Non-aqueous electrolyte secondary battery
The non-aqueous electrolyte secondary battery addresses the challenge of high capacity and rapid charging by employing a multilayer negative electrode structure with optimized porosity and density ratios and carboxymethylcellulose content, enhancing liquid circulation and capacity retention.
Patent Information
- Application Number
- PCT/JP2024/019401
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-27
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional non-aqueous electrolyte secondary batteries face challenges in achieving both high capacity and good rapid charging cycle characteristics, with capacity retention rates decreasing due to poor liquid circulation in the negative electrode active material layer during rapid charging.
A non-aqueous electrolyte secondary battery design featuring a negative electrode with a multilayer structure, where the first and second negative electrode active material layers have specific porosity and density ratios, and contain carboxymethylcellulose or its salt, improving liquid circulation and rapid charging cycle characteristics.
The battery achieves improved capacity retention rates and excellent rapid charging cycle characteristics by enhancing liquid circulation within the negative electrode active material layer, significantly exceeding previous performance expectations.
Smart Images

Figure JP2024019401_05122024_PF_FP_ABST
Abstract
Description
Nonaqueous electrolyte secondary battery
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery.
[0002] In recent years, non-aqueous electrolyte secondary batteries such as lithium ion batteries have been widely used in applications requiring high capacity, such as automotive applications and power storage applications. Furthermore, non-aqueous electrolyte secondary batteries are required to have various performance characteristics, such as rapid charging performance and good cycle characteristics. Because electrodes, which are the main components of batteries, have a significant impact on these performance characteristics, many studies have been conducted on electrodes. For example, Patent Document 1 discloses a negative electrode having a two-layer structure in which the negative electrode active material layer has a higher porosity on the surface side of the negative electrode than on the layer on the negative electrode current collector side, with the aim of achieving high capacity.
[0003] Japanese Patent Application Laid-Open No. 2003-77463
[0004] Conventionally, methods for increasing the capacity of batteries have been proposed, such as using a silicon-containing material with a high theoretical capacity density as the negative electrode active material or increasing the packing density of the negative electrode active material. However, batteries using such methods suffer from a significant capacity loss during rapid charge cycles. Achieving both high capacity and good rapid charge cycle characteristics is an important challenge. Conventional technologies, including those described in Patent Document 1, still have significant room for improvement in achieving both high capacity and good rapid charge cycle characteristics.
[0005] A non-aqueous electrolyte secondary battery according to the present disclosure is a non-aqueous electrolyte secondary battery including an electrode assembly including a positive electrode, a negative electrode, and a separator, and a non-aqueous electrolyte, wherein the negative electrode has a negative electrode current collector, a first negative electrode active material layer provided on the negative electrode current collector, and a second negative electrode active material layer provided on the negative electrode current collector via the first negative electrode active material layer, and the first and second negative electrode active material layers contain negative electrode active material particles and carboxymethyl cellulose or a salt thereof, and the first negative electrode active material layer is a a ratio (S2 / S1) of the interparticle porosity (S2) of the second negative electrode active material layer to the interparticle porosity (S1) of the material layer is 1.1 or more and 2.0 or less; a ratio (D2 / D1) of the density (D2) of the second negative electrode active material layer to the density (D1) of the first negative electrode active material layer is 0.9 or more and 1.1 or less; and a degree of etherification of carboxymethyl cellulose or a salt thereof contained in the first and second negative electrode active material layers is 0.7 or more and 1.8 or less.
[0006] According to the nonaqueous electrolyte secondary battery according to the present disclosure, the capacity retention rate during rapid charge cycles can be improved, and for example, both high capacity and good rapid charge cycle characteristics can be achieved.
[0007] 1 is a cross-sectional view of a non-aqueous electrolyte secondary battery according to an embodiment of the present invention;
[0008] As described above, it is important to improve the capacity retention rate during rapid charge cycles while increasing the capacity of batteries. In particular, for automotive batteries, there is a strong demand for high capacity and minimal capacity loss during repeated rapid charge cycles, i.e., excellent rapid charge cycle characteristics. However, in high-capacity batteries, the electrolyte does not sufficiently penetrate into the negative electrode active material layer during rapid charge, which tends to result in poor liquid circulation. Therefore, repeated rapid charge cycles are thought to accelerate deterioration of the negative electrode and significantly decrease capacity.
[0009] As a result of extensive research into the above-mentioned problems, the inventors have found that excellent rapid charge cycle characteristics can be obtained by using a multilayer negative electrode active material layer, setting the ratio (S2 / S1) of the interparticle porosity (S2) of the second negative electrode active material layer on the negative electrode surface side to the interparticle porosity (S1) of the first negative electrode active material layer on the negative electrode current collector side to be 1.1 or more and 2.0 or less, and setting the degree of etherification of carboxymethyl cellulose or a salt thereof contained in the negative electrode active material layer to be 0.7 or more and 1.8 or less. The application of this configuration is believed to effectively improve the liquid circulation of the negative electrode, thereby achieving a much greater improvement in rapid charge cycle characteristics than expected.
[0010] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations obtained by selectively combining the respective components of the multiple embodiments and variations described below are included within the scope of the present disclosure.
[0011] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical outer can 16 with a bottom is exemplified as a nonaqueous electrolyte secondary battery, but the outer can of the battery is not limited to a cylindrical outer can. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery having a prismatic outer can, a coin battery having a coin-shaped outer can, or a laminate battery having an outer can made of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, and may be a laminated type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween.
[0012] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 is a cylindrical battery including an electrode assembly 14, a nonaqueous electrolyte, a cylindrical outer can 16 with a bottom that houses the electrode assembly 14 and the nonaqueous electrolyte, and a sealing member 17 that closes the opening of the outer can 16. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The outer can 16 has a groove 22 formed in its sidewall, and the sealing member 17 is supported by the groove 22 and closes the opening of the outer can 16. Hereinafter, for convenience of explanation, the sealing member 17 side of the nonaqueous electrolyte secondary battery 10 is referred to as the top, and the bottom side of the outer can 16 is referred to as the bottom.
[0013] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as
[0014] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all long, strip-like bodies that are spirally wound and alternately stacked in the radial direction of the electrode assembly 14. The negative electrode 12 is formed to be slightly larger than the positive electrode 11 in order to prevent lithium precipitation. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal and width directions. The separator 13 is formed to be at least slightly larger than the positive electrode 11, and, for example, two separators 13 are arranged to sandwich the positive electrode 11. The electrode assembly 14 has a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the outer can 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, and the outer can 16 serves as the negative electrode terminal.
[0016] The negative electrode 12 is disposed on the outer peripheral surface of the electrode body 14, and an exposed portion may be provided in which the surface of the negative electrode current collector 30 (see FIG. 2 described later) constituting the negative electrode 12 is exposed. In this case, the exposed portion may be in contact with the inner peripheral surface of the outer can 16, and the negative electrode 12 and the outer can 16 may be electrically connected.
[0017] A gasket 28 is provided between the outer can 16 and the sealing body 17, ensuring airtightness inside the battery and preventing electrical contact between the outer can 16 and the sealing body 17. The outer can 16 has a groove 22 formed on its side surface that protrudes inward and supports the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the outer can 16 by the groove 22 and the open end of the outer can 16 that is crimped to the sealing body 17.
[0018] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0019] The positive electrode 11, the negative electrode 12, and the separator 13 that constitute the electrode assembly 14, with the negative electrode 12 being particularly described in detail below.
[0020] [Positive Electrode] The positive electrode 11 includes a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. The positive electrode current collector can be a foil of a metal stable within the potential range of the positive electrode 11, such as aluminum, an aluminum alloy, stainless steel, or titanium, or a film with such a metal disposed on its surface. The positive electrode active material layer contains a positive electrode active material, a conductive agent, and a binder, and is preferably provided on both sides of the positive electrode current collector except for the portion where the positive electrode lead 21 is connected. A protective layer containing inorganic particles and a binder may be provided between the positive electrode current collector and the positive electrode active material layer, or on the positive electrode active material layer. The positive electrode 11 can be fabricated, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, and a binder to the positive electrode current collector, drying the coating, and then compressing it to form positive electrode active material layers on both sides of the positive electrode current collector.
[0021] The positive electrode active material uses a lithium transition metal composite oxide containing transition metal elements such as Ni, Co, and Mn. Examples of metal elements contained in the lithium transition metal composite oxide include Ni, Co, Mn, Al, Be, B, Na, Mg, Si, K, Ca, Sc, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Y, Zr, Nb, Mo, In, Sn, Sb, Ba, Ta, W, Pb, and Bi. Among these, it is preferable to contain at least one of Ni, Co, and Mn. Examples of suitable composite oxides include lithium transition metal composite oxides containing Ni, Co, and Mn, and lithium transition metal composite oxides containing Ni, Co, and Al. One type of lithium transition metal composite oxide may be used alone, or multiple types may be used in combination.
[0022] The lithium transition metal composite oxide has, for example, a layered rock salt structure. Examples of the layered rock salt structure include a layered rock salt structure belonging to the space group R-3m and a layered rock salt structure belonging to the space group C2 / m. Among these, a layered rock salt structure belonging to the space group R-3m is preferred from the viewpoint of high capacity and stability of the crystal structure. The density of the positive electrode active material layer is 3.3 g / cm from the viewpoint of high capacity. 3An example of the upper limit of the density of the positive electrode active material layer is 3.8 g / cm 3 is.
[0023] Examples of the conductive agent contained in the positive electrode active material layer include carbon black such as acetylene black and ketjen black, graphite, carbon nanotubes (CNT), carbon nanofibers, graphene, metal fibers, metal powder, conductive whiskers, etc. One type of conductive agent may be used alone, or multiple types may be used in combination.
[0024] Examples of binders contained in the positive electrode active material layer include fluorine-containing resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), olefin resins such as polyethylene, polypropylene, ethylene-propylene-isoprene copolymer, and ethylene-propylene-butadiene copolymer, and acrylic resins such as polyacrylonitrile (PAN), polyimide, polyamide, and ethylene-acrylic acid copolymer. These resins may also be used in combination with carboxymethyl cellulose (CMC) or a salt thereof, polyethylene oxide (PEO), or the like. One type of binder may be used alone, or multiple types may be used in combination.
[0025] [Negative Electrode] Fig. 2 is a cross-sectional view of the negative electrode 12 cut in the longitudinal direction. As shown in Fig. 2, the negative electrode 12 has a negative electrode current collector 30 and a negative electrode active material layer 33 provided on the negative electrode current collector 30. The negative electrode active material layer 33 has a multi-layer structure and includes a first negative electrode active material layer 31 provided on the negative electrode current collector 30 and a second negative electrode active material layer 32 provided on the negative electrode current collector 30 via the first negative electrode active material layer 31. As will be described in detail later, the ratio (S2 / S1) of the inter-particle porosity (S2) of the second negative electrode active material layer 32 to the inter-particle porosity (S1) of the first negative electrode active material layer 31 is 1.1 or more and 2.0 or less, and the ratio (D2 / D1) of the density (D2) of the second negative electrode active material layer 32 to the density (D1) of the first negative electrode active material layer 31 is 0.9 or more and 1.1 or less.
[0026] The negative electrode current collector 30 can be a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper, a copper alloy, stainless steel, nickel, or a nickel alloy, or a film having such a metal disposed on its surface. The negative electrode active material layer 33 contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode current collector 30 except for the portion where the negative electrode lead 21 is connected. A protective layer containing inorganic particles and a binder may be provided between the negative electrode current collector 30 and the negative electrode active material layer 33 or on the negative electrode active material layer 33. The negative electrode 12 can be produced, for example, by sequentially applying two types of negative electrode mixture slurries containing a negative electrode active material and a binder to the surface of the negative electrode current collector 30, drying the coating, and then compressing it to form negative electrode active material layers 33 containing two layers on both sides of the negative electrode current collector 30.
[0027] The negative electrode active material generally uses a carbon material that reversibly absorbs and releases lithium ions. The negative electrode active material may be an element that alloys with Li, such as silicon (Si) or tin (Sn), or a material containing such an element. Among these, a Si-containing material containing Si is preferred. Furthermore, lithium titanate, which has a higher charge / discharge potential relative to metallic lithium than carbon materials, may also be used as the negative electrode active material. One type of negative electrode active material may be used alone, or multiple types may be used in combination. The negative electrode active material layer 33 may contain a conductive agent such as CNT. The conductive agent may be the same as that used in the positive electrode 11.
[0028] The carbon material functioning as the negative electrode active material is, for example, at least one selected from the group consisting of natural graphite, artificial graphite, soft carbon, and hard carbon. Among them, graphite is preferably used as the carbon material. The graphite may be artificial graphite such as massive artificial graphite (MAG) or graphitized mesophase carbon microbeads (MCMB), natural graphite such as flake graphite, massive graphite, or amorphous graphite, or a mixture thereof.
[0029] The volume-based D50 of graphite is, for example, 1 μm or more and 30 μm or less, preferably 5 μm or more and 25 μm or less. The D50 of the negative electrode active material particles means the particle size at which the cumulative frequency of the particles in the volume-based particle size distribution is 50% from the smallest particle size. The particle size distribution of the lithium transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II manufactured by Microtrac-Bell Co., Ltd.) with water as the dispersion medium.
[0030] The Si-containing material functioning as the negative electrode active material may be any material containing Si, and examples thereof include silicon alloys, silicon compounds, and Si-containing composite materials. Among these, Si-containing composite materials are preferred. The D50 of the Si-containing material is generally smaller than the D50 of graphite. The volume-based D50 of the Si-containing material is, for example, 1 μm or more and 20 μm or less, or 1 μm or more and 15 μm or less.
[0031] A suitable Si-containing material (composite material) is a composite particle containing an ion-conducting phase and a Si phase dispersed in the ion-conducting phase. An example of a suitable ion-conducting phase is at least one selected from the group consisting of a silicate phase, a carbon phase, a silicide phase, and a silicon oxide phase. The silicide phase is a phase of a compound consisting of Si and an element more electropositive than Si, such as NiSi, Mg 2 Si, TiSi 2 The Si phase is formed by dispersing Si in the form of fine particles, and the ion-conducting phase is a continuous phase formed by an aggregation of particles that are finer than the Si phase.
[0032] The composite material may have a conductive layer covering the surface of the ion-conducting phase. The conductive layer is made of a material with higher conductivity than the ion-conducting layer and forms a good conductive path in the negative electrode active material layer 33. The conductive layer is, for example, a carbon coating made of a conductive carbon material. Examples of the conductive carbon material that can be used include carbon black such as acetylene black and ketjen black, graphite, and amorphous carbon (amorphous carbon) with low crystallinity.
[0033] An example of a suitable Si-containing composite material has a sea-island structure in which fine Si is dispersed almost uniformly in an amorphous silicon oxide phase, and the overall structure is represented by the general formula SiO x The silicon oxide may be mainly composed of silicon dioxide. The silicon oxide phase may be doped with Li. The oxygen to Si content (x) is, for example, 0.5≦x<2.0, and preferably 0.8≦x≦1.5.
[0034] Another example of a suitable Si-containing composite material is a composite particle having a sea-island structure in which fine Si particles are uniformly dispersed in an amorphous silicate phase. A suitable silicate phase is a lithium silicate phase containing Li. The lithium silicate phase can be, for example, a compound represented by the general formula Li 2z SiO (2+z) (0<z<2). The lithium silicate phase contains Li 4 SiO 4 It is preferable that (Z=2) is not included. 4 SiO 4 is an unstable compound and reacts with water to become alkaline, which may cause Si to change and lead to a decrease in charge / discharge capacity. The lithium silicate phase is considered to be a suitable phase for Li, from the viewpoints of stability, productivity, Li ion conductivity, etc. 2 SiO 3 (Z=1) or Li 2 Si 2 O 5 It is preferable that (Z=1 / 2) is used as the main component.
[0035] Another example of a suitable Si-containing composite material is composite particles having a sea-island structure in which fine Si particles are substantially uniformly dispersed in a carbon phase. The carbon phase is preferably an amorphous carbon phase. The carbon phase may contain a crystalline phase component, but preferably contains a larger amount of amorphous phase components. The composite material may contain particles whose ion-conducting phase is an amorphous carbon phase. The amorphous carbon phase is, for example, composed of a carbon material having an average interplanar spacing of (002) planes of more than 0.34 nm as measured by X-ray diffraction. The composite material containing a carbon phase may or may not have a conductive layer separate from the carbon phase.
[0036] As described above, the negative electrode active material layer 33 has, in order from the negative electrode current collector 30 side, a first negative electrode active material layer 31 and a second negative electrode active material layer 32. The first negative electrode active material layer 31 and the second negative electrode active material layer 32 are layers with different interparticle porosities, and the interparticle porosity (S2) of the second negative electrode active material layer 32 is greater than the interparticle porosity (S1) of the first negative electrode active material layer 31. The negative electrode active material layer 33 may include a third negative electrode active material layer as long as the object of the present disclosure is not impaired, but preferably has a two-layer structure consisting of the first negative electrode active material layer 31 and the second negative electrode active material layer 32.
[0037] The first negative electrode active material layer 31 and the second negative electrode active material layer 32 contain negative electrode active material particles and carboxymethyl cellulose (CMC) or a salt thereof. Each negative electrode active material layer preferably contains graphite and Si or a Si-containing material as the negative electrode active material particles. In particular, a combination of graphite and a Si-containing material is preferred. This facilitates achieving both high capacity and good cycle characteristics. The graphite content is, for example, 80% to 99% by mass, 85% to 98% by mass, or 90% to 97% by mass of the total mass of the negative electrode active material. The Si-containing material content is, for example, 1% to 20% by mass, 2% to 15% by mass, or 3% to 10% by mass of the total mass of the negative electrode active material.
[0038] The CMC or salt thereof contained in the first negative electrode active material layer 31 and the second negative electrode active material layer 32 functions as a binder and also as a thickener for imparting an appropriate viscosity to the negative electrode mixture slurry. As will be described in detail later, CMC or a salt thereof having an etherification degree of 0.7 or more and 1.8 or less improves the liquid permeability of the negative electrode active material layer and contributes to improving the rapid charge cycle characteristics. Furthermore, each negative electrode active material layer preferably contains a binder other than CMC or a salt thereof. Each negative electrode active material layer may contain the same binder as that in the positive electrode 11, but preferably contains styrene-butadiene rubber (SBR).
[0039] The content of the negative electrode active material is, for example, 90% by mass or more and 99.5% by mass or less, or 95% by mass or more and 99% by mass or less, relative to the mass of the negative electrode active material layer 33. The content of CMC or a salt thereof is, for example, 0.1% by mass or more and 2.5% by mass or less, or 0.5% by mass or more and 1.5% by mass or less, relative to the mass of the negative electrode active material layer 33. In this case, it becomes easy to achieve both high capacity and good cycle characteristics.
[0040] The thickness of the negative electrode active material layer 33 is determined by observing a cross section of the active material layer using a scanning electron microscope (SEM). The thickness of the negative electrode active material layer 33 is generally uniform, but unless otherwise specified, "thickness" in this specification refers to the average thickness. The thicknesses of the first negative electrode active material layer 31 and the second negative electrode active material layer 32 may be different from each other, but are preferably approximately the same from the viewpoint of achieving both high capacity and good cycle characteristics. When the negative electrode active material layer 33 has a two-layer structure, the thickness of the first negative electrode active material layer 31 is preferably 30% to 70% of the total thickness of the negative electrode active material layer 33, and more preferably 40% to 60%.
[0041] The densities (D1, D2) of the first negative electrode active material layer 31 and the second negative electrode active material layer 32 are set to 1.3 g / cm 3 from the viewpoint of increasing capacity. 3 More preferably, 1.4 g / cm 3 The upper limit of the density (D1, D2) is, for example, 2.0 g / cm 3 From the viewpoint of achieving both high capacity and good cycle characteristics, an example of a suitable range of the densities (D1, D2) is 1.3 g / cm 3 2.0g / cm or more 3 The following is the result.
[0042] The ratio (D2 / D1) of the density (D2) of the second negative electrode active material layer 32 to the density (D1) of the first negative electrode active material layer 31 is 0.9 or more and 1.1 or less. The densities (D1, D2) may be different from each other, but from the viewpoint of achieving high capacity, it is preferable that the difference between the densities (D1, D2) is small, and the ratio (D2 / D1) is adjusted to satisfy 0.9 or more and 1.1 or less. For example, if the density (D2) of the second negative electrode active material layer 32 is significantly reduced, the electrolyte circulation property is improved, but in that case, the capacity will be significantly reduced. The negative electrode 12 can improve the electrolyte circulation property and achieve excellent rapid charge cycle characteristics without significantly reducing the density (D2).
[0043] [Method for calculating density of negative electrode active material layer] The thicknesses of the first negative electrode active material layer 31 and the second negative electrode active material layer 32 are measured from a cross-sectional SEM image (the same image as that used to determine the interparticle porosity) of the negative electrode active material layer 33. Then, the mass of the negative electrode active material layer per unit area is determined, and the density (mass of the negative electrode active material layer per unit area × 100 / (unit area + thickness of the negative electrode active material layer)) is calculated.
[0044] The interparticle porosity (S2) of the second negative electrode active material layer 32 is higher than the interparticle porosity (S1) of the first negative electrode active material layer 31. The interparticle porosity of the active material layer refers to the ratio of the area of the voids between particles of the negative electrode active material to the cross-sectional area of the active material layer, and voids within the active material particles are not counted in the interparticle porosity. Increasing the interparticle porosity (S2) of the second negative electrode active material layer 32 improves the permeability of the electrolyte throughout the entire negative electrode active material layer 33.
[0045] As described above, the ratio (S2 / S1) of the interparticle porosity (S2) of the second negative electrode active material layer 32 to the interparticle porosity (S1) of the first negative electrode active material layer 31 is set to 1.1 or more and 2.0 or less. The ratio (S2 / S1) is more preferably 1.1 or more and 1.7 or less, and particularly preferably 1.2 or more and 1.5 or less. In this case, it becomes easy to achieve both high capacity and good cycle characteristics. The negative electrode 12 is designed to increase the interparticle porosity (S2) while suppressing a decrease in the density (D2) of the second negative electrode active material layer 32.
[0046] A specific example of a method for forming the first negative electrode active material layer 31 and the second negative electrode active material layer 32 is to use particles A with many internal voids as the graphite particles that make up the first negative electrode active material layer 31, and particles B with few internal voids as the graphite particles that make up the second negative electrode active material layer 32. In this way, by adjusting the internal voids of particles A and B, the interparticle void ratios (S1, S2) can be controlled within a desired range. Alternatively, the interparticle void ratios (S1, S2) can also be controlled by changing the particle size distribution of the negative electrode active material in each active material layer.
[0047] Artificial graphite can be synthesized, for example, by crushing coke to a particle size of 12 μm to 20 μm, adding pitch that functions as a binder to agglomerate the crushed particles, and firing at a high temperature of 2500° C. or higher. In this process, the amount of voids inside the particles can be controlled by the degree of crushing of the coke, the amount of pitch added, whether or not agglomerates are formed, etc. Generally, increasing the particle size of the crushed coke reduces the internal voids, and increasing the amount of pitch added increases the internal voids.
[0048] The interparticle porosity (S1) of the first negative electrode active material 31 is preferably 2.5% or more and 25% or less. The interparticle porosity (S2) of the second negative electrode mixture layer 32 is preferably 3% or more and 50% or less. The ratio (S2 / S1) is controlled to be 1.1 or more and 2.0 or less.
[0049] [Method for Measuring Interparticle Porosity of Negative Electrode Active Material Layer] The interparticle porosity (S2 / S1) of each negative electrode active material layer is determined by the following method. (1) A cross section of the negative electrode active material layer 33 is exposed using an ion milling device (IM4000PLUS, manufactured by Hitachi High-Tech Corporation), and a backscattered electron image of the exposed cross section of the negative electrode active material layer 33 is taken using an SEM at 800x magnification. (2) The obtained cross-sectional image is imported into a computer, and portions of the first negative electrode active material layer 31 and the second negative electrode active material layer 32 are cut out. (3) The cut-out cross-sectional image is binarized using image analysis software to obtain a binarized image in which the particle cross sections of the negative electrode active material in the cross-sectional image are converted to white and the interparticle voids are converted to black. The image analysis software used is ImageJ manufactured by the National Institutes of Health. Note that the binarization is performed so that voids inside the particles are white. (4) The interparticle porosity (area of black interparticle voids × 100 / (area of black interparticle voids + area of white negative electrode active material particles)) is calculated from the ratio of the white and black areas. Note that the calculation of the interparticle porosity uses the electrode plate of a battery that has undergone initial low-rate cycle measurement (see Examples described later).
[0050] As described above, the CMC or a salt thereof contained in the first negative electrode active material layer 31 and the second negative electrode active material layer 32 has a degree of etherification of 0.7 or more and 1.8 or less. In this case, the permeability of the electrolyte in the negative electrode active material layer is improved, and the rapid charge cycle characteristics are improved. CMC is a water-soluble polymer in which some of the hydroxyl groups in the cellulose skeleton are substituted with carboxymethyl groups. The degree of substitution by carboxymethyl groups is expressed as the degree of etherification.
[0051] The first negative electrode active material layer 31 and the second negative electrode active material layer 32 preferably contain a salt in which the carboxyl groups of CMC have been neutralized. Examples of CMC salts include sodium salt, ammonium salt, lithium salt, potassium salt, rubidium salt, and cesium salt, with sodium salt (CMC-Na) being preferred. CMC-Na is generally a partially neutralized salt in which some of the carboxyl groups have been neutralized. The weight-average molecular weight of CMC-Na is, for example, 200,000 or more and 1,000,000 or less, and preferably 200,000 or more and 500,000 or less.
[0052] The degree of etherification of CMC-Na is more preferably 0.8 or more and 1.4 or less, and particularly preferably 0.9 or more and 1.2 or less. If the degree of etherification of CMC-Na is too high, it is thought that the adhesion of the negative electrode active material layer 33 to the negative electrode current collector 30 will decrease, and although the permeability of the electrolyte will improve, the effect of improving the cycle characteristics may not be obtained. If the degree of etherification is within the above range, the rapid charge cycle characteristics can be greatly improved.
[0053] The degree of etherification of the CMC or a salt thereof contained in the second anode active material layer 32 is preferably higher than the degree of etherification of the CMC or a salt thereof contained in the first anode active material layer 31. In this case, the effect of improving the rapid charge cycle characteristics becomes more significant. The ratio (DS2 / DS1) of the degree of etherification (DS2) of the CMC or a salt thereof contained in the second anode active material layer 32 to the degree of etherification (DS1) of the CMC or a salt thereof contained in the first anode active material layer 31 is, for example, 1.5 or more and 2.3 or less.
[0054] [Method for measuring the degree of etherification of carboxymethyl cellulose] Approximately 1 g of sample is weighed into a flask and dissolved in an appropriate amount of pure water. Approximately 5 mL of 0.05 M (N / 10) aqueous sulfuric acid is added using a pipette, boiled for several minutes, and cooled. After this, phenolphthalein indicator is added and titration is performed with 0.1 M (N / 10) aqueous sodium hydroxide. The alkalinity is calculated using the following formula: Alkalinity = 5 x F' - mL of 0.1 M (N / 10) aqueous sodium hydroxide x F / sample (g of anhydrous equivalent), where F is the factor of the 0.1 M (N / 10) aqueous sodium hydroxide solution, F' is the factor of the 0.05 M (N / 10) aqueous sulfuric acid solution, and approximately 1 g of sample is weighed out and placed in a crucible and incinerated at 500°C or higher. After cooling, the crucible is transferred to a beaker, an appropriate amount of pure water is added, and then 50 mL of 0.05 M (N / 10) aqueous sulfuric acid is accurately added and boiled for several tens of minutes. After cooling, add phenolphthalein indicator and titrate with 0.1M (N / 10) aqueous sodium hydroxide solution. A blank titration is carried out in the same manner using this method. The degree of etherification is calculated using the following formula: A = (blank titration mL - sample titration mL) x F / sample (anhydrous equivalent g) - alkalinity F: Factor of 0.1M (N / 10) aqueous sodium hydroxide solution The above A refers to the number of mL of 0.05M (N / 10) aqueous sulfuric acid consumed to neutralize the bound sodium in 1 g of sample. The above A is used to calculate the degree of etherification as follows: Degree of etherification (DS) = 162A / (10000 - 80A)
[0055] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of porous sheets include microporous thin films, woven fabrics, and nonwoven fabrics. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. The separator 13 may have, for example, a multi-layer structure including a thermoplastic resin layer such as polyolefin and a cellulose fiber layer, a two-layer structure of polyethylene (PE) / polypropylene (PP), or a three-layer structure of PE / PP / PE. A filler layer including an inorganic filler or a layer of a highly heat-resistant resin such as aramid resin may be provided on the surface of the separator 13.
[0056] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0057] Experimental Example 1 [Fabrication of Positive Electrode] Aluminum-containing lithium nickel cobalt oxide (LiNi) was used as the positive electrode active material. 0.88 Co 0.09 Al 0.03 O 2 ) was used. A positive electrode active material, graphite, and polyvinylidene fluoride were mixed in a solid content mass ratio of 100:1:0.9, and a positive electrode mixture slurry was prepared using N-methyl-2-pyrrolidone (NMP) as a dispersion medium. Next, the positive electrode mixture slurry was applied to both sides of a positive electrode current collector made of aluminum foil (thickness 15 μm) by a doctor blade method, and the coating was dried and compressed using a rolling roller. Thereafter, the positive electrode current collector was cut to a predetermined electrode size, and a positive electrode in which a positive electrode active material layer was formed on both sides of the positive electrode current collector was obtained.
[0058] [Synthesis of Graphite Particles B] Coke (precursor) was pulverized to a D50 of 13 μm, and pitch (binder) was added to aggregate the particles to a D50 of 18 μm. The aggregates were calcined at a temperature of 2800° C. to graphitize them, and then sieved to obtain graphite particles B having a D50 of 23 μm.
[0059] [Synthesis of Graphite Particles A] Coke was pulverized to a D50 of 17 μm, and pitch was added to agglomerate the agglomerate. The agglomerate was isotropically compressed to a density of 1.6 g / cm 3 1.9g / cm or more 3 The resulting block-shaped body was fired at a temperature of 2800°C to graphitize it, and then crushed and sieved to obtain graphite particles A having a D50 of 23 µm. Note that by using a larger amount of pitch in the synthesis of graphite particles A than in the synthesis of graphite particles B, graphite particles A having a higher porosity than graphite particles B were obtained.
[0060] [Fabrication of Negative Electrode] As the negative electrode active material, graphite particles A and SiO XA mixture was used in which a Si-containing material represented by (X = 1) was mixed at a mass ratio of 95:5. The negative electrode active material, a dispersion of styrene butadiene rubber (SBR), and a sodium salt of carboxymethyl cellulose (CMC-Na) having a degree of etherification (DS) of 1.0 were mixed at a solids mass ratio of 100:1:1, and negative electrode mixture slurry A was prepared using water as the dispersion medium. Similarly, negative electrode mixture slurry B was prepared using graphite particles B instead of graphite particles A.
[0061] Next, the negative electrode mixture slurry A was applied to both sides of a negative electrode current collector made of copper foil by a doctor blade method to form a first coating film. After the first coating film was dried, the negative electrode mixture slurry B was applied to the first coating film to form a second coating film, and the second coating film was dried. At this time, the application amount of each negative electrode mixture slurry per unit area was the same. Thereafter, the coating film was compressed using a rolling roller, and the negative electrode current collector was cut to a predetermined electrode size to obtain a negative electrode in which a two-layer structure negative electrode active material layer including a first layer and a second layer was formed on both sides of the negative electrode current collector.
[0062] The density (D1) of the first negative electrode active material layer measured by the above method is 1.59 g / cm 3 , the density (D2) of the second negative electrode active material layer is 1.49 g / cm 3 The D2 / D1 ratio was 0.94, and the S2 / S1 ratio measured by the above method was 1.39.
[0063] [Preparation of non-aqueous electrolyte] Ethylene carbonate and dimethyl carbonate were mixed at a volume ratio of 1:3 (at 25°C), and then 5 mass % of vinylene carbonate and LiPF 6 were added to the mixed solvent. 6 was added to give a concentration of 1 mol / L to obtain a non-aqueous electrolyte solution.
[0064] [Preparation of Test Cell (Non-Aqueous Electrolyte Secondary Battery)] The positive electrode, in which the positive electrode lead was welded to the positive electrode current collector, and the negative electrode, in which the negative electrode lead was welded to the negative electrode current collector, were spirally wound with a separator interposed therebetween to prepare a wound electrode assembly. Insulating plates were placed on the top and bottom of the electrode assembly, and the negative electrode lead was welded to the inner bottom of a cylindrical outer can with a bottom, and the positive electrode lead was welded to a sealing member, and the electrode assembly was then housed in the outer can. The non-aqueous electrolyte was poured into the outer can under reduced pressure, and the opening of the outer can was sealed with a sealing member via a gasket to obtain a test cell.
[0065] Example 2 A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in preparing negative electrode mixture slurries A and B, CMC-Na having a DS of 1.4 was used.
[0066] Example 3 A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in preparing negative electrode mixture slurries A and B, CMC-Na having a DS of 1.6 was used.
[0067] Example 4 A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in preparing negative electrode mixture slurries A and B, CMC-Na having a DS of 0.9 was used.
[0068] Comparative Example 1 A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in preparing negative electrode mixture slurries A and B, CMC-Na having a DS of 0.6 was used.
[0069] Comparative Example 2 A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in preparing negative electrode mixture slurries A and B, CMC-Na having a DS of 2.0 was used.
[0070] <Comparative Example 3> A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that in fabricating the negative electrode, the order of application of the negative electrode mixture slurries A and B was changed so that the negative electrode mixture slurry B was applied first. In this case, D2 / D1 was 1.02, and S2 / S1 was 0.70.
[0071] <Comparative Example 4> A negative electrode and a test cell were fabricated in the same manner as in Example 1, except that a single-layer negative electrode active material layer was formed using a slurry in which the same amounts of negative electrode mixture slurries A and B were mixed. In this case, the density of the negative electrode active material layer was 1.51 g / cm 3 It was.
[0072] The performance of each test cell in the Examples and Comparative Examples was evaluated by the following method, and the evaluation results, along with the physical properties of the negative electrode, are shown in Table 1. The capacity retention rates shown in Table 1 are relative values when the capacity retention rate of Example 1 is set to 100, and a higher value indicates better rapid charge cycle characteristics.
[0073] [Initial Low-Rate Cycle Conditions] In a temperature environment of 25°C, each test cell of the Examples and Comparative Examples was subjected to constant current charging at 0.2 C (920 mA) until the cell voltage reached 4.2 V, and then constant voltage charging at 4.2 V up to C / 50. Subsequently, constant current discharging was performed at 0.2 C until the cell voltage reached 2.5 V. After repeating this charge / discharge cycle for 5 cycles, the cell was disassembled, the negative electrode was removed, and the interparticle porosity was determined by the method described above.
[0074] [Evaluation of rapid charge cycle characteristics (capacity retention)] In a temperature environment of 25°C, each test cell of the examples and comparative examples was subjected to constant current charging at 1 C (4600 mA) until the cell voltage reached 4.2 V, and then constant voltage charging at 4.2 V up to C / 50. Thereafter, constant current discharging was performed at 0.5 C until the cell voltage reached 2.5 V. This charge / discharge cycle was repeated 100 times, and the capacity retention was calculated using the following formula: Capacity retention = (discharge capacity at 100th cycle / discharge capacity at 1st cycle) × 100
[0075]
[0076] As shown in Table 1, the test cells of the examples have a capacity equivalent to that of the test cells of the comparative examples, while exhibiting a higher capacity retention rate during rapid charge cycles than the test cells of the comparative examples. When a negative electrode having a single-layer structure negative electrode active material layer is used, or when a negative electrode in which the interparticle porosity ratio (S2 / S1) of each negative electrode active material layer is less than 1.1 is used, the capacity retention rate is significantly lower than that of the test cells of the examples (see Comparative Examples 3 and 4). Furthermore, the test cells of Comparative Examples 1 and 2, which differ from the test cells of the examples only in the degree of etherification (DS) of CMC-Na contained in the negative electrode active material layer, do not exhibit the excellent rapid charge cycle characteristics of the test cells of the examples.
[0077] The present disclosure will be further described by the following embodiments. Configuration 1: A non-aqueous electrolyte secondary battery including an electrode assembly including a positive electrode, a negative electrode, and a separator, and a non-aqueous electrolyte, wherein the negative electrode has a negative electrode current collector, a first negative electrode active material layer provided on the negative electrode current collector, and a second negative electrode active material layer provided on the negative electrode current collector via the first negative electrode active material layer, the first and second negative electrode active material layers containing negative electrode active material particles and carboxymethyl cellulose or a salt thereof, and interparticle spaces in the first negative electrode active material layer A nonaqueous electrolyte secondary battery, wherein a ratio (S2 / S1) of the interparticle porosity (S2) of the second negative electrode active material layer to the porosity (S1) of the first negative electrode active material layer is 1.1 or more and 2.0 or less, a ratio (D2 / D1) of the density (D2) of the second negative electrode active material layer to the density (D1) of the first negative electrode active material layer is 0.9 or more and 1.1 or less, and a degree of etherification of carboxymethyl cellulose or a salt thereof contained in the first and second negative electrode active material layers is 0.7 or more and 1.8 or less. Configuration 2: The nonaqueous electrolyte secondary battery according to Configuration 1, wherein the ratio (S2 / S1) is 1.1 or more and 1.7 or less. Configuration 3: The densities (D1, D2) of the first and second negative electrode active material layers are 1.3 g / cm or less. 3 2.0g / cm or more 3The nonaqueous electrolyte secondary battery according to Configuration 1 or 2, wherein: Configuration 4: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the first and second negative electrode active material layers contain graphite and silicon or a silicon-containing material as the negative electrode active material particles; Configuration 5: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein the carboxymethyl cellulose or a salt thereof contained in the first and second negative electrode active material layers has a weight average molecular weight of 200,000 or more and 500,000 or less; Configuration 6: The nonaqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein the carboxymethyl cellulose salt contained in the first and second negative electrode active material layers contains at least one of a sodium salt, an ammonium salt, a lithium salt, a potassium salt, a rubidium salt, and a cesium salt as the salt.
[0078] REFERENCE SIGNS LIST 10 Non-aqueous electrolyte secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 16 Outer can, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Grooved portion, 23 Internal terminal plate, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket, 30 Negative electrode current collector, 31 First negative electrode active material layer, 32 Second negative electrode active material layer, 33 Negative electrode active material layer
Claims
1. A non-aqueous electrolyte secondary battery comprising an electrode assembly including a positive electrode, a negative electrode, and a separator, and a non-aqueous electrolyte, wherein the negative electrode has a negative electrode current collector, a first negative electrode active material layer provided on the negative electrode current collector, and a second negative electrode active material layer provided on the negative electrode current collector via the first negative electrode active material layer, the first and second negative electrode active material layers contain negative electrode active material particles and carboxymethyl cellulose or a salt thereof, a ratio (S2 / S1) of an interparticle porosity (S2) of the second negative electrode active material layer to an interparticle porosity (S1) of the first negative electrode active material layer is 1.1 or more and 2.0 or less, and a ratio (D2 / D1) of a density (D2) of the second negative electrode active material layer to a density (D1) of the first negative electrode active material layer is 0.9 or more and 1.1 or less, a degree of etherification of carboxymethyl cellulose or a salt thereof contained in the first and second negative electrode active material layers is 0.7 or more and 1.8 or less.
2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the ratio (S2 / S1) is 1.1 or more and 1.7 or less.
3. The density (D1, D2) of the first and second negative electrode active material layers is 1.3 g / cm 3 2.0g / cm or more 3 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein:
4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the first and second negative electrode active material layers contain graphite and silicon or a silicon-containing material as the negative electrode active material particles.
5. The nonaqueous electrolyte secondary battery according to claim 1, wherein the weight average molecular weight of the carboxymethyl cellulose or a salt thereof contained in the first and second negative electrode active material layers is 200,000 or more and 500,000 or less.
6. The nonaqueous electrolyte secondary battery according to claim 1, wherein the carboxymethyl cellulose salt contained in the first and second negative electrode active material layers includes at least one of a sodium salt, an ammonium salt, a lithium salt, a potassium salt, a rubidium salt, and a cesium salt as a salt.
Citation Information
Patent Citations
Lithium secondary battery and its manufacturing method
JP2003077463A
Nonaqueous electrolyte secondary battery
JP2010238365A
Nonaqueous electrolyte secondary battery
JP2013073718A
Negative electrode for electricity storage devices, and electricity storage device
WO2014141403A1
Negative electrode for lithium ion secondary batteries, and lithium ion secondary battery