Negative electrode body and method for manufacturing negative electrode body

The negative electrode body with a roughened current collector and specific SiOxLi y particles, along with an ion conductive and solid electrolyte layer, addresses the challenges of silicon-based lithium-ion batteries, achieving high capacity and safety by minimizing expansion and improving conductivity.

WO2024247872A1PCT designated stage expired Publication Date: 2024-12-05SHIN ETSU CHEMICAL CO LTD
View PDF 28 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018978
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries using silicon as the negative electrode material face challenges in maintaining high capacity and safety due to volumetric expansion, which leads to conductive path breakage and reduced energy density, especially when using solid electrolytes.

Method used

A negative electrode body with a roughened current collector, a multilayer active material structure, and an ion conductive layer, featuring SiOxLi y particles with specific oxygen and lithium ratios, and a solid electrolyte layer to enhance ionic conductivity and stability, reducing expansion and improving cycle characteristics.

Benefits of technology

The solution significantly increases battery capacity while maintaining excellent battery characteristics by reducing expansion and improving ionic conductivity, leading to enhanced cycle life and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018978_05122024_PF_FP_ABST
    Figure JP2024018978_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention is a negative electrode body that has a negative electrode including a negative electrode current collector having a roughened surface, a negative electrode active material layer provided on the negative electrode current collector, and an ion conductive layer having lithium ion conductivity on the surface of the negative electrode active material layer, and has a solid electrolyte layer adjacent to the ion conductive layer, wherein the negative electrode body is characterized in that: the negative electrode active material layer contains negative electrode active material particles having a compound containing lithium, silicon, and oxygen; the negative electrode active material particles can be represented by SiOx1Liy1; and the value of x1 is more than 0.8 and 1.2 or less, and the value of y1 is 0.5 or more and 3.4 or less. It is thereby possible to provide a negative electrode body having a negative electrode in which capacitance can be dramatically increased while maintaining exceptional battery characteristics, and expansion under full charging can be suppressed.
Need to check novelty before this filing date? Find Prior Art

Description

Anode body and method for manufacturing the anode body

[0001] The present invention relates to an anode body and a method for manufacturing the anode body.

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of achieving high energy density has been progressing. The application of these secondary batteries is being considered not only for small electronic devices but also for large electronic devices such as automobiles and power storage systems such as those for homes.

[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and can provide a higher energy density than lead-acid batteries or nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte solution, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have called for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material has been considered. This is because the theoretical capacity of silicon (4199 mAh / g) is more than 10 times greater than that of graphite (372 mAh / g), and a significant improvement in battery capacity can be expected. The development of silicon materials as negative electrode active materials is being considered not only for silicon itself, but also for compounds such as alloys and oxides. Furthermore, the active material shape is being considered, ranging from the standard coated type for carbon-based active materials to an integrated type deposited directly on the current collector.

[0006] However, when silicon is used as the main raw material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, mainly near the surface of the negative electrode active material. Furthermore, ionic substances are generated within the active material, making it prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reactive area of ​​the active material. At this time, the electrolyte decomposes on the new surface, and a coating made of the electrolyte decomposition product is formed on the new surface, consuming the electrolyte. This can lead to a decrease in cycle performance.

[0007] To date, various studies have been conducted on negative electrode materials and electrode configurations for lithium-ion secondary batteries that use silicon materials as the main material in order to improve the initial battery efficiency and cycle characteristics.

[0008] Specifically, to achieve good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a vapor-phase method (see, for example, Patent Document 1). Furthermore, to achieve high battery capacity and safety, a carbon material (electron conductor) is provided on the surface of silicon oxide particles (see, for example, Patent Document 2). Furthermore, to improve cycle characteristics and achieve high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio near the current collector is formed (see, for example, Patent Document 3). Furthermore, to improve cycle characteristics, oxygen is incorporated into the silicon active material, and the silicon active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is higher near the current collector (see, for example, Patent Document 4).

[0009] In addition, in order to improve the initial charge / discharge efficiency, Si phase, SiO 2A nanocomposite containing metal oxides, such as MyO, is used (see, for example, Patent Document 5). To improve cycle performance, SiOx (0.8≦x≦1.5, particle size range = 1 μm to 50 μm) is mixed with a carbon material and sintered at high temperatures (see, for example, Patent Document 6). To improve cycle performance, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled so that the difference between the maximum and minimum molar ratios near the active material / current collector interface is 0.4 or less (see, for example, Patent Document 7). To improve battery load characteristics, a lithium-containing metal oxide is used (see, for example, Patent Document 8). To improve cycle performance, a hydrophobic layer, such as a silane compound, is formed on the surface of the silicon material (see, for example, Patent Document 9). To improve cycle performance, silicon oxide is used and a graphite coating is formed on the surface to impart conductivity (see, for example, Patent Document 10). In Patent Document 10, broad peaks appear at 1330 cm-1 and 1580 cm-1 in the shift values ​​obtained from the RAMAN spectrum of a graphite coating, and their intensity ratio I1330 / I1580 is 1.5<I1330 / I1580<3. Furthermore, to achieve high battery capacity and improved cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). Furthermore, to improve overcharge and overdischarge characteristics, silicon oxide is used in which the atomic ratio of silicon to oxygen is controlled to 1:y (0<y<2) (see, for example, Patent Document 12).

[0010] As for lithium ion secondary batteries using silicon oxide, Hitachi Maxell began shipping square secondary batteries for smartphones that use nanosilicon composites in June 2010 (see, for example, Non-Patent Document 1). The silicon oxide proposed by Hohl is Si 0+ ~Si 4+ It is a composite material with various oxidation states (see Non-Patent Document 2). Kapaklis also reported that applying a thermal load to silicon oxide results in the formation of Si and SiO 2 have proposed a disproportionated structure that is divided into Si and SiO, which contribute to charge and discharge among silicon oxides having a disproportionated structure (see Non-Patent Document 3). 2have focused on the above (see Non-Patent Document 4), and Yamada et al. have proposed the following reaction formula between silicon oxide and Li (see Non-Patent Document 5):

[0011] 2SiO(Si+SiO 2 ) + 6.85Li + + 6.85e - → 1.4 Li 3.75 Si + 0.4Li 4 SiO 4 + 0.2SiO 2

[0012] The above reaction formula is the reaction of Si and SiO 2 reacts with Li to form Li silicide, Li silicate, and partially unreacted SiO 2 This indicates that the two will be separated.

[0013] The Li silicate produced here is irreversible, and once formed, it is considered to be a stable substance that does not release Li. The capacity per weight calculated from this reaction formula is close to the experimental value, and is recognized as the reaction mechanism of silicon oxide. Kim et al. 4 SiO 4 As such, 7 Li-MAS-NMR 29 The identification was carried out using Si-MAS-NMR (see Non-Patent Document 6).

[0014] This irreversible capacity is the weakest point of silicon oxide, and improvement is required. Kim et al. have used a Li pre-doping method to form Li silicate in advance, which significantly improved the initial efficiency of the battery and produced a negative electrode that can withstand practical use (see Non-Patent Document 7).

[0015] Furthermore, instead of doping the electrode with Li, a method of treating the powder has also been proposed, which has achieved an improvement in irreversible capacity (see Patent Document 13).

[0016] Silicon oxide, which has improved irreversible capacity, can be used to replace a carbon anode at a high ratio, significantly increasing the battery capacity. However, increasing the ratio of silicon oxide in the anode increases the risk of fire in the event of a malfunction in a battery using a liquid electrolyte, reducing the safety of the battery.

[0017] Therefore, in order to ensure the safety of batteries, various all-solid-state batteries in which the liquid electrolyte is replaced with a solid electrolyte have been developed (see Patent Documents 14 to 17).

[0018] Japanese Patent Application Laid-Open No. 2001-185127 Japanese Patent Application Laid-Open No. 2002-042806 Japanese Patent Application Laid-Open No. 2006-164954 Japanese Patent Application Laid-Open No. 2006-114454 Japanese Patent Application Laid-Open No. 2009-070825 Japanese Patent Application Laid-Open No. 2008-282819 Japanese Patent Application Laid-Open No. 2008-251369 Japanese Patent Application Laid-Open No. 2008-177346 Japanese Patent Application Laid-Open No. 2007-234255 Japanese Patent Application Laid-Open No. 2009-212074 Japanese Patent Application Laid-Open No. 2009-205950 JP 25765 A JP 2015-156355 A JP 11-007942 A JP 2017-033647 A JP 2018-142431 A JP 2022-165490 A JP 2003-059492 A JP 2015-220196 A JP 2017-068929 A JP 2020-068104 A JP 2020-030919 A ​​JP 2021-128857 A

[0019] Battery Industries Association, May 1, 2003, issue "Denchi", page 10. A. Hohl, T. Wieder, PA van Aken, TE Weirich, G. Denninger, M. Vidal, S. Oswald, C. Deneke, J. Mayer, and H. Fuess: J. Non-Cryst. Solids, 320, (2003), 255. V. Kapaklis, J. Non-Crystalline Solids, 354 (2008) 612. Mariko Miyachi, Hironori Yamamoto, and Hidemasa Kawai, J. Electrochem. Soc. 2007 volume 154, issue 4, A376-A380. M. Yamada, M. Inaba, A. Ueda, K. Matsumoto, T. Iwasaki, T. Ohzuku, J. Electrochem. Soc., 159, A1630 (2012) Taeahn Kim, Sangjin Park, and Seung M. Oh, J. Electrochem. Soc. volume 154, (2007), A1112-A1117. Hye Jin Kim, Sunghun Choi, Seung Jong Lee, Myung Won Seo, Jae Goo Lee, Erhan Deniz, Yong Ju Lee, Eun Kyung Kim, and Jang Wook Choi,. Nano Lett. 2016, 16, 282-288. Sato Noboru, "Frontiers in the Development of Automotive Lithium-ion Batteries," Society Publishing, November 27, 2020, pp. 96-111

[0020] As mentioned above, in recent years, small electronic devices, such as mobile terminals, have become increasingly sophisticated and multifunctional, necessitating increased battery capacity for their main power sources: lithium-ion secondary batteries. One approach to solving this problem is the development of lithium-ion secondary batteries with anodes primarily made of silicon materials. Furthermore, lithium-ion secondary batteries using silicon materials are expected to have initial charge-discharge characteristics and cycle characteristics comparable to those of lithium-ion secondary batteries using carbon-based active materials. Therefore, by using silicon oxide modified by Li insertion and partial deintercalation as the anode active material, cycle characteristics and initial charge-discharge characteristics have been improved. Recently, by incorporating Li into silicon oxide as the primary material and forming Li silicate, the irreversible capacity, a disadvantage of silicon oxide, has been reduced, and batteries have actually begun to be marketed. Prototype batteries have been fabricated by replacing a high proportion of carbon anode material with Li—SiO—C (Non-Patent Document 8), which uses Li in silicon oxide, and by replacing the carbon anode material with Li. Although this has enabled significant capacity increases, increasing the amount of silicon oxide added reduces safety.

[0021] It has been reported that the use of a solid electrolyte as the electrolyte can address this safety issue and achieve high safety (Patent Documents 18 to 20). However, when using a graphite anode, the increase in capacity that can be expected from silicon oxide cannot be expected. While lithium anodes and silicon-based compound anodes can improve Coulomb efficiency, they still face the issue of reduced cycle performance due to disconnection of the conductive path caused by volume expansion (Patent Document 21). Even when using a silicon-based anode to suppress volume expansion, the presence of a void layer or the incorporation of a solid electrolyte into the anode results in a decrease in energy density (Patent Documents 22 and 23).

[0022] The present invention has been made in view of the above problems, and has an object to provide an anode body having an anode that can significantly increase capacity while maintaining excellent battery characteristics and can suppress expansion during full charge, and a method for manufacturing an anode body that can manufacture such an anode body.

[0023] In order to solve the above problems, the present invention provides an anode assembly having an anode including an anode current collector having a roughened surface, an anode active material layer provided on the anode current collector, and an ion conduction layer having lithium ion conductivity on the surface of the anode active material layer, and having a solid electrolyte layer adjacent to the ion conduction layer, wherein the anode active material layer contains anode active material particles having a compound containing lithium, silicon, and oxygen, and the anode active material particles are SiO x1 Li y1 The negative electrode body is characterized in that the value of x1 is greater than 0.8 and not greater than 1.2, and the value of y1 is not less than 0.5 and not greater than 3.4.

[0024] Such an anode body has an anode active material layer containing anode active material particles having a compound of lithium, silicon, and oxygen, thereby improving battery capacity. Furthermore, the anode body of the present invention can directly support the anode active material layer on the roughened surface of the anode current collector without using a binder, a conductive additive, or the like, thereby reducing the area of ​​the electrode not involved in charge and discharge, and reducing excess voids, thereby significantly improving the energy density of the electrode. Furthermore, the anode body of the present invention has a layer (ion conduction layer) having lithium ion conductivity on the surface (outermost surface) of the anode active material layer, and the ion conduction layer and the solid electrolyte layer are adjacent to each other, thereby improving the ionic conductivity between the solid electrolyte and the anode active material compared to conventional anode active material layers using silicon powder or silicon-based compound powder, thereby improving battery characteristics. Furthermore, the anode body of the present invention can be an anode body that can suppress expansion during full charge. Furthermore, the anode body of the present invention can be an anode body in which the composition formula of the anode active material particles is SiO x1 Li y1 When the value of x1 is greater than 0.8 and less than or equal to 1.2 and the value of y1 is greater than or equal to 0.5 and less than or equal to 3.4, excellent battery characteristics can be maintained. In the description of the present invention, the negative electrode and solid electrolyte integrated together will be referred to as a negative electrode body.

[0025] In this case, the negative electrode active material layer has a multilayer structure consisting of two or more layers, and when the negative electrode active material particles are defined as primary particles, the negative electrode active material layer forms secondary particles that are aggregates of the primary particles, and the secondary particles have a morphology that is separated from each other in the in-plane direction, and the thickness T1 of the negative electrode active material layer before charging and the thickness T2 when fully charged can have a relationship of T2 / T1≦1.4.

[0026] In this way, the anode body of the present invention can have a multilayer structure, and the anode active material particles can form secondary particles. A anode active material layer having a multilayer structure consisting of two or more layers can mitigate expansion and contraction of the anode active material layer. Therefore, the anode body of the present invention can suppress changes in thickness before and after charge. If the thickness T1 of the anode active material layer before charge and the thickness T2 after full charge satisfy the relationship T2 / T1≦1.4, expansion and contraction of the active material during charge and discharge is suppressed, electronic contact is less likely to be broken, and excellent battery characteristics can be maintained.

[0027] It is also preferable that the negative electrode active material layer having a multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity between at least one of the layers constituting the multilayer structure.

[0028] Such a negative electrode body has improved ionic conductivity and can reduce the resistance between the negative electrode active material layers, thereby improving battery performance.

[0029] The negative electrode active material layer contains Li 4 SiO 4 , Li 2 Si 2 O 5 , Li 2 SiO 3 and Li 6 Si 2 O 7 It is preferable that at least one of the above is included.

[0030] By containing at least one of these Li silicates, the battery is stable against charge and discharge, and can therefore exhibit excellent cycle characteristics.

[0031] The ion conduction layer having lithium ion conductivity is preferably made of at least one of a carbonate of Li, a phosphate of Li, a fluoride of Li, a carbonate of Al, a phosphate of Al, a fluoride of Al, a compound having a silyl group, and a carbonized material containing a polycyclic aromatic hydrocarbon.

[0032] By using such an ion-conducting layer, it is possible to suppress reactions with moisture and oxygen, suppress deterioration of the material, and facilitate the introduction of Li, thereby maintaining excellent battery characteristics.

[0033] Furthermore, the secondary particles of the negative electrode active material layer preferably consist of four or more primary particles on average.

[0034] Such a negative electrode body can more effectively prevent electrode collapse due to charge and discharge, and can maintain a stable negative electrode active material layer.

[0035] In the negative electrode body of the present invention, the solid electrolyte layer may be made of a sulfide-based solid electrolyte.

[0036] There is a risk that sulfide-based solid electrolytes will react with lithium released from silicon-based active materials and generate heat, but the negative electrode body of the present invention has an ion-conducting layer on the surface, which can suppress this reaction. This makes it possible to design a safe battery that is less likely to generate heat while maintaining high ion conductivity.

[0037] In this case, the sulfide-based solid electrolyte may contain at least one of lithium, indium, sulfur, and phosphorus.

[0038] The sulfide-based solid electrolyte is Li 2 S, P 2 S 5 , SiS 2 , LiI, LiBr, P 2 O 5 , Li 3 P.O. 4 and GeS 2 It may have at least one of the above.

[0039] In the negative electrode body of the present invention, the sulfide-based solid electrolyte may be suitably selected from those described above.

[0040] In the anode body of the present invention, the solid electrolyte layer may be made of an oxide-based solid electrolyte.

[0041] Oxide-based solid electrolytes are stable in air and easy to handle, making it possible to design safe batteries.

[0042] In this case, the oxide-based solid electrolyte may have a perovskite structure.

[0043] In this case, the oxide-based solid electrolyte may contain at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

[0044] The oxide-based solid electrolyte has a composition formula of A x2 BO 3 (0<x2<1), wherein the element A includes at least one of La and Li, and the element B includes at least one of Mg, W, Nb, and Ti.

[0045] The oxide-based solid electrolyte may contain a Nasicon-type phosphate compound.

[0046] In this case, the solid electrolyte containing the Nasicon-type phosphate compound may contain at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

[0047] The Nasicon-type phosphate compound is Li (1+x3) M1 (x3) M2 (2-x3) (P.O. 4 ) 3 wherein the element M1 includes at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 includes at least one selected from the group consisting of Ti, Ge, and Zr, and x3 satisfies 0≦x3≦2.

[0048] The oxide-based solid electrolyte may have a garnet-type crystal structure.

[0049] The solid electrolyte having a garnet-type crystal structure may contain at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

[0050] The solid electrolyte having the garnet-type crystal structure is Li(7-3x4+y4-z4)M x4 La (3-y4) A' (y4) Zr (2-z4) T (z4) O 12 (The element M is one or more of Al and Ga, the element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.)

[0051] In the anode body of the present invention, the above-mentioned oxide-based solid electrolytes can be suitably used.

[0052] The present invention also provides a method for manufacturing an anode body for manufacturing any of the above anode bodies, the method comprising the steps of: winding the anode current collector around a can roll having a curvature; vapor-depositing a film containing silicon and / or silicon monoxide and having a multilayer structure consisting of two or more layers on the anode current collector while running the anode current collector on the can roll; spraying an oxygen-containing gas onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on the top of each layer; inserting and desorbing lithium into and from the multilayer structure layer to form the anode active material layer; forming the ion-conducting layer having lithium ion conductivity on the surface of the anode active material layer; and forming the solid electrolyte layer adjacent to the ion-conducting layer.

[0053] The method for producing an anode body of the present invention makes it possible to produce an anode body that can significantly increase capacity while maintaining battery characteristics.

[0054] In this case, it is preferable that the method further comprises the steps of: forming layers of the multilayer structure, each layer of which contains silicon oxide including silicon dioxide, in the step of forming layers of the multilayer structure; vapor-depositing an anode active material layer containing silicon oxide on the anode current collector; immersing the anode active material layer containing silicon oxide in a solution containing lithium; and modifying the silicon oxide by an electrochemical method, thereby generating the compound containing lithium, silicon, and oxygen, and forming the ion-conducting layer.

[0055] Such a method for producing an anode body allows lithium to be inserted by an electrochemical method, so that an anode body that can significantly increase capacity while maintaining battery characteristics can be more reliably produced.

[0056] As described above, the anode body of the present invention can achieve high initial efficiency, high capacity, and excellent cycle characteristics when used as a component of a secondary battery. Furthermore, the method for producing the anode body of the present invention can produce an anode body that has high capacity and excellent initial charge-discharge characteristics when used as an anode body constituting a secondary battery while also achieving good cycle characteristics.

[0057] 1 is a schematic cross-sectional view showing an example of the configuration of the negative electrode body of the present invention; 2 is a schematic exploded view showing an example of the configuration of a lithium ion secondary battery including the negative electrode body of the present invention; 3 is an SEM image of the surface of the negative electrode active material layer of the example negative electrode body of the present invention;

[0058] As mentioned above, one method for increasing the battery capacity of lithium-ion secondary batteries has been investigated: using a negative electrode made primarily of silicon oxide. Lithium-ion secondary batteries using silicon oxide are expected to have initial charge-discharge characteristics comparable to those of lithium-ion secondary batteries using carbon-based active materials. While the use of Li-doped SiO, which can improve the initial charge-discharge characteristics, can significantly increase capacity, further improvements in capacity are required for automotive applications.

[0059] Therefore, the present inventors conducted extensive research to obtain a negative electrode that, when used as a negative electrode for a secondary battery, can achieve high cycle characteristics, improve initial charge-discharge characteristics, and increase battery capacity, and have arrived at the present invention.

[0060] That is, one aspect of the present invention is an anode assembly having an anode including an anode current collector having a roughened surface, an anode active material layer provided on the anode current collector, and an ion conduction layer having lithium ion conductivity on the surface of the anode active material layer, and having a solid electrolyte layer adjacent to the ion conduction layer, wherein the anode active material layer contains anode active material particles having a compound containing lithium, silicon, and oxygen, and the anode active material particles are SiO x1 Li y1 The anode body of the present invention is characterized in that the value of x1 is greater than 0.8 and not greater than 1.2, and the value of y1 is not less than 0.5 and not greater than 3.4. Thus, the anode body of the present invention has an anode and a solid electrolyte layer.

[0061] Another aspect of the present invention is a method for producing the above-mentioned anode body of the present invention, comprising the steps of: winding the anode current collector around a can roll having a curvature; vapor-depositing a film containing silicon and / or silicon monoxide and having a multilayer structure consisting of two or more layers on the anode current collector while running the anode current collector on the can roll; spraying an oxygen-containing gas onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on the top of each layer; inserting and desorbing lithium into and from the multilayer structure layer to form the anode active material layer; forming the ion-conducting layer having lithium ion conductivity on the surface of the anode active material layer; and forming the solid electrolyte layer adjacent to the ion-conducting layer.

[0062] The present invention will be described in detail below, but the present invention is not limited thereto.

[0063] <Negative Electrode Body> First, the configuration of the negative electrode body of the present invention will be described with reference to the drawings.

[0064] FIG. 1 shows a schematic cross-sectional view of an example of an anode body of the present invention. As shown in FIG. 1, the anode body 10 includes an anode current collector 11 and an anode active material layer 12 provided on the surface 11a of the anode current collector 11. The anode active material layer 12 may be provided on both surfaces 11a of the anode current collector 11 as shown in FIG. 1, or may be provided on only one surface 11a. The anode body 10 further includes an ion conduction layer 14 having lithium ion conductivity on the surface of the anode active material layer 12. That is, the anode structure includes the anode current collector 11, the anode active material layer 12, and the ion conduction layer 14. The anode body 10 further includes a solid electrolyte layer 16 adjacent to the ion conduction layer 14.

[0065] The surface 11 a of the negative electrode current collector 11 is a roughened surface. That is, the negative electrode active material layer 12 is provided on the roughened surface 11 a of the negative electrode current collector 11 .

[0066] The negative electrode current collector 11 and the negative electrode active material layer 12 will be described below.

[0067] [Negative electrode current collector] The negative electrode current collector 11 is made of a highly conductive material that has excellent mechanical strength. Examples of conductive materials that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). This conductive material is preferably a material that does not form an intermetallic compound with lithium (Li).

[0068] The negative electrode current collector 11 preferably contains carbon (C) and sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector is improved. In particular, when an active material layer that expands during charging is included, if the current collector contains the above elements, it is effective in suppressing deformation of the electrode including the current collector. The contents of the above contained elements are not particularly limited, but are preferably 100 mass ppm or more each. This is because a higher deformation suppression effect can be obtained. Such a deformation suppression effect can further improve cycle characteristics.

[0069] The surface 11a of the negative electrode current collector 11 must be roughened, and preferably the ten-point mean roughness Rz of the surface is 1.5 μm or more and 5.0 μm or less. An anode body 10 including a negative electrode current collector 11 having a surface 11a with such a desirable mean roughness Rz can not only more stably support the negative electrode active material layer 12 but also ensure an appropriate density of the negative electrode active material particles in the negative electrode active material layer 12, resulting in superior battery characteristics. The roughened negative electrode current collector 11 can be, for example, a metal foil that has been subjected to electrolytic treatment, embossing treatment, or chemical etching treatment.

[0070] [Negative Electrode Active Material Layer] The negative electrode active material layer 12 of the negative electrode body 10 of the present invention contains negative electrode active material particles having a compound containing lithium, silicon, and oxygen (silicon compound particles). That is, the layer contains silicon compound particles containing lithium and oxygen, and is provided on the negative electrode current collector 11. It can be said that the negative electrode body 10 has, as part of its structure, a structure in which the negative electrode active material particles are directly supported on the roughened surface 11a of the negative electrode current collector 11.

[0071] The anode body 10 of the present invention contains anode active material particles that are silicon compound particles, thereby improving battery capacity. Furthermore, unlike typical electrodes, the anode body 10 of the present invention can directly support the anode active material layer 12 on the roughened surface 11a of the anode current collector 11 without using a binder, a conductive additive, or the like, thereby reducing the area of ​​the electrode that is not involved in charge and discharge and reducing excess voids, thereby significantly improving the energy density of the electrode.

[0072] In this way, by using the negative electrode body 10 having the densely supported negative electrode active material layer 12, it is possible to increase the energy density of the battery, which cannot be achieved with, for example, a powder electrode.

[0073] Furthermore, in the anode active material layer 12, anode active material particles containing a compound containing lithium, silicon, and oxygen can be adjacent to each other. As described above, an ion conduction layer 14 having lithium ion conductivity is formed on the surface of the anode active material layer 12. The ion conduction layer 14 is preferably composed of at least one of Li carbonate, Li phosphate, Li fluoride, Al carbonate, Al phosphate, Al fluoride, a compound having a silyl group, and a carbide containing a polycyclic aromatic hydrocarbon. Examples of carbides include those containing aromatic compounds as the main component, and particularly preferred are carbides containing polycyclic aromatic hydrocarbons as the main component. The coating that forms the ion conduction layer 14 serves as a protective layer that protects the interface between the anode active material layer 12 and the solid electrolyte layer 16. The presence of such a coating allows the anode body 10 of the present invention to exhibit excellent cycle characteristics.

[0074] Examples of the silyl group in the silyl group-containing compound include silyl groups having an organic group such as an alkyl group. In this case, a silyl group having an organic group having 1 to 5 carbon atoms is preferred. More preferred is a silyl group having an alkyl group having 1 to 5 carbon atoms. In this case, the alkyl group is preferably a methyl group, ethyl group, propyl group, isopropyl group, butyl group, tertiary butyl group, or isobutyl group. Examples of silyl groups having such alkyl groups include trialkylsilyl groups such as trimethylsilyl group and triethylsilyl group. In this case, the three alkyls may be the same or different, as described above. The organic group having 1 to 5 carbon atoms may contain an unsaturated bond. Furthermore, the alkyl group may contain a fluorine atom.

[0075] Furthermore, in the negative electrode body 10 of the present invention, the negative electrode active material particles are SiO x1 Li y1The value of x1 is greater than 0.8 and not greater than 1.2, and the value of y1 is greater than 0.5 and not greater than 3.4. If x1 is greater than 0.8, the oxygen ratio is higher than that of silicon alone, resulting in good cycle characteristics. It is more preferable that x1 is 0.9 or greater. If x1 is 1.2 or less, the resistance of the silicon oxide does not become too high, which is preferable. Among these, SiO x1 Li y1 The value of x1 is preferably closer to 1, because this results in high cycle characteristics. The composition of the silicon compound in the present invention does not necessarily mean 100% purity, and may contain trace amounts of impurity elements. If the value of y1 is 0.5 or more, the irreversible SiO component generated during the initial charge / discharge can be fixed in advance, significantly improving the energy density of the electrode. If the value of y1 is 3.4 or less, the negative electrode active material particles are stable against oxygen and moisture, allowing for the assembly of a higher-capacity battery.

[0076] That is, the negative electrode body 10 of the present invention can significantly increase the capacity while maintaining the battery characteristics.

[0077] On the other hand, if the value of x1 is 0.8 or less, the capacity increases, but the Si 0+ The area that reacts with the electrolyte increases, deteriorating the cycle characteristics. Furthermore, if the value of x1 exceeds 1.2, it becomes a load substance, which also deteriorates the battery characteristics. It is desirable that the value of x1 be as close to 1 as possible.

[0078] In the anode body 10 of the present invention, the anode active material layer 12 preferably has a multilayer structure consisting of two or more layers. Anode body 10 having a multilayer anode active material layer 12 is more preferable because it can mitigate expansion and contraction of the anode active material layer 12 and improve the capacity retention rate.

[0079] Furthermore, as will be described later, when manufacturing the anode body 10 of the present invention, Li is introduced into the anode active material layer 12. To introduce Li more smoothly, it is preferable to form the anode active material layer 12 into a multilayer structure consisting of two or more layers at the timing of forming the anode active material layer 12. The anode active material layer 12 having a multilayer structure consisting of two or more layers can realize smooth insertion of Li while suppressing decomposition of the electrolyte.

[0080] When the negative electrode active material layer 12 has a multilayer structure, each layer of the multilayer structure preferably has a layer made of a high-valence silicon compound containing at least one of lithium and oxygen on the surface thereof. By having a layer made of a silicon compound on the surface, expansion and contraction of the negative electrode active material layer 12 due to charge and discharge can be alleviated, and the negative electrode active material layer 12 can be maintained stable.

[0081] Furthermore, when the above-described negative electrode active material particles are defined as primary particles, the negative electrode active material layer 12 forms secondary particles that are aggregates of the primary particles, and it is preferable that the secondary particles have a morphology in which they are separated from each other in the in-plane direction.

[0082] In the manufacturing method of the anode body 10 of the present invention described below, the anode active material particles grow in a vapor phase due to the roughened portion of the surface 11a of the anode current collector 11. If these are defined as primary particles, it is preferable that secondary particles, which are aggregates of the primary particles, are formed. This can be controlled by changing the roughened state of the surface 11a of the anode current collector 11. For example, if the roughened spacing is wide, the secondary particle group becomes small. On the other hand, if the roughened spacing is narrow and the primary particles are too densely packed, secondary particles are less likely to be generated during charging and discharging.

[0083] It is desirable that the secondary particles are separated from each other in the in-plane direction. By performing charge and discharge in this state, a stable negative electrode active material layer 12 can be maintained.

[0084] With this configuration, the anode body 10 of the present invention can suppress thickness changes in the anode active material layer 12 due to charge and discharge. In particular, the relationship between the thickness T1 of the anode active material layer 12 before charge and the thickness T2 after full charge can be T2 / T1≦1.4. With this configuration, expansion during full charge can be suppressed to a state close to that of graphite.

[0085] In addition, in the anode body 10 of the present invention, the number of primary particles forming the secondary particles of the anode active material particles in the anode active material layer 12 is preferably four or more on average. This number of four or more ensures a suitable surface area for the anode active material layer, thereby suppressing material degradation due to battery charging and discharging. In other words, this number of four or more ensures stable battery characteristics while suppressing material degradation. The average number of primary particles in the secondary particles can be measured by observation with a scanning electron microscope. Figure 3 shows an SEM image of the surface of the anode active material layer 12 constituting the anode body 10 of the present invention.

[0086] The negative electrode active material layer 12 contains Li 4 SiO 4 , Li 2 Si 2 O 5 , Li 2 SiO 3 and Li 6 Si 2 O 7 It is preferable to have at least one of the following: 2 SiO 3 In addition to Li 4 SiO 4 , Li 6 Si 2 O 7 Li silicates such as these are relatively more stable than other Li compounds, and therefore silicon-based active materials containing these Li compounds can achieve more stable battery characteristics. 2 It can be obtained by selectively changing a part of the components to Li compounds and modifying silicon compounds.

[0087] Furthermore, in the anode body 10 of the present invention, when the anode active material layer 12 has a multilayer structure, it is preferable that at least one of the interlayers of the multilayer structure has an ion-conducting layer (interlayer lithium-ion-conducting layer) having lithium ion conductivity. The presence of an ion-conducting layer (interlayer lithium-ion-conducting layer) between the layers of the multilayer structure in this manner facilitates the movement of lithium between the layers, thereby improving the battery characteristics.

[0088] [Solid Electrolyte Layer] The solid electrolyte layer 16 shown in FIG. 1 is adjacent to the ion-conducting layer 14 on the outermost surface of the negative electrode active material.

[0089] The solid electrolyte constituting the solid electrolyte layer 16 is preferably either a sulfide-based solid electrolyte or an oxide-based solid electrolyte.

[0090] [Sulfide-Based Solid Electrolyte] First, a case where the solid electrolyte layer 16 is made of a sulfide-based solid electrolyte will be described. A known sulfide-based solid electrolyte can be used as the sulfide-based solid electrolyte. The sulfide-based solid electrolyte may react with lithium released from the silicon-based active material to generate heat. However, the negative electrode body of the present invention has an ion-conducting layer on its surface, which can suppress this reaction. This allows for the design of a safe battery that is less likely to generate heat while maintaining high ion conductivity.

[0091] The sulfide-based solid electrolyte may contain at least one of lithium, indium, sulfur, and phosphorus. 2 S, P 2 S 5 , SiS 2 , LiI, LiBr, P 2 O 5 , Li 3 P.O. 4 and GeS 2 The sulfide-based solid electrolyte may have at least one of the following: 2 S-P 2 S 5 , Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2, LiI-Si 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiI-LiBr, LiI-Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 O 5 , LiI-Li 3 P.O. 4 -P 2 S 5 , Li 2 S-P 2 S 5 -GeS 2 The following can be mentioned:

[0092] [Oxide-Based Solid Electrolyte] Next, a case where the solid electrolyte layer 16 is made of an oxide-based solid electrolyte will be described. The oxide-based solid electrolyte is stable in air and easy to handle, making it possible to design a safe battery.

[0093] [Compound Having Perovskite Structure] The oxide-based solid electrolyte that can be used in the present invention can have a perovskite structure. The compound having a perovskite structure has a composition formula represented by the general formula A X2 BO 3 (where 0<X2<1 is satisfied). In this compound having a perovskite structure, element A contains at least one of La and Li, and element B contains at least one of Mg, W, Nb, and Ti. By including Li in element A, Li ion conductivity can be imparted. Furthermore, it is preferable that element B contains Mg and W. This perovskite-type ion-conducting oxide (solid electrolyte) has a basic composition formula (Li 3a , La 2/3-a ) (Mg b , W 1-b ) O 3(However, 0<a≦1 / 3, 0.4≦b≦0.6 are satisfied. In this case, the Li substitution amount a is preferably 0.04 or more, more preferably in the range of 0.05 to 0.30, and even more preferably in the range of 0.07 to 0.22. In such a range, the Li ion conductivity can be further increased, which is preferable. Furthermore, the Mg content b is preferably in the range of 0.48 to 0.52, and the closer the amounts of Mg and W are to be equal, the more preferable, and 0.5 is more preferable. This perovskite-type ion-conductive oxide has a basic composition formula (Li 3 a, La 2/3-a ) (Mg 1/2 , W 1/2 ) O 3 (wherein a is 1 / 6, 1 / 4, or 1 / 3) is more preferable. 2/3 ) (Mg 1/2 , W 1/2 ) O 3 However, the perovskite-type ion-conducting oxide of the present disclosure has a structure in which part of the La is substituted with Li.

[0094] [Phosphate compound with Nasicon crystal structure] The oxide-based solid electrolyte that can be used in the present invention can have a Nasicon-type phosphate compound.The phosphate compound with Nasicon-type crystalline structure is not particularly limited as long as it is a Nasicon-type phosphate compound, but for example, it can have at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.In addition, this Nasicon-type phosphate compound can be represented by the general formula (1) Li 1+x3 M1 x3 M2 2-x3 (P.O. 4 ) 3 It is preferable that the compound is a Nasicon-type phosphate compound represented by formula (1), where M1 is at least one selected from the group consisting of Al, Y, Ga and In, M2 is at least one selected from the group consisting of Ti, Ge and Zr, and x3 is 0≦x3≦2.

[0095] The metal M1 is preferably at least one selected from the group consisting of Al, Y, and Ga, and more preferably Al. The metal M2 is preferably at least one selected from the group consisting of Ge and Ti, and more preferably Ge. That is, the general formula (2) Li 1+x3 Al x3 Ge 2-x3 (P.O. 4 ) 3 (wherein x3 is 0≦x≦2) is preferably a Nasicon-type phosphate compound (LAGP). Among Nasicon-type phosphate compounds, the compound represented by formula (2) has high ionic conductivity.

[0096] The range of x3 is preferably 0.1≦x3≦1.9, and more preferably 0.3≦x3≦0.7. In particular, the solid electrolyte material is 1.5 Al 0.5 Ge 1.5 (P.O. 4 ) 3 It is preferable that:

[0097] [Compound Having a Garnet-Type Crystal Structure] The oxide-based solid electrolyte that can be used in the present invention can be a solid electrolyte having a garnet-type crystal structure. The solid electrolyte having a garnet-type crystal structure preferably contains at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen. The compound having a garnet-type crystal structure is Li(7-3x4+y4-z4)M x4 La (3-y4) A' (y4) Zr (2-z4) T (z4) O 12 (Element M is one or more of Al and Ga, element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.) In particular, the solid electrolyte having a garnet-type crystal structure is preferably a solid electrolyte having a composition formula: Li 7-3x4+α La 3 Zr 2Al x4 O 12-y4 Li 3 BO 3 (wherein 0≦x4<2, 1.1<(7−3x4+α) / (7−3x4)≦1.5, and 0.3≦y4≦2.0). When a compound having a garnet-type crystal structure has the above composition, it becomes a cubic crystal at room temperature, and therefore has the effect of having high ionic conductivity at room temperature. In addition, the compound having a garnet-type crystal structure according to the embodiment of the present invention has the composition formula: Li 7-3x4+α La 3 Zr 2 Al x4 O 12-y4 Li 3 BO 3 In this case, the stoichiometric ratio of Li is "Li 7-3x4 " has Li in excess of "α" compared to ", and is Li-excessive. In addition, in the above formula, 0≦x4<1 may be satisfied. In addition, Li 3 BO 3 Regarding "y4" indicating the substance amount ratio, 0.3≦y4≦1.5 may be satisfied.

[0098] [Method for Manufacturing Anode Body] The method for manufacturing an anode body of the present invention preferably includes the steps of: winding the anode current collector around a curvature-provided can roll; vapor-depositing a multilayered silicon and / or silicon monoxide film having two or more layers on the anode current collector while the anode current collector is running on the can roll; spraying an oxygen-containing gas onto the silicon and / or silicon monoxide film to form a multilayered silicon dioxide-containing layer on each layer; inserting and desorbing lithium into and from the multilayered layer to form the anode active material layer; forming the ion conduction layer having lithium ion conductivity on the surface of the anode active material layer; and forming the solid electrolyte layer adjacent to the ion conduction layer. Such a method for manufacturing an anode body of the present invention makes it possible to manufacture an anode body that can significantly increase capacity while maintaining battery characteristics.

[0099] In this case, it is preferable that the method further comprises the steps of: forming a multilayer structure in which each layer contains silicon oxide including silicon dioxide in the step of forming layers of the multilayer structure; vapor-depositing a silicon oxide-containing anode active material layer on the anode current collector in the vapor phase; immersing the silicon oxide-containing anode active material layer in a solution containing lithium; and modifying the silicon oxide by an electrochemical method to produce the compound containing lithium, silicon, and oxygen and form the ion-conducting layer. Such a method for producing an anode body allows lithium to be inserted by an electrochemical method, thereby more reliably producing an anode body that can significantly increase capacity while maintaining battery characteristics.

[0100] The anode body of the present invention can be manufactured by the above-described manufacturing method of the anode body of the present invention, but the method for manufacturing the anode body of the present invention is not limited to the manufacturing method of the present invention described here.

[0101] An example of a method for producing an anode body of the present invention will be specifically described below, but the method for producing an anode body of the present invention is not limited to the example described below.

[0102] First, a multilayered film containing silicon and / or silicon monoxide consisting of two or more layers is fabricated. Here, a multilayered film containing silicon and / or silicon monoxide is vapor-deposited on a negative electrode current collector. The silicon-containing film can contain silicon particles. The silicon monoxide-containing film can contain silicon monoxide particles, which are silicon compound (silicon oxide) particles containing oxygen. Therefore, the multilayered film containing silicon and / or silicon monoxide consisting of two or more layers can contain silicon-containing particles.

[0103] This multilayered film containing silicon and / or silicon monoxide can be formed by depositing, for example, a silicon vapor stream or silicon oxide gas on a surface-roughened negative electrode current collector, for example, a roughened foil (for example, a roughened copper foil) having a surface ten-point mean roughness Rz of 1.5 μm to 5.0 μm (for example, 2.5 μm). In the method for producing a negative electrode body of the present invention, the negative electrode current collector is wound around a can roll having a curvature. The curvature (R) of the can roll is, for example, 4 m -1More than 20m -1 It is preferable to do the following:

[0104] A specific example of a method for forming a multilayered film containing silicon and / or silicon monoxide is as follows.

[0105] A silicon monoxide film can be formed, for example, by the following procedure. First, a raw material that generates silicon oxide gas is heated under reduced pressure at a temperature of 1100°C or higher to generate silicon oxide gas. A mixture of metal silicon powder and silicon dioxide powder can be used as the raw material. Considering the presence of oxygen on the surface of the metal silicon powder and trace amounts of oxygen in the reactor, it is desirable for the molar ratio of the mixture to be in the range of 0.9<metal silicon powder / silicon dioxide powder<1.2.

[0106] Silicon oxide can also be formed by vapor deposition using metallic silicon and introducing oxygen gas into the deposited silicon, but in this case, valence control is not possible, resulting in a composite in which silicon separates into a zero-valent state and a tetravalent compound state. Similarly, it is possible to introduce a reducing gas (hydrogen) into silicon dioxide gas, but it is difficult to introduce sufficient hydrogen into vapor that moves at speeds close to the speed of sound. As a result, in the method for producing an anode body of the present invention, it is preferable to use metallic silicon and silicon dioxide powder as raw materials for the silicon monoxide film.

[0107] The silicon oxide gas generated as described above is deposited on the roughened portion of the surface of the negative electrode current collector, and becomes primary particles having a columnar structure.

[0108] The silicon film can be formed by vapor deposition using, for example, metallic silicon.

[0109] When forming the silicon film and / or silicon monoxide film, the structure of the primary particles can also be changed by changing the roughened structure of the surface of the negative electrode current collector.

[0110] The heat of solidification during deposition and the radiant heat from the heating unit promote crystallization of the negative electrode active material layer. Therefore, in the method for producing a negative electrode body of the present invention, the negative electrode current collector is run on a can roll having a curve, thereby reducing the thermal load and enabling vapor deposition to occur without causing crystallization of Si.

[0111] In particular, silicon oxide, unlike silicon, is sublimable, allowing for rapid deposition, and is not subject to the radiant heat from molten silicon that is a problem with silicon films. Therefore, it can be said to be suitable for forming active materials by vapor deposition.

[0112] In the method for manufacturing a negative electrode of the present invention, multilayer film formation (e.g., reciprocating multilayer film formation) is performed while the negative electrode current collector is running on a can roll having a curve, so that part of the surface of each layer is deposited at an angle, resulting in voids.

[0113] Vapor deposition can also be performed on both roughened surfaces of the negative electrode current collector. For example, vapor deposition can be performed on one roughened surface of the negative electrode current collector, and then the negative electrode current collector can be turned over and vapor deposition can be performed on the other roughened surface of the negative electrode current collector.

[0114] A gas containing oxygen is blown onto the silicon and / or silicon monoxide-containing film formed as described above, and a multilayer structure containing silicon dioxide is formed on top of each layer.

[0115] The oxygen-containing gas is not particularly limited as long as it contains oxygen, but may be, for example, nitrogen gas containing oxygen.

[0116] By blowing the oxygen-containing gas, oxygen can enter the voids in the upper part of each layer, and oxygen can be introduced into each layer. This also makes it possible to convert at least a portion of the silicon and / or silicon monoxide in the upper part of each layer into silicon dioxide. In other words, by blowing the oxygen-containing gas, it is possible to form a multilayer structure in which each layer contains silicon oxides including silicon dioxide.

[0117] Next, the multilayer structure containing silicon dioxide on the top of each layer prepared as described above is doped (inserted) with Li. This results in a negative electrode active material layer containing negative electrode active material particles containing silicon oxide particles into which lithium has been inserted. That is, this modifies the silicon oxide particles, and Li compounds are generated inside the silicon oxide particles.

[0118] [Electrochemical Modification] In electrochemical modification, a negative electrode active material layer containing silicon oxide particles is immersed in a liquid nonaqueous electrolyte (electrolyte) as an anode and a lithium metal cathode, and lithium is inserted by supplying a current. This electrolyte contains an electrolyte salt dissolved in a solvent and may contain other materials such as additives.

[0119] The solvent can be, for example, a non-aqueous solvent. Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, and tetrahydrofuran. Among these, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. This is because better properties can be obtained. In this case, more advantageous properties can be obtained by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. This is because the dissociation property and ion mobility of the electrolyte salt are improved.

[0120] In particular, it is desirable for the solvent to contain at least one of a halogenated chain carbonate or a halogenated cyclic carbonate. This allows a stable coating to be formed on the surface of the negative electrode active material during charge and discharge, particularly during charging. Here, the halogenated chain carbonate is a chain carbonate having a halogen as a constituent element (i.e., at least one hydrogen atom is substituted with a halogen). Furthermore, the halogenated cyclic carbonate is a cyclic carbonate having a halogen as a constituent element (i.e., at least one hydrogen atom is substituted with a halogen).

[0121] Although the type of halogen is not particularly limited, fluorine is preferred because it forms a better coating than other halogens. Furthermore, the more halogens there are, the more desirable they are because the resulting coating is more stable and the decomposition reaction of the electrolyte is reduced.

[0122] Examples of halogenated chain carbonates include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of halogenated cyclic carbonates include 4-fluoro-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, etc.

[0123] It is preferable that the solvent additive contains an unsaturated carbon-bond cyclic carbonate. This is because a stable coating is formed on the surface of the negative electrode active material layer during charge and discharge, and decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bond cyclic carbonate include vinylene carbonate and vinylethylene carbonate.

[0124] It is also preferable that the solvent additive contains sultone (cyclic sulfonic acid ester), which improves the chemical stability of the battery. Examples of sultones include propane sultone and propene sultone.

[0125] Furthermore, it is preferable that the solvent contains an acid anhydride, because this improves the chemical stability of the electrolyte solution. Examples of acid anhydrides include propanedisulfonic acid anhydride.

[0126] The electrolyte salt may include, for example, one or more light metal salts such as lithium salts. Examples of the lithium salt include lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ) etc.

[0127] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because high ionic conductivity can be obtained.

[0128] After lithium insertion, lithium can be desorbed by supplying current to a negative electrode active material layer containing silicon oxide particles as a cathode and a lithium metal anode. The state of the filled coating (composite compound) can be controlled by adjusting the solvent temperature, the type and concentration of the polyphenylene compound or polycyclic aromatic compound contained in the solvent, and the concentration of the polycyclic aromatic compound complexed with Li. The resulting silicon active material particles may be heat-treated in an inert gas atmosphere. Heat treatment can stabilize the Li compound.

[0129] The resulting complex compound may contain multiple types of compounds.

[0130] [Formation of a coating having lithium ion conductivity] A coating having lithium ion conductivity (ion conductive layer) is formed on the negative electrode active material layer obtained by electrochemical modification. A lithium carbonate coating can be formed on the surface and between the layers by spraying carbon dioxide gas onto the negative electrode active material layer. In addition, a coating can be formed by adding aluminum phosphate to the electrolyte solution during lithium insertion and deintercalation. By not removing the electrolyte salt after lithium insertion and deintercalation, Li can be formed on the surface. 3 P.O. 4 , LiF, Li 2 CO 3 A coating consisting of the above can be formed.

[0131] The compound having a silyl group is preferably formed by alkylsilazane treatment. In this way, the treatment occurs on the surface of the material, and a layer containing a compound having a silyl group can be efficiently formed. More specifically, for example, a layer containing a compound having a silyl group can be formed by the following procedure. It is considered that OH groups are present on the surface of the negative electrode active material layer, and these OH groups react with the decomposition product of the alkylsilazane, thereby introducing trialkylsilyl groups into the surface of the silicon compound particles or the carbon material.

[0132] First, dehydrated toluene, a negative electrode active material in an amount equal to one-fourth the mass of the dehydrated toluene, and HMDS (hexamethyldisilazane) in an amount equivalent to 3 mass% of the negative electrode active material are placed in a container and left to stand for 1 hour. Thereafter, the negative electrode active material layer is dried to form a coating film of a compound having a silyl group.

[0133] A carbonized material whose main component is an aromatic compound (polycyclic aromatic hydrocarbon) is preferably formed by coal tar pitch treatment. Specifically, a coating can be formed by applying coal tar or pitch to the negative electrode active material layer and then heat treating it. The coal tar or pitch is thermally decomposed to form a carbonized material that is an aromatic compound (polycyclic aromatic hydrocarbon), and a coating is formed on the negative electrode active material layer. The thermal decomposition temperature is not particularly limited.

[0134] [Formation of Solid Electrolyte Layer] After forming the ion conductive layer, a solid electrolyte layer adjacent to the ion conductive layer is formed. This step can be performed by disposing the solid electrolyte layer adjacent to the ion conductive layer and then applying pressure.

[0135] In this manner, the negative electrode body of the present invention can be produced.

[0136] <Lithium-ion secondary battery> The negative electrode body of the present invention can be used in the negative electrode body of an all-solid-state battery, for example, a lithium-ion secondary battery.

[0137] Next, an example of an all-solid-state battery in which the negative electrode body of the present invention can be used will be described.

[0138] The structure of the lithium secondary battery is not particularly limited, and an example thereof is the structure shown in FIG. 2 . FIG. 2 is an explanatory diagram showing an example of the structure of an all-solid-state lithium secondary battery 20. This all-solid-state lithium secondary battery has the above-mentioned solid electrolyte layer 16, a positive electrode active material layer 21 formed on one surface of the solid electrolyte layer 16 and containing a positive electrode active material that absorbs and releases lithium, and a negative electrode active material layer 12 formed on the other surface of the solid electrolyte layer 16 and containing a negative electrode active material that absorbs and releases lithium. A positive electrode current collector 22 is formed on the surface of the positive electrode active material layer 21, and a negative electrode current collector 11 is formed on the surface of the negative electrode active material layer 12. The solid electrolyte layer 16 and the negative electrode active material layer 12 may form a composite to form an anode body 10.

[0139] EXAMPLES The present invention will be specifically explained below using examples and comparative examples, but the present invention is not limited to these.

[0140] Comparative Example 1 To serve as a reference for the Examples, the following particulate coated active material was first produced.

[0141] (Preparation of negative electrode structure) A particle composite apparatus (NOB-MINI, manufactured by Hosokawa Micron Corporation) was used to prepare a coated active material. First, a negative electrode active material (a powder of Li-doped SiO2 coated with carbon (referred to as "Li-SiO-C")), a sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5), average particle size 0.5 μm), and a conductive additive (spherical carbon, specific surface area 93 m2 / g) were added to the treatment vessel of the apparatus in a total amount of 30 g in the proportions shown in Table 1 below. Next, the spacing between the rotating blades (blades) of the compression shear rotor and the inner wall of the treatment vessel was set to 1 mm, the pressure to 100 Pa, the blade peripheral speed to 26.4 m / s, and the treatment time to 12.5 minutes, and a compression shear treatment was performed to obtain a coated active material.

[0142] Li-SiO-C was prepared by the following procedure. First, silicon and silicon dioxide were mixed as raw materials, vaporized at 1300°C, and then deposited on a deposition substrate and rapidly cooled to produce SiO blocks. This SiO block was pulverized to a median diameter of 7 μm, and then doped with Li using an oxidation-reduction method. After doping, samples were prepared by heat treatment to stabilize the Li silicate.

[0143] The obtained active material, sulfide solid electrolyte (10LiI-15LiBr-75(0.75LiS-0.25P2S5), average particle size 0.5 μm), conductive additive (VGCF), and binder (PVdF) were prepared and weighed out to a weight ratio of negative electrode active material:sulfide solid electrolyte:conductive additive:binder = 53:41:4:2, and mixed with a dispersion medium (heptane). The obtained mixture was dispersed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a negative electrode slurry.

[0144] The obtained negative electrode slurry was applied onto a negative electrode current collector (copper foil) and dried at 100°C for 30 minutes. 2 The negative electrode structure having the negative electrode layer and the negative electrode current collector was obtained by punching out the negative electrode sheet into a size of 1 cm. 2A sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li 2 S-0.25P 2 S 5 ), average particle size 0.5 μm) was added at 4 ton / cm 2 The resulting solid electrolyte layer and the negative electrode structure were placed together and pressed with a pressure of 4 ton / cm 2 The thickness of the negative electrode layer was 46 μm.

[0145] (Preparation of Positive Electrode Structure) Positive electrode active material (LiNi 1/3 Co 1/3 Mn 1/3 O 2 ) and sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li 2 S-0.25P 2 S 5 ), average particle size 0.5 μm), conductive additive (VGCF), and binder (PVdF) were prepared, and these were weighed out so that the weight ratio of positive electrode active material: sulfide solid electrolyte: conductive additive: binder was 85:13:1:1, and mixed with a dispersion medium (heptane). The resulting mixture was dispersed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a positive electrode slurry.

[0146] The obtained positive electrode slurry was applied onto a positive electrode current collector (aluminum foil) and dried at 100°C for 30 minutes. 2 The thickness of the positive electrode layer was 50 μm.

[0147] (Preparation of Evaluation Battery) The positive electrode structure and the negative electrode structure were arranged, and a pressure of 4 ton / cm 2 Thereafter, a stainless steel rod was inserted into each of the positive electrode side and the negative electrode side, and the mixture was constrained at 5 MPa to obtain an all-solid-state battery (battery for evaluation).

[0148] Comparative Example 2 The electrode of Comparative Example 2 was prepared by the following procedure: A surface-roughened copper foil having a ten-point average roughness (roughness) Rz of 2.5 μm was used as the negative electrode current collector.

[0149] [Preparation of Negative Electrode Active Material Layer] Gravel-like metallic silicon was placed in a carbon crucible, and the silicon was melted and vaporized under vacuum using an electron gun. Using a rolling device, a surface-roughened copper foil (to become a negative electrode current collector) was placed on a roll, and five silicon films were formed on the surface-roughened copper foil while the roll was running.

[0150] [Lithium Insertion and Extraction] Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed to prepare a non-aqueous solvent, and then an electrolyte salt (lithium hexafluorophosphate: LiPF ) was added to the non-aqueous solvent. 6 ) was dissolved to prepare an electrolyte solution (nonaqueous electrolyte). In this case, the solvent composition was EC:DMC = 30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. Using this electrolyte solution, the obtained negative electrode active material layer was modified by electrochemically inserting and deintercalating lithium into the silicon compound particles. Lithium insertion was completed when the potential difference between the anode and cathode became zero. Lithium deintercalation was completed when the potential difference between the anode and cathode became 1.2 V. After lithium deintercalation was completed, the obtained negative electrode active material layer was washed with a nonaqueous solvent of dimethyl carbonate to remove the electrolyte salt.

[0151] [Formation of Surface Coating (Ion Conducting Layer)] Carbon dioxide gas was sprayed onto the negative electrode active material layer obtained by electrochemical modification, thereby forming a lithium carbonate coating (ion conducting layer) on the surface and between the layers (between each layer of the multilayer structure).

[0152] The obtained negative electrode structure and the solid electrolyte layer were placed adjacent to each other, and the negative electrode structure was applied with a pressure of 4 ton / cm 2 The negative electrode body was obtained by pressing.

[0153] Comparative Example 3 In Comparative Example 3, metal silicon and silicon dioxide were placed in a carbon crucible. -2 The vapor was taken out by heating at 1200° C. in an atmosphere of a vacuum degree of 100 Pa. The vapor was directly supported on the roughened copper foil as in Comparative Example 2, and five layers were formed.

[0154] In Comparative Example 3, the roughened copper foil, the negative electrode active material layer containing silicon oxide provided on the roughened copper foil, and the solid electrolyte layer were arranged adjacent to each other, and a pressure of 4 ton / cm 2The negative electrode body was obtained by pressing.

[0155] (Comparative Examples 4 and 5 and Example 1) In Comparative Examples 4 and 5 and Example 1, anode bodies were prepared in the same manner as in Comparative Example 2, except that water vapor was introduced into the silicon vapor flow during film formation to attempt forced oxidation.

[0156] Example 2 In Example 2, a roughened copper foil was obtained in the same manner as in Comparative Example 3, and an anode active material layer containing silicon oxide was provided on the roughened copper foil. Lithium was inserted and extracted, and a surface coating (ion conductive layer) was formed, in the same manner as in Comparative Example 2. The obtained anode structure and a solid electrolyte layer were disposed adjacent to each other, and a 4 ton / cm 2 The negative electrode body was obtained by pressing.

[0157] Comparative Example 6 In Comparative Example 6, a negative electrode body was produced in the same manner as in Example 2, except that the surface coating (ion-conducting layer) was not formed.

[0158] (Examples 3 and 4 and Comparative Example 7) In Examples 3 and 4 and Comparative Example 7, the SiO of the negative electrode active material particles was x1 Li y1 The negative electrode body was produced in the same manner as in Example 2, except that the film formation rate was adjusted so that the value of x1 was the value shown in Table 1, and hydrogen or oxygen was blown into the steam as necessary to form the film.

[0159] (Examples 5 and 6) In Examples 5 and 6, each negative electrode body was produced in the same manner as in Example 2, except that the film formation rate was controlled to form one layer and 20 layers, respectively, in the formation of the negative electrode active material layer.

[0160] Example 7 In Example 7, a negative electrode body was produced in the same manner as in Example 2, except that the roughness Rz of the surface-roughened copper foil was set to 0.5.

[0161] In Examples 8 to 10, negative electrode bodies were fabricated in the same manner as in Example 2, except that the depth of charge during lithium intercalation was changed to change the thickness (T1) of the battery before charging and the thickness (T2) of the battery when fully charged. The depth of charge was defined as 0% before charging, and the amount of Li intercalated when the potential difference between the anode and cathode became zero was defined as 100%.

[0162] (Examples 11 to 14) In Example 11, an anode body was prepared in the same manner as in Example 2, except that aluminum phosphate was added to the electrolyte solution during lithium insertion and deintercalation, and carbon dioxide gas was not sprayed onto the anode body. In Example 12, Li was applied to the surface in the same manner as in Example 2, except that the electrolyte salt was not removed after lithium insertion and deintercalation. 3 P.O. 4 , LiF, Li 2 CO 3 A negative electrode body was fabricated having a negative electrode active material layer on which a coating (ion conduction layer) consisting of the above was present. In Example 13, a negative electrode body was fabricated in the same manner as in Example 2, except that the negative electrode active material layer obtained after lithium insertion and extraction was treated with alkylsilazane. In Example 14, a negative electrode body was fabricated in the same manner as in Example 2, except that the negative electrode active material layer obtained after lithium insertion and extraction was washed with a dimethyl carbonate nonaqueous solvent containing 3 vol% tar to remove the electrolyte salt, and then heat-treated.

[0163] Example 15 In Example 15, a negative electrode body was produced in the same manner as in Example 2, except that the carbon dioxide gas to be sprayed onto the negative electrode active material layer obtained by electrochemical modification was mixed with Ar and diluted to a concentration of 1.0 vol %, thereby forming a lithium carbonate coating (ion conduction layer) only on the surface.

[0164] (Examples 16 to 18) In Examples 16 to 18, negative electrode bodies were produced in the same manner as in Example 2, except that the average number of primary particles in the secondary particles was adjusted by setting the roughness Rz of the surface-roughened copper foil to 1.0, 1.5, and 2.5, respectively.

[0165] Example 19 In Example 19, the solid electrolyte adjacent to the ion-conducting layer on the outermost surface of the negative electrode active material was Li, which is a compound having a perovskite structure. 0.5 La 0.5 Mg 0.5 W 0.5 O 3 A negative electrode body was produced in the same manner as in Example 2, except for the change in the above.

[0166] [Preparation of Compounds Having Perovskite Structure] Basic composition formula Li 0.5 La 0.5 Mg 0.5 W 0.5 O3 So that Li 2 CO 3 (Kojundo Kagaku), La(OH) 3 (Kojundo Kagaku), MgO (Kojundo Kagaku), WO 3 (manufactured by Kojundo Chemical Co., Ltd.) was weighed. 2 A ball mill pot and beads (3 mmf) made of SUS304 were prepared, and the weighed powder was added. Ethanol was added as a solvent. The mixture was stirred at 300 rpm for 3 minutes, followed by a 2-minute break. This grinding process was repeated 20 times. The contents were poured into a stainless steel tray and dried in a dryer at 90°C for 2 hours. The powder was collected through a sieve (#500 mesh). The resulting powder was then placed in an alumina crucible and heated in air at 900°C for 10 hours, and the above-mentioned grinding process was carried out. The resulting powder was then pressed at 10 MPa in a mold molding machine and molded into a pellet-shaped compact. This compact was sintered at 1100°C for 12 hours.

[0167] Example 20 In Example 20, the solid electrolyte adjacent to the ion-conducting layer on the outermost surface of the negative electrode active material was a Nasicon-type phosphate compound, Li 3 In 2 (P.O. 4 ) 3 A negative electrode body was produced in the same manner as in Example 2, except for the change in the above.

[0168] [Preparation of Nasicon-type phosphate compound] In was used as the In-containing active material, and glassy Li was used as the amorphous phosphate compound. 1.5 Al 0.5 Ge 1.5 (P.O. 4 ) 3 An intermediate is prepared by using In and LAGP in contact with each other. Then, the intermediate is fired at a predetermined temperature to react In and LAGP, resulting in Li 3 In 2 (P.O. 4 ) 3 A sintered body for a battery containing an active material having the above crystalline phase is obtained.

[0169] Example 21 In Example 21, the solid electrolyte adjacent to the ion-conducting layer on the outermost surface of the negative electrode active material was Li, which is a compound having a garnet-type crystal structure. 6.8 (La 2.95 Ca 0.05 ) (Zr 1.75 Nb 0.25 ) O 12 A negative electrode body was produced in the same manner as in Example 2, except that the material was changed to (LLZ-CN).

[0170] [Preparation of a compound having a garnet-type crystal structure] The starting material was LiOH(H 2 O), La(OH) 3 , Ca(OH) 2 , ZrO 2 , Nb 2 O 5 The starting materials were weighed to achieve the stoichiometric ratio, mixed, and pulverized. The mixing and pulverization were carried out in ethanol using a planetary ball mill (300 rpm) using zirconia balls for 1 hour. Then, the powder was pre-fired (700°C, 48 hours). After pre-fired, LiOH (H 2 O) was added in excess. Then, mixing and pulverization were carried out again under the same conditions. Then, pre-sintering (700°C, 10 hours) was carried out again. The powder that had been pre-sintered twice was identified for its crystalline phase by XRD, and it was confirmed that no unreacted raw materials remained. Then, the LLZ-CN powder was immersed in water to exchange Li with H. The immersion conditions were a ratio of 4 g of LLZ-CN to 50 mg of water, and the powder was left to stand at room temperature (near 25°C) for 30 minutes to exchange Li with H. Analysis of the composition after the exchange of Li with H under these conditions revealed (Li 5.6 , H 1.2 ) (La 2.95 , Ca 0.05 ) (Zr 1.75 , Nb 0.25 ) O 12 (LLZ-HCN). Here, the amount of H was identified as follows: First, the powder after H substitution was subjected to TG / DTA-MASS measurement, and H was extracted from the sample by the MASS measurement. 2The temperature range in which O (molecular weight 18) evaporated was determined, and the weight loss in that temperature range was quantified at Tg. The atomic weight of H contained in LLZ-HCN was calculated from the mass and molecular weight of LLZ-CN and the mass and molecular weight of evaporated water.

[0171] [Evaluation of Discharge Capacity and Cycle Characteristics] The prepared test battery was placed in a thermostatic chamber at 25° C. and discharged to a discharge end potential of 2.0 V (vs. Li / Li + ), charge end potential 4.8V (vs.Li / Li + ), CC charge and discharge were repeated at a current density of 0.1 C. The first discharge capacity was taken as the reference (100%), and the discharge capacity retention rate (%) after 100 cycles was calculated.

[0172]

[0173] [Results] Tables 1 and 2 above show the results of the capacity retention rate and discharge capacity up to 100 cycles.

[0174] As is clear from Tables 1 and 2, the negative electrode bodies of Examples 1 to 21 all maintained a capacity retention rate of 80% after 100 cycles, while also exhibiting battery characteristics of a discharge capacity of 240 mAh / g.

[0175] On the other hand, the anode body of Comparative Example 1, which was produced using powdered Li—SiO, had a lower discharge capacity than the anode bodies of Examples 1 to 20. This is thought to be because the anode body of Comparative Example 1 used powder rather than vapor deposition, and therefore contained a binder that is not involved in charge and discharge, and furthermore had many excess voids.

[0176] Furthermore, the negative electrode body of Comparative Example 2 was significantly inferior in cycle characteristics to those of Examples 1-21.

[0177] In Comparative Example 3, both the cycle characteristics and discharge capacity were significantly lower than in Examples 1 to 21. This is thought to be due to the fact that Li was not inserted into the silicon oxide.

[0178] Silicon oxide is produced from silicon and silicon dioxide, so it is difficult to increase or decrease the amount of oxygen. x1 Li y1In the case of silicon oxide (Comparative Example 4) in which x1 is 0.7, the valence could not be controlled, and a considerable amount of silicon element remained.

[0179] To achieve even lower oxygen levels, it is necessary not only to introduce hydrogen into the vapor to actively reduce it, but also to significantly reduce the film formation rate.

[0180] The negative electrode bodies of Comparative Examples 4 and 5 were made of SiO x1 Li y1 When x1 was set to 0.7 and 0.8, the discharge capacity was lower than that of the negative electrodes of Examples 1 and 2. This is because the negative electrode bodies of Comparative Examples 4 and 5 had a lower SiO x1 Li y1 This is thought to be because, when x1 was set to 0.7 and 0.8, the area where zero-valent Si reacts with the electrolyte became too large, causing the conductive path to break during discharge.

[0181] On the other hand, when the amount of oxygen was increased, the film formation rate was also reduced and oxygen was blown directly into the vapor flow, but as the amount of oxygen increased, it became difficult to prepare the silicon oxide film.

[0182] The negative electrode body of Comparative Example 7 was made of SiO x1 Li y1 As a result of setting x1 to 1.3, the discharge capacity was lower than that of the anode bodies of Examples 1 to 4. This is because the anode body of Comparative Example 7 had a lower SiO x1 Li y1 This is thought to be due to the fact that the amount of the load material was too large because x1 was set to 1.3. As the discharge capacity tends to decrease as x increases, it is preferable to set x1 to 1.2 or less.

[0183] The discharge capacity of the negative electrode body of Comparative Example 6 was reduced as a result of the absence of the ion-conducting layer on the outermost surface of the negative electrode active material layer, which is believed to be due to an increase in interfacial resistance with the solid electrolyte caused by the absence of the ion-conducting layer on the outermost surface of the negative electrode active material layer.

[0184] The negative electrode bodies of Examples 1 to 4 have a lower SiO x1 Li y1 As a result of setting x1 to 0.9 to 1.2, the irreversible components of the negative electrode body are suppressed, and both the initial efficiency and the cycle characteristics can be improved.

[0185] In Example 5, the anode active material layer is a single-layer film, which reduces interlayer resistance and improves discharge capacity, but makes it difficult to alleviate expansion and contraction during charge and discharge, resulting in a decrease in capacity retention. Anode bodies with a multilayer structure such as those in Examples 2 and 6 are more preferable because they can alleviate expansion and contraction of the anode active material layer in the anode body and therefore improve capacity retention.

[0186] It is believed that the capacity retention rate decreased in Example 7 because secondary particles were not formed compared to Example 2, making it difficult to alleviate the expansion and contraction of the negative electrode active material layer in the negative electrode body. It is preferable that secondary particles are formed as in Example 2.

[0187] Examples 8 to 10 are examples aimed at finding the optimum thickness (T1) of the negative electrode active material before charging and the optimum thickness (T2) after full charging.

[0188] It is believed that the smaller the value of T2 / T1, the more the expansion and contraction during charge and discharge is suppressed, and therefore the capacity retention rate can be improved.

[0189] The presence of the coating (ion-conducting layer) shown in Examples 3 and 11 to 14 on the outermost surface of the negative electrode active material layer is thought to suppress reaction with moisture and oxygen, suppress deterioration of the material, and maintain excellent battery characteristics. Therefore, the presence of such a coating (ion-conducting layer) is preferable.

[0190] The anode body of Example 15 has a lower discharge capacity than that of Example 3 due to the absence of an ion-conducting layer between the anode active material layers. Therefore, it is considered that the anode body in which an ion-conducting layer is present between the anode active material layers as in Example 3 has improved ion conductivity and can maintain excellent battery characteristics. Therefore, it is preferable to have an ion-conducting layer between the anode active material layers.

[0191] Examples 16 to 18 are examples aimed at exploring the optimum number of primary particles among secondary particles. It is believed that a large number of primary particles among secondary particles can alleviate the stress of expansion during charge and discharge, thereby improving the capacity retention rate.

[0192] Examples 19 to 21 are examples aimed at exploring the type of solid electrolyte adjacent to the ion conduction layer. The negative electrode active materials of Examples 19 to 21 can exhibit excellent battery characteristics when combined with any solid electrolyte.

[0193] This specification includes the following aspects: [1]: An anode body having an anode including an anode current collector having a roughened surface, an anode active material layer provided on the anode current collector, and an ion conduction layer having lithium ion conductivity on the surface of the anode active material layer, and having a solid electrolyte layer adjacent to the ion conduction layer, wherein the anode active material layer includes anode active material particles having a compound containing lithium, silicon, and oxygen, and the anode active material particles are SiO x1 Li y1 where x1 is greater than 0.8 and less than 1.2, and y1 is greater than 0.5 and less than 3.4. [2]: The anode body of [1] above, wherein the anode active material layer has a multilayer structure consisting of two or more layers, and when the anode active material particles are defined as primary particles, the anode active material layer forms secondary particles which are aggregates of the primary particles, and the secondary particles have a morphology separated from each other in an in-plane direction, and the relationship between the thickness T1 of the anode active material layer before charge and the thickness T2 when fully charged is T2 / T1 ≦ 1.4. [3]: The anode body of [2] above, wherein the anode active material layer having a multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity between at least one of the layers constituting the multilayer. [4]: ​​The anode active material layer is formed by dissolving Li 4 SiO 4 , Li 2 Si 2 O 5 , Li 2 SiO 3 and Li 6 Si 2 O 7The anode body of any of [1] to [3] above, wherein the ion-conducting layer having lithium ion conductivity is made of at least one of Li carbonate, Li phosphate, Li fluoride, Al carbonate, Al phosphate, Al fluoride, a compound having a silyl group, and a carbide containing a polycyclic aromatic hydrocarbon. [6]: The anode body of any of [2] to [5] above, wherein the secondary particles of the anode active material layer are made of an average of four or more primary particles. [7]: The anode body of any of [1] to [6] above, wherein the solid electrolyte layer is made of a sulfide-based solid electrolyte. [8]: The anode body of [7] above, wherein the sulfide-based solid electrolyte contains at least one of lithium, indium, sulfur, and phosphorus. [9]: The sulfide-based solid electrolyte is made of Li 2 S, P 2 S 5 , SiS 2 , LiI, LiBr, P 2 O 5 , Li 3 P.O. 4 and GeS 2 The anode body of [7] or [8] above, wherein the solid electrolyte layer is made of an oxide-based solid electrolyte.

[10] : The anode body of any of [1] to [6] above, wherein the solid electrolyte layer is made of an oxide-based solid electrolyte.

[11] : The anode body of

[10] above, wherein the oxide-based solid electrolyte has a perovskite structure.

[12] : The anode body of

[10] or

[11] above, wherein the oxide-based solid electrolyte contains at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

[13] : The oxide-based solid electrolyte is represented by the composition formula A x2 BO 3The anode body of any one of the above

[10] to

[12] , which is represented by (0<x2<1), wherein the element A includes La and Li, and the element B includes Mg, W, Nb, and Ti.

[14] : The anode body of the above

[10] , wherein the oxide-based solid electrolyte has a Nasicon-type phosphate compound.

[15] : The anode body of the above

[14] , wherein the solid electrolyte having the Nasicon-type phosphate compound has at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

[16] : The Nasicon-type phosphate compound is Li (1+x3) M1 (x3) M2 (2-x3) (P.O. 4 ) 3 wherein the element M1 includes at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 includes at least one selected from the group consisting of Ti, Ge, and Zr, and x3 satisfies the condition 0≦x3≦2.

[17] : The anode body of the above

[10] , wherein the oxide-based solid electrolyte has a garnet-type crystal structure.

[18] : The anode body of the above

[17] , wherein the solid electrolyte having a garnet-type crystal structure includes at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

[19] : The solid electrolyte having a garnet-type crystal structure is Li(7-3x4+y4-z4)M x4 La (3-y4) A' (y4) Zr (2-z4) T (z4) O 12The negative electrode body of the above

[17] or

[18] , wherein the element M is one or more of Al and Ga, the element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.

[20] : A method for producing the anode body according to any one of [1] to

[19] above, comprising: a step of winding the anode current collector around a can roll having a curvature; a vapor deposition step of vapor-depositing a film containing silicon and / or silicon monoxide and having a multilayer structure consisting of two or more layers on the anode current collector while running the anode current collector on the can roll; a step of spraying an oxygen-containing gas onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on an upper portion of each layer; a step of inserting and desorbing lithium into and from the multilayer structure layer to form the anode active material layer; a step of forming the ion conduction layer having lithium ion conductivity on a surface of the anode active material layer; and a step of forming the solid electrolyte layer adjacent to the ion conduction layer.

[21] : A method for producing the anode body of

[20] , comprising the steps of: in the step of forming layers of the multilayer structure, forming layers of the multilayer structure, each layer containing a silicon oxide including silicon dioxide; in the vapor phase growth step, vapor-depositing an anode active material layer containing silicon oxide on the anode current collector; and immersing the anode active material layer containing silicon oxide in a solution containing lithium to modify the silicon oxide by an electrochemical method, thereby producing the compound containing lithium, silicon, and oxygen and forming the ion-conducting layer.

[0194] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A negative electrode body having a negative electrode current collector with a roughened surface, a negative electrode active material layer provided on the negative electrode current collector, and an ion conduction layer having lithium ion conductivity on the surface of the negative electrode active material layer, and having a solid electrolyte layer adjacent to the ion conduction layer, wherein the negative electrode active material layer contains negative electrode active material particles having a compound containing lithium, silicon and oxygen, and the negative electrode active material particles can be represented by SiO x1 Li y1 and the value of x1 exceeds 0.8 and is 1.2 or less, and the value of y1 is 0.5 or more and 3.4 or less.

2. The negative electrode active material layer has a multilayer structure composed of two or more layers. When the negative electrode active material particles are defined as primary particles, the negative electrode active material layer forms secondary particles that are aggregates of the primary particles. The secondary particles are separated from each other in the in-plane direction. The negative electrode body according to claim 1, wherein the thickness T1 of the negative electrode active material layer before charging and the thickness T2 when charged to full charge satisfy the relationship T2 / T1 ≤ 1.

4.

3. The negative electrode body according to claim 2, wherein at least one of the layers constituting the multilayer structure of the negative electrode active material layer having the multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity.

4. The negative electrode active material layer contains Li 4 SiO 4 、Li 2 Si 2 O 5 、Li 2 SiO 3 and Li 6 Si 2 O 7 The negative electrode body according to claim 1, characterized in that it contains at least any one of them.

5. The negative electrode body according to claim 1, wherein the ion conductive layer having lithium ion conductivity is composed of at least one of a carbonate of Li, a phosphate of Li, a fluoride of Li, a carbonate of Al, a phosphate of Al, a fluoride of Al, a compound having a silyl group, and a carbide containing a polycyclic aromatic hydrocarbon.

6. The negative electrode body according to claim 2, wherein the secondary particles of the negative electrode active material layer are composed of an average of four or more primary particles.

7. The negative electrode body according to claim 1, wherein the solid electrolyte layer is composed of a sulfide-based solid electrolyte.

8. The negative electrode body according to claim 7, wherein the sulfide-based solid electrolyte has at least one of lithium, indium, sulfur, and phosphorus.

9. The sulfide-based solid electrolyte is Li 2 S, P 2 S 5 , SiS 2 , LiI, LiBr, P 2 O 5 , Li 3 PO 4 and GeS 2 and has at least one of them, and the negative electrode body according to claim 7 is characterized by this.

10. The negative electrode body according to claim 1, wherein the solid electrolyte layer is composed of an oxide-based solid electrolyte.

11. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has a perovskite structure.

12. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

13. The oxide-based solid electrolyte has a composition formula of A x2 BO 3 (0 < x2 < 1), and at least one of La and Li is included in the element A, and at least one of Mg, W, Nb, and Ti is included in the element B. The negative electrode body according to claim 10, characterized in that.

14. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has a NASICON-type phosphate compound.

15. The negative electrode body according to claim 14, wherein the solid electrolyte having the NASICON-type phosphate compound has at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

16. The nasicon-type phosphate compound is Li (1+x3) M1 (x3) M2 (2-x3) (PO 4 ) 3 represented by the formula, wherein the element M1 includes at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 includes at least one selected from the group consisting of Ti, Ge, and Zr, and x3 satisfies 0 ≦ x3 ≦ 2. The negative electrode body according to claim 14, characterized by the above.

17. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has a garnet-type crystal structure.

18. The negative electrode body according to claim 17, wherein the solid electrolyte having a garnet-type crystal structure contains at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

19. The solid electrolyte having the garnet-type crystal structure is Li(7 - 3x4 + y4 - z4)M x4 La (3-y4) A' ((y4) Zr (2-z4) T (z4) O 12 (Element M is one or more of Al and Ga, element A' is either one of Ca and Sr, T is either one of Nb and Ta, and 0 ≤ x4 ≤ 0.18, 0 ≤ y4 ≤ 0.18, 0 ≤ z4 ≤ 1.5), and the negative electrode body according to claim 17, characterized in that 20. A method for manufacturing a negative electrode body for manufacturing the negative electrode body according to any one of claims 1 to 19, the method including: a step of winding the negative electrode current collector around a can roll having a curvature; a vapor deposition step of vapor-depositing a film containing silicon and / or silicon monoxide having a multilayer structure composed of two or more layers on the negative electrode current collector while the negative electrode current collector travels on the can roll; a step of spraying a gas containing oxygen onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on the upper part of each layer; a step of inserting and desorbing lithium into and from the multilayer structure layer to form the negative electrode active material layer; a step of forming the ion conduction layer having lithium ion conductivity on the surface of the negative electrode active material layer; and a step of forming the solid electrolyte layer adjacent to the ion conduction layer.

21. The method for manufacturing a negative electrode body according to claim 20, including: in the step of forming the multilayer structure layer, forming the multilayer structure layer in which each layer contains a silicon oxide containing silicon dioxide; in the vapor deposition step, vapor-depositing a negative electrode active material layer containing silicon oxide on the negative electrode current collector; immersing the negative electrode active material layer containing silicon oxide in a solution containing lithium, and reforming the silicon oxide by an electrochemical method to generate a compound containing lithium, silicon, and oxygen, and a step of forming the ion conduction layer.

Citation Information

Patent Citations

  • Nonaqueous electrolytic secondary battery and its manufacture

    JP1994325765A

  • Total solid lithium battery

    JP1999007942A

  • Lithium secondary battery

    JP2001185127A

  • Non-aqueous electrolyte secondary battery

    JP2002042806A

  • Lithium secondary battery and its manufacturing method

    JP2003059492A