Liquid crystal polyester composition and method for producing same
The liquid crystal polyester composition with controlled fibrous filler proportions and aromatic hydroxycarboxylic acid content addresses gas generation issues in high-temperature environments by promoting the volatilization of high boiling point components, thereby reducing gas formation in molded articles.
Patent Information
- Application Number
- PCT/JP2024/017705
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional liquid crystal polyester compositions experience gas generation, particularly high boiling point components, in high-temperature environments, which is a concern for molded articles.
A liquid crystal polyester composition with a specific proportion of fibrous fillers, where the proportion of fibrous filler with a fiber length of 50 μm or less is 0.5% by mass or less, and the proportion of fibrous filler with a fiber length of 10 μm or more and 75 μm or less is 0% by mass or more and 1% by mass or less, is used, along with glass fibers and a high content of monomer units derived from aromatic hydroxycarboxylic acids, to suppress gas generation during molding.
The composition effectively reduces gas generation in high-temperature environments by exposing fibrous fillers with longer lengths to the surface, allowing high boiling point components to volatilize and be discharged during molding, resulting in a molded article with minimal gas formation.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Liquid crystal polyester composition and method for producing the same
[0001] The present disclosure relates to a liquid crystal polyester composition and a method for producing the same.
[0002] Liquid crystal polyesters are used in a variety of applications due to their high fluidity, heat resistance and dimensional accuracy.
[0003] Liquid crystal polyesters are usually used as liquid crystal polyester compositions containing fillers and the like to satisfy required properties depending on the application. For example, Patent Document 1 describes a liquid crystal polyester composition containing glass fibers having a non-circular cross-sectional shape.
[0004] Japanese Patent Application Laid-Open No. 2008-013703
[0005] However, conventional liquid crystal polyester compositions have a problem in that a small amount of gas is generated from the surface of the molded article in a high temperature environment.
[0006] An object of the present disclosure is to provide a liquid crystalline polyester composition capable of forming a molded article in which generation of gas (particularly high-boiling point components) under high temperature environments is suppressed. Another object of the present disclosure is to provide a method for producing the liquid crystalline polyester composition.
[0007] The present disclosure provides, for example, the following: [1] A liquid crystal polyester composition comprising a liquid crystal polyester and a fibrous filler (A), wherein a proportion of fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) is 0.5 mass% or less. [2] The liquid crystal polyester composition according to [1], wherein a proportion of fibrous filler (A-2) having a fiber length of 10 μm or more and 75 μm or less in the fibrous filler (A) is 0 mass% or more and 1 mass% or less. [3] The liquid crystal polyester composition according to [1] or [2], wherein the fibrous filler (A) contains glass fiber. [4] The liquid crystal polyester composition according to any one of [1] to [3], wherein the content of the fibrous filler (A) is 5 mass% or more and 35 mass% or less. [5] The liquid crystal polyester composition according to any one of [1] to [4], wherein the liquid crystal polyester contains a monomer unit derived from an aromatic hydroxycarboxylic acid. [6] The liquid crystal polyester composition according to [5], wherein the content of the monomer unit is 50 mol % or more relative to the total of all monomer units constituting the liquid crystal polyester. [7] A method for producing a liquid crystal polyester composition, comprising a mixing step of mixing a liquid crystal polyester with a fibrous filler to obtain a liquid crystal polyester composition, wherein the mixing step is a step of mixing the liquid crystal polyester with the fibrous filler so that a proportion of fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) in the liquid crystal polyester composition is 0.5 mass % or less.
[0008] According to the present disclosure, it is possible to provide a liquid crystal polyester composition capable of forming a molded article in which generation of gas (particularly high-boiling point components) in a high-temperature environment is suppressed. Furthermore, according to the present disclosure, it is possible to provide a method for producing the liquid crystal polyester composition.
[0009] A preferred embodiment of the present disclosure will be described in detail below.
[0010] The liquid crystal polyester composition of this embodiment (hereinafter also simply referred to as "liquid crystal polyester composition") contains a liquid crystal polyester and a fibrous filler (fibrous filler (A)). The proportion of the fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) is 0.5 mass% or less.
[0011] According to the liquid crystal polyester composition of the present embodiment, a molded article can be formed in which generation of gas (particularly high boiling point components) in a high temperature environment is suppressed.
[0012] The reason why such an effect is achieved is thought to be as follows. The liquid crystal polyester composition of this embodiment has a small amount of fibrous filler (A-1) with a fiber length of 50 μm or less and a large amount of fibrous filler (A') with a fiber length of more than 50 μm. In this embodiment, since there is a large amount of fibrous filler with a fiber length of more than 50 μm, the fibrous filler (A') is likely to be exposed to the surface when the liquid crystal polyester composition is molded. When the fibrous filler (A') is exposed to the surface, gas components (particularly high-boiling point components) inside the composition are likely to be volatilized by heating during molding and discharged to the outside of the composition. That is, it is thought that a molded article formed from the liquid crystal polyester composition of this embodiment has components that cause gas generation removed in advance by heating during molding, and therefore generates less gas in a high-temperature environment.
[0013] (1) Liquid Crystalline Polyester The liquid crystal polyester may be any polyester that exhibits liquid crystallinity in a molten state. The liquid crystal polyester composition may contain only one type of liquid crystal polyester, or may contain two or more types of liquid crystal polyester.
[0014] The flow initiation temperature of the liquid crystal polyester may be 250° C. or higher, or 270° C. or higher. The flow initiation temperature of the liquid crystal polyester may be 400° C. or lower, 360° C. or lower, or 340° C. or lower. That is, the flow initiation temperature of the liquid crystal polyester may be, for example, 250° C. or higher and 400° C. or lower, 250° C. or higher and 360° C. or lower, 250° C. or higher and 340° C. or lower, 270° C. or higher and 400° C. or lower, 270° C. or higher and 360° C. or lower, or 270° C. or higher and 340° C. or lower.
[0015] In this specification, the flow initiation temperature of the liquid crystal polyester is measured using a flow tester, and the liquid crystal polyester is subjected to a pressure of 9.8 MPa (100 kg / cm 2 The liquid crystalline polyester is melted while being heated at a rate of 4°C / min under a load of 1000 kJ / min, and the molten liquid crystalline polyester is extruded from a nozzle having an inner diameter of 1 mm and a length of 10 mm, and the temperature is the temperature at which the viscosity of the extruded liquid crystalline polyester is 4800 Pa·s (48,000 poise).
[0016] The liquid crystal polyester has constituent units (also referred to as monomer units) derived from raw material monomers. The liquid crystal polyester may have a main monomer unit (for example, 90 mol% or more, 95 mol% or more, or 99 mol% or more of the monomer units relative to the total of all monomer units, preferably all monomer units) derived from an aromatic compound. A liquid crystal polyester in which all monomer units are derived from an aromatic compound is also referred to as a wholly aromatic liquid crystal polyester.
[0017] Typical examples of liquid crystal polyesters include polymers having monomer units derived from aromatic hydroxycarboxylic acids (preferably polymers having two or more types of monomer units derived from aromatic hydroxycarboxylic acids), polymers having monomer units derived from aromatic dicarboxylic acids and monomer units derived from aromatic diols, and polymers having monomer units derived from aromatic hydroxycarboxylic acids, monomer units derived from aromatic dicarboxylic acids and monomer units derived from aromatic diols.
[0018] Examples of the monomer unit derived from an aromatic hydroxycarboxylic acid include a monomer unit represented by the following formula (I): Examples of the monomer unit derived from an aromatic dicarboxylic acid include a monomer unit represented by the following formula (II): Examples of the monomer unit derived from an aromatic diol include a monomer unit represented by the following formula (III) (wherein X and Y are oxygen atoms):
[0019] In this specification, "derived" means that in the monomer units of the liquid crystal polyester formed by polymerization of the raw material monomers, the chemical structure of the functional group that contributes to polymerization of the raw material monomers has changed, but other structural changes have not occurred. Here, "derived" is a concept that also includes cases where the monomer unit is derived from a polymerizable derivative of the raw material monomer (for example, a compound obtained by converting the functional group that contributes to polymerization of the raw material monomers into another polymerizable group).
[0020] The liquid crystal polyester may have a monomer unit represented by the following formula (I) (hereinafter also referred to as "monomer unit (I)"). In this specification, CO in the formula represents a carbonyl group. 1 -CO- (I) [wherein, Ar 1 represents a phenylene group, a naphthylene group, or a biphenylylene group. 1 Some or all of the hydrogen atoms in the group represented by the formula (I) may be substituted with a halogen atom, an alkyl group, or an aryl group.
[0021] The liquid crystal polyester may further have a monomer unit represented by the following formula (II) (hereinafter also referred to as "monomer unit (II)") and / or a monomer unit represented by the following formula (III) (hereinafter also referred to as "monomer unit (III)"). 2 -CO- (II) -X-Ar 3 -Y- (III) [wherein, Ar 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following formula (IV): X and Y each independently represent an oxygen atom or an imino group (—NH—). 2 Some or all of the hydrogen atoms of the group represented by Ar may be substituted with a halogen atom, an alkyl group or an aryl group. 3 Some or all of the hydrogen atoms of the group represented by the formula (I) may be substituted with a halogen atom, an alkyl group or an aryl group. 4 -Z-Ar 5 - (IV) [wherein, Ar 4 and Ar5 each independently represents a phenylene group or a naphthylene group, and Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkanediyl group.
[0022] Ar 1 , Ar 2 or Ar 3 Examples of halogen atoms that can substitute for hydrogen atoms in include fluorine, chlorine, bromine and iodine atoms.
[0023] Ar 1 , Ar 2 or Ar 3 The alkyl group that can substitute for a hydrogen atom in may be linear, branched, or cyclic. The alkyl group may be, for example, an alkyl group having 1 to 10 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, and an n-decyl group.
[0024] Ar 1 , Ar 2 or Ar 3 The aryl group capable of substituting a hydrogen atom in may be a single ring or a condensed ring. The aryl group may be, for example, an aryl group having 6 to 20 carbon atoms. Examples of the aryl group include a phenyl group, an o-tolyl group, an m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group. The aryl group may be a group in which a hydrogen atom in an aromatic ring is substituted with an alkyl group, such as a tolyl group.
[0025] Ar 1 , Ar 2 or Ar 3 When a hydrogen atom of is substituted with the above-mentioned group, the number of substitutions may be one or two, or may be one.
[0026] The alkanediyl group in Z may be linear or branched. The alkanediyl group may be an alkanediyl group having 1 to 10 carbon atoms. Examples of the alkanediyl group include a methylene group, an ethanediyl group, a propanediyl group (e.g., a propane-2,2-diyl group), a butanediyl group, and an octanediyl group (e.g., an octane-3,3-diyl group).
[0027] The monomer unit (I) can be, for example, Ar 1 is a phenylene group, 1 is a naphthylene group or a monomer unit Ar 1 may be a monomer unit in which Ar is a biphenylylene group; 1 is a phenylene group or a monomer unit Ar 1 may be a monomer unit in which Ar is a naphthylene group, 1 is a 1,4-phenylene group or a monomer unit Ar 1 The liquid crystal polyester may have one or more kinds of monomer units (I).
[0028] The monomer unit (II) is, for example, Ar 2 is a phenylene group, 2 is a naphthylene group, 2 is a biphenylylene group, or Ar 2 is a diphenylether-diyl group, and Ar 2 is a phenylene group, 2 is a naphthylene group, or Ar 2 may be a monomer unit in which Ar is a biphenylylene group, 2 is a phenylene group, or Ar 2may be a monomer unit in which the monomer unit (II) is a naphthylene group. The phenylene group may be a 1,4-phenylene group or a 1,3-phenylene group. The naphthylene group may be a 2,6-naphthylene group or a 2,7-naphthylene group. The biphenylylene group may be a 4,4'-biphenylylene group. The diphenylether-diyl group may be a diphenylether-4,4'-diyl group. The liquid crystal polyester may have one or more types of monomer units (II).
[0029] The monomer unit (II) is, for example, Ar 2 is a 1,4-phenylene group, 2 is a 1,3-phenylene group, 2 is a 2,6-naphthylene group, 2 is a 2,7-naphthylene group, 2 is a 4,4'-biphenylylene group, or Ar 2 is a diphenylether-4,4'-diyl group, and Ar 2 is a 1,4-phenylene group, 2 is a 1,3-phenylene group, or Ar 2 may be a monomer unit in which the aryl group is a 2,6-naphthylene group.
[0030] The monomer unit (III) is, for example, Ar 3 is a phenylene group, 3 is a naphthylene group, or Ar 3 may be a monomer unit in which Ar is a biphenylylene group; 3 is a phenylene group, or Ar 3 may be a monomer unit in which Ar is a biphenylylene group, 3 is a 1,4-phenylene group, or Ar 3 The liquid crystal polyester may have one or more kinds of monomer units (III).
[0031] The monomer unit (III) may be a monomer unit (III) in which X and Y are each an oxygen atom.
[0032] The monomer unit (I) may be a monomer unit represented by the following formula (Ia) (hereinafter also referred to as "monomer unit (Ia)"), the monomer unit (II) may be a monomer unit represented by the following formula (IIa) (hereinafter also referred to as "monomer unit (IIa)"), and the monomer unit (III) may be a monomer unit represented by the following formula (IIIa) (hereinafter also referred to as "monomer unit (IIIa)"): 11 -CO- (Ia) -CO-Ar 12 -CO- (IIa) -O-Ar 13 -O- (IIIa) [wherein, Ar 11 represents a 1,4-phenylene group or a 2,6-naphthylene group. 12 represents a 1,4-phenylene group, a 1,3-phenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, a 4,4'-biphenylylene group, or a diphenylether-4,4'-diyl group. 13 represents a 1,4-phenylene group or a 4,4'-biphenylylene group. 11 , Ar 12 or Ar 13 Some or all of the hydrogen atoms in the group represented by the formula (I) may be independently substituted with a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms.]
[0033] The liquid crystal polyester may be, for example, a polymer having the monomer unit (Ia), a polymer having the monomer unit (Ia) and the monomer unit (IIa), or a polymer having the monomer unit (Ia), the monomer unit (IIa), and the monomer unit (IIIa).
[0034] The liquid crystal polyester preferably has a monomer unit derived from an aromatic hydroxycarboxylic acid (hereinafter also referred to as "monomer unit A"). The majority of the monomer units (e.g., 50 mol % or more) may be monomer unit A, or all of the monomer units may be monomer unit A.
[0035] The liquid crystal polyester may have, as the monomer unit A, at least one monomer unit selected from the group consisting of a monomer unit derived from p-hydroxybenzoic acid and a monomer unit derived from 2-hydroxy-6-naphthoic acid.
[0036] The number of monomer units A in the liquid crystal polyester having monomer units A may be 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 55 mol% or more, or 60 mol% or more, relative to the total of all monomer units of the liquid crystal polyester. Furthermore, the number of monomer units A in the liquid crystal polyester having monomer units A may be 100 mol% or less, 95 mol% or less, 90 mol% or less, 85 mol% or less, or 80 mol% or less, relative to the total of all monomer units of the liquid crystal polyester. That is, the number of the monomer units A in the liquid crystal polyester having the monomer units A is, for example, 20 mol% or more and 100 mol% or less, 20 mol% or more and 95 mol% or less, 20 mol% or more and 90 mol% or less, 20 mol% or more and 85 mol% or less, 20 mol% or more and 80 mol% or less, 30 mol% or more and 100 mol% or less, 30 mol% or more and 95 mol% or less, 30 mol% or more and 90 mol% or less, 30 mol% or more and 85 mol% or less, 30 mol% or more and 80 mol% or less, 40 mol% or more and 100 mol% or less, 40 mol% or more and 95 mol% or less, 40 mol% or more and 90 mol% or less, 40 mol% or more and 90 mol% or less, 40 mol% or more and 85 mol% or less, 40 mol% or more and 80 mol% or less, 50 mol% or more and 100 mol% or less, 50 mol% or more and 95 mol% or less, 50 mol% or more and 90 mol% or less, 50 mol% or more and 85 mol% or less, 50 mol% or more and 80 mol% or less, 55 mol% or more and 100 mol% or less, 55 mol% or more and 95 mol% or less, 55 mol% or more and 90 mol% or less, 55 mol% or more and 85 mol% or less, 55 mol% or more and 80 mol% or less, 60 mol% or more and 100 mol% or less, 60 mol% or more and 95 mol% or less, 60 mol% or more and 90 mol% or less, 60 mol% or more and 85 mol% or less, or 60 mol% or more and 80 mol% or less.
[0037] When the liquid crystal polyester is a polymer having two or more kinds of monomer units (I), at least one Ar of the monomer units (I) 1 When the liquid crystal polyester is a polymer having the monomer unit (I) and the monomer unit (II), Ar of the monomer unit (I) may be a naphthylene group. 1 and Ar of the monomer unit (II) 2 When the liquid crystal polyester is a polymer having the monomer unit (I), the monomer unit (II), and the monomer unit (III), at least one of Ar of the monomer unit (I) may be a naphthylene group. 1 , Ar of the monomer unit (II) 2 and Ar of the monomer unit (III) 3 At least one of the groups may be a naphthylene group.
[0038] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (I) may be, for example, 30 mol% or more, 40 mol% or more, 45 mol% or more, 50 mol% or more, or 55 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (I) may be, for example, 80% or less, or 70% or less, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (I) may be, for example, 30 mol% or more and 80 mol% or less, 30 mol% or more and 70 mol% or less, 40 mol% or more and 80 mol% or less, 40 mol% or more and 70 mol% or less, 45 mol% or more and 80 mol% or less, 45 mol% or more and 70 mol% or less, 50 mol% or more and 80 mol% or less, 50 mol% or more and 70 mol% or less, 55 mol% or more and 80 mol% or less, or 55 mol% or more and 70 mol% or less, based on the total of all the monomer units of the liquid crystal polyester.
[0039] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (II) may be, for example, 35 mol% or less, or 30 mol% or less, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (II) may be, for example, 5 mol% or more, 10 mol% or more, or 15 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (II) may be, for example, 5 mol% or more and 35 mol% or less, 5 mol% or more and 30 mol% or less, 10 mol% or more and 35 mol% or less, 10 mol% or more and 30 mol% or less, 15 mol% or more and 35 mol% or less, or 15 mol% or more and 30 mol% or less, relative to the total of all the monomer units of the liquid crystal polyester.
[0040] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (III) may be, for example, 35 mol% or less, or 30 mol% or less, based on the total of all the monomer units of the liquid crystal polyester. Also, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II) and the monomer unit (III), the number of the monomer unit (III) may be, for example, 5 mol% or more, 10 mol% or more, or 15 mol% or more, based on the total of all the monomer units of the liquid crystal polyester. That is, when the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the number of the monomer unit (III) may be, for example, 5 mol% or more and 35 mol% or less, 5 mol% or more and 30 mol% or less, 10 mol% or more and 35 mol% or less, 10 mol% or more and 30 mol% or less, 15 mol% or more and 35 mol% or less, or 15 mol% or more and 30 mol% or less, relative to the total of all the monomer units of the liquid crystal polyester.
[0041] When the liquid crystal polyester has the monomer unit (I), the monomer unit (II), and the monomer unit (III), the ratio of the number of the monomer units (II) to the number of the monomer units (III) ([number of the monomer units (II)] / [number of the monomer units (III)]) may be 0.9 / 1 to 1 / 0.9, 0.95 / 1 to 1 / 0.95, or 0.98 / 1 to 1 / 0.98.
[0042] The liquid crystal polyester may have monomer units other than the monomer unit (I), the monomer unit (II) and the monomer unit (III), but the number of such monomer units is preferably 10% or less, more preferably 5% or less, even more preferably 2% or less, still more preferably 1% or less, and particularly preferably 0%, based on the total number of all monomer units of the liquid crystal polyester.
[0043] In this specification, the number of each monomer unit contained in the liquid crystal polyester is determined by the analytical method described in JP 2000-19168 A. Specifically, the liquid crystal polyester is depolymerized by reacting it with a lower alcohol in a supercritical state, and the depolymerization product (monomers that derive each monomer unit) is quantified by liquid chromatography, whereby the number of each monomer unit relative to the total monomer units can be calculated.
[0044] The liquid crystal polyester can be produced by polymerizing raw material monomers corresponding to the monomer units that constitute the polyester, for example, according to the method described in Japanese Patent No. 6439027.
[0045] The content of the liquid crystal polyester may be, for example, 60% by mass or more, 70% by mass or more, or 80% by mass or more, based on the total amount of the liquid crystal polyester composition. Furthermore, the content of the liquid crystal polyester may be, for example, 95% by mass or less, 90% by mass or less, or 88% by mass or less, based on the total amount of the liquid crystal polyester composition. That is, the content of the liquid crystal polyester may be, for example, 60% by mass or more to 95% by mass or less, 60% by mass or more to 90% by mass or less, 60% by mass or more to 88% by mass or less, 70% by mass or more to 95% by mass or less, 70% by mass or more to 90% by mass or less, 70% by mass or more to 88% by mass or less, 80% by mass or more to 95% by mass or less, 80% by mass or more to 90% by mass or less, or 80% by mass or more to 88% by mass or less, based on the total amount of the liquid crystal polyester composition.
[0046] (2) Fibrous Filler The liquid crystal polyester composition contains a fibrous filler (A).
[0047] Examples of the fibrous filler (A) include glass fiber and carbon fiber, and among these, glass fiber is preferred. The proportion of glass fiber in the fibrous filler (A) may be, for example, 90% by mass or more, 95% by mass or more, 99% by mass or more, or 100% by mass.
[0048] The proportion of the fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) is 0.5 mass % or less, and may be 0.3 mass % or less, 0.1 mass % or less, or 0.05 mass % or less.
[0049] The proportion of the fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) may be 0% by mass. Alternatively, the fibrous filler (A) may contain a small amount of the fibrous filler (A-1) having a fiber length of 50 μm or less, and in this case, the proportion of the fibrous filler (A-1) may be, for example, 0.001% by mass or more, 0.005% by mass or more, or 0.01% by mass or more.
[0050] The proportion of the fibrous filler (A-2) having a fiber length of 10 μm or more and 75 μm or less in the fibrous filler (A) may be, for example, 0% by mass or more, 0.001% by mass or more, or 0.005% by mass or more, which tends to more effectively exhibit the reinforcing effect of the fibrous filler.
[0051] The proportion of the fibrous filler (A-2) having a fiber length of 10 μm or more and 75 μm or less in the fibrous filler (A) may be, for example, 2.0 mass % or less, 1.0 mass % or less, 0.5 mass % or less, 0.3 mass % or less, or 0.1 mass % or less, which tends to further increase the mechanical strength of the molded article.
[0052] The number average fiber length of the fibrous filler (A) may be, for example, 50 μm or more, 100 μm or more, or 200 μm or more, which tends to increase the mechanical strength of the molded article.
[0053] The number average fiber length of the fibrous filler (A) may be, for example, 1500 μm or less, 1000 μm or less, or 500 μm or more, which tends to further improve the detail filling ability in the molded article.
[0054] The fiber length distribution of the fibrous filler (A) (proportion of fibrous filler (A-1), proportion of fibrous filler (A-2), number average fiber length) is measured by the following method. <Measurement of fiber length distribution> 4 g of a liquid crystal polyester composition is heated at 600°C for 4 hours to obtain ash. The obtained ash is dispersed in ethylene glycol to prepare a preparation, which is observed under an optical microscope at a magnification of 500. Of the fibers that fall within the field of view (i.e., fibers whose both ends are within the field of view), the fiber lengths of fibers that have a length equal to or greater than the fiber diameter are measured. The fiber lengths of 500 or more fibers are measured to determine the fiber length distribution.
[0055] The fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 5 μm or more, 6 μm or more, or 9 μm or more. The fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 17 μm or less, 15 μm or less, or 12 μm or less. That is, the fiber diameter (single fiber diameter) of the fibrous filler (A) may be, for example, 5 μm or more and 17 μm or less, 5 μm or more and 15 μm or less, 5 μm or more and 12 μm or less, 6 μm or more and 17 μm or less, 6 μm or more and 15 μm or less, 6 μm or more and 12 μm or less, 9 μm or more and 17 μm or less, 9 μm or more and 15 μm or less, or 9 μm or more and 12 μm or less.
[0056] The content of the fibrous filler (A) may be, for example, 5% by mass or more, 10% by mass or more, or 12% by mass or more, based on the total amount of the liquid crystal polyester composition. Furthermore, the content of the fibrous filler (A) may be, for example, 40% by mass or less, 30% by mass or less, or 20% by mass or less, based on the total amount of the liquid crystal polyester composition. That is, the content of the fibrous filler (A) may be, for example, 5% by mass or more to 40% by mass or less, 5% by mass or more to 30% by mass or less, 5% by mass or more to 20% by mass or less, 10% by mass or more to 40% by mass or less, 10% by mass or more to 30% by mass or less, 10% by mass or more to 20% by mass or less, 12% by mass or more to 40% by mass or less, 12% by mass or more to 30% by mass or less, or 12% by mass or more to 20% by mass or less.
[0057] The liquid crystal polyester composition may contain one or more resins other than the liquid crystal polyester, such as polyolefins, cyclic polyolefins, polyvinyl chloride, polysulfones, (meth)acrylic resins, polyphenylene ether resins, polyacetal resins, polyamide resins, imide resins, polystyrene resins, cellulose resins, polyether ether ketone resins, fluororesins, polycarbonate resins, and thermosetting resins.
[0058] The liquid crystal polyester composition may contain one or more additives other than the fibrous filler, such as a filler, a colorant, a dispersant, a plasticizer, an antioxidant, a curing agent, a flame retardant, a heat stabilizer, an ultraviolet absorber, an antistatic agent, a surfactant, a lubricant, and a mold release agent.
[0059] The liquid crystal polyester composition may be in the form of powder, particles (for example, granules, pellets, etc.), film, sheet, plate, or the like.
[0060] The liquid crystal polyester composition of the present embodiment may be produced, for example, by the following method.
[0061] (Method for producing liquid crystal polyester composition) The method for producing the liquid crystal polyester composition of this embodiment may include a mixing step of mixing a liquid crystal polyester with a fibrous filler (hereinafter also referred to as fibrous filler (a)) to obtain a liquid crystal polyester composition.
[0062] In the mixing step, the liquid crystal polyester and the fibrous filler (a) are mixed so that the proportion of the fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) in the liquid crystal polyester composition is 0.5 mass % or less.
[0063] The fibrous filler (a) may be, for example, a fiber bundle obtained by bundling fibrous fillers with a bundling agent.
[0064] In the mixing step, the fibrous filler blended in the liquid crystal polyester is broken, for example, to form a fibrous filler with a short fiber length. If the fibrous filler is crushed without being broken, a significantly short fibrous filler (A-1) is likely to be formed. Therefore, in the mixing step, by selecting a mixing method that reduces crushing of the fibrous filler, a liquid crystal polyester composition having a proportion of fibrous filler (A-1) of 0.5 mass % or less can be easily obtained.
[0065] An example of a mixing method in the mixing step is a method in which a fibrous filler (a) is introduced into a melt of the liquid crystal polyester and kneaded. In such a method, for example, by increasing the time from introducing the fibrous filler (a) into the melt of the liquid crystal polyester to kneading (for example, by increasing the length from the introduction port of the fibrous filler (a) to the kneading disk), the crushing of the fibrous filler tends to be reduced. By increasing the time from introducing the fibrous filler (a) to kneading, the fibrous filler (a) is loosened in the melt, and the formation of a fibrous filler (A-1) due to the crushing of aggregates of the fibrous filler (a) (for example, fiber bundles bonded with a sizing agent) is suppressed.
[0066] The mixing step may be carried out using, for example, a twin-screw extruder.
[0067] The liquid crystal polyester composition of the present embodiment may be in the form of, for example, particles (e.g., granules, pellets, etc.), a film, a sheet, a plate, etc. That is, the mixing step may be a step of mixing the liquid crystal polyester and a fibrous filler (hereinafter also referred to as fibrous filler (a)), and molding the mixture to obtain a molded article of the liquid crystal polyester composition.
[0068] The liquid crystal polyester composition of the present embodiment can be suitably applied to parts for communication devices, electrical devices, electronic devices, medical devices, automobiles, home appliances, industrial machinery, daily necessities, etc. The parts can be produced, for example, by molding the liquid crystal polyester composition by injection molding, compression molding, extrusion molding, blow molding, etc.
[0069] Although one embodiment of the invention according to the present disclosure has been described above, the invention according to the present disclosure is not limited to the above embodiment.
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, percentages and parts representing the content or amount used are by mass unless otherwise specified.
[0071] Example 1 (1) Production of Liquid Crystal Polyester A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 1118.8 g (8.10 mol) of p-hydroxybenzoic acid, 547.4 g (3.00 mol) of 2-hydroxy-6-naphthoic acid, 1235.3 g (12.1 mol) of acetic anhydride, and 0.17 g of 1-methylimidazole. After thoroughly purging the reactor with nitrogen gas, the temperature was raised to 140°C over 15 minutes under a nitrogen gas stream, and the temperature was maintained at 140°C and refluxed for 1 hour. Thereafter, the temperature was raised to 280°C over 3 hours and 40 minutes while distilling off the by-product acetic acid. The point at which an increase in torque was observed was considered the end of the reaction, and the contents were removed. The flow initiation temperature of the resulting solid content was 235°C. The obtained solid was cooled to room temperature and crushed in a coarse crusher. The mixture was heated from room temperature (25°C) to 235°C over 1 hour in a nitrogen atmosphere, then heated from 235°C to 240°C over 4 hours and 10 minutes, and held at 240°C for 5 hours to carry out solid-state polymerization. The obtained solid-state polymer was cooled to room temperature to obtain a powdered liquid crystal polyester (1). The flow initiation temperature of the obtained liquid crystal polyester (1) was 277°C.
[0072] (2) Preparation of Liquid Crystal Polyester Composition Using a twin-screw extruder (Shibaura Machinery, TEM48S), liquid crystal polyester (1) and glass fiber were kneaded to produce pellets of the liquid crystal polyester composition. Specifically, liquid crystal polyester (1) was fed through the main feed port of the twin-screw extruder, glass fiber was fed through the side feed port, and kneading was performed. The kneaded mixture was extruded from the nozzle of the extruder to obtain strands. The feed amounts were 85 parts by mass of liquid crystal polyester (1) and 15 parts by mass of glass fiber. The strands were cooled by spraying water to solidify them, and then further cooled while blowing air to remove the water. The solidified strands were cut with a pelletizer to obtain pellets of the liquid crystal polyester composition.
[0073] (Comparative Example 1) Pellets of a liquid crystal polyester composition were obtained in the same manner as in Example 1, except that the position of the side feed port was moved downstream, the length from the side feed port to the kneading disc section was set to 0.9 times that of Example 1, and the length of the kneading disc section was set to 0.5 times that of Example 1.
[0074] <Measurement of Fiber Length Distribution of Glass Fiber> The fiber length distribution of the glass fiber was measured for the pellets of the liquid crystal polyester composition obtained in Example 1 and Comparative Example 1 using the following method. 4 g of pellets were heated at 600°C for 4 hours to obtain ash. The obtained ash was dispersed in ethylene glycol to prepare a preparation, which was then observed under an optical microscope at a magnification of 500x. Of the fibers that fell within the field of view, the fiber lengths of fibers having a length equal to or greater than the fiber diameter were measured. The fiber lengths of 500 or more fibers were measured to determine the fiber length distribution. From the obtained fiber length distribution, the proportion of fibrous filler (A-1) having a fiber length of 50 μm or less, the proportion of fibrous filler (A-2) having a fiber length of 10 μm or more and 75 μm or less, and the number-average fiber length of the fibrous fillers were determined. The results are shown in Table 1.
[0075]
[0076] <Evaluation of Gas Generation Amount> The amount of gas generated was evaluated for the pellets of the liquid crystal polyester composition obtained in Example 1 and Comparative Example 1 by the following method. A dumbbell test piece with a thickness of 0.8 mm was prepared by injection molding using the pellets. The parallel portion of this test piece was cut into a 5 mm square to obtain a measurement sample of 5 mm x 5 mm x 0.8 mm. 4 g of the measurement sample was sealed in a vial and sealed with a septum. The sample sealed in the vial was heated at 120°C for 20 hours, and then the amount of gas generated was measured under the following conditions using a headspace gas chromatograph (GC-2030AF, manufactured by Shimadzu Corporation). <Conditions> Column: Restek Rtx-1301 (inner diameter: 0.25 mm, length: 60 m, film thickness: 1.4 μm) Column temperature: held at 60°C for 5 minutes, heated to 220°C at 10°C / min, held at 220°C for 15 minutes Carrier gas: helium Split ratio: 10 Carrier gas flow rate: 10 mL / min Acetone, acetic acid, phenol, and acetic phenol were quantified using a calibration curve, and peaks from other components were quantified by converting components with retention times of 15.5 minutes or less to acetone and components with retention times greater than 15.5 minutes to phenol. The measured amounts of low-boiling components with retention times of 15.5 minutes or less and high-boiling components with retention times greater than 15.5 minutes are shown in Table 2.
[0077]
[0078] As shown in Table 2, in the liquid crystal polyester composition of Example 1, compared with the liquid crystal polyester composition of Comparative Example 1, generation of gas (particularly high boiling point components) in a high temperature environment was suppressed.
Claims
1. A liquid crystal polyester composition comprising a liquid crystal polyester and a fibrous filler (A), wherein the proportion of fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) is 0.5 mass % or less.
2. The liquid crystal polyester composition according to claim 1, wherein the proportion of fibrous filler (A-2) having a fiber length of 10 μm or more and 75 μm or less in the fibrous filler (A) is 2.0 mass % or less.
3. The liquid crystal polyester composition according to claim 1, wherein the fibrous filler (A) comprises glass fibers.
4. The liquid crystal polyester composition according to claim 1, wherein the content of the fibrous filler (A) is 5% by mass or more and 40% by mass or less.
5. The liquid crystalline polyester composition according to claim 1, wherein the liquid crystalline polyester contains monomer units derived from an aromatic hydroxycarboxylic acid.
6. The liquid crystal polyester composition according to claim 5, wherein the content of said monomer unit is 50 mol % or more based on the total of all monomer units constituting said liquid crystal polyester.
7. A method for producing a liquid crystal polyester composition, comprising a mixing step of mixing a liquid crystal polyester with a fibrous filler to obtain a liquid crystal polyester composition, wherein the mixing step is a step of mixing the liquid crystal polyester with the fibrous filler such that a proportion of fibrous filler (A-1) having a fiber length of 50 μm or less in the fibrous filler (A) in the liquid crystal polyester composition is 0.5 mass % or less.
Citation Information
Patent Citations
Liquid crystal resin composition and precision formed product of the composition
JP1999209590A
Liquid crystal polyester resin molded article, liquid crystal polyester resin pellet and production method of liquid crystal polyester resin pellet
JP2021028384A
Liquid crystal polyester resin composition, and molded article made from the same
JP2024061926A
Process for producing resin composition containing fibrous filler in high concentration and resin composition pellet