Porous cellulose particles and method for producing same
Cellulose porous particles with a collagen coating and optimized pore structure address the limitations of existing microcarriers by enhancing cell adhesion and resistance to shear stress, achieving efficient high-density cell culture.
Patent Information
- Application Number
- PCT/JP2024/019915
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Current microcarriers, such as Cytodex 1, lack a porous structure, limiting cell proliferation and being susceptible to shear stress during agitation culture, which reduces culture efficiency.
Development of cellulose porous particles with a large surface area, collagen coating, and specific pore structure to enhance cell adhesion and resistance to shear stress, allowing for efficient cell culture at high densities.
The cellulose porous particles with collagen coating improve cell adhesion and proliferation, especially in the early stages of culture, and reduce cell shedding during agitation, leading to high-density cell culture efficiency.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Cellulose porous particles and their manufacturing method
[0001] The present invention relates to porous cellulose particles and a method for producing the same.
[0002] In recent years, there has been a demand for efficient mass cultivation of cells, tissues, microorganisms, etc. in fields such as the production of vaccines and antibody drugs, and regenerative medicine. As a mass cultivation technique for the above cells, compared to the conventional monolayer culture method using flasks or roller bottles, which has a small culture surface area / volume ratio, the culture method using microcarriers can expand the culture surface area in a small volume while simultaneously maintaining a high cell density per culture volume, and is therefore currently widely adopted in the cultivation of anchorage-dependent cells.
[0003] A widely used microcarrier is Cytodex 1 (manufactured by Cytiva), which has a charge capacity of approximately 1.5 mmol / g and is made by modifying dextran particles with cationic diethylaminoethyl groups. However, because the particles do not have a porous structure and cells are cultured only on the surface, there is a limit to the proliferation capacity. Furthermore, when agitation culture is performed in a reactor, there is a problem that shear stress is applied to the cells, which causes them to fall off, significantly reducing the culture efficiency.
[0004] To solve the above problems, porous microcarriers with large surface areas have also been developed. Patent Document 1 below describes culture using porous cellulose particles characterized by interconnected pores with a pore size of approximately 2 μm or larger. When culturing using such porous particles, the large surface area allows efficient cell culture, and furthermore, because the cells are positioned inside the particles, they are less susceptible to shear stress during agitation culture.
[0005] Japanese Unexamined Patent Publication No. 2-208331
[0006] In the culture microcarrier using porous cellulose particles described in Patent Document 1, cells are adsorbed to the surface of the porous microcarrier by introducing a charge onto the surface of the carrier, but there is room for further improvement in cell adhesion and culture efficiency.
[0007] In view of the above-mentioned current state of the art, the problem to be solved by the present invention is to provide porous cellulose particles that have excellent cell adhesiveness and allow cells to grow efficiently.
[0008] As a result of extensive research and experimentation to solve these problems, the inventors unexpectedly discovered that by having collagen on the surface of porous cellulose particles, cells are less likely to fall off even when cultured at high density, and cell proliferation, particularly in the early stages of culture, is excellent. Based on this finding, the present invention was completed.
[0009] That is, the present invention is as follows. [1] Porous cellulose particles made of cellulose, having collagen on the surface of the porous cellulose particles, wherein the amount of collagen immobilized in a dry state is 10 μg / g or more and 25 mg / g or less (0.001 to 2.5 wt %) per gram of the porous cellulose particles. [2] The porous cellulose particles according to [1] above, having a large number of pores with an average pore size of 5 μm or more and 100 μm or less. [3] The porous cellulose particles according to [1] or [2] above, having a continuous pore structure in which adjacent pores are interconnected by openings in a membrane separating them. [4] The porous cellulose particles according to any one of [1] to [3] above, having an average particle size of 100 μm or more and 1,000 μm or less. [5] The porous cellulose particles according to any one of [1] to [4] above, having a sphericity of 0.7 or more. [6] The cellulose porous particles have a specific surface area of 0.3 m when dried. 2 / g or more 4.4m 2 / g or less. [7] The porous cellulose particle according to any of [1] to [6], wherein the amount of collagen immobilized in a dry state is 1 mg / g or more and 10 mg / g or less (0.1 to 1.0 wt %) per gram of the porous cellulose particle. [8] The porous cellulose particle according to any of [1] to [7], wherein the surface of the porous cellulose particle is modified with a cationic substituent. [9] The porous cellulose particle according to [8], wherein the cationic substituent is at least one selected from the group consisting of a primary amino group, a secondary amino group, and a tertiary amino group.
[10] The porous cellulose particle according to any of [1] to [9], wherein the charge capacity of the porous cellulose particle is 0 mmol / g or more and 5.0 mmol / g or less.
[11] The porous cellulose particle according to any of [1] to
[10] , wherein the collagen is fibrous collagen.
[12] The cellulose porous particles according to any one of [1] to
[10] above, wherein the collagen is cross-linked collagen.
[13] The cellulose porous particles according to any one of [1] to
[12] above, wherein the cellulose constituting the cellulose porous particles is cuprammonium regenerated cellulose.
[14] A method for producing the cellulose porous particles according to any one of [1] to
[13] above, comprising the following steps: a step of impregnating the cellulose porous particles with a collagen solution; a step of neutralizing the collagen solution to a pH of 6 to 8; a dehydration step of removing the collagen solution; and a drying step of drying the cellulose porous particles.
[0010] When the porous cellulose particles of the present invention are used as microcarriers, which are support bodies for cell culture, they can efficiently adsorb cells even in the early stages of culture when intercellular adhesion to the substrate is not yet fully developed. Furthermore, even when cultured at high density, cell detachment from the particles due to shear stress can be reduced, allowing cells to proliferate efficiently.
[0011] An embodiment of the present invention will be described in detail below. An embodiment of the present invention is a porous cellulose particle made of cellulose, which has collagen on the surface of the porous cellulose particle. Here, the porous cellulose particle of this embodiment has an immobilized amount of collagen in a dry state of 10 μg / g or more and 25 mg / g or less (0.001 to 2.5 wt %) per gram of the porous cellulose particle. In this specification, the "surface" in the term "porous cellulose particle surface" includes not only the outer surface of the porous cellulose particle but also the surfaces of the pores inside the particle.
[0012] The type of cellulose constituting the porous cellulose particles of this embodiment is not particularly limited, but known celluloses such as cuprammonium regenerated cellulose, viscose regenerated cellulose, cotton, pulp, and polynosic are used. Cuprammonium regenerated cellulose and viscose regenerated cellulose are preferred, and cuprammonium regenerated cellulose is more preferred. Cuprammonium regenerated cellulose has a low degree of crystallinity, making it highly reactive when modified with various functional groups, and even porous particles can be highly densely and uniformly modified with cationic substituents, even inside the particles. Furthermore, cuprammonium regenerated cellulose has a lower zeta potential than general crystalline cellulose. Therefore, interactions such as electrostatic adsorption and repulsion with collagen molecules are less likely to occur, making it possible to uniformly introduce collagen into the porous inner surface. The lower limit of the density of the material used for the microcarrier is 1.0 g / cm. 3 More preferably, it is 1.2 g / cm or more. 3 More preferably, 1.4 g / cm 3 The upper limit of the density of the material used for the microcarrier is 2.0 g / cm 3 More preferably, it is less than 1.8 g / cm 3 Particularly preferably 1.6 g / cm 3 The density is 2.0 g / cm or less. 3 When the density is less than 1.0 g / cm, the cells can be suspended even with a small stirring force, the shear stress is small, and damage to the cells is reduced. 3At this density, the microcarriers sink in water and the cells are no longer in contact with air, allowing them to be used for agitation culture. 3 This is a preferable density for the material used in the microcarrier.
[0013] The shape of the porous cellulose particles of this embodiment is preferably spherical, more preferably having a sphericity of 0.70 to 1.00, even more preferably 0.90 to 1.00. In this specification, the term "sphericity" refers to a value representing the shape of a particle, and is defined as the value obtained by dividing the shortest diameter of a projected circle of the particle, as seen in an optical microscope image, by the longest diameter after swelling the porous particle with water and removing excess water. Specifically, the swelling process for the porous particles involved immersing 1 mg of porous particles in 10 ml of physiological saline for half a day to allow swelling, and then filtering off excess water using an empty column (BIO-RAD, 7311550) to remove the particles to the extent that they would fall under their own weight. While this measurement method only measures each particle in a plane, using an average value obtained by measuring at least 100 particles allows for consideration of variations in the observation direction, thereby enabling the degree of sphericity of the particles to be measured in three dimensions. The closer this value is to 1.00, the more spherical the particle shape is, with a perfect sphere being 1.00. Spherical porous microcarriers have no anisotropy in the internal liquid permeability, allowing collagen to be uniformly modified even inside the particles, allowing cells to spread uniformly inside the particles. Furthermore, compared to other shapes such as cubes, buoyancy can be achieved with less stirring force, reducing shear stress and preventing cells from falling out.
[0014] The lower limit of the average particle size of the porous cellulose particles of this embodiment is preferably 100 μm or more, more preferably 200 μm or more. An average particle size greater than 100 μm increases the number of cells retained per microcarrier, facilitating separation from the culture medium. The upper limit of the average particle size of the porous cellulose particles of this embodiment is preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 400 μm or less. An average particle size smaller than 1000 μm ensures sufficient supply of nutrients and oxygen to cells in the center of the microcarrier, resulting in a favorable culture environment. Furthermore, an average particle size smaller than 1000 μm reduces the stirring force required to suspend and disperse the microcarriers, thereby reducing shear stress. As a result, cell detachment is less likely to occur, making the particles suitable for high-density culture. In this specification, the term "average particle size" refers to the average particle size measured by swelling porous particles with water, removing excess water, and measuring 20 or more particles using an optical microscope at an appropriate magnification. In detail, the swelling process of the porous particles was carried out by immersing 1 mg of porous particles in 10 ml of physiological saline for half a day to allow the particles to swell, and then filtering out excess water using an empty column (manufactured by BIO-RAD, 7311550) until the particles fell under their own weight.
[0015] The lower limit of the average pore size of the pores in the porous cellulose particles of this embodiment is preferably 5 μm or more, more preferably 10 μm or more. By setting the average pore size to 5 μm or more, the degree of freedom of movement of cells and culture medium within the microcarrier is increased, allowing cells to enter the interior of the microcarrier and efficiently proliferate. The upper limit of the average pore size is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. An average pore size of 100 μm or less ensures a sufficient surface area for cell proliferation, resulting in efficient cell proliferation. Furthermore, the porous cellulose particles of this embodiment preferably have a continuous pore structure in which adjacent pores are interconnected by openings in the membrane separating them. Forming a continuous pore structure increases the specific surface area, allowing cells to spread even within the microcarrier, thereby increasing the number of cells that can adhere. In this specification, the term "average pore size" refers to the maximum value of the pore size distribution measured by a mercury intrusion porosimeter after solvent substitution of porous particles with water, ethanol, and t-butanol in that order, followed by removal of the remaining excess solvent by freeze-drying.
[0016] The lower limit of the surface area (specific surface area) per 1 g of the cellulose porous particles of this embodiment when dried is 0.3 m 2 / g or more, more preferably 0.6m 2 / g or more, and more preferably 0.8m 2 The surface area required for cell culture is 0.3 m / g or more from the viewpoint of efficient cell proliferation and further from the viewpoint of reducing the amount of collagen per unit area so that adhesion between particles due to the fixation of collagen molecules is unlikely to occur. 2 The upper limit of the specific surface area is preferably 4.4 m / g or more. 2 / g or less, and 2 / g or less is more preferable, and 2.0m 2 / g or less is more preferable, and 1.7m 2 From the viewpoint of preventing a decrease in the charge per unit area, the amount of collagen, and the rate of cell attachment, and further preventing cells from dropping off due to shear stress when cultured at high density, the specific surface area is 4.4 m 2In this specification, the term "specific surface area" refers to the surface area per 1 g of dry weight measured by the BET method.
[0017] In this specification, the cellulose constituting the cellulose porous particles is preferably modified with a cationic substituent, which is preferably at least one selected from the group consisting of a primary amino group, a secondary amino group, and a tertiary amino group, more preferably a tertiary amino group, and even more preferably a diethylaminoethyl group.
[0018] Unlike particles such as polystyrene and gelatin, the charge capacity of the porous cellulose particles of this embodiment must take into account the influence of hydroxyl groups contained in the base material, cellulose. It is also necessary to consider the significant differences in intramolecular hydrogen bonds and crystallinity compared to polysaccharide particles such as dextran particles. It is also important to consider that the optimal charge range for good cell adhesion differs between cationized cellulose with immobilized collagen and cationized cellulose without immobilized collagen. The upper limit of the charge capacity of the porous cellulose particles of this embodiment is preferably 5.0 mmol / g or less, more preferably 3.0 mmol / g or less, and particularly preferably 2.0 mmol / g or less. A charge capacity below 5.0 mmol / g is less likely to inhibit cell growth. The lower limit of the charge capacity of the porous cellulose particles is preferably 0 mmol / g or more, more preferably greater than 0 mmol / g, more preferably 0.005 mmol / g or more, more preferably 0.1 mmol / g or more, more preferably 0.3 mmol / g or more, and particularly preferably 0.5 mmol / g or more. When the lower limit of the charge capacity of the porous cellulose particles is within this range, cells can be efficiently adsorbed onto the particles. In this specification, the term "charge capacity" refers to an evaluation method in which chloride ions are adsorbed to the amines in the porous particles using hydrochloric acid, and the adsorbed chloride ions are then washed away with a sodium sulfate solution, and the chloride ion concentration of the resulting solution is titrated with 1N silver nitrate using potassium chromate as an indicator, and the average value of measurements for three or more samples is taken as the charge capacity. More specifically, the charge capacity can be calculated using the following measurement method.
[0019] [Charge Capacity Measurement] 5.0 g of porous particles were weighed and washed twice with 30 mL of distilled water using a funnel and suction filter, followed by water replacement. The particles were then washed twice with 30 mL of 0.3 N hydrochloric acid and four times with 50 mL of 10-4 N hydrochloric acid. Then, using a funnel and suction filter, the particles were washed four times with 50 mL of 10% sodium sulfate aqueous solution, and the filtrate was recovered. The recovered filtrate was then added with 2 mL of 0.1 N potassium chromate aqueous solution and stirred. The sample was then titrated with a 1 N silver nitrate aqueous solution, and the titer A (mL) at the moment when the reddish-brown precipitate of silver chromate began to form was determined. Separately, a sample that had been washed with 10% sodium sulfate aqueous solution in the above-mentioned process was washed four times with 50 mL of pure water, dried at 105°C for at least 15 hours, and weighed on a balance to determine the dry weight B (g). The charge capacity is calculated using the titer A (mL) measured above and the dry weight B (g) of the sample according to the following formula (1) (N=3): Charge capacity (mmol / g) = 1 (N) (mol / L) × A (mL) / B (g) (1)
[0020] The amount of collagen immobilized is preferably 10 μg / g or more and 25 mg / g or less (0.001 to 2.5 wt %) per 1 g of the cell culture carrier (dry porous cellulose particles). The lower limit of the amount of collagen immobilized is preferably 10 μg / g or more, more preferably 100 μg / g or more, more preferably 500 μg / g or more, more preferably 1 mg / g or more, and particularly preferably 2 mg / g or more per 1 g of the cell culture carrier (dry porous cellulose particles). When converted into an immobilization amount per unit area of the culture carrier, the lower limit is preferably 1 ng / cm. 2 More preferably, 10 ng / cm 2 More preferably, 50 ng / cm 2 More preferably, 100 ng / cm 2 More preferably, 200 ng / cm 2 The upper limit is preferably 25 mg / g or less, more preferably 20 mg / g or less, more preferably 15 mg / g or less, and particularly preferably 10 mg / g. When converted into an immobilization amount per unit area of the cultivation carrier, it is preferably 2.5 μg / cm 2 or less, more preferably 2 μg / cm 2or less, more preferably 1.51 μg / cm 2 Below, particularly preferably 1 μg / cm 2 The lower limit is within the above range, which can improve the adhesiveness and extensibility of cells, and the upper limit is within the above range, which can prevent poor dispersion due to the pores of cellulose particles being buried by fibrous collagen molecules or the adhesion of collagen molecules to each other, resulting in adhesion of particles to each other. The amount of collagen in this embodiment was quantified by a hydroxyproline assay. More specifically, the amount of collagen can be calculated using the following measurement method.
[0021] [Measurement of Collagen Amount] In this embodiment, the collagen amount may be quantified using a hydroxyproline assay kit (QuickZyme, Total Collagen Assay Kit). 10 mg of a collagen-coated sample is weighed, 1 ml of PBS buffer is added, and the mixture is stirred using a rotator at a stirring speed of 20 rpm for 7 days. After 7 days, the sample is filtered using a spin column (BIO PHARMA, EP-31101), and centrifuged for 1 minute in a 2000 G mini-centrifuge (MILLIPORE, CHIBITAN-R, CT6M) to separate the particles and the supernatant. After removing the supernatant, 1 ml of PBS was added to remove any remaining supernatant from the particles. The mixture was then centrifuged at 2000 g for 1 minute in a small centrifuge (MILLIPORE, CHIBITAN-R, CT6M) to recover the washed particles. Separating the particles from the supernatant removed the collagen eluted in the supernatant, allowing the amount of collagen immobilized on the particles to be measured. 500 μl of 6 M hydrochloric acid was added to the particles and heated at 95°C for 24 hours to hydrolyze the collagen and produce hydroxyproline. After heating, 500 μl of the sample was neutralized by adding 120 μl of 48% sodium hydroxide and 130 μl of pure water. The neutralized sample was passed through a 0.2 μl PES syringe filter to remove any fine particles that remained unhydrolyzed. To prepare a standard curve, 500 μl of 1000 μg / ml collagen solution was measured, 500 μl of 12 M hydrochloric acid was added, and the solution was heated at 95°C for 24 hours. To 1 ml of the standard curve sample, 240 μl of 48% sodium hydroxide and 260 μl of pure water were added to neutralize the solution. The neutralized sample was diluted to prepare seven samples with collagen concentrations of 0 μg / ml, 7.8 μg / ml, 15.6 μg / ml, 31.3 μg / ml, 62.5 μg / ml, 125 μg / ml, and 250 μg / ml. 35 μl of each of the neutralized sample and the sample for preparing the standard curve was added to a 96-well microplate.Thereafter, 70 μl of chloramine T solution (a mixture of 1.86 g of sodium hydroxide, 2.18 g of citric acid monohydrate, 2.75 g of anhydrous sodium acetate, 0.5 g of glacial acetic acid, and 0.84 g of chloramine T, made up to 74 ml with water, and then 26 ml of 2-propanol was added) was added to each well and allowed to react at room temperature for 20 minutes to convert to pyrrole. Subsequently, 70 μl of Ehrlich's reagent was added to each well, and the mixture was allowed to react at 60°C for 30 minutes. Absorbance at a wavelength of 560 nm was measured using a microplate reader (Corona, SH-1000Lab). The intercept t and slope k were calculated from a calibration curve with the collagen concentration on the horizontal axis and the absorbance on the vertical axis, and the collagen concentration C of the sample solution was calculated from the absorbance A of each sample using the following formula: C [μg / ml] = (A - t) / k When absorbance A is an extrapolation of the calibration curve, the sample solution can be diluted appropriately, the absorbance remeasured, and the collagen concentration corrected taking into account the dilution factor. The amount of immobilized collagen (amount of detached collagen) is calculated using the following formula, where M [mg] is the amount of sample used: Amount of immobilized collagen (mg / g) = C [μg / ml] × (dilution rate at neutralization: 1.5) × (amount of sample before neutralization: 0.5 ml) / M [mg].
[0022] The collagen can be introduced onto the cellulose surface by physical adsorption or chemical bonding. More specifically, collagen can be introduced onto the cellulose surface by a method of impregnating cellulose with a collagen solution and adsorbing it through the interaction between cellulose and collagen in the liquid; a method of impregnating the cellulose with collagen, neutralizing it with a buffer, and then drying it to precipitate and immobilize collagen fibers on the cellulose surface; or a method of modifying the cellulose surface by chemical bonding, such as condensation of a primary amino group with a carboxylic acid. In this embodiment, the introduction method is not particularly limited, but a method of neutralizing the collagen, drying it, and precipitating and immobilizing it on the cellulose surface is preferred. Neutralizing the collagen with a buffer at around pH 7 causes the collagen to become fibrous, and subsequent drying allows the collagen to be firmly attached to the cellulose surface. When collagen is immobilized onto cellulose by this method, the collagen remains intact for a long period of time, even when the particles are added with a liquid and stirred. Furthermore, since a large amount of collagen can be introduced into the particles, cells can be effectively attached.
[0023] After being introduced into the cellulose particles, the collagen may be chemically crosslinked with a crosslinking agent. The type of crosslinking agent is not particularly limited, but examples thereof include glutaraldehyde, formaldehyde, 1-[3-(dimethylamino)propyl]-3-ethylcarbodiimide, N,N'-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, N,N'-carbonyldiimidazole, 1,1'-carbonyldi(1,2,4-triazole), 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride hydrate, (4,6-dimethoxy-1,3,5-triazin-2-yl)-( Crosslinking can be performed using crosslinkers such as 2-octoxy-2-oxoethyl)dimethylammonium, 1H-benzotriazol-1-yloxytris(dimethylamino)phosphonium hexafluorophosphate, 1H-benzotriazol-1-yloxytripyrrolidinophosphonium hexafluorophosphate, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate, and O-(7-azabenzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate. Furthermore, in addition to the crosslinking agent, a carboxylic acid activating reagent such as N-hydroxysuccinimide can also be added. Crosslinking collagen strengthens adhesion to cellulose, allowing cell adhesion effects to be maintained even during agitation culture.
[0024] The porous cellulose particles of this embodiment can be produced by a method in which a solution containing dissolved cellulose is formed into a desired shape while being cooled to a temperature below the solidification temperature of the solution to freeze it, and then the solvent is extracted and removed or the dissolving ability is lost. In general, the freezing temperature is preferably not set to a temperature lower than the freezing temperature of the solvent or the like by 40°C or more, and is usually selected in the range of 0 to 20°C lower than the freezing temperature.
[0025] The frozen cellulose solution or cellulose derivative solution is then subjected to extraction and removal of the solvent dissolving the cellulose or cellulose derivative, or reduction of its dissolving power (hereinafter, these processes are collectively referred to as "solvent removal, etc."), resulting in a solidified porous cellulose body. The conditions for solvent removal, etc., are not particularly limited. Typically, the frozen body can be quickly placed in a coagulation bath or regeneration bath, but it is preferable and recommended that the coagulation bath or regeneration bath be kept below the freezing temperature of the solution. However, in the case of cellulose derivatives, a cellulose regeneration process is required, and this regeneration is carried out simultaneously with or sequentially (i.e., after solvent removal, etc.). The regeneration itself can be carried out by conventional methods. Using the above production method, there is no need to add foreign substances such as porosifying agents to the polymer solution during production, making it easy to produce droplets of uniform diameter, and particle size control is possible. The diameter and shape of the pores are essentially determined by the size and shape of the solvent crystals formed when the solvent in the solution freezes and solidifies. Therefore, the shape and diameter of the pores can be adjusted by changing the type of polymer solution, the freezing and solidification conditions such as the temperature.
[0026] In this specification, the porous cellulose particles can be granulated cellulose particles as they are, but are preferably crosslinked before use. There are no limitations on the crosslinking method, but any crosslinking agent having two or more functional groups capable of reactively bonding with the hydroxyl groups of cellulose can be used for intermolecular crosslinking of porous cellulose materials. Examples include bifunctional organic substances. Examples include X-R-Z type compounds (where R represents an aliphatic residue containing a carbon atom, and X and Z are various halogens, epoxy, etc., bonded to the carbon atoms of the aliphatic residue) that react relatively easily in the presence of an alkaline reactant. Examples of bifunctional compounds suitable for the above reaction include epichlorohydrin, dichlorohydrin, 1,2- or 3,4-diepoxybutane, bisepoxypropyl ether, ethylene glycol-bis-epoxypropyl ether, 1,4-butanediol-bis-epoxypropyl ether, and closely related compounds, but are not limited to these. Crosslinking allows the crystalline structure of cellulose to be maintained even when modified with many cationic substituents, thereby keeping the particle structure stable.
[0027] In the production of the porous cellulose particles of this embodiment, the method for modifying the cellulose constituting the porous cellulose particles with a cationic substituent is not particularly limited, and multiple methods are possible for introduction, such as a method of directly modifying a hydroxyl group or a method of modifying via a functional group having an epoxy group. The introduction of tertiary amino groups is preferably a method of directly modifying the hydroxyl groups of the cellulose using 2-(diethylamino)ethyl chloride hydrochloride or the like. Because cellulose has many hydroxyl groups, direct modification with the hydroxyl groups makes it possible to modify the particles with a large amount of cationic tertiary amino groups uniformly, even within the particle.
[0028] The porous cellulose particles of this embodiment can be used as microcarriers for culture. In this specification, "microcarriers for culture" refers to microcarriers used to attach and grow the culture target. During culture, the cells themselves may be the target of production, or a virus for vaccine production or the like may be the target cell growth product. In such cases, appropriate cells may be selected as the host. Depending on the purpose, it may be preferable to use genetically modified cells into which a production gene for the target cell growth product has been introduced. Regarding culture, for example, suspension culture and static culture may be used, but the use is not limited to these.
[0029] The cells used for the culture are not particularly limited, but include fungi, yeast, plant cells, and animal cells including fish and insects, and are preferably primate or human stem cells or induced pluripotent stem cells.Human stem cells include, but are not limited to, dental pulp stem cells, neural stem cells, skin stem cells, hematopoietic stem cells, mesenchymal stem cells, mammary stem cells, endothelial stem cells, and embryonic stem cells.
[0030] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples. The following describes methods for measuring the physical properties of the structure.
[0031] (1) Charge capacity: 1.0 g of a sample containing water was weighed out and, using a funnel and a suction filter, was diluted twice with 30 mL of 0.3 N hydrochloric acid solution. -4The sample was washed four times with 50 mL of 10% sodium sulfate aqueous solution. Then, using a funnel and a suction filter, the sample was washed four times with 50 mL of 10% sodium sulfate aqueous solution, and the filtrate was recovered. The recovered filtrate was added with 2 mL of 0.1 N potassium chromate aqueous solution and stirred. The sample was then titrated with 1 N silver nitrate aqueous solution, and the titer A (mL) at the moment when reddish-brown precipitation of silver chromate began to occur was determined. Separately, a sample that had been washed with 10% sodium sulfate aqueous solution in the above process was washed four times with 50 mL of pure water, dried at 105°C for 15 hours or more, and weighed on a balance to determine the dry weight B (g). The charge capacity was calculated using the measured titer A (mL) and the dry weight B (g) of the sample according to the following formula (1) (N = 3): Charge capacity (mmol / g) = 1 (N) (mol / L) × A (mL) / B (g)... formula (1)
[0032] (2) Measurement of Collagen Amount The collagen amount in this embodiment was quantified using a hydroxyproline assay kit (QuickZyme, Total Collagen Assay Kit). 10 mg of the collagen-coated sample was weighed, 1 ml of PBS buffer was added, and the mixture was stirred for 7 days at a stirring speed of 20 rpm using a rotator. After 7 days, the sample was filtered using a spin column (BIO PHARMA, EP-31101), and centrifuged for 1 minute using a 2000 G mini-centrifuge (MILLIPORE, CHIBITAN-R, CT6M) to separate the particles and the supernatant. After removing the supernatant after separation, 1 ml of PBS was added to remove any remaining supernatant from the particles, and the mixture was centrifuged for 1 minute at 2000 g in a small centrifuge (MILLIPORE, CHIBITAN-R, CT6M) to recover the washed particles. Separating the particles from the supernatant removed the collagen eluted in the supernatant, allowing the amount of collagen immobilized on the particles to be measured. 500 μl of 6 M hydrochloric acid was added to the particles, and the mixture was heated at 95°C for 24 hours to hydrolyze the collagen and produce hydroxyproline. After heating, 500 μl of the sample was neutralized by adding 120 μl of 48% sodium hydroxide and 130 μl of pure water. The neutralized sample was passed through a 0.2 μl PES syringe filter to remove any fine particles that remained unhydrolyzed. To prepare a calibration curve, 500 μl of 1000 μg / ml collagen solution was weighed out, 500 μl of 12 M hydrochloric acid was added, and the solution was heated at 95°C for 24 hours. 240 μl of 48% sodium hydroxide and 260 μl of pure water were added to 1 ml of the calibration curve sample to neutralize it. The neutralized sample was diluted to prepare seven samples with collagen concentrations of 0 μg / ml, 7.8 μg / ml, 15.6 μg / ml, 31.3 μg / ml, 62.5 μg / ml, 125 μg / ml, and 250 μg / ml. 35 μl of each of the neutralized sample and the calibration curve sample was added to a 96-well microplate. Thereafter, 70 μl of chloramine T solution (a mixture of the above reagents, 1.86 g of sodium hydroxide, 2.18 g of citric acid monohydrate, 2.75 g of anhydrous sodium acetate, 0.5 g of glacial acetic acid, and 0.84 g of chloramine T, diluted to 74 ml with water, and then 26 ml of 2-propanol was added) was added to each well, and the mixture was allowed to react at room temperature for 20 minutes to convert to pyrrole.Next, 70 μl of Ehrlich's reagent was added to each well, and the mixture was incubated at 60°C for 30 minutes. Absorbance at a wavelength of 560 nm was measured using a microplate reader (Corona, SH-1000Lab). The intercept t and slope k were calculated from a calibration curve with collagen concentration on the horizontal axis and absorbance on the vertical axis. The collagen concentration C of each sample solution was calculated from the absorbance A of each sample using the following formula: C [μg / ml] = (A - t) / k. When absorbance A is an extrapolation of the calibration curve, the sample solution can be appropriately diluted, the absorbance remeasured, and corrected to a collagen concentration that takes the dilution factor into account. The amount of collagen immobilized (amount removed) was calculated using the following formula, where M [mg] is the amount of sample used: Amount of immobilized collagen (mg / g) = C [μg / ml] × (1.5x dilution rate upon neutralization) × (0.5 ml sample volume before neutralization) / M [mg].
[0033] The method for producing porous cellulose particles is described below. [Production of Cellulose Particles] 500 mL of a cellulose-copper-ammonium solution prepared using purified linters as a raw material, with a viscosity of 2 poise at 5°C, a cellulose concentration of 2%, a copper concentration of 1.2%, and an ammonia concentration of 4%, was sprayed using a two-fluid nozzle along with nitrogen gas and stirred into 10 L of silicone oil (SH200, 1.5 cs, Toray Industries, Inc.) cooled to -40°C. The silicone oil was heated to -20°C and stirred for 20 minutes, after which 10 L of 40% sulfuric acid cooled to -35°C was added. After adding the sulfuric acid, stirring was continued for 8 hours, and the mixture was heated to 20°C. The silicone oil was removed, and the remainder was extracted and washed with water to obtain porous cellulose particles. Using a classification sieve (mesh openings 250 μm and 125 μm), porous cellulose particles with an average particle size of 240 μm and an average pore size of 30 μm were obtained. Next, to perform epichlorohydrin crosslinking, 50 g of the obtained particles were weighed out, and 2010 ml of pure water, 0.12 mg of sodium dodecyl sulfate, 97.9 ml of 48% aqueous sodium hydroxide solution, and 28.9 g of epichlorohydrin were added, followed by reaction with stirring for 1 hour in a thermostatic chamber at 60° C. Thereafter, the sample was washed three times with 8000 ml of pure water using a funnel and a suction filter, and the cellulose particles before cationization modification were designated as Particles 1.
[0034] [Cationization of Cellulose Particles] 6.66 g of Particles 1 was weighed out, and pure water, anhydrous sodium sulfate, sodium dodecyl sulfate, and a 50% aqueous solution of 2-(diethylamino)ethyl chloride hydrochloride were added in the amounts shown in Table 1 below, followed by stirring. A reaction initiation liquid (48% aqueous sodium hydroxide solution) was immediately added, and the reaction was carried out with stirring for 1 hour in a thermostatic chamber at 70°C. After 1 hour, 36% hydrochloric acid was added to neutralize the mixture until the pH reached 7, and the sample was washed three times with 8,000 mL of pure water by suction filtration to obtain Particles 2 to 8, which are cationic porous cellulose particles. The charge capacity of the dried particles was measured.
[0035]
[0036] [Collagen Coating by Drying Method] Next, 5 ml of collagen solution at pH 3.0 with the concentration shown in Table 2 below was added to particles 1 to 8 (100 mg) and incubated at 30°C for 1 hour. After incubation, 5 ml of PBS at pH 7.4 was added and the mixture was neutralized by inversion. The pH after neutralization was confirmed to be around 7.0. Using an empty column (BIO-RAD, 7311550), the reaction solution was filtered to remove the remaining solution until it fell under its own weight. The filtered particles were dried at 30°C for 2 days. The reaction solution (5 ml of MES buffer adjusted to pH 5.5, 5 mg of EDCI.HCl, and 1.15 mg of NHS) was added to the resulting dried particles and allowed to react at 37°C for 1 hour. After the reaction, the particles were centrifuged at 2000 rpm for 1 minute using an empty column (BIO-RAD, 7311550), and then washed by adding 5 ml of PBS and centrifuging five times. The washed particles were transferred to a tray, and 6 ml of PBS was added and dried at 30°C to obtain collagen-modified particles 9 to 26. The amount of collagen in the dried particles was evaluated by a hydroxyproline assay.
[0037]
[0038] [Collagen Coating by Wet Method] 5 ml of a 0.5 mg / ml collagen solution was added to Particle 1 (100 mg) and incubated at 30°C for 1 hour. After incubation, 5 ml of PBS was added, the mixture was mixed by inversion, and filtered using an empty column (BIO-RAD, 7311550) until the mixture fell under its own weight. 5 ml of PBS was passed through the column three times for washing, yielding Particle 27. This method is referred to as the wet method. The amount of collagen immobilized on Particle 27 was evaluated and found to be 0.1 mg / g. This was significantly lower than the amount of collagen immobilized on Particle 9, which was prepared using the same Particle 1 and the same collagen concentration by the dry method, with an immobilization amount of 3.8 mg / g.
[0039] [Crosslinked Collagen-Coated Particles Using Glutaraldehyde] 5 ml of a 0.5 mg / ml collagen solution was added to 100 mg of Particle 6 and incubated at 30°C for 1 hour. After incubation, 5 ml of PBS was added, the mixture was mixed by inversion, and the mixture was filtered using an empty column (BIO-RAD, 7311550) until the particles fell under their own weight. The filtered particles were dried at 30°C for 2 days. A reaction solution (5 ml of PBS buffer, 50 μl of glutaraldehyde) was added to the dried particles and reacted at 37°C for 1 hour. After the reaction, the particles were centrifuged at 2000 rpm using an empty column (BIO-RAD, 7311550), and then washed by adding 5 ml of PBS and centrifuging five times. The washed particles were transferred to a tray, 6 ml of PBS was added, and the mixture was dried at 30°C for 2 days to obtain collagen-modified Particles 28. The amount of collagen in the dried particles was evaluated by hydroxyproline assay, and the immobilized amount was 2.0 mg / g.
[0040] [Uncrosslinked collagen-coated particles] 5 ml of a collagen solution with a concentration of 0.5 mg / ml was added to Particle 6 (100 mg) and incubated at 30°C for 1 hour. After incubation, 5 ml of PBS was added, the mixture was mixed by inversion, and filtered using an empty column (BIO-RAD, 7311550) until the particles fell under their own weight. The filtered particles were dried at 30°C for 2 days to obtain Particle 29. The amount of collagen in the dried particles was evaluated by a hydroxyproline assay, and the immobilized amount was 2.0 mg / g.
[0041] [Collagen-coated cellulose particles with an average pore size of 1 μm] A cellulose-copper-ammonium solution with a viscosity of 2 poise at 5 ° C, a cellulose concentration of 2%, a copper concentration of 1.2%, and an ammonia concentration of 4%, prepared using purified linters as a raw material, was sprayed in an amount of 500 mL with nitrogen gas using a two-fluid nozzle and stirred into 10 L of silicone oil (SH200, 1.5 cs, Toray Industries, Inc.) cooled to -55 ° C. The silicone oil was kept at -55 ° C and stirred for 50 minutes, and then 10 L of 40% sulfuric acid cooled to -55 ° C was added. After adding the sulfuric acid, stirring was continued for 8 hours, and the temperature was raised to 20 ° C. The silicone oil was removed, and the remainder was extracted and washed with water to obtain porous cellulose particles. Using a classification sieve (openings 250 μm and 125 μm), porous cellulose particles with an average particle size of 240 μm and an average pore size of 1 μm were obtained. Next, 5 ml of a 0.5 mg / ml collagen solution was added to the resulting particles and incubated at 30°C for 1 hour. After incubation, 5 ml of PBS was added, the mixture was mixed by inversion, and filtered using an empty column (BIO-RAD, 7311550) until the particles fell under their own weight. The filtered particles were dried at 30°C for 2 days. A reaction solution (5 ml of MES buffer adjusted to pH 5.5, 5 mg of EDCI·HCl, and 1.15 mg of NHS) was added to the resulting dried particles and reacted at 37°C for 1 hour. After the reaction, the particles were centrifuged at 2000 rpm using an empty column, and then washed by adding 5 ml of PBS and centrifuging five times. The washed particles were transferred to a tray, 6 ml of PBS was added, and the particles were dried at 30°C for 2 days to obtain collagen-modified particles 30. The amount of collagen in the dried particles was evaluated by a hydroxyproline assay, and the immobilized amount was 2.0 mg / g.
[0042] The cell culture evaluation of the collagen porous particles obtained as described above will be described below. [Culture Evaluation] The following Tables 3-1 and 3-2 show the results of the culture evaluation using particles 1, 6, and 9 to 30. In Examples 1 to 17, 24 to 27, and Comparative Examples 1 to 3, human dental pulp-derived stem cells (DPSC) were used for the evaluation, and in Examples 18 to 23, human adipose-derived mesenchymal stem cells (MSC) were used for the evaluation.
[0043] [Static culture method of human dental pulp-derived stem cells (DPSCs)] Using a 6-well suspension culture plate manufactured by IWAKI (product number 1810-006), 5.0 × 10 human dental pulp-derived stem cells (PT-5025 manufactured by Lonza) were cultured in each well. 4 The cells were added with 3 ml of Lonza DPSC Bullet Kit (PT-3005) medium and 6 mg of microcarriers, and cultured statically for 6 days in an incubator at 37° C. The medium was changed on the fourth day of culture.
[0044] [Static culture method for human adipose tissue-derived mesenchymal stem cells (MSCs)] Using a 6-well suspension culture plate manufactured by IWAKI (product number 1810-006), 5.0 × 10 human adipose tissue-derived mesenchymal stem cells (product number C-12977) manufactured by Promocell were placed in each well. 4 3 ml of Mesenchymal Stem Cell Growth Medium 2 (product number C-28009) manufactured by Promocell and 6 mg of microcarriers were added, and the cells were cultured stationary for 6 days in an incubator at 37° C. The medium was changed on the 4th day of culture.
[0045] <Evaluation of cell proliferation using a fluorescence microscope> After culturing, 6 mg of the microcarriers were washed by removing the supernatant and adding 2 ml of PBS buffer three times. After washing, the microcarriers were washed with calcein-containing assay buffer (AAT, manufactured by Bioquest, Live or Dead). TMCell Viability Assay Kit) was added and allowed to stand for 5 minutes. After standing, 2 ml of PBS buffer was added and the supernatant was removed. This process was repeated three times for washing. Using a fluorescence microscope (Leica, DMi8), live cells were observed with a FITC filter (excitation 480 nm, absorption 527 nm) at 4x magnification. The ratio of the fluorescence area to the particle area was calculated using analysis software (Image J), and the initial cell adhesion and proliferation were evaluated.
[0046] <Evaluation of cell proliferation> The fluorescence area ratio on day 6 of culture relative to the fluorescence area ratio on day 1 was evaluated as follows: an area increase ratio of 800% or more was scored as "5", an area increase ratio of less than 800% and 600% or more was scored as "4", an area increase ratio of less than 600% and 400% or more was scored as "3", an area increase ratio of less than 400% and 300% or more was scored as "2", and an area increase ratio of less than 300% was scored as "1".
[0047] <Evaluation of initial adhesion> The initial cell adhesion amount was evaluated as follows: when the ratio of the fluorescent area of the control sample to the fluorescent area on day 1 of Comparative Example 1 was less than 100%, it was rated as "1"; when the area ratio was 100% or more but less than 200%, it was rated as "2"; when the area ratio was 200% or more but less than 300%, it was rated as "3"; when the area ratio was 300% or more but less than 400%, it was rated as "4"; and when it was 400% or more, it was rated as "5".
[0048] <Evaluation of cell adhesion to the inside of the carrier> Cells were fixed to the particles with 2.5% glutaraldehyde, then the medium was replaced with ethanol and t-butanol, and the particles were freeze-dried. After coating with osmium, the particles were sectioned with an ion beam, and the cross-sections were observed with an SEM. 20 or more particles were observed, and the average number of cells per cross-section was scored as "1" if it was less than 0.5, "2" if it was 0.5 to 1, "3" if it was 2 to 5, "4" if it was 6 to 10, and "5" if it was 11 or more.
[0049] <Evaluation of particle aggregation degree> 1 ml of PBS was added to 10 mg of particles in a 2 ml tube, and the evaluation was as follows: if the particles broke apart individually after 10 inversions, the evaluation was "5"; if the particles broke apart individually after 10 pipettings using a 1 ml micropipette (Eppendorf, 3123000063), the evaluation was "4"; if the particles broke apart partially after 10 pipettings, the evaluation was "3"; if the particles did not break apart at all after 10 pipettings, the evaluation was "2"; and if the particles did not break apart at all after 30 pipettings and then after 10 minutes of vibration at intensity 6 using a vortex mixer (Vortex-Genie 2, Scientific Industries), the evaluation was "1".
[0050] <Evaluation of Overall Score> The total score was calculated by adding up the scores for cell proliferation, initial adhesion, cell adhesion to the inside of the carrier, and particle aggregation. As shown in the table below, it was confirmed that Examples 1 to 27 achieved superior results in the evaluation items of, for example, cell proliferation, cell adhesion to the inside of the carrier, and / or overall score compared to Comparative Examples 1 to 3. For example, it was confirmed that Examples 1 to 7 achieved superior results in the evaluation item of overall score compared to Comparative Example 3, which shared various conditions. Furthermore, it was confirmed that Examples 8 to 11 achieved superior results in the evaluation item of overall score compared to Comparative Example 2, which shared various conditions.
[0051]
[0052]
[0053] When the porous cellulose particles of the present invention are used as a culture support (culture microcarrier), they can efficiently adsorb and spread cells even in the early stages of culture when intercellular substrate adhesion is underdeveloped, and further, even when cultured at high density, cell detachment from the particles due to shear stress can be reduced, allowing cells to proliferate highly efficiently.
Claims
1. A cellulose porous particle made of cellulose, having collagen on the surface of the cellulose porous particle, and an immobilized amount of the collagen in a dry state of 10 μg / g or more and 25 mg / g or less (0.001 to 2.5 wt %) per 1 g of the cellulose porous particle.
2. The cellulose porous particles according to claim 1, wherein the cellulose porous particles have a large number of pores with an average pore size of 5 μm or more and 100 μm or less.
3. The cellulose porous particle according to claim 1 or 2, wherein the cellulose porous particle forms a continuous pore structure in which adjacent pores are interconnected by openings in the membrane that separate the pores.
4. The cellulose porous particles according to claim 1 or 2, wherein the average particle size of the cellulose porous particles is 100 μm or more and 1000 μm or less.
5. The cellulose porous particles according to claim 1 or 2, wherein the sphericity of the cellulose porous particles is 0.7 or more.
6. The specific surface area of the cellulose porous particles when dried is 0.3 m 2 / g or more 4.4m 2 The cellulose porous particle according to claim 1 or 2, wherein the molecular weight is 1 / g or less.
7. The cellulose porous particles according to claim 1 or 2, in which the amount of collagen immobilized in a dry state is from 1 mg / g to 10 mg / g (0.1 wt % to 1.0 wt %) per gram of the cellulose porous particles.
8. The cellulose porous particle according to claim 1 or 2, wherein the surface of the cellulose is modified with a cationic substituent.
9. The cellulose porous particle according to claim 8, wherein the cationic substituent is at least one selected from the group consisting of a primary amino group, a secondary amino group, and a tertiary amino group.
10. The cellulose porous particles according to claim 1 or 2, wherein the charge capacity of the cellulose porous particles is 0 mmol / g or more and 5.0 mmol / g or less.
11. The cellulose porous particle according to claim 1 or 2, wherein the collagen is fibrous collagen.
12. The cellulose porous particle according to claim 1 or 2, wherein the collagen is cross-linked collagen.
13. The cellulose porous particles according to claim 1 or 2, wherein the cellulose constituting the cellulose porous particles is cuprammonium regenerated cellulose.
14. A method for producing cellulose porous particles according to claim 1 or 2, comprising the following steps: a step of impregnating cellulose porous particles in a collagen solution; a step of neutralizing the collagen solution to a pH of 6 or more and 8 or less; a dehydration step of removing the collagen solution; and a drying step of drying the cellulose porous particles.
Citation Information
Patent Citations
JP1974118998A
Bone defficient part and void part filling material
JP1983058041A
cosmetic
JP1986282307A
Production of wool-like acrylic fiber fabric having durable pill resistance