Adhesive for power storage device packaging material, power storage device packaging material, container for power storage device, and power storage device
The adhesive composition for power storage device packaging materials, incorporating a polyisocyanate and a polyol with a specific partial structure, addresses the challenges of adhesive strength and durability by enhancing adhesion and moldability, even with reduced adhesive application and short curing times, achieving effective performance under high temperature and humidity conditions.
Patent Information
- Application Number
- PCT/JP2024/019141
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Packaging materials for power storage devices, such as lithium-ion batteries, face challenges with adhesive strength and durability under high temperature and humidity conditions, particularly when the adhesive amount is reduced and curing time is shortened, leading to insufficient adhesion and moldability issues.
An adhesive composition for power storage device packaging materials containing a polyisocyanate and a polyol, where the polyol includes a polyester polyol and a partial structure represented by a specific general formula, enhancing adhesion and flexibility, even with reduced adhesive application and shortened curing time, while maintaining long-term durability.
The adhesive composition achieves high adhesiveness, flexibility, and excellent moldability and durability under high temperature and humidity conditions, ensuring strong adhesion and resistance to moisture, even with minimal adhesive application and short curing times.
Smart Images

Figure JP2024019141_05122024_PF_FP_ABST
Abstract
Description
Adhesive for packaging material for power storage devices, packaging material for power storage devices, container for power storage devices, and power storage devices
[0001] The present disclosure relates to an adhesive for packaging materials for electricity storage devices used to form containers for electricity storage devices such as lithium ion batteries, and relates to an adhesive for packaging materials for electricity storage devices that has a good appearance and excellent adhesive strength and formability.
[0002] The rapid growth of electronic devices such as mobile phones and portable personal computers has led to an increasing demand for power storage devices, such as secondary batteries (e.g., lithium-ion batteries and nickel-metal hydride batteries) and electrochemical capacitors (e.g., electric double-layer capacitors). Among these, small lithium-ion batteries have attracted attention due to their high energy density and light weight. While metal cans have traditionally been used as the exterior housings for lithium-ion batteries, packaging materials made of laminated plastic films or metal foils are becoming mainstream due to their lighter weight and productivity.
[0003] In the field of packaging materials for such electrical storage devices, for example, Patent Document 1 discloses that a laminate adhesive composition for battery packaging containing a polyol-modified polyisocyanate, which is a compound of an aromatic isocyanate having tri- or higher functional isocyanate groups in its molecular structure and a polyester polyol, and a polyester polyol, has excellent adhesive properties and heat resistance and can shorten the curing period.
[0004] JP 2018-110086 A
[0005] In recent years, as applications such as in-vehicle and home energy storage have expanded, there has been a demand for larger capacity secondary batteries, and packaging materials for energy storage devices are now required to have good formability. Meanwhile, further weight reductions are required for in-vehicle applications, and packaging materials are required that maintain the adhesive strength between the layers of the packaging material, such as plastic films and metal foils, even after molding and long-term durability tests, and that have no abnormalities in appearance, even when the amount of adhesive applied is reduced. Furthermore, along with the reduction in the amount of adhesive applied, there is also a demand for further shortening of the curing period and improvement of productivity.
[0006] However, the adhesive described in Patent Document 1 does not contain the partial structure represented by general formula (1), and therefore the urethane reaction does not proceed quickly. As a result, in the harsh usage environments that have recently been required, such as reducing the amount of adhesive applied and shortening the curing period, it takes time for adhesive properties to develop, and there are problems with reduced adhesive strength after molding and after long-term durability testing.
[0007] Therefore, an object of the present disclosure is to provide an adhesive for packaging materials for electricity storage devices that exhibits high adhesion and flexibility, and is capable of achieving both excellent formability and long-term durability at high temperatures and high humidity, even when a small amount of adhesive is applied and the curing time is shortened, as well as to provide packaging materials for electricity storage devices, containers for electricity storage devices, and electricity storage devices that use the adhesive and have excellent formability and long-term durability.
[0008] As a result of extensive research into solving the above problems, the present inventors have found that the above problems can be solved by the following embodiments, and have thus completed the present disclosure.
[0009] <1> That is, the present disclosure relates to an adhesive for packaging materials for electricity storage devices, which contains a polyisocyanate (A) and a polyol (B), wherein the polyol (B) contains a polyester polyol (b1), the polyol (B) accounts for 20 to 60 mass % based on the mass of the polyisocyanate (A), and the adhesive contains a partial structure represented by the following general formula (1) in an amount of 0.5 to 12.0 mass % based on the mass of the solid content of the adhesive: General formula (1): [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.]
[0010] <2> The present disclosure relates to the adhesive for packaging materials for electricity storage devices according to <1>, in which the polyisocyanate (A) includes a reaction product of a polyisocyanate and a polyol including a polyester polyol (a2).
[0011] <3> The present disclosure relates to the adhesive for packaging materials for storage batteries according to <1> or <2>, in which the polyisocyanate (A) comprises a reaction product of a polyisocyanate including an aromatic polyisocyanate adduct (a1) and a polyol including a polyester polyol (a2).
[0012] <4> The present disclosure relates to the adhesive for packaging materials for electricity storage devices according to <2> or <3>, in which the polyhydric alcohol that is a constituent component of the polyester polyol (a2) contains 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by general formula (1) relative to 100 mol % of the polyhydric alcohol.
[0013] <5> The present disclosure relates to the adhesive for packaging materials for electricity storage devices according to any one of <1> to <4>, in which the polyol (B) further contains a hydroxyl group-containing epoxy resin (b2) in an amount of 5 to 50 mass% based on the mass of the polyol (B).
[0014] <6> The present disclosure relates to the adhesive for packaging materials for electricity storage devices according to <5>, in which the hydroxyl group-containing epoxy resin (b2) is a bisphenol A-type epoxy resin.
[0015] <7> The present disclosure relates to a packaging material for an electricity storage device having a configuration in which at least an outer layer resin film layer, an outer layer adhesive layer, a metal foil layer, an inner layer adhesive layer, and a heat seal layer are laminated in this order, and the outer layer adhesive layer is a cured product of the adhesive for electricity storage device packaging according to any one of <1> to <6>.
[0016] <8> The present disclosure relates to a container for an electricity storage device formed from the electricity storage device packaging material described in <7>, in which the outer layer side resin film layer forms a convex surface and the heat seal layer forms a concave surface.
[0017] <9> The present disclosure relates to an electricity storage device including the electricity storage device container according to <8>.
[0018] The present disclosure makes it possible to provide an adhesive for packaging materials for electricity storage devices that exhibits high adhesion and flexibility, and that is capable of achieving both excellent formability and long-term durability at high temperatures and high humidity, even when a small amount of adhesive is applied and the curing time is shortened, as well as electricity storage device packaging materials, electricity storage device containers, and electricity storage devices that use the adhesive and have excellent formability and long-term durability.
[0019] 1 is a schematic cross-sectional view of a packaging material for an electricity storage device according to the present disclosure; 2 is a schematic perspective view of one embodiment of a container for an electricity storage device according to the present disclosure (tray-shaped);
[0020] <Adhesive for Electricity Storage Device Packaging> The adhesive for electricity storage device packaging (hereinafter also referred to as adhesive) of the present disclosure is an adhesive containing a polyisocyanate (A) and a polyol (B), characterized in that the polyol (B) contains a polyester polyol (b1), the polyol (B) accounts for 20 to 60 mass % based on the mass of the polyisocyanate (A), and the partial structure represented by general formula (1) above accounts for 0.5 to 12.0 mass % based on the mass of the solids content of the adhesive.
[0021] First, by containing 0.5 to 12.0 mass% of the highly hydrophilic partial structure represented by the general formula (1), affinity with water is enhanced, accelerating the reaction between the polyisocyanate (A) and water. This reaction forms urea bonds with high cohesive strength, and a self-crosslinking reaction progresses during curing, improving cohesive strength. This allows for high adhesiveness even with a small application amount and a short curing time. Furthermore, because the partial structure has a flexible skeleton, having a predetermined amount of such a flexible partial structure allows for excellent moldability. The content of the partial structure is preferably 5.0 to 10.0 mass%. A content of 5.0 mass% or more facilitates curing even with a short curing time, while a content of 10 mass% or less provides excellent moist heat resistance. The partial structure of general formula (1) may be contained in at least one of the polyisocyanate (A) and the polyol (B), or may be contained in both. From the viewpoints of improving the compatibility between the polyisocyanate (A) and the polyol (B) and further improving the appearance, it is preferable that both the polyisocyanate (A) and the polyol (B) contain the partial structure of general formula (1). R in general formula (1) is preferably a hydrogen atom. When R is a hydrogen atom, affinity with water is further increased, which is preferable from the viewpoint of shortening the curing period, and the cohesive strength of the adhesive layer is increased, improving adhesion and moldability.
[0022] Furthermore, it is important that the adhesive of the present disclosure contains 20 to 60 mass % of polyol (B) containing polyester polyol (b1) based on the mass of polyisocyanate (A), more preferably in the range of 25 to 45 mass %. If it is less than 20 mass %, the cured film becomes excessively rigid, and adhesion and conformability to the substrate are insufficient, making it impossible to achieve both adhesive strength and moldability. If it exceeds 60 mass %, the cohesive strength of the adhesive decreases, and further, the amount of hydroxyl groups in the adhesive increases and the number of isocyanate groups decreases, resulting in a decrease in affinity with the substrate and insufficient adhesive strength and moist heat resistance. Furthermore, when polyol (B) contains polyester polyol (b1), adhesion to the substrate is improved, and high adhesion and moldability can be exhibited even when the application amount is small and the curing period is short.
[0023] In other words, the adhesive for packaging materials for electricity storage devices of the present disclosure has synergistic effects based on the fact that the amount of polyol (B) containing polyester polyol (b1) is 20 to 60 mass % relative to the polyisocyanate (A) and that the adhesive contains a partial structure represented by general formula (1) in an amount of 0.5 to 12.0 mass % based on the mass of the solid content of the adhesive, and even when the application amount is small and the curing period is short, the adhesive exhibits high cohesive strength, substrate conformability, and flexibility, and can achieve excellent adhesive strength, moldability, and moist heat resistance.
[0024] <Polyisocyanate (A)> Polyisocyanate (A) crosslinks with the hydroxyl groups in the polyol (B), increasing the molecular weight of the adhesive layer and improving the internal cohesive strength that exhibits energy resilience. Furthermore, the isocyanate groups in the polyisocyanate (A) can react with water to form urea bonds with high cohesive strength, so the cohesive strength of the adhesive layer can be increased by self-crosslinking during curing. Thus, the use of polyisocyanate (A) makes it possible to form a strong adhesive layer and improve adhesive strength.
[0025] Examples of the polyisocyanate (A) include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, and various derivatives derived from the above polyisocyanates.
[0026] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, and 2,6-diisocyanate methyl caproate.
[0027] Examples of alicyclic polyisocyanates include 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, and 1,3-bis(isocyanatomethyl)cyclohexane.
[0028] Examples of aromatic polyisocyanates include m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanate benzene, 2,4,6-triisocyanate toluene, and 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate.
[0029] Examples of the araliphatic polyisocyanate include 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or a mixture thereof.
[0030] Examples of derivatives derived from the polyisocyanates include adducts of the polyisocyanates with low-molecular-weight polyols having a molecular weight of less than 200, such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3′-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol, or castor oil; trimers (also referred to as trimers or nurates) of the diisocyanates; biurets; allophanates; polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide and the diisocyanates; and polyurethane polyisocyanates obtained by reacting a polyisocyanate with a polyol under conditions in which the isocyanate group is in excess.
[0031] The polyol to be reacted with the polyisocyanate may be any conventionally known polyol, such as polyester polyol, polyether polyol, polycarbonate polyol, acrylic polyol, or polybutadiene polyol.
[0032] (Polyesterurethane Polyisocyanate) From the viewpoint of achieving both excellent high-temperature durability and high cohesive strength and processability, the polyisocyanate (A) preferably contains a polyesterurethane polyisocyanate which is a reaction product of a polyisocyanate and a polyol containing a polyester polyol (a2). As the polyisocyanate for forming the polyesterurethane polyisocyanate, an aromatic polyisocyanate is preferably used, and among these, one containing an adduct (a1) of an aromatic polyisocyanate such as tolylene diisocyanate or MDI is particularly preferably used.
[0033] (Aromatic Polyisocyanate Adduct (a1)) Examples of the aromatic polyisocyanate adduct (a1) include adducts obtained by adding an aromatic diisocyanate monomer to a polyhydric alcohol. Examples of the diisocyanate monomer include m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, and 4,4'-diphenyl ether diisocyanate. Examples of the polyhydric alcohol include Examples of the aromatic polyisocyanate adduct (a1) include low molecular weight polyols having a molecular weight of less than 200, such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol, and castor oil. Suitable examples of the aromatic polyisocyanate adduct (a1) include an adduct of tolylene diisocyanate with trimethylolpropane, an adduct of tolylene diisocyanate with trimethylolpropane and diethylene glycol, and an adduct of 4,4'-diphenyl diisocyanate with trimethylolpropane, dipropylene glycol, and tripropylene glycol. That is, the polyester urethane polyisocyanate is preferably a polyisocyanate obtained by reacting a polyisocyanate containing an aromatic polyisocyanate adduct (a1) with a polyol containing a polyester polyol (a2). By having an ester structure derived from such a polyester polyol and a urethane structure, the polyester urethane polyisocyanate can have both flexibility and cohesive strength, and can exhibit excellent adhesive performance.
[0034] The polyisocyanate for forming the polyester urethane polyisocyanate may contain a polyisocyanate other than the adduct (a1) of an aromatic polyisocyanate. Examples of such a polyisocyanate include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, and various derivatives derived from the polyisocyanates described above in the section <Polyisocyanate (A)>.
[0035] (Polyester Polyol (a2)) In the present disclosure, the polyester polyol (a2) is not limited to the following, but examples thereof include polyester polyols obtained by reacting a polybasic acid with a polyhydric alcohol; or polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone).
[0036] Examples of the polybasic acid include dibasic acids having an aromatic ring, such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, and phthalic anhydride; aliphatic dibasic acids, such as adipic acid, azelaic acid, sebacic acid, succinic acid, glutaric acid, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, maleic anhydride, and itaconic anhydride; and dialkyl esters thereof, or mixtures thereof.
[0037] Examples of the polyhydric alcohol include diols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, butylene glycol, neopentyl glycol, dineopentyl glycol, trimethylolpropane, glycerin, 1,6-hexanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, 1,9-nonanediol, polyoxyethylene glycol, polyoxypropylene glycol, polytetramethylene ether glycol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, and polyurethane polyol; or mixtures thereof. The polybasic acids and polyhydric alcohols may each be used alone, but it is preferable to use two or more of them in combination.
[0038] The polyhydric alcohol constituting the polyester polyol (a2) preferably contains, per 100 mol % of the polyhydric alcohol, 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by the following general formula (1): When the content is 5 mol % or more, affinity with water is increased, and the effect of shortening the curing time is easily achieved. When the content is 30 mol % or less, the polyisocyanate (A) does not become too flexible, and excellent adhesion at high temperatures is achieved.
[0039] General formula (1) [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.]
[0040] Examples of polyhydric alcohols having the above partial structure include diethylene glycol, triethylene glycol, dipropylene glycol, and tripropylene glycol. Furthermore, the polyhydric alcohols having the above partial structure may be polyoxyalkylene glycols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran with a low-molecular-weight polyol such as water, ethylene glycol, propylene glycol, trimethylolpropane, or glycerin as an initiator. From the viewpoints of reactivity and moderate hydrophilicity, those having an oxyethylene structure are preferred. Furthermore, from the viewpoint of compatibility between the polyhydric alcohol and other raw materials, diethylene glycol is preferred.
[0041] The weight-average molecular weight (Mw) of the polyester polyol (a2) is preferably 5,000 to 30,000. When the weight-average molecular weight is 5,000 or more, adhesion to the substrate is further improved and processability is excellent. When the weight-average molecular weight is 30,000 or less, it is possible to easily prevent the concentration of hydroxyl groups at the terminals of the polyester polyol (a2) from becoming excessively low, and it is possible to easily prevent the reaction time from being prolonged when the polyester polyol (a2) is reacted with a trifunctional or higher aromatic polyisocyanate (a1) to obtain the polyisocyanate (A).
[0042] The hydroxyl value (OHV) of the polyester polyol (a2) is preferably 2 to 35 mgKOH / g, more preferably 10 to 20 mgKOH / g. The hydroxyl groups are used in a reaction with the trifunctional or higher aromatic polyisocyanate (a1), and as the reaction progresses, the adhesive becomes highly molecular weight, thereby improving the heat resistance of the adhesive as a packaging material. The hydroxyl value can be determined by a method in accordance with JIS K 1557-1.
[0043] The glass transition temperature (Tg) of the polyester polyol (a2) is preferably in the range of −20 to 5° C., more preferably −10 to 0° C. By setting the glass transition temperature (Tg) within the above range, it becomes easy to control the cohesive strength of the adhesive, and it is possible to obtain an appropriate cohesive strength depending on the adherend substrate, required performance, etc.
[0044] The reaction temperature for urethanization of the tri- or higher functional aromatic polyisocyanate (a1) and the polyester polyol (a2) is preferably 50 to 180° C., and more preferably 60 to 100° C. A temperature of 50 to 180° C. is preferred because the urethanization reaction proceeds efficiently.
[0045] The NCO% contained in the polyisocyanate (A) is preferably 1.0 to 8.0 mass% and more preferably 4.0 to 6.0 mass% in terms of solid content. When it is 1.0 mass% or more, the amount of urethane bonds after curing becomes sufficient, increasing the cohesive force and improving the adhesive strength. When it is 8.0 mass% or less, the time required for curing can be shortened and poor appearance due to foaming and the like can be suppressed.
[0046] <Polyol (B)> The polyol (B) used in the present disclosure is characterized by containing a polyester polyol (b1). By containing the polyester polyol (b1), adhesion to the substrate is improved, and excellent adhesive strength and moldability can be exhibited. In addition, the polyester polyol (b1) is suitable from the viewpoint of ease of introducing the partial structure of general formula (1).
[0047] (Polyester Polyol (b1)) Examples of the polyester polyol (b1) include polyester polyols obtained by reacting a polybasic acid with a polyhydric alcohol; or polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone). Examples of such polyester polyols (b1) include those described in the section (Polyester Polyol (a2)) under <Polyisocyanate (A)> above. Similarly to polyester polyol (a2), the polyhydric alcohol that constitutes polyester polyol (b1) may contain a polyhydric alcohol having a partial structure represented by general formula (1). The content of the polyhydric alcohol having the partial structure is preferably 5 to 30 mol % relative to 100 mol % of the polyhydric alcohol.
[0048] The weight-average molecular weight of the polyester polyol (b1) is preferably 5,000 to 60,000. When the weight-average molecular weight is 5,000 or more, the adhesion to the substrate is further improved and the processability is excellent. When the weight-average molecular weight is 60,000 or less, the compatibility when mixed with the polyisocyanate (A) is excellent and the appearance is good.
[0049] The polyester polyol (b1) preferably has a hydroxyl value of 5 to 20 mgKOH / g, and a glass transition temperature of -20 to 50°C, more preferably -5 to 35°C.
[0050] (Hydroxyl-containing epoxy resin (b2)) From the viewpoint of adhesive strength and moist heat resistance, it is preferable that the polyol (B) further contains a hydroxyl-containing epoxy resin (b2). By using the hydroxyl-containing epoxy resin (b2) in combination, the high-temperature adhesive strength to metal materials such as metal foil, and the heat resistance and heat durability of the molded product are improved. The content of the hydroxyl-containing epoxy resin (b2) is preferably 5 to 50 mass% based on the mass of the polyol (B). When it is 5 mass% or more, the adhesive strength and moist heat resistance are excellent. When it is 50 mass% or less, the moldability is excellent. From the viewpoint of the balance of adhesive strength, moldability, and moist heat resistance, it is more preferably 10 to 30 mass%.
[0051] Examples of the hydroxyl group-containing epoxy resin (b2) include bisphenol A type epoxy resin, bisphenol F type epoxy resin, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, and trimethylolpropane polyglycidyl ether. From the viewpoint of adhesiveness and durability of molded products, bisphenol A type epoxy resin is preferred. These hydroxyl group-containing epoxy resins may be used alone or in combination of two or more.
[0052] (Other Polyols) The polyol (B) may further contain a known polyol other than (b1) and (b2), as long as the effects of the present disclosure are not impaired. Examples of such polyols include polyether polyols, polyurethane polyols, polycarbonate polyols, and acrylic polyols, and may further be polyols that have been reacted with polyisocyanate to introduce urethane bonds.
[0053] <Solvent> The adhesive of the present disclosure may contain a solvent to the extent that it does not affect the substrate during the drying process, in order to adjust the coating liquid to an appropriate viscosity when the adhesive is applied to a substrate. Examples of the solvent include ketone compounds such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester compounds such as methyl acetate, ethyl acetate, butyl acetate, ethyl lactate, and methoxyethyl acetate; ether compounds such as diethyl ether and ethylene glycol dimethyl ether; aromatic compounds such as toluene and xylene; aliphatic compounds such as pentane and hexane; and halogenated hydrocarbon compounds such as methylene chloride, chlorobenzene, and chloroform.
[0054] <Production of adhesive for packaging material for electricity storage device> The adhesive of the present disclosure contains at least the polyisocyanate (A) and a polyol (B) containing the polyester polyol (b1), and the content of the polyol (B) is 20 to 60 mass% based on the mass of the polyisocyanate (A), and the content of the partial structure represented by the general formula (1) is 0.5 to 12.0 mass% based on the mass of the solid content of the adhesive.
[0055] In the adhesive of the present disclosure, when polyisocyanate (A) and polyol (B) are blended, the ratio of the number of isocyanate groups in polyisocyanate (A) to the number of hydroxyl groups in polyol (B) (number of NCO moles / number of OH moles) is preferably 5 to 20, more preferably 8 to 12. When the ratio is 5 or more, the amount of urethane bonds after curing becomes sufficient, increasing the cohesive strength and improving the heat resistance and heat durability of the molded product. When the ratio is 20 or less, the time required for curing can be shortened and poor appearance due to foaming and the like can be suppressed.
[0056] The adhesive of the present disclosure may further contain other components within a range that does not impair the effects of the present disclosure. Such optional components may be blended with either or both of the polyisocyanate (A) and the polyol (B), or may be added when blending the polyisocyanate (A) and the polyol (B). Each of these may be used alone or in combination of two or more.
[0057] (Antioxidant) The adhesive of the present disclosure may contain an antioxidant to suppress thermal oxidative degradation. Examples of antioxidants include monophenolic antioxidants such as 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, and stearin-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), and 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-tetramethylphenyl; Examples of suitable antioxidants include bisphenol-based antioxidants such as laoxaspiro[5,5]undecane; and polymeric phenol-based antioxidants such as 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis-(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, 1,3,5-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, and triphenol. Among these, high-molecular-weight hindered phenol-based antioxidants such as tetraphenols and triphenols are preferred.
[0058] (Reaction Accelerator) The adhesive of the present disclosure may further contain a reaction accelerator to accelerate the urethanization reaction. Examples of reaction accelerators include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dimaleate; tertiary amines such as 1,8-diazabicyclo(5,4,0)undecene-7 and 1,5-diazabicyclo(4,3,0)nonene-5,6-dibutylamino-1,8-diazabicyclo(5,4,0)undecene-7; and reactive tertiary amines such as triethanolamine.
[0059] (Silane Coupling Agent) The adhesive of the present disclosure may further contain a silane coupling agent to improve adhesive strength to metal materials such as metal foil. Examples of silane coupling agents include trialkoxysilanes having a vinyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane; and trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-glycidoxypropyltriethoxysilane. The content of the silane coupling agent is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 3 parts by mass, per 100 parts by mass of the solid content of the adhesive for packaging materials for electrical storage devices. Adding a silane coupling agent in the above range can further improve adhesive strength to metal foil.
[0060] (Phosphorus Oxygen Acid or Derivative Thereof) The adhesive of the present disclosure may contain a phosphorus oxyacid or a derivative thereof to improve adhesive strength to metal materials such as metal foil. The phosphorus oxyacid may be any acid having at least one free oxyacid, and examples thereof include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid; and condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid. Derivatives of phosphorus oxyacids include, for example, the above phosphorus oxyacids partially esterified with alcohols while leaving at least one free oxyacid. Examples of the alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. The content of the phosphorus oxyacid or its derivative is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.05 to 1 part by mass, per 100 parts by mass of the solid content of the adhesive for packaging materials for electrical storage devices.
[0061] (Leveling Agent or Antifoaming Agent) The adhesive of the present disclosure may further contain a leveling agent or antifoaming agent to improve the laminate appearance of the packaging material. Examples of leveling agents include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl-containing polydimethylsiloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, acrylic copolymer, methacrylic copolymer, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymer, methacrylic acid alkyl ester copolymer, and lecithin. Examples of antifoaming agents include silicone resin, silicone solution, and copolymers of alkyl vinyl ether, acrylic acid alkyl ester, and methacrylic acid alkyl ester.
[0062] (Additives) The adhesive of the present disclosure may contain various additives to the extent that the effects of the present disclosure are not impaired. Examples of additives include inorganic fillers such as silica, alumina, mica, talc, aluminum flakes, and glass flakes, layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, UV absorbers, hydrolysis inhibitors, etc.), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, and catalysts for adjusting the curing reaction.
[0063] <Packaging Material for Electricity Storage Device> The adhesive of the present disclosure can be used as an adhesive for forming an adhesive layer of a packaging material for an electricity storage device. In particular, it can be suitably used as an outer layer adhesive for forming an outer layer adhesive layer of a packaging material for an electricity storage device. The packaging material for an electricity storage device of the present disclosure has a configuration in which at least an outer layer resin film layer, an outer layer adhesive layer, a metal foil layer, and a heat seal layer are laminated in this order from the outside, and is characterized in that the outer layer adhesive layer is a cured product of the adhesive for electricity storage device packaging material described above. The manufacturing method of the packaging material for an electricity storage device is not particularly limited, and the packaging material can be manufactured by a known method. For example, the packaging material can be manufactured by laminating an outer layer resin film layer and a metal foil layer using the adhesive for electricity storage device packaging material that forms the outer layer adhesive layer to obtain an intermediate laminate having a configuration of outer layer resin film layer / outer layer adhesive layer / metal foil layer, and then laminating a heat seal layer on the surface of the metal foil layer of the intermediate laminate using an inner layer adhesive (hereinafter referred to as manufacturing method 1). Alternatively, the package can be manufactured by laminating a metal foil layer and a heat seal layer using an inner layer adhesive to obtain an intermediate laminate having a configuration of metal foil layer / inner layer adhesive layer / heat seal layer, and then laminating the metal foil layer of the intermediate laminate and an outer layer resin film layer using an adhesive for packaging materials for electricity storage devices (hereinafter, manufacturing method 2).
[0064] In the case of manufacturing method 1, it is preferable to apply the adhesive for electricity storage device packaging materials to one surface of the substrate of either the outer layer side resin film layer or the metal foil layer, volatilize the solvent, and then overlap the other substrate with the uncured outer layer side adhesive layer under heat and pressure, followed by aging at room temperature to less than 100°C to cure the outer layer side adhesive layer. If the aging temperature is less than 100°C, thermal shrinkage of the outer layer side resin film layer does not occur, so there is no decrease in breaking elongation or breaking stress that affects molding, and no decrease in molding productivity due to film curl. The coating amount of the outer layer side adhesive after drying is 1 to 15 g / m 2 Similarly, in the case of production method 2, the adhesive for packaging materials for electricity storage devices may be applied to either the outer layer side resin film layer or the metal foil layer surface of the intermediate laminate.
[0065] Examples of methods for forming the outer adhesive layer include methods using a comma coater, dry laminator, roll knife coater, die coater, roll coater, bar coater, gravure roll coater, reverse roll coater, blade coater, gravure coater, and microgravure coater.
[0066] [Outer Resin Film Layer] The outer resin film layer is not particularly limited, but is preferably at least one stretched film selected from the group consisting of polyamide, polyester, and polyimide. From the viewpoints of stretchability during molding and heat resistance, polyester film is more preferred. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, and polycyclohexanedimethylene terephthalate. The outer resin film layer may be colored with pigments such as carbon black or titanium oxide. The non-laminated surface of the outer resin film layer may be coated with a coating agent for scratch prevention and electrolyte resistance, a slip agent for providing slippage during molding, or a printing ink for decorative purposes. The outer resin film layer may also be a laminate film in which two or more layers of film are pre-laminated. The thickness of the outer resin film layer is not particularly limited, but is preferably 12 to 100 μm.
[0067] [Metal Foil Layer] The metal foil layer is not particularly limited, but may be a stainless steel foil layer or an aluminum foil layer. The thickness of the metal foil layer is not particularly limited, but is preferably 20 to 80 μm. The surface of the metal foil layer is preferably subjected to a known antiseptic treatment such as chromate phosphate treatment, chromate chromate treatment, trivalent chromium treatment, zinc phosphate treatment, zirconium phosphate treatment, zirconium oxide treatment, titanium phosphate treatment, hydrofluoric acid treatment, cerium treatment, or hydrotalcite treatment. The antiseptic treatment can suppress corrosion degradation of the metal foil surface due to the battery electrolyte. Furthermore, it is preferable that a known organic component such as a phenolic resin, an amide resin, an acrylic resin, polyvinyl alcohol, or a coupling agent is applied to the antiseptic-treated surface, or a mixture of the antiseptic treatment component and the organic component is applied, and the metal foil layer is baked at a high temperature of approximately 200°C. Applying such an organic primer treatment can more firmly bond the metal foil and adhesive, further suppressing lifting between the metal foil and adhesive.
[0068] [Heat-seal layer] The heat-seal layer is not particularly limited, and is preferably an unstretched film made of at least one thermoplastic resin selected from the group consisting of polyester, polyethylene, polypropylene, olefin copolymers, acid-modified products thereof, and ionomers. The thickness of the heat-seal layer is not particularly limited, but is preferably 20 to 150 μm.
[0069] [Inner Layer Adhesive Layer] The adhesive forming the inner layer adhesive layer is not particularly limited, but is preferably one that does not reduce the adhesive strength between the metal foil layer and the heat seal layer due to the electrolyte solution of the energy storage device. In addition to the adhesive for energy storage device packaging materials of the present disclosure, known adhesives can be used. The inner layer adhesive layer can be formed, for example, by applying an adhesive combining a polyolefin resin and a polyisocyanate or an adhesive combining a polyol and a polyisocyanate to the metal foil layer using a gravure coater or the like, drying the solvent, laminating a heat seal layer on the adhesive layer under heat and pressure, and then aging at room temperature or under elevated temperature. Alternatively, the inner layer adhesive layer can be formed by melt-extruding an adhesive such as acid-modified polypropylene onto the metal foil layer using a T-die extruder to form an adhesive layer, laminating a heat seal layer on the adhesive layer, and bonding the metal foil layer and the heat seal layer together. When both the outer layer adhesive layer and the inner layer adhesive layer require aging, aging may be performed all at once after obtaining a laminate having a configuration in which the outer layer resin film layer, the uncured outer layer adhesive layer, the metal foil layer, the uncured inner layer adhesive layer, and the heat seal layer are laminated in this order from the outside.
[0070] <Container for Electricity Storage Device> The container for an electricity storage device of the present disclosure can be obtained by molding the packaging material for an electricity storage device of the present disclosure so that the outer layer side resin film layer forms a convex surface and the heat seal layer forms a concave surface. Note that the "concave surface" in this disclosure means a surface having a depression capable of accommodating an electrolyte solution when the packaging material for an electricity storage device in a flat state is molded into a tray shape as shown in Fig. 2, and the "convex surface" in this disclosure means the back surface of the surface having the depression.
[0071] <Electricity Storage Device> The electricity storage device of the present disclosure uses the electricity storage device container, and examples thereof include secondary batteries such as lithium-ion batteries, nickel-metal hydride batteries, and lead-acid batteries, as well as electrochemical capacitors such as electric double-layer capacitors. A typical electricity storage device includes a battery element including electrodes, leads extending from the electrodes, and a container that houses them. In the electricity storage device of the present disclosure, the electricity storage device container is used as the housing container. The housing container may be formed from a packaging material for an electricity storage device so that the heat seal layers are on the inside, by overlapping two packaging materials with the heat seal layers facing each other and heat-sealing the peripheral edges of the overlapped packaging materials, or by folding one packaging material over the other and similarly heat-sealing the peripheral edges of the packaging materials.
[0072] The present disclosure will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0073] <Measurement of Acid Value (AV)> Approximately 1 g of sample (polyester polyol solution) was precisely weighed into a stoppered Erlenmeyer flask, and 100 mL of a toluene / ethanol (volume ratio: toluene / ethanol = 2 / 1) mixture was added and dissolved. Phenolphthalein test solution was added as an indicator and the mixture was allowed to stand for 30 seconds. The solution was then titrated with 0.1 N alcoholic potassium hydroxide solution until it turned a pale pink color, and the acid value (mg KOH / g) was calculated using the following formula: Acid Value (mg KOH / g) = (5.611 × a × F) / S, where S is the amount of sample collected (g), a is the amount of 0.1 N alcoholic potassium hydroxide solution consumed (mL), and F is the titer of the 0.1 N alcoholic potassium hydroxide solution.
[0074] <Measurement of hydroxyl value (OHV)> Approximately 1 g of sample (polyester polyol, hydroxyl group-containing urethane resin, etc.) was precisely weighed into a stoppered Erlenmeyer flask and dissolved in 100 mL of a toluene / ethanol (volume ratio: toluene / ethanol = 2 / 1). Exactly 5 mL of an acetylating agent (a solution prepared by dissolving 25 g of acetic anhydride in pyridine to a volume of 100 mL) was then added and stirred for approximately 1 hour. Phenolphthalein test solution was added as an indicator and the mixture was stirred for 30 seconds. The solution was then titrated with 0.5 N alcoholic potassium hydroxide solution until it turned pale pink, and the hydroxyl value (mg KOH / g) was calculated using the following formula: Hydroxyl value (mg KOH / g) = [{(b - a) x F x 28.05} / S] + D where S: sample amount (g) a: amount of 0.5N alcoholic potassium hydroxide solution consumed (mL) b: amount of 0.5N alcoholic potassium hydroxide solution consumed in blank experiment (mL) F: titer of 0.5N alcoholic potassium hydroxide solution D: acid value (mg KOH / g)
[0075] <Method for measuring NCO content (mass%)> Approximately 1 g of sample was weighed into a 200 mL Erlenmeyer flask, and 10 mL of 0.5 N di-n-butylamine toluene solution and 10 mL of toluene were added to dissolve the sample. Next, phenolphthalein test solution was added as an indicator, and after holding for 30 seconds, the solution was titrated with 0.25 N hydrochloric acid solution until it turned pale pink. The NCO content (mass%) was calculated using the following formula (3): (Formula 3): NCO (mass%) = {(b - a) × 4.202 × F × 0.25} / S, where S is the amount of sample collected (g), a is the amount of 0.25 N hydrochloric acid solution consumed (mL), b is the amount of 0.25 N hydrochloric acid solution consumed in a blank experiment (mL), and F is the titer of the 0.25 N hydrochloric acid solution.
[0076] <Measurement of Weight Average Molecular Weight (Mw), Number Average Molecular Weight (Mn), and Molecular Weight Distribution (Mw / Mn)> The weight average molecular weight and number average molecular weight were measured using Showdex (registered trademark) (manufactured by Showa Denko K.K.) columns: KF-805L, KF-803L, and KF-802 (all trade names, manufactured by Showa Denko K.K.) at a column temperature of 40°C, THF as an eluent, a flow rate of 0.2 mL / min, detection by RI, and a sample concentration of 0.02% by mass, and values were used in terms of standard polystyrene. The molecular weight distribution was calculated from the obtained values.
[0077] <Glass transition temperature (Tg)> The glass transition temperature was measured by DSC (differential scanning calorimetry). Specifically, approximately 2 mg of the compound to be measured was weighed on an aluminum pan, the aluminum pan was set in a DSC measurement holder, and the endothermic peak in the chart obtained at a temperature rise condition of 5°C / min was read, and the peak temperature at this time was taken as the glass transition temperature.
[0078] <<Production of Polyisocyanate (A)>> <Synthesis of Aromatic Polyisocyanate Adduct (a1)> (Aromatic Polyisocyanate Adduct (a1-1)) 239 parts of tolylene diisocyanate was charged, and 61 parts of molten trimethylolpropane was added dropwise with stirring at room temperature, followed by reaction at 60°C for 2 hours. Next, the mixture was diluted with ethyl acetate, the nonvolatile content was adjusted to 50%, and the mixture was discharged. The resulting aromatic polyisocyanate adduct (a1-1) had an NCO% of 19.0% on a solids basis, and the amount of the partial structure of general formula (1) was 0%.
[0079] (Aromatic Polyisocyanate Adduct (a1-2)) 238 parts of tolylene diisocyanate was charged, and a mixed liquid of 46 parts of molten trimethylolpropane and 15 parts of diethylene glycol was added dropwise with stirring at room temperature, followed by reaction at 60°C for 2 hours. Next, the mixture was diluted with ethyl acetate, the nonvolatile content was adjusted to 50%, and the mixture was discharged. The resulting aromatic polyisocyanate adduct (a1-2) had an NCO% of 19.4% on a solids basis, and the amount of the partial structure of general formula (1) was 4.4%.
[0080] (Aromatic Polyisocyanate Adduct (a1-3)) 244 parts of 4,4'-diphenylmethane diisocyanate was charged, and a mixed liquid of 32 parts of molten trimethylolpropane and 15 parts of dipropylene glycol was added dropwise while stirring at 40°C, and then the reaction was carried out at 60°C for 2 hours. Next, the mixture was diluted with ethyl acetate, the nonvolatile content was adjusted to 50%, and the mixture was discharged. The resulting aromatic polyisocyanate adduct (a1-3) had an NCO% of 14.0% on a solid basis, and the amount of the partial structure of general formula (1) was 5.9%.
[0081] <Synthesis of Polyester Polyol (a2)> (Polyester Polyol (a2-1)) 166 parts of isophthalic acid, 166 parts of terephthalic acid, 293 parts of adipic acid, 87 parts of ethylene glycol, 146 parts of neopentyl glycol, and 142 parts of 1,6-hexanediol were charged and subjected to an esterification reaction for 8 hours at 170 to 230 ° C. After distilling off a predetermined amount of water, 0.13 parts of tetraisobutyl titanate was added, and the pressure was gradually reduced to 1.3 to 2.6 hPa and 230 to 250 ° C. for 3 hours to perform a transesterification reaction. A number average molecular weight of 9,620, a weight average molecular weight of 190,700, a molecular weight distribution of 2.05, a hydroxyl value of 10.1 mg KOH / g, and a glass transition temperature of -1.2 ° C. were obtained. When the total amount of the polybasic acid and the polyhydric alcohol is 200 mol %, the composition of the obtained polyester polyol (a2-1) is isophthalic acid: terephthalic acid: adipic acid: ethylene glycol: neopentyl glycol: 1,6-hexanediol=30:30:40:35:35:30 (mol %), as shown in Table 1-2.
[0082] (Polyester polyols (a2-2) to (a2-14)) Polybasic acids and polyhydric alcohols were reacted in the same manner as for polyester polyol (a2-1), to obtain polyester polyols (a2-2) to (a2-14), except that the blending amounts were changed so that the mole percentages of each component, when the total of the polybasic acid and polyhydric alcohol was 200 mole %, were as shown in Table 1-2.
[0083] The composition ratio (mass %) and composition ratio (mol %) of the resulting polyester polyol (a2) are shown in Table 1-1 and Table 1-2 (hereinafter abbreviated as Table 1).
[0084]
[0085]
[0086] The abbreviations in Table 1 and Table 3 described below are as follows: PA: phthalic anhydride IPA: isophthalic acid TPA: terephthalic acid AdA: adipic acid SeA: sebacic acid AzA: azelaic acid EG: ethylene glycol NPG: neopentyl glycol 1,6-HD: 1,6-hexanediol MPO: 2-methyl-1,3-propanediol DEG: diethylene glycol TEG: triethylene glycol PEG: polyethylene glycol (hydroxyl value 281 mg KOH / g, molecular weight 400) PPG: polypropylene glycol (hydroxyl value 280 mg KOH / g, molecular weight 400)
[0087] <Synthesis of Polyisocyanate (A)> (Polyisocyanate (A-1)) 100 parts of polyester polyol (a2-1), 2.5 parts of 1,4-butanediol, and 102.5 parts of ethyl acetate were charged into a four-neck flask, heated to 100°C, and stirred until the solution became homogeneous. To this was added 65 parts, in solids equivalent, of the aromatic polyisocyanate adduct (a1-1), and the reaction was carried out at 80°C for 4 hours. After completion of the reaction, the nonvolatile content was adjusted to 50% with ethyl acetate and the solution was removed. The obtained polyisocyanate (A-1) had an NCO% in solids equivalent of 5.6%, and the content of the partial structure represented by general formula (1) was 0.0% by mass.
[0088] (Polyisocyanates (A-2) to (A-22)) Polyols and polyisocyanates were reacted in the same manner as for polyisocyanate (A-1), except that the blending amounts were changed to those shown in Table 2, and polyisocyanates (A-2) to (A-22) were obtained by adjusting the nonvolatile content to 50% with ethyl acetate.
[0089]
[0090] The abbreviations in Table 2 are as follows: 1,4-BD: 1,4-butanediol NPG: neopentyl glycol
[0091] <<Production of Polyol (B)>> <Synthesis of Polyester Polyol (b1)> (Polyester Polyols (b1-1) to (b1-8)) Polybasic acids and polyhydric alcohols were reacted in the same manner as for polyester polyol (a2-1), except that the blending amounts were changed so that the mole percentages of each component, when the total of the polybasic acid and polyhydric alcohol was 200 mole %, were as shown in Table 3-1, to obtain polyester polyols (b1-1) to (b1-8).
[0092] The composition ratio (mass %) and composition ratio (mol %) of the resulting polyester polyol (b1) are shown in Tables 3-1 and 3-2.
[0093]
[0094]
[0095] <Preparation of Polyol (B)> (Polyols (B-1) to (B-16)) Polyols (B-1) to (B-16) were obtained by mixing and dissolving polyester polyol (b1), hydroxyl group-containing epoxy resin (b2), and ethyl acetate as a solvent in the amounts shown in Table 4, and adjusting the nonvolatile content to 50%.
[0096]
[0097] The abbreviations in Table 4 are as follows: NPEL-134: bisphenol A type epoxy resin (manufactured by NANYA PLASTICS, epoxy equivalent weight 230 to 270) jER152: phenol novolac type multifunctional epoxy resin (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight 178)
[0098] <Production of Adhesive for Packaging Materials for Electricity Storage Devices> [Example 1] 100 parts of a 50% non-volatile solution of polyisocyanate (A-1), 36 parts of a 50% non-volatile solution of polyol (B-3), 1.0 part of glycidopropyltrimethoxysilane (Si coupling agent) as an additive, 0.010 parts of dibutyltin dilaurate (DBTDL) as a catalyst, and ethyl acetate were adjusted to a solids concentration of 30%, and the mixture was stirred for 10 minutes to obtain an adhesive.
[0099] [Examples 2 to 38, Comparative Examples 1 to 7] Adhesives with a solids concentration of 30% were obtained in the same manner as in Example 1, except that the polyisocyanate (A), polyol (B), Si coupling agent, and type and amount of catalyst were changed to those shown in Tables 5 and 6.
[0100] <Evaluation of Adhesive for Packaging of Electricity Storage Devices> Packaging materials were produced using the obtained adhesives, and the following evaluations were carried out. The results are shown in Tables 5 and 6.
[0101] [Production of packaging material] The adhesive obtained above was applied to one side of an aluminum foil having a thickness of 40 μm using a dry laminator as an outer adhesive layer. After the solvent was evaporated, a stretched polyamide film having a thickness of 30 μm was laminated thereon to obtain an intermediate laminate. The amount of the adhesive applied after drying was 3 g / m. 2 Next, using a dry laminator, the adhesive for the inner layer side adhesive layer described below was applied to the other side of the aluminum foil of the obtained intermediate laminate. After the solvent was evaporated, an unstretched polypropylene film having a thickness of 30 μm was laminated to obtain a laminate. The amount of the adhesive applied after drying was 4 g / m. 2 Next, aging was carried out for 2 days and 4 days under conditions of 40°C and 60% RH (relative humidity) to cure the outer and inner adhesive layers, thereby obtaining a packaging material having a configuration of outer resin film layer / outer adhesive layer / metal foil layer / inner adhesive layer / heat seal layer.
[0102] <<Adhesive for inner adhesive layer>> AD-502 (trade name, polyester polyol, manufactured by Toyo-Morton Co., Ltd.) was used as the base agent, and CAT-10L (trade name, isocyanate-based curing agent, manufactured by Toyo-Morton Co., Ltd.) was used as the curing agent, blended at a base agent / curing agent ratio of 100 / 10 (mass ratio), and adjusted with ethyl acetate to a solids concentration of 30%. This was used as the adhesive for the inner adhesive layer.
[0103] [Lamination Strength] The packaging materials aged for two days at 40°C and 60% RH were each cut into 200 mm x 15 mm pieces and subjected to a T-peel test using a tensile tester to measure the peel strength (N / 15 mm width) between the stretched polyamide film and the aluminum foil. The measurement was performed in an environment of 20°C and 65% RH at a load rate of 300 mm / min, and the average value of five test pieces was evaluated according to the following criteria: S: Average peel strength of 7 N or more (very good); A: Average peel strength of 4 N or more but less than 7 N (good); B: Average peel strength of 2 N or more but less than 4 N (usable); C: Average peel strength of less than 2 N (unusable).
[0104] [Moldability] The packaging material aged for 2 days at 40°C and 60% RH and the packaging material aged for 4 days under the same conditions were each cut into 80 x 80 mm pieces, and with the stretched polyamide film facing outward, a one-stage overhang molding was performed using a height-adjustable straight mold. The maximum molding height at which the aluminum foil did not break or the layers did not float was determined, and moldability was evaluated according to the following criteria. The punch shape of the mold used was a square with sides of 30 mm, a corner R of 2 mm, and a punch shoulder R of 1 mm. The die hole shape of the mold used was a square with sides of 34 mm, a die hole corner R of 2 mm, and a die hole shoulder R of 1 mm. The clearance between the punch and the die hole was 2 mm on each side, and this clearance caused a slope corresponding to the molding height. S: The maximum molded height is 6 mm or more (very good) A: The maximum molded height is 4 mm or more and less than 6 mm (good) B: The maximum molded height is 2 mm or more and less than 4 mm (usable) C: The maximum molded height is less than 2 mm (unusable)
[0105] [Heat and humidity resistance] The packaging materials aged for 2 days at 40°C and 60% RH were each cut into 80 x 80 mm pieces, and with the stretched polyamide film facing outward, they were subjected to a one-stage molding process with a height-adjustable straight mold, overhanging the mold to a height of 3 mm, to obtain molded products. The molded products were then placed in a constant temperature and humidity chamber under an atmosphere of 85°C and 85% RH and left to stand for 168 hours. After being removed from the chamber, they were visually inspected for any floating and evaluated according to the following criteria. The punch shape of the mold used was a square with sides of 30 mm, a corner R of 2 mm, and a punch shoulder R of 1 mm. The die hole shape of the mold used was a square with sides of 34 mm, a die hole corner R of 2 mm, and a die hole shoulder R of 1 mm. S: No lifting (very good) A: Lifting occurs on one of the four sides (good) B: Lifting occurs on two of the four sides (usable) C: Lifting occurs on three or more of the four sides (unusable)
[0106]
[0107]
[0108] According to Tables 5 and 6, the adhesive of the present disclosure, in which the polyol (B) contains the polyester polyol (b1), is 20 to 60% by mass relative to the polyisocyanate (A), and further contains 0.5 to 12.0% by mass of the partial structure represented by general formula (1), has a coating amount of the adhesive of 3 g / m 2 Even when the curing time was shortened to two days, high adhesion and flexibility were exhibited, and excellent moldability and long-term durability at high temperatures and high humidity were achieved. In particular, those containing 5 to 50 mass% of the hydroxyl group-containing epoxy resin (b2) relative to the polyol (B) exhibited excellent laminate strength and moist heat resistance. Furthermore, those using a bisphenol A-type epoxy resin as the hydroxyl group-containing epoxy resin (b2) exhibited excellent laminate strength and moldability.
[0109] On the other hand, Comparative Example 1 does not have the partial structure represented by general formula (1), so the curing reaction proceeds insufficiently. When the amount of adhesive applied is reduced and the curing period is shortened to two days, the laminate strength and moldability are not satisfactory. Comparative Examples 5 and 6 correspond to examples of JP 2018-110086 A, and like Comparative Example 1, do not have the partial structure represented by general formula (1). Therefore, when the amount of adhesive applied is reduced and the curing period is shortened to two days, the curing reaction proceeds insufficiently, and satisfactory adhesive performance cannot be achieved. Comparative Example 2, in which the amount of the partial structure represented by general formula (1) exceeds 12.0% by mass, has too high an affinity with water, so it easily traps moisture in the air and cannot achieve satisfactory moist heat resistance. Furthermore, Comparative Example 3, in which the amount of polyol (B) is less than 20%, results in an adhesive layer that is too rigid, making it impossible to achieve both adhesive strength and moldability. In Comparative Example 4, in which the amount of polyol (B) exceeds 60%, the urethane concentration in the adhesive layer decreases, resulting in a decrease in the cohesive strength of the adhesive. Furthermore, affinity with the substrate also decreases, resulting in failure to achieve satisfactory adhesive strength and moist heat resistance. Comparative Example 7 contains a hydroxyl group-containing epoxy resin (b2) but does not contain a polyester polyol (b1), resulting in a decrease in the flexibility of the adhesive layer. Therefore, even when the amount of adhesive applied is reduced and the curing period is shortened to two days, it is not possible to achieve both moldability and moist heat resistance of the molded product.
[0110] This application claims priority based on Japanese Patent Application No. 2023-087150, filed May 26, 2023, the disclosure of which is incorporated herein by reference in its entirety.
[0111] (1): Outer resin film layer (2): Outer adhesive layer (3): Metal foil layer (4): Inner adhesive layer (5): Heat seal layer
Claims
1. An adhesive for packaging materials for electrical storage devices, comprising a polyisocyanate (A) and a polyol (B), wherein the polyol (B) comprises a polyester polyol (b1), the polyol (B) accounts for 20 to 60 mass% based on the mass of the polyisocyanate (A), and the adhesive for packaging materials for electrical storage devices comprises a partial structure represented by the following general formula (1) in an amount of 0.5 to 12.0 mass% based on the solid content mass of the adhesive: General formula (1): [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.] 2. The adhesive for packaging materials for storage devices according to claim 1, wherein the polyisocyanate (A) comprises a reaction product of a polyisocyanate and a polyol including a polyester polyol (a2).
3. The adhesive for packaging materials for storage devices according to claim 1, wherein the polyisocyanate (A) comprises a reaction product of a polyisocyanate including an adduct (a1) of an aromatic polyisocyanate and a polyol including a polyester polyol (a2).
4. An adhesive for packaging materials for storage devices according to claim 2 or 3, wherein the polyhydric alcohol which is a component of the polyester polyol (a2) contains 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by general formula (1) per 100 mol % of the polyhydric alcohol.
5. An adhesive for packaging materials for electric storage devices according to any one of claims 1 to 3, wherein the polyol (B) further contains a hydroxyl group-containing epoxy resin (b2) in a range of 5 to 50 mass % based on the mass of the polyol (B).
6. The adhesive for packaging materials for storage battery devices according to claim 5, wherein the hydroxyl-containing epoxy resin (b2) is a bisphenol A type epoxy resin.
7. A packaging material for an electricity storage device having a configuration in which at least an outer layer resin film layer, an outer layer adhesive layer, a metal foil layer, an inner layer adhesive layer and a heat seal layer are laminated in that order, wherein the outer layer adhesive layer is a cured product of the adhesive for electricity storage device packaging materials described in any one of claims 1 to 3.
8. A container for an electricity storage device formed from the electricity storage device packaging material according to claim 7, in which the outer resin film layer forms a convex surface and the heat seal layer forms a concave surface.
9. An electricity storage device comprising the container for an electricity storage device according to claim 8.
Citation Information
Patent Citations
Polyisocyanate curing agent and polyurethane coating composition and polyurethane adhesive composition using the same
JP1994199987A
Packing material for electronic parts
JP2002187233A
Packing material for battery case and battery case molded with packing material
JP2005063685A
Covering material for lithium ion battery
JP2011187385A
Lithium ion secondary battery outer packaging material
JP2014060013A