate.
[0127] [Sintering of metal particle aggregate] The metal particle aggregate prepared by the method described above was impregnated with a sintering solvent (unit: mass %) having the composition shown in Table 2, and the temperature was increased from room temperature to 200°C at a rate of 40°C / min in a nitrogen atmosphere. After reaching 200°C, the mixture was heated for 30 minutes to prepare a sintered body of the metal particles.
[0128]
[0129] (Metal particle aggregate and sintered body of Example 1) Figure 2 shows SEM images of the metal particle aggregate (after drying) and the sintered body (after sintering) of Example 1. Within the metal particle aggregate, each particle maintains its particle state, but is in an aggregated state due to nanoparticles generated within the system between adjacent particles and weak necking between particles. After sintering this metal particle aggregate with a sintering solvent, necking between the metal particles was observed to be progressing.
[0130] (Metal particle aggregate and sintered body of Example 5) Figure 3 shows SEM images of the metal particle aggregate (after drying) and sintered body (after sintering) of Example 5. While each of the sub-micron-sized particles blended within the metal particle aggregate maintains its particle state, it has become aggregated due to nanoparticles generated within the system between adjacent particles and fine necking between particles. It was also observed that the surfaces of the blended microparticles were deformed due to the generated nanoparticles. After the metal particle aggregate was sintered with a sintering solvent, necking progressed between the sub-microparticles, and necking also progressed between the microparticles and the sub-microparticles.
[0131] (Metal particle aggregate and sintered body of Example 7) Figure 4 shows SEM images of the metal particle aggregate (after drying) and sintered body (after sintering) of Example 7. While each submicron-sized particle blended within the metal particle aggregate maintains its particle state, it is aggregated due to nanoparticles generated within the system and fine necking between particles between adjacent particles. Furthermore, clumps of nanoparticles generated within the system were observed in areas where the solvent was concentrated during solvent evaporation. The presence of nanoparticles could be more clearly confirmed in 50,000x (50k) photographs. After the metal particle aggregate was sintered with the sintering solvent, strong necking developed between the submicron particles, and the nanoparticles generated within the system were consumed by the necking between the particles and were no longer observed.
[0132] (Metal particle aggregate and sintered body of Example 10) Figure 5 shows SEM images of the metal particle aggregate (after drying) and sintered body (after sintering) of Example 10. Each sub-micron-sized particle blended within the metal particle aggregate maintains its particle state, but is in an aggregated state due to nanoparticles generated within the system between adjacent particles and fine necking between particles. After sintering the metal particle aggregate with a sintering solvent, strong necking developed between the sub-micron particles, and strong necking also formed between the blended flake-like microparticles. In the 50k photograph, it was clearly possible to confirm that nanoparticles had been generated on the surface of some of the sub-micron particles and between the sub-micron particles.
[0133] Example 12 [Preparation of Metal Particle Aggregate] Metal particle aggregates were prepared in the same manner as in Example 11, except that the heating temperature was 120°C instead of 200°C. Example 12 is an example for confirming the formation of metal nanoparticles in the metal particle aggregate. Figure 6 shows an SEM image of the metal particle aggregate (after drying) of Example 12. While each of the submicron-sized particles blended within the metal particle aggregate maintains its particle state, it has become aggregated due to nanoparticles generated in the system between adjacent particles and thin necking between particles. Furthermore, it was clearly confirmed that nanoparticles were generated on the surface of some of the submicron particles.
[0134] (Metal particle aggregate of Comparative Example 1) Fig. 7 shows an SEM image of the metal particle aggregate of Comparative Example 1. Since Comparative Example 1 did not contain a coordinating organic compound, the nanoparticles generated in the system could not be maintained in a nanoparticle state, and necking between particles had already progressed under the aggregate formation conditions.
[0135] [Adhesion Test of Metal Particle Aggregates (Tape Peeling)] A weak adhesive tape (product name "Karitome No. 207" manufactured by Nichiban Co., Ltd.) with an adhesive strength of 0.94 N / 10 mm was attached to a 4 mm x 4 mm x 64 metal particle aggregate layer on copper foil obtained by preparing the metal particle aggregate described above in a horizontal row of eight patterns. The weak adhesive tape was peeled off in one go from the edge, and the metal particle aggregate layer was observed for peeling or chipping. This test was performed on all 64 patterns, and a rating of ⊚ was given when three or fewer (5% or less) 4 mm x 4 mm square patterns had chips at the edge. A rating of ◯ was given when 22 or fewer (35% or less) 4 mm x 4 mm square patterns had chips at the edge or peeled off entirely. A rating of △ was given when 42 or fewer (65% or less) 4 mm x 4 mm square patterns had chips at the edge or peeled off entirely. The case where 43 or more 4 mm x 4 mm square patterns had chips at the edges or peeled off entirely (defects occurred in 65% or more of the patterns) was rated as x.
[0136] As shown in Table 1, Examples 1 to 3 had few defects upon tape peeling and were rated as Excellent. Examples 4 to 6 and Example 9 contained many microparticles, resulting in a low aggregation density of the metal particle aggregates and a tendency for the metal particle aggregates to have slightly weaker strength, resulting in ratings of Fair to Excellent. Examples 7, 8, and 10 had strong aggregation, as can be seen from the SEM images of the metal particle aggregates, and had few defects upon tape peeling and were rated as Excellent. Furthermore, Example 12 was dried at a lower temperature than Example 11, resulting in slightly weaker strength of the metal particle aggregates than Example 11 and an Excellent rating. As a result, the square pattern was maintained to some extent upon tape peeling, and the Examples were rated as having excellent strength. On the other hand, Comparative Example 4 did not contain a thermoplastic resin, resulting in significantly weaker adhesion between the copper foil used as the substrate and the metal particle aggregates, and most of the particle aggregates adhered to the tape during tape peeling, resulting in an Excellent rating. The inclusion of a thermoplastic resin increases the adhesion strength between the substrate and the metal particle aggregates, making it easier to handle for subsequent sintering.
[0137] [Evaluation of Conductivity of Metal Particle Sintered Body] The prepared metal paste was applied with a squeegee to a glass slide masked on all four sides with masking tape (polyester film adhesive tape, product name "631U #12", manufactured by Teraoka Seisakusho Co., Ltd.) to form a metal paste film with a thickness of 25 μm. This metal paste film was heated in a nitrogen atmosphere from room temperature to 200 °C at a temperature increase rate of 20 °C / min, and then held at 200 °C for 5 minutes to form a metal particle aggregate on the glass slide. A sintering solvent prepared with the blending ratio shown in Table 2 was applied to this metal particle aggregate film, and the temperature was increased from room temperature to 200 °C at a rate of 40 °C / min in a nitrogen atmosphere. After reaching 200 °C, the sintered body was heated for 30 minutes to obtain a metal particle sintered body. The conductivity of this metal particle sintered body was evaluated by measuring the volume resistivity using a resistivity meter (product name "Loresta GP MCP-T610", manufactured by Nitto Seiko Analytech Co., Ltd.).
[0138] As shown in Table 1, the sintered bodies obtained from metal pastes containing small submicroparticles as the main component, such as those in Example 1, Examples 7 and 8, and Example 10, exhibited extremely high conductivity with a volume resistivity of 8 to 18 μΩ cm. The metal pastes of Examples 4 to 6 and 9 were mainly composed of large microparticles, and therefore exhibited lower volume resistivities than those of Example 1 above, but exhibited high conductivity of 100 μΩ cm or less. Furthermore, no voids were observed in the metal particle aggregates or metal particle sintered bodies in any of the examples.
[0139] [Bonding Evaluation] 5 mm x 5 mm Cu-Cu Bonding (Bonding Test (1) of Example 7) The metal paste of Example 7 was printed on a 35 mm x 35 mm x 1 mm oxygen-free copper substrate using a squeegee with a metal mask having a 5 mm x 5 mm x 100 μm opening pattern. The copper substrate with the printed metal paste was heated in a nitrogen atmosphere from room temperature to 200 °C at a temperature increase rate of 20 °C / min, and then held at 200 °C for 5 minutes to obtain a copper substrate with a 5 mm x 5 mm metal particle aggregate printed thereon. A sintering solvent listed in Table 2 was applied from above the 5 mm x 5 mm metal particle aggregate, impregnating the entire aggregate layer with the sintering solvent. A 5 mm x 5 mm x 1 mm oxygen-free copper plate was then placed on top of the aggregate layer. The metal particle aggregate impregnated with the sintering solvent sandwiched between the copper plates was placed in a pressure sintering apparatus and pressed from above with a force of 10 MPa (250 N / 1 sample). While maintaining this pressurized state, the temperature was raised from room temperature to 200°C at a rate of 40°C / min in a nitrogen atmosphere, and after reaching 200°C, the temperature was maintained for 30 minutes, thereby obtaining a bonded body in which the copper plates were bonded together by the metal sintered body. The bond strength of this bonded body was measured using a die shear tester (product name "SERIES4000", manufactured by DAGE Corporation) at room temperature, a test speed of 50 μm / s, and a test height of 50 μm. The bond strength was 50 MPa or more, which was sufficient.
[0140] (Bonding Test (1) of Example 8) When the same bonding test as above was carried out using the metal paste of Example 8, the bonding strength was 48 MPa, which was sufficient.
[0141] 10 mm x 10 mm Cu-Cu bonding (Bonding test (2) of Example 7) The same test was carried out using the metal paste of Example 7, except that the conditions of the above bonding test were changed to a metal paste printing area of 10 mm x 10 mm x 100 μm, a copper plate mounted on top of a 10 mm x 10 mm x 1 mm copper plate, and a pressure of 10 MPa (1000 N / 1 sample). To determine the quality of the bond, an ultrasonic imaging inspection was carried out using a "FINE SAT II" (50 MHz probe) manufactured by Hitachi Power Solutions Co., Ltd., and it was found that the bond was complete with no peeling except for some voids caused by printing. The SAT image is shown in Figure 8.
[0142] 20 mm x 20 mm Cu-Cu bonding (Bonding test (2) of Example 8) The same test was carried out using the metal paste of Example 8, except that the conditions of the above bonding test were changed to a metal paste printing area of 20 mm x 20 mm x 100 μm, the copper plate mounted on top was the same 35 mm x 35 mm x 1 mm copper plate used for printing, and the pressure was 10 MPa (4000 N). When the presence or absence of voids or peeling inside the bonded body was confirmed by cross-sectional SEM, it was confirmed that a good bonded body had been obtained. The cross-sectional SEM observation results are shown in FIG. 9.
[0143] (Bonding test of Example 9) Similarly, a bonded body was produced using the metal paste of Example 9, in which copper plates measuring 35 mm × 35 mm × 1 mm were bonded together under printing conditions of 20 mm × 20 mm × 100 μm. The presence or absence of voids or peeling inside the bonded body was confirmed by cross-sectional SEM, and it was confirmed that a good bonded body had been obtained. The cross-sectional SEM observation results are shown in FIG.
[0144] 35mm x 35mm Cu-Cu Bonding (Bonding Test of Example 10) The metal paste of Example 10 was printed on a 35mm x 35mm x 1mm copper substrate using a screen printing plate (product name "SUS200-40, mesh thickness 80, 23B NU-55", 10µm thick, manufactured by Nakanuma Art Screen Co., Ltd.) with four 10mm x 10mm opening patterns. The copper substrate with this metal paste printed on it was heated in a nitrogen atmosphere from room temperature to 200°C at a heating rate of 20°C / min, and then held at 200°C for 5 minutes, resulting in a copper substrate with four 10mm x 10mm metal particle aggregate patterns printed on it. The sintering solvent listed in Table 2 was applied to this metal particle aggregate, and the entire aggregate layer was impregnated with the sintering solvent. After that, a copper plate of the same size as the copper substrate was placed on top so that all four metal particle aggregate patterns were covered. Then, using a pressure sintering apparatus, the temperature was raised from room temperature to 200°C at a rate of 40°C / min under a pressure of 4000 N (10 MPa) in a nitrogen atmosphere, and after reaching 200°C, the temperature was held for 30 minutes to obtain a bonded body in which the copper plates were bonded together using a metal sintered body. SAT measurements were performed to determine the quality of this bonded body, and no peeling or large voids were observed in any of the four patterns on which the metal paste was printed, indicating that a good bonded body had been obtained. The SAT image is shown in Figure 11.
[0145] 5mm x 5mm Cu-Cu Bonding (Bonding Test of Comparative Example 3) The metal paste of Comparative Example 3 was printed on a copper substrate in the same manner as in the bonding test (1) of Example 7. A 5mm x 5mm x 1mm oxygen-free copper plate was mounted on the printed metal paste, and the temperature was raised from room temperature to 200°C at a heating rate of 5°C / min in a nitrogen atmosphere. After reaching 200°C, the temperature was held for 1 hour to obtain a bonded body in which the copper plates were bonded together using a metal sintered body. The bond strength of the bonded body produced in Comparative Example 3 was 15 MPa, which was weaker than that of a bonded body obtained by forming metal particle aggregates and then pressure sintering. Figure 12 shows the cross-sectional SEM observation results of the bonded body obtained in Comparative Example 3. Because the bonded body produced in Comparative Example 3 was sintered without drying the metal paste, large voids originating from the reducing agent and other organic components in the metal paste were observed in some areas, and these voids prevented sufficient bond strength from being obtained.
[0146] Variations of the invention according to the present disclosure are described below. [Appendix 1] A metal paste comprising metal particles, a reducing organic substance, a basic compound, a coordinating organic compound excluding compounds corresponding to the basic compound, and a resin, wherein the molar ratio of the basic groups of the basic compound to the acidic groups of the reducing organic substance (basic groups / acidic groups) is 0.4 or more. [Appendix 2] The metal paste according to Appendices 1, wherein the metal particles contain copper. [Appendix 3] The metal paste according to Appendices 1 or 2, wherein the reducing organic substance contains formic acid. [Appendix 4] The metal paste according to any one of Appendices 1 to 3, wherein the content of the reducing organic substance is 5 mass% or less. [Appendix 5] The basic compound is represented by the following formula (1): (In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c are not simultaneously hydrogen atoms. A double line including a dashed line represents a single bond or a double bond. When it is a double bond, R c does not exist. a ~R cwherein any two of the nitrogen-containing compounds may be bonded to each other to form a ring together with the adjacent nitrogen atom. [Appendix 6] The metal paste according to any one of Appendices 1 to 5, wherein the coordinating organic compound is a compound having a carboxy group. [Appendix 7] The metal paste according to any one of Appendices 1 to 6, wherein the resin is a thermoplastic resin. [Appendix 8] The metal paste according to Appendices 7, wherein the thermoplastic resin is polyvinyl butyral. [Appendix 9] The metal paste according to any one of Appendices 1 to 8, wherein the resin content is 1.0 mass% or less. [Appendix 10] A metal paste containing metal particles, wherein the metal paste is heated from room temperature to 200°C at a heating rate of 20°C / min in a nitrogen atmosphere, and heated for 5 minutes after reaching 200°C to be molded, whereby metal particles are generated on the surfaces of the metal particles, and the particle diameter of the generated metal particles is smaller than the number average particle diameter of the metal particles in the metal paste. [Appendix 11] A metal particle aggregate which is a molded product of the metal paste according to any one of Appendices 1 to 10. [Appendix 12] A method for producing a metal particle aggregate, comprising molding and heating the metal paste according to any one of Appendices 1 to 10 to obtain a metal particle aggregate. [Appendix 13] A method for producing a sintered body, comprising firing the metal particle aggregate according to Appendices 11 to obtain a sintered body. [Appendix 14] A method for producing a bonded body, comprising contacting a base material and a body to be bonded via the metal particle aggregate according to Appendices 11 and firing the resulting body. [Appendix 15] An electronic device comprising a base material, a body to be bonded, and a sintered body which is a fired product of the metal particle aggregate according to Appendices 11 that contacts the base material and the body to be bonded and bonds the base material and the body to be bonded.
Claims
1. A metal paste comprising metal particles, a reducing organic substance, a basic compound, a coordinating organic compound other than compounds corresponding to the basic compound, and a resin, wherein the molar ratio of the basic group of the basic compound to the acidic group of the reducing organic substance (basic group / acidic group) is 0.4 or more.
2. The metal paste of claim 1, wherein the metal particles include copper.
3. The metal paste of claim 1, wherein the reducing organic material comprises formic acid.
4. A metal paste according to any one of claims 1 to 3, wherein the content of the reducing organic substance is 5 mass % or less.
5. The basic compound is represented by the following formula (1): (In formula (1), R a ~R c are the same or different and each represents a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and is at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c A double line including a dashed line represents a single bond or a double bond. c does not exist. a ~R c The metal paste according to any one of claims 1 to 3, wherein the nitrogen-containing compound is represented by the following formula:
6. The metal paste according to any one of claims 1 to 3, wherein the coordinating organic compound is a compound having a carboxy group.
7. The metal paste according to any one of claims 1 to 3, wherein the resin is a thermoplastic resin.
8. The metal paste of claim 7, wherein the thermoplastic resin is polyvinyl butyral.
9. A metal paste according to any one of claims 1 to 3, wherein the resin content is 1.0 mass% or less.
10. A metal paste containing metal particles, wherein when the metal paste is heated in a nitrogen atmosphere from room temperature to 200°C at a heating rate of 20°C / min, and then heated for 5 minutes after reaching 200°C and molded, metal particles are generated on the surfaces of the metal particles, and the particle diameter of the generated metal particles is smaller than the number average particle diameter of the metal particles in the metal paste.
11. A metal particle aggregate which is a molded product of the metal paste according to any one of claims 1 to 3 and 10.
12. A method for producing a metal particle aggregate, comprising forming and heating the metal paste according to any one of claims 1 to 3 and 10 to obtain a metal particle aggregate.
13. A method for producing a sintered body, comprising sintering the metal particle aggregate according to claim 11 to obtain a sintered body.
14. A method for producing a bonded body, comprising contacting a substrate and a body to be bonded via the metal particle aggregate according to claim 11, and firing the resulting body.
15. An electronic device comprising a substrate, an object to be joined, and a sintered body which is a sintered product of the metal particle aggregate according to claim 11, which is in contact with the substrate and the object to be joined and joins the substrate and the object to be joined.
Citation Information
Patent Citations
Dispersion medium for metal particle sintering, and electroconductive paste
WO2021166627A1
Method for manufacturing metal coating film pattern, method for manufacturing connection member, and metal coating film pattern
WO2022264964A1