Method for polishing object to be polished
The use of a nitrogen-containing compound in the polishing liquid with an aliphatic polyester binder pad enhances polishing rate stability and prevents pad degradation at low pH, addressing exposure and replacement issues in semiconductor polishing.
Patent Information
- Application Number
- PCT/JP2024/020022
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-26
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Polishing methods using binder resins in semiconductor device polishing pads face challenges with abrasive grain exposure and replacement, leading to decreased polishing rates, especially when using low pH polishing liquids which can also damage equipment.
A polishing method employing a polishing pad with an aliphatic polyester binder and abrasive grains, using a nitrogen-containing compound like ammonia in the polishing liquid to facilitate aminolysis or ammonolysis reactions, maintaining high polishing rates even at low pH by promoting decomposition of the binder.
The method maintains a stable polishing rate and prevents excessive pad degradation, even under low pH conditions, reducing equipment damage and ensuring consistent performance.
Smart Images

Figure JP2024020022_05122024_PF_FP_ABST
Abstract
Description
Method for polishing an object
[0001] The present invention relates to a method for polishing an object to be polished.
[0002] 2. Description of the Related Art In polishing a substrate used for a semiconductor device or the like, a method using a fixed-abrasive polishing pad having a polishing layer containing a binder resin and abrasive grains fixed by the binder resin is known.
[0003] As the binder resin, a curable resin such as a phenol resin, an epoxy resin, or an acrylic phenol resin is usually used (see, for example, Patent Document 1).
[0004] JP 2018-51733 A
[0005] However, in polishing pads using the binder resin described above, the abrasive grains inside the binder resin are less likely to be exposed to the surface of the polishing layer, and replacement of the grains is less likely to occur. As a result, there is a problem that, over time during polishing, the abrasive grains protruding from the surface of the polishing layer wear and become dull, which tends to reduce the polishing rate.
[0006] In response to this, the inventors have investigated a method of using a degradable resin such as glycolic acid polymer as the binder resin and an alkaline aqueous solution such as a sodium hydroxide aqueous solution as the polishing liquid to hydrolyze the resin in the polishing pad and cause an appropriate change in grain size, thereby minimizing the decrease in polishing rate.
[0007] However, when using the above-mentioned alkaline aqueous solution, hydrolysis of the decomposable resin does not proceed easily under low pH conditions. As a result, the polishing pad is less likely to be replaced, and the polishing rate is likely to decrease. On the other hand, under high pH conditions, although the decrease in polishing rate can be suppressed, there is a concern that the high pH alkaline aqueous solution may damage the polishing apparatus when used for a long period of time. Therefore, a polishing method in which the decrease in polishing rate is small even when a polishing solution with a low pH is used is desired.
[0008] The present invention has been made in view of the above circumstances, and has as its object to provide a method for polishing an object to be polished in which the decrease in polishing rate is small even when a polishing liquid with a low pH is used.
[0009] [1] A method for polishing an object to be polished, comprising the step of polishing the object to be polished by supplying a polishing liquid to the surface of a polishing pad having a polishing layer containing a composition containing an aliphatic polyester and abrasive grains, while sliding the polishing pad and the object to be polished relative to each other, wherein the polishing liquid contains a nitrogen-containing compound represented by the following formula (1) and water. Formula (1): H-N(((CH 2 ) n X) m -R 1 ) R 2 (In formula (1), R 1 and R 2 is H or a hydrocarbon group having 1 to 22 carbon atoms, and R 1 and R 2 may be bonded to each other to form a ring, X is a divalent group selected from the group consisting of -O-, -NH-, -S-, and -COO-, m is an integer of 0 to 3, and n is an integer of 0 to 6, and when m is 2 or more, the number of n and the type of atom of X may be different from each other.) [2] The method for polishing an object to be polished according to [1], wherein the nitrogen-containing compound includes ammonia, hydrazine, or hydroxylamine. [3] The method for polishing an object to be polished according to [1] or [2], wherein the aliphatic polyester contains polyglycolic acid as a main component. [4] The method for polishing an object to be polished according to any one of [1] to [3], wherein the pH of the polishing liquid is 7 or more but less than 13.
[0010] According to the present invention, it is possible to provide a method for polishing an object to be polished in which the polishing rate is not likely to decrease even when a polishing liquid with a low pH is used.
[0011] Fig. 1 is a schematic cross-sectional view showing a polishing method for a workpiece according to one embodiment of the present invention. Figs. 2A to 2C are schematic cross-sectional views showing the molding process in an example. Fig. 3A is a graph showing the change in the polishing rate of SiC over time in a polishing test, and Fig. 3B is a graph showing the change in the removal rate of a polishing pad over time. Fig. 4 is a graph summarizing the results of Figs. 3A and 3B.
[0012] The present inventors have found that an aqueous solution containing a specific nitrogen-containing compound, such as ammonia, a primary amine, or a secondary amine, is less likely to decrease the polishing rate even in a low pH range.
[0013] Although the mechanism behind this is unclear, it is presumed that when a polishing liquid containing a specific nitrogen-containing compound is used, decomposition reactions due to aminolysis or ammonolysis occur more predominantly than hydrolysis reactions.
[0014] Specifically, a hydrogen atom is eliminated from the amino group of a specific nitrogen-containing compound, and the nitrogen-containing compound from which the hydrogen atom is eliminated nucleophilically attacks the ester bond of the aliphatic polyester of the polishing pad to form an amide bond. Meanwhile, the hydrogen atom eliminated from the nitrogen-containing compound is bonded to the oxygen atom eliminated from the ester bond of the aliphatic polyester to form a compound containing OH. In this way, it is thought that the reaction in which the aliphatic polyester is decomposed into a compound having an amide bond and a compound containing OH (decomposition reaction by aminolysis or ammonolysis) occurs predominantly.
[0015] The equilibrium constant of such a decomposition reaction by aminolysis or ammonolysis is much larger than the equilibrium constant of a conventional hydrolysis reaction, and the decomposition reaction rate is high. Therefore, it is thought that the decomposition rate of the aliphatic polyester is unlikely to decrease even at a low pH.
[0016] Hereinafter, a method for polishing an object to be polished according to one embodiment of the present invention will be described. First, a polishing pad used in the method for polishing an object to be polished will be described, and then the method for polishing an object to be polished will be described.
[0017] 1. Polishing Pad The polishing pad according to this embodiment includes a polishing layer.
[0018] 1-1. Abrasive Layer The abrasive layer contains a composition including a matrix containing an aliphatic polyester and abrasive grains held in the matrix.
[0019] 1-1-1 Aliphatic Polyester The aliphatic polyester is not particularly limited as long as it is decomposed by the aminolysis reaction or ammonolysis reaction described above.
[0020] Such aliphatic polyesters may be polyesters obtained by homopolymerization or copolymerization of hydroxycarboxylic acids and / or lactones, esterification reaction of aliphatic dicarboxylic acids with aliphatic diols, or copolymerization of aliphatic dicarboxylic acids, aliphatic diols, and hydroxycarboxylic acids and / or lactones. Among these, polyesters that are rapidly decomposed and dissolved by aminolysis or ammonolysis in the presence of water at about 20 to 100°C are preferred.
[0021] Examples of hydroxycarboxylic acids include aliphatic hydroxycarboxylic acids having 2 to 8 carbon atoms, such as glycolic acid, lactic acid, malic acid, hydroxypropionic acid, hydroxybutyric acid, hydroxypentanoic acid, hydroxycaproic acid, hydroxyheptanoic acid, and hydroxyoctanoic acid.
[0022] Examples of lactones include lactones having 3 to 10 carbon atoms, such as propiolactone, butyrolactone, valerolactone, and ε-caprolactone.
[0023] Examples of the aliphatic dicarboxylic acid include saturated aliphatic dicarboxylic acids having 2 to 8 carbon atoms, such as oxalic acid, malonic acid, succinic acid, glutaric acid, and adipic acid, and unsaturated aliphatic dicarboxylic acids having 4 to 8 carbon atoms, such as maleic acid and fumaric acid.
[0024] Examples of the aliphatic diol include alkylene glycols having 2 to 6 carbon atoms, such as ethylene glycol, propylene glycol, butanediol, and hexanediol, and polyalkylene glycols having 2 to 4 carbon atoms, such as polyethylene glycol, polypropylene glycol, and polybutylene glycol.
[0025] These components may be used alone or in combination of two or more. In addition, the aliphatic polyester may further contain structural units derived from an aromatic dicarboxylic acid such as terephthalic acid, an aromatic diol such as bisphenol A, or an aromatic hydroxycarboxylic acid such as hydroxybenzoic acid, as long as it is decomposed by an aminolysis reaction or an ammonolysis reaction.
[0026] Among these, hydroxycarboxylic acid-based aliphatic polyesters such as polylactic acid (hereinafter also referred to as "PLA") and polyglycolic acid (hereinafter also referred to as "PGA"); lactone-based aliphatic polyesters such as poly-ε-caprolactone (hereinafter also referred to as "PCL"); and diol-dicarboxylic acid-based aliphatic polyesters such as polyethylene succinate and polybutylene succinate are preferred. PGA and PLA are preferred, with PGA being more preferred, from the viewpoint of having higher strength and degradability suitable for the binder resin of the polishing layer. That is, it is preferred that the aliphatic polyester contains polyglycolic acid as the main component. "Containing polyglycolic acid as the main component" means that the content of polyglycolic acid relative to the total amount of the aliphatic polyester is 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.
[0027] Polyglycolic acid is a copolymer of glycolic acid-derived structural units (-(-O-CH 2 Polyglycolic acid is a polymer containing a structural unit derived from glycolic acid, and is a polymer containing a structural unit derived from glycolic acid as a main component. Polyglycolic acid may be a homopolymer of glycolic acid or a copolymer of glycolic acid and a monomer copolymerizable therewith.
[0028] Examples of copolymerizable monomers include the above-mentioned oxycarboxylic acids other than glycolic acid, the above-mentioned lactones, aliphatic dicarboxylic acids, aliphatic diols, aromatic dicarboxylic acids, aromatic diols, and aromatic hydroxycarboxylic acids. Among these, lactic acid is preferred.
[0029] The term "mainly composed of structural units derived from glycolic acid" means that the content of structural units derived from glycolic acid is 50% by mass or more relative to the total amount of structural units constituting polyglycolic acid. The content of structural units derived from glycolic acid is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. When the content of structural units constituting glycolic acid is 50% by mass or more, the strength of the polyglycolic acid can be increased, and therefore sufficient strength can be obtained when used in a polishing pad.
[0030] Polylactic acid is a polymer containing structural units derived from L-lactic acid or D-lactic acid. Polylactic acid may be a homopolymer of L-lactic acid or D-lactic acid, or a copolymer of L-lactic acid or D-lactic acid with a monomer copolymerizable therewith. Examples of copolymerizable monomers include the above-mentioned oxycarboxylic acids other than lactic acid, the above-mentioned lactones, aliphatic dicarboxylic acids, aliphatic diols, aromatic dicarboxylic acids, aromatic diols, and aromatic hydroxycarboxylic acids.
[0031] The content of structural units derived from L-lactic acid or D-lactic acid in polylactic acid can be preferably 50% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more, based on the total amount of structural units constituting polylactic acid.
[0032] The weight-average molecular weight of the aliphatic polyester is not particularly limited, but is preferably 70,000 or more and 500,000 or less. When the weight-average molecular weight of the aliphatic polyester is 70,000 or more, the strength of the aliphatic polyester is higher, thereby further improving the retention and durability of the abrasive grains. Furthermore, even if the decomposition rate of the nitrogen-containing compound is fast, excessive collapse in a short period of time can be further suppressed. When the weight-average molecular weight of the aliphatic polyester is 500,000 or less, moldability can be further maintained. From the same viewpoint, the weight-average molecular weight of the aliphatic polyester is more preferably 90,000 or more and 400,000 or less, even more preferably 100,000 or more and 350,000 or less, and particularly preferably 110,000 or more and 300,000 or less.
[0033] The weight-average molecular weight of the aliphatic polyester can be measured by gel permeation chromatography (GPC). The measurement conditions can be as follows: (Measurement conditions) Apparatus: "Shodex-104" manufactured by Showa Denko Column: Two HFIP-606M columns connected in series with one HFIP-G column as a pre-column Column temperature: 40°C Eluent: HFIP solution containing 5 mM sodium trifluoroacetate Flow rate: 0.6 mL / min Detector: RI (differential refractive index) detector Molecular weight calibration: Five types of standard polymethyl methacrylate with different molecular weights
[0034] The content of the aliphatic polyester is preferably 20% by mass or more and 99% by mass or less, more preferably 30% by mass or more and 95% by mass or less, even more preferably 30% by mass or more and 90% by mass or less, and particularly preferably 50% by mass or more and 90% by mass or less, relative to the polishing layer (or the total amount of the composition).When the content of the aliphatic polyester is 20% by mass or more, the strength of the polishing layer containing abrasive grains is increased, which is preferable.When the content of the aliphatic polyester is 99% by mass or less, the proportion of abrasive grains is not too small, and the polishing rate is not too slow, which is preferable.When the content of the aliphatic polyester is above this level, excessive collapse of the polishing layer is suppressed, and a more stable polishing rate is easily obtained due to the dressing effect.
[0035] 1-1-2. Abrasive Grains The material of the abrasive grains is not particularly limited, and examples thereof include diamond, silicon carbide, boron carbide, boron nitride, silicon nitride, cerium oxide, aluminum oxide, zirconium oxide, silicon oxide, iron oxide, manganese oxide, magnesium oxide, calcium oxide, barium oxide, zinc oxide, titanium oxide, chromium oxide, barium carbonate, and calcium carbonate. Among these, diamond, boron carbide, and boron nitride are preferred from the viewpoint of further increasing the polishing rate, and diamond is more preferred from the viewpoint of facilitating processing of high-hardness substrates such as SiC substrates.
[0036] The median diameter of the abrasive grains varies depending on the desired degree of polishing, but is preferably 0.01 μm or more and 50 μm or less, more preferably 0.1 μm or more and 40 μm or less, even more preferably 1 μm or more and 20 μm or less, and particularly preferably 3 μm or more and 15 μm or less.
[0037] The median diameter of the abrasive grains can be determined from the particle size distribution measured in accordance with particle size analysis - laser diffraction and scattering method (ISO 13320:2020). Specifically, it can be measured using a laser diffraction particle size analyzer (e.g., Malvern Mastersizer 3000) at a measurement temperature of 21°C, using ion-exchanged water as the dispersion medium, with a refractive index of 1.330, and using the Mie theory as the light scattering model.
[0038] The content of the abrasive grains is not particularly limited, but is preferably 1% by mass or more and 80% by mass or less relative to the polishing layer (or the total amount of the composition). When the content of the abrasive grains is 1% by mass or more, the polishing rate can be further increased. When the content of the abrasive grains is 80% by mass or less, the formability or processability into a polishing pad can be further improved. From the same viewpoint, the content of the abrasive grains is more preferably 5% by mass or more and 70% by mass or less relative to the polishing layer (or the total amount of the composition), even more preferably 10% by mass or more and 70% by mass or less, and particularly preferably 10% by mass or more and 50% by mass or less.
[0039] The content of abrasive grains can be measured by thermogravimetric analysis (TGA).Specifically, on the surface of the polishing layer of unused polishing pad, when any straight line passing through the center O of the polishing layer is designated as line L, and the straight line passing through the center O of the polishing layer perpendicular to line L is designated as line M, the center O of the polishing layer, the midpoint between the center O of the polishing layer and the end of the polishing layer on line L are designated as a1 and a2, and the midpoint between the center O of the polishing layer and the end of the polishing layer on line M are designated as b1 and b2, then, from the range including the measurement points of O, a1, a2, b1 and b2, 100 mg or more of measurement samples are taken from the polishing layer, and suitably pulverized, and used as the measurement samples from each measurement point.20±2 mg of measurement sample is placed in a platinum pan, and in an air atmosphere, it is heated from room temperature to 800 ° C at a rate of 10 ° C / min, and kept at 800 ° C for 30 minutes, and components other than abrasive grains are burned off, and the remaining sample weight is divided by the mass of the measurement sample to determine the content of abrasive grains in the polishing layer at each measurement point. In the present application, the arithmetic mean value of the abrasive grain content at each of the five points was taken as the representative value of the abrasive grain content of the polishing layer.
[0040] 1-1-3. Other Components The base material containing an aliphatic polyester may further contain other components in addition to the aliphatic polyester and abrasive grains. Examples of other components include resins other than the aliphatic polyester and hydrolysis accelerators. In particular, from the viewpoint of further increasing the polishing rate, the base material may further contain a hydrolysis accelerator. One type of hydrolysis accelerator may be used alone, or two or more types may be used in combination.
[0041] The hydrolysis accelerator is a compound that accelerates the hydrolysis reaction of the aliphatic polyester, and is preferably a compound that dissolves in the polishing solution to accelerate the penetration of the solution into the aliphatic polyester, and more preferably a compound that generates an acid or alkali in the presence of water. Examples of such decomposition accelerators include carboxylic acid anhydrides, phosphorus compounds, cyclic esters, and basic metal oxides.
[0042] Examples of carboxylic acid anhydrides include hexanoic anhydride, octanoic anhydride, decanoic anhydride, lauric anhydride, myristic anhydride, palmitic anhydride, stearic anhydride, benzoic anhydride, succinic anhydride, maleic anhydride, phthalic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, butanetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, diphenylsulfonetetracarboxylic dianhydride, biphenyltetracarboxylic dianhydride, ethylene glycol bisanhydrotrimellitate, and glycerin bisanhydrotrimellitate monoacetate. Among these, phthalic anhydride, trimellitic anhydride, benzoic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and benzene-1,2,4,5-tetracarboxylic anhydride (pyromellitic anhydride) are preferred.
[0043] The phosphorus compound is preferably an organic phosphorus compound such as a phosphate ester or a phosphite ester, and more preferably an organic phosphorus compound having at least one selected from the group consisting of a long-chain alkyl group having 8 to 24 carbon atoms, an aromatic ring, and a pentaerythritol skeleton.
[0044] Examples of phosphate esters having a long-chain alkyl group having 8 to 24 carbon atoms include mono- or di-stearyl acid phosphate or a mixture thereof, and di-2-ethylhexyl acid phosphate. Examples of phosphites having an aromatic ring include tris(nonylphenyl)phosphite. Examples of phosphites having a pentaerythritol skeleton include cyclic neopentanetetraylbis(2,6-di-tert-butyl-4-methylphenyl)phosphite, cyclic neopentanetetraylbis(2,4-di-tert-butylphenyl)phosphite, and cyclic neopentanetetraylbis(octadecyl)phosphite.
[0045] Examples of cyclic esters include glycolide, lactide, ε-caprolactone, γ-valerolactone, δ-valerolactone, diglycolic anhydride, and glutaric anhydride.
[0046] Examples of basic metal oxides include magnesium oxide, zinc oxide, calcium oxide, sodium oxide, and copper oxide.
[0047] The content of the hydrolysis accelerator is not particularly limited, but can be, for example, 30% by mass or less based on the total amount of the aliphatic polyester.
[0048] The thickness of the polishing layer is not particularly limited, but when used for processing a substrate of a semiconductor device, for example, it is preferably 0.1 mm or more and 50 mm or less, more preferably 0.3 mm or more and 30 mm or less, even more preferably 0.4 mm or more and 10 mm or less, and particularly preferably 0.5 mm or more and 5 mm or less. A thickness of 0.1 mm or more is preferable from the viewpoint that the polishing layer can sufficiently hold abrasive grains.
[0049] 1-1-4 Physical Properties It is preferable that the strength of the matrix containing the aliphatic polyester is appropriately high.
[0050] (Tensile strength) The tensile strength of the base material at 25°C is preferably 55 MPa or more. If the tensile strength is 55 MPa or more, the abrasive grain retention force can be further increased. From the same viewpoint, the tensile strength of the base material is more preferably 60 MPa or more. There is no particular upper limit to the tensile strength of the base material, but it can be, for example, 1000 MPa or less. The tensile strength can be measured in accordance with ISO 527.
[0051] (Tensile Modulus) The tensile modulus of the base material at 25°C is preferably 1 GPa or more. When the tensile modulus is 1 GPa or more, when a polishing pad is brought into contact with the workpiece and a load is applied, the abrasive grains protruding from the surface are less likely to be pushed back into the base material. This makes it possible to reduce the decrease in polishing rate even when using small abrasive grains. In addition, it is possible to reduce the edge sagging of the workpiece after polishing (a phenomenon in which the edge is intensively scraped, resulting in a decrease in dimensional accuracy). From the same perspective, the tensile modulus of the base material is more preferably 3 GPa or more, and even more preferably 5 GPa or more. The upper limit of the tensile modulus of the base material is not particularly limited, but can be, for example, 50 GPa or less. The tensile modulus can be measured in accordance with ISO 527.
[0052] The tensile strength and tensile modulus of the base material can be adjusted by the type and content of the aliphatic polyester, the type and content of the hydrolysis accelerator, the weight average molecular weight, the cooling step during molding, etc. For example, if the content of the hydrolysis accelerator is low, the tensile strength and tensile modulus tend to be large.
[0053] 1-1-5. Shape The surface of the polishing layer may have grooves for supplying or discharging the polishing liquid to the polishing surface. This allows the polishing liquid to be easily distributed over the entire surface of the polishing layer through the grooves, and also allows shavings generated by hydrolysis of the hydrolyzable resin to be easily discharged to the outside through the grooves.
[0054] The grooves may have a circular, radial, lattice, or linear shape in plan view. The convex portions of the concave-convex pattern formed by the grooves may be arranged in an island shape.
[0055] 1-2. Other Layers The polishing pad may be composed of a polishing layer, or may further include other layers as necessary. Examples of other layers include a substrate layer and an adhesive layer. The substrate layer may be, for example, a resin film. In this case, the polishing layer may be disposed uniformly over the entire substrate layer, or may be disposed in a pattern. The adhesive layer may be an adhesive layer for attaching the polishing pad 100 to a polishing platen (platen 210, described below).
[0056] 1-3. Manufacturing Method The polishing pad according to this embodiment can be manufactured by any method. For example, the polishing pad can be manufactured through the steps of 1) obtaining a composition containing a base material containing an aliphatic polyester and abrasive grains, and 2) molding the obtained composition.
[0057] In step 1), the composition can be obtained by kneading, for example, the aliphatic polyester and the abrasive grains. Examples of kneading machines that can be used include rolls, kneaders, Banbury mixers, and extruders (single-screw or multi-screw). Kneading is preferably performed under heating to improve processability.
[0058] In step 2), the obtained composition is molded into a predetermined shape. The molding method is not particularly limited, and may be, for example, any of injection molding, melt extrusion molding, solidification extrusion molding, and compression molding.
[0059] 2. Method for Polishing an Object to be Polished A method for polishing an object to be polished according to one embodiment of the present invention will now be described with reference to the drawings.
[0060] 1 is a schematic diagram showing a polishing apparatus 200 using a polishing pad 100 according to the present embodiment. Note that detailed illustration of the polishing pad 100 is omitted in FIG.
[0061] 1, polishing apparatus 200 includes polishing pad 100, a disc-shaped surface plate 210 that supports polishing pad 100, a disc-shaped polishing head 230 that holds an object to be polished 220, a weight 240, and a supply nozzle 250 that supplies polishing liquid W. Surface plate 210 is rotatable by a rotation shaft (not shown), and polishing head 230 is rotatable by a rotation shaft 230A.
[0062] In this embodiment, the polishing pad 100 and the object to be polished 220 are slid relative to each other while the polishing liquid W is supplied to the surface of the polishing layer of the polishing pad 100, thereby polishing the object to be polished 220.
[0063] Specifically, first, the polishing pad 100 is attached to the surface plate 210. Next, the workpiece 220 held by the polishing head 230 is pressed against the polishing surface of the polishing pad 100, and the surface plate 210 and / or the polishing head 230 are rotated while supplying the polishing liquid W from the supply nozzle 250. This causes the polishing pad 100 and the workpiece 220 to slide relative to each other, polishing the processed surface (surface to be polished) of the workpiece 220.
[0064] (Polished object) The material of the polished object 220 is not particularly limited and may be a ceramic material, a glass material, or the like. Examples of ceramic materials include Si (silicon), SiC (silicon carbide), GaN (silicon nitride), GaAs (gallium arsenide), sapphire, etc., preferably SiC or GaN. Specifically, the polished object 220 may be a material for a semiconductor device or electronic component, particularly a Si substrate, a SiC substrate, a GaAs substrate, glass, or a substrate for a hard disk or LCD (liquid crystal display). Among these, a semiconductor wafer is preferred, a SiC substrate, a sapphire substrate, or a GaN substrate used in a power device is more preferred, and a SiC substrate or a GaN substrate is even more preferred.
[0065] (Polishing Liquid) The polishing liquid may contain a nitrogen-containing compound represented by formula (1) and water. Formula (1): H—N(((CH 2 ) n X) m -R 1 ) R 2
[0066] R in formula (1) 1 and R 2 is H or a hydrocarbon group having 1 to 22 carbon atoms. The hydrocarbon group may be linear or cyclic. Furthermore, the hydrocarbon group may be saturated or unsaturated.
[0067] Examples of chain hydrocarbon groups include alkyl groups having 1 to 22 carbon atoms, preferably 1 to 6 carbon atoms. Examples of cyclic hydrocarbon groups include cycloalkyl groups having 3 to 8 carbon atoms and aryl groups having 6 to 22 carbon atoms, preferably 6 to 10 carbon atoms. R 1 and R 2 may be bonded to each other to form a ring.
[0068] X in formula (1) is a divalent group selected from the group consisting of —O—, —NH—, —S—, and —COO—.
[0069] In formula (1), m is an integer of 0 to 3. n is an integer of 0 to 6. When m is 2 or more, the number of n and the type of atom of X may be different from each other.
[0070] The number of amino groups or groups represented by --NH-- in one molecule of the nitrogen-containing compound is not particularly limited, and may be one or two or more.
[0071] Such a nitrogen-containing compound may be any of ammonia, hydrazine, hydroxyamine, primary amine, secondary amine, or a corresponding polyamine. The nitrogen-containing compound may be used alone or in combination of two or more kinds.
[0072] Examples of primary amines include monoalkylamines [e.g., C1-10 alkylamines such as methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, and decylamine], alkanolamines [e.g., mono-C2-6 alkylamines such as monoethanolamine (2-aminoethyl alcohol), monopropanolamine, monoisopropanolamine, butanolamine, hexanolamine, 2-amino-2-methyl-1-propanol, and 2-amino-2-methyl-1,3-propanediol], and the like. canolamine or an ethylene oxide adduct thereof], cycloalkylamines (for example, C4-10 cycloalkylamines such as cyclopentylamine and cyclohexylamine), arylamines (for example, C6-10 arylamines such as aniline, toluidine, anisidine, phenetidine, and aminonaphthalene), aralkylamines (for example, benzylamine), thiolamines (for example, 2-aminoethanethiol, 2-(methylthio)ethanamine)), and aminoesters (for example, β-alanine, methyl 3-aminopropanoate, and 4-aminobutyric acid).
[0073] Examples of secondary amines include dialkylamines (e.g., diC1-10 alkylamines such as dimethylamine, diethylamine, dipropylamine, diisopropylamine, and dibutylamine), alkylalkanolamines (e.g., N-C1-3 alkylmono C2-6 alkanolamines such as N-methylethanolamine or ethylene oxide adducts thereof), dialkanolamines (e.g., diC2-6 alkanolamines such as diethanolamine, dipropanolamine, and diisopropanolamine or ethylene oxide adducts thereof), dithiolamines (e.g., 2,2'-azanediylbis(ethane-1-thiol), alkylcycloalkylamines (e.g., methylcyclohexylamine), alkylarylamines (e.g., N-methylaniline), alkylaralkylamines (e.g., N-methylbenzylamine), and cyclic amines (e.g., 5- to 8-membered cyclic amines such as pyrrolidine, piperidine, hexamethyleneimine, and morpholine).
[0074] Examples of the polyamines include polyamines corresponding to the monoamines described above. Examples of the linear primary polyamines include alkanediamines (C2-10 alkanediamines such as ethylenediamine, propylenediamine, tetramethylenediamine, and hexamethylenediamine), polyalkylenepolyamines (or polyalkyleneimines, for example, polyC2-4 alkylenepolyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine), alkanolamines (2-(3-aminopropylamino)ethanol, etc.), and aromatic primary polyamines (for example, xylylenediamine). Examples of the linear secondary polyamine include alkanamines (e.g., N,N'-dimethylethylenediamine, N,N'-dimethyl-1,3-diaminopropane), aromatic secondary polyamines (e.g., N,N'-dimethylxylylenediamine), and heterocyclic secondary polyamines (e.g., piperazine, 1,4,8,11-tetraazacyclotetradecane, triethylenediamine).
[0075] Among these, the nitrogen-containing compound preferably contains ammonia, hydrazine or hydroxyamine, and more preferably contains ammonia.
[0076] The pKa of the nitrogen-containing compound is preferably 11.5 or less, and more preferably 10.5 or less. A pKa of 11.5 or less can reduce damage to the polishing apparatus. The lower limit of the pKa of the nitrogen-containing compound is not particularly limited, but can be set to, for example, 5.97 or more in order to increase the decomposition reaction rate. The acid dissociation constant pKa of the nitrogen-containing compound may be determined by a known method commonly used in the technical field. For simple evaluation, literature values (e.g., Maruzen Experimental Chemistry Lectures, 2nd Edition, Vol. 5) or known values provided by reagent companies (e.g., Bordwell pKa Table (organicchemistrydata.org)) may be referenced. Methods for determining pKa include, for example, neutralization titration, absorptiometry, and capillary electrophoresis.
[0077] The pKa of a nitrogen-containing compound can be adjusted by the structure of the nitrogen-containing compound. For example, the fewer the number of hydrocarbon groups bonded to the nitrogen atom (or the more hydrogen atoms there are), the lower the pKa tends to be.
[0078] The content of the nitrogen-containing compound in the polishing liquid varies depending on the type of nitrogen-containing compound, but is, for example, 0.0001 to 15 M (mol / dm 3 ) is preferable. When the content of the nitrogen-containing compound is 0.0001M or more, the decomposition reaction rate of the aliphatic polyester contained in the polishing pad can be further increased. When the content of the nitrogen-containing compound is 15M or less, the decomposition reaction rate does not become too high, so excessive decomposition of the aliphatic polyester in the polishing pad can be suppressed and collapse in a short period of time can be further suppressed. From the same viewpoint, the content of the nitrogen-containing compound is more preferably 0.0001 to 10M.
[0079] The polishing liquid may further contain other components as necessary, provided that the effects of the present invention are not impaired. These other components include other alkaline substances, such as sodium hydroxide (NaOH) and potassium hydroxide (KOH). In an aqueous solution containing other alkaline substances, carboxylic acid terminals formed by hydrolysis remain as carboxylate ions, and oligomers of the polymer formed by hydrolysis are likely to be eluted into the solution. Therefore, the inclusion of other alkaline substances can further promote hydrolysis.
[0080] The pH of the polishing solution may be set so as to achieve the desired height of abrasive grain protrusion on the surface of the polishing layer, and although it depends on the type of aliphatic polyester, it is usually preferably at least 7 and less than 13. The pH of the polishing solution W is a value measured with a pH meter at 20°C.
[0081] The pH of the polishing liquid W can be adjusted by the content of the nitrogen-containing compound in the polishing liquid.
[0082] The temperature of the polishing liquid W is not particularly limited, but can be set to 1°C or higher and 60°C or lower.
[0083] In the above embodiment, the polishing liquid containing a specific nitrogen-containing compound and water is supplied to polish the workpiece 220. As a result, even under low pH conditions, the decomposition rate of the aliphatic polyester in the polishing pad is unlikely to decrease, and therefore the polishing rate is unlikely to decrease.
[0084] The present disclosure will be described below with reference to examples, which should not be construed as limiting the scope of the present disclosure.
[0085] 1. Preparation of materials 1-1. Polishing pad materials 1-1-1. Binder resin - PGA (homopolymer of glycolic acid, weight average molecular weight 298,000, tensile strength 112.8 MPa)
[0086] The weight average molecular weight and tensile strength of the PGA were measured by the following methods.
[0087] (Measurement of Weight-Average Molecular Weight) The weight-average molecular weight was measured by gel permeation chromatography (GPC). The measurement conditions were as follows: Apparatus: "Shodex-104" manufactured by Showa Denko K.K. Column: Two HFIP-606M columns connected in series with one HFIP-G column as a pre-column Column temperature: 40°C Eluent: HFIP solution containing 5 mM sodium trifluoroacetate Flow rate: 0.6 mL / min Detector: RI (differential refractive index) detector Molecular weight calibration: Five types of standard polymethyl methacrylate with different molecular weights
[0088] (Measurement of Tensile Strength) The tensile strength of the PGA was measured in accordance with ISO527.
[0089] 1-1-2. Abrasive grains Polycrystalline diamond powder (manufactured by Global Diamond, median diameter (D50): 5.93 μm, irregular shape)
[0090] The median diameter of the abrasive grains was measured by the following method.
[0091] (Measurement of median diameter) Using a laser diffraction particle size measuring instrument Mastersizer 3000 (Malvern), the measurement temperature is 21 ° C, the dispersion medium is ion-exchanged water, the dispersion medium refractive index is 1.330, the light scattering model is Mie theory, the particle absorption rate of polycrystalline diamond powder is 0.100, the particle refractive index is 2.418, and the measurement conditions are set. The amount of abrasive grains added to the dispersion medium is adjusted so that the laser scattering intensity is 4% or more and 10% or less.
[0092] 1-2. Materials for polishing solution 1-2-1. Alkaline components ・NH 3 (ammonia, pKa = 9.25) NaOH (sodium hydroxide) DBU (1,8-diazabicyclo[5.4.0]-7-undecene, tertiary amine) TEOA (triethanolamine, tertiary amine) TEA (triethylamine, tertiary amine) The pKa of ammonia used was the value given in Maruzen Experimental Chemistry Lectures, 2nd edition, Vol. 5.
[0093] 2. Decomposition test 2-1. Preparation of test pieces The PGA was injection molded to obtain ISO 1 dumbbell pieces, which were then cut into 10 mm x 10 mm x 4 mm thick to obtain test pieces.
[0094] 2-2. Preparation of alkaline aqueous solutions 1 to 8 The alkaline components shown in Table 1 were added to water to give the concentrations shown in the table to prepare alkaline aqueous solutions 1 to 8. The pH of the alkaline aqueous solutions was confirmed using pH test paper.
[0095] 2-3. Decomposition Test (Tests 1-1 to 1-8) 90 mL of the alkaline aqueous solution shown in Table 1 was placed in a vial, and three of the test pieces prepared above were immersed in the solution. The immersion was carried out at 23°C for 1 hour, 3 hours, and 168 hours, respectively, and the test pieces were removed after each immersion time, and the weights of the three test pieces were measured. The weight change rate was calculated by applying the average weight of the three test pieces after immersion and the average weight of the three test pieces before immersion to the following formula: Weight change rate (%) = [1 - (average weight of test pieces after immersion / average weight of test pieces before immersion)] x 100
[0096] The results of tests 1-1 to 1-8 are shown in Table 1.
[0097]
[0098] As shown in Table 1, it can be seen that the alkaline aqueous solution 1 containing ammonia (Tests 1-1 to 1-3) exhibits a weight change rate (particularly the weight change rate after 168 hours) equal to or greater than that of the alkaline aqueous solution 8 containing sodium hydroxide, even at a low pH. It can also be seen that the alkaline aqueous solution 1 containing ammonia exhibits a higher weight change rate (particularly the weight change rate after 168 hours) than the alkaline aqueous solutions 4 to 7 containing tertiary amines such as TEOA, TEA, and DBU, even at a low pH.
[0099] 3. XPS Analysis 3-1. Preparation of Test Pieces The PGA was press-molded to obtain a sheet of 100 mm × 100 mm × t 0.5 mm, which was then annealed at 120° C. for 2 hours. The obtained sheet was then cut into a 6 mm × 6 mm square to obtain a test piece.
[0100] 10 mL of the treatment solution shown in Table 2 was placed in a vial, and one of the test pieces prepared above was immersed in it for 1 hour at 23° C. Thereafter, the test piece was removed from the treatment solution, washed with pure water, and then air-dried overnight at room temperature (Conditions 2 to 5).
[0101] 3-3. XPS Measurement After Immersion The elemental composition ratios of C, N, O, Si, and Na in the surface-modified region of the test piece were measured using an X-ray photoelectron spectrometer (e.g., JPS 9010MC, manufactured by JEOL Ltd.) under the following conditions for each binding energy range. The measurement was performed without removing the measurement sample from the measurement device and without changing the measurement environment during the process of measuring the spectrum corresponding to each element. The measurement conditions were as follows: MgKα radiation was used as the X-ray source without being converted to monochromatic light; acceleration voltage was 12 kV; analysis diameter was 3 mmΦ; photoelectron take-off angle was 90°; pass energy was 10 eV; energy step was 0.1 eV; and a neutralization gun was used at 2 mA and 2 V to irradiate the X-rays. The background was subtracted using the Shirley method from the spectrum obtained by integrating 8 or more times, the peak area was determined, and the abundance (atom%) of each atom was calculated using the following formula. Amount of atom present=Peak area / Correlation sensitivity coefficient For comparison, the test piece before immersion (Condition 1) was also measured in the same manner.
[0102] The analysis results of the test pieces before immersion (condition 1) and after immersion (conditions 2 to 5) are shown in Table 3.
[0103]
[0104] As shown in Table 2, when the test piece was immersed in an aqueous sodium hydroxide solution (conditions 3 and 4), almost no nitrogen atoms were detected from the test piece after immersion. In contrast, when the test piece was immersed in an aqueous ammonia solution (condition 5), nitrogen atoms were detected from the test piece after immersion.
[0105] These results suggest that the nitrogen atoms detected in the test specimen treated with an aqueous ammonia solution originate from decomposition products with amide bonds remaining on the test specimen, indicating that ammonolysis, rather than hydrolysis, is occurring.
[0106] 4. Preparation and evaluation of polishing pad [Test 2-1] (1) Preparation of polishing pad (1.1) Kneading process The abrasive grains were weighed to be 50% by mass relative to the PGA binder resin, and kneaded using a Laboplastomill (manufactured by Toyo Seiki Seisakusho) to obtain a composition. Kneading was carried out at a predetermined heater temperature, with a preheating time of 1 minute, a kneading time of 5 minutes, and a rotation speed of 50 rpm. The heater temperature was set to 250 ° C.
[0107] (1.2) Molding Step Figures 2A to 2C are schematic diagrams showing the components of the molding apparatus 300 used in the examples. In these figures, reference numeral 301 denotes a SUS plate, and 302 denotes aluminum foil. A 0.5 mm thick SUS mold 303 with a hole 150 mm in diameter was arranged as shown in Figure 2A, and the kneaded composition 304 was placed in the SUS mold 303 and press-molded to obtain a polishing pad 100 consisting of a polishing layer 0.5 mm thick (see Figures 2B and 2C). The temperature of the press was set to the same temperature as the heater temperature of the Labo Plastomill.
[0108] (2) Polishing Test The polishing test was performed by mounting a polishing pad on a polishing apparatus 200 as shown in Fig. 1. Specifically, the polishing pad was attached to a surface plate 210 (polishing plate) using a double-sided adhesive film (e.g., AS ONE OCA50-A4). The double-sided adhesive sheet was attached to the polishing pad and polishing plate using a rubber roller or the like to prevent air bubbles from being trapped when the sheet was attached to the polishing pad and polishing plate.
[0109] Next, a SiC substrate (20 x 20 mm square) was pressed against the rotating polishing pad as the workpiece 220 to perform polishing. The polishing conditions were as follows. At this time, the load of the jig (polishing head 230) and weight 240 was applied to the substrate. (Polishing conditions) Polishing device: Dialap ML-150P (manufactured by Marutoh Co., Ltd.) Polishing disc rotation speed: 100 rpm Polishing disc diameter: 150 mm diameter Forced drive or oscillation of workpiece: None Surface pressure: 250 gf / cm 2 Polishing liquid flow rate: 75 mL / h Polishing liquid: 1 M NH 3 Aqueous solution (20° C.), pH=11.7. The pH of the polishing solution was measured using a compact pH meter (manufactured by HORIBA) before the start of the polishing test.
[0110] (3) Evaluation (3.1) Polishing rate of the workpiece The thickness of the workpiece was measured using an electric micrometer Millimar 1240 (manufactured by Mahr) while the workpiece was attached to a jig. The thickness of the workpiece was measured at five locations and the average value was used. The polishing rate was calculated from the polishing time (min) and the thickness reduction value (removal amount, μm).
[0111] (3.2) Removal rate of polishing pad The thickness of the polishing pad was measured using an electric micrometer Millimar 1240 (manufactured by Mahr) while the polishing pad was attached to a jig. The thickness of the polishing pad was measured at three locations and the average value was used. The removal rate was calculated from the polishing time (min) and the thickness reduction value (removal amount, μm).
[0112] [Test 2-2] The same method as in Test 1 was used, except that the polishing liquid was changed to a 0.01 M NaOH aqueous solution (20° C.) with a pH of 12.1.
[0113] [Test 2-3] Test 2-3 was carried out in the same manner as Test 1, except that the polishing liquid was changed to a 0.1 M NaOH aqueous solution (20° C.) with a pH of 13.0.
[0114] A graph showing the change in the polishing rate of the workpiece over time is shown in Figure 3A, and a graph showing the change in the removal rate of the polishing pad over time is shown in Figure 3B. In these graphs, the horizontal axis represents the polishing time (minutes), and the vertical axis represents the polishing rate (µm / h). The results are summarized in Figure 4.
[0115] As shown in Figures 3A and 4, Test 2-1 (pH = 11.7) using an aqueous ammonia solution can maintain a polishing rate for the workpiece equal to or greater than that of Test 2-2 (pH = 12.1) and Test 2-3 (pH = 12.9) using an aqueous sodium hydroxide solution.
[0116] Furthermore, as shown in Figures 3B and 4, Test 2-1 (pH = 11.7) using an aqueous ammonia solution had a higher polishing pad removal rate than Test 2-2 (pH = 12.1) and Test 2-3 (pH = 13.0) using an aqueous sodium hydroxide solution.
[0117] These results show that by using an aqueous ammonia solution, even at a low pH, the PGA is worn down to a level equal to or greater than that when an aqueous sodium hydroxide solution is used, and the polishing rate for SiC can be maintained at a high level.
[0118] This application claims priority based on Japanese Patent Application Nos. 2023-91781 and 2023-091782, filed June 2, 2023, Japanese Patent Application No. 2023-119986, filed July 24, 2023, and Japanese Patent Application No. 2024-050250, filed March 26, 2024. The contents of the specifications and drawings of these applications are incorporated herein by reference in their entirety.
[0119] According to the present invention, it is possible to provide a method for polishing an object to be polished in which the polishing rate is not likely to decrease even when a polishing liquid with a low pH is used.
[0120] REFERENCE SIGNS LIST 100 Polishing pad 110 Polishing layer 110A Groove 111 Aliphatic polyester 112 Abrasive grains 200 Polishing device 210 Surface plate 220 Object to be polished 230 Polishing head 230A Rotating shaft 240 Weight 250 Supply nozzle 301 Ferro plate 302 Aluminum foil 303 Aluminum punching sheet 304 SUS mold 305 Composition
Claims
1. A method for polishing an object to be polished, comprising the steps of supplying a polishing liquid to a surface of a polishing pad having a polishing layer containing a composition containing an aliphatic polyester and abrasive grains, while sliding the polishing pad and the object to be polished relative to each other, thereby polishing the object to be polished, wherein the polishing liquid contains a nitrogen-containing compound represented by the following formula (1) and water. Formula (1): H-N(((CH 2 ) n X) m -R 1 ) R 2 (In formula (1), R 1 and R 2 is H or a hydrocarbon group having 1 to 22 carbon atoms, R 1 and R 2 may be bonded to each other to form a ring, X is a divalent group selected from the group consisting of -O-, -NH-, -S-, and -COO-, m is an integer of 0 to 3, n is an integer of 0 to 6, and when m is 2 or more, the number of n and the type of atom of X may be different from each other.
2. The method for polishing an object to be polished according to claim 1, wherein the nitrogen-containing compound includes ammonia, hydrazine or hydroxylamine.
3. The method for polishing an object to be polished according to claim 1 or 2, wherein the aliphatic polyester has polyglycolic acid as a main component.
4. The method for polishing an object to be polished according to any one of claims 1 to 3, wherein the pH of the polishing liquid is 7 or more and less than 13.
Citation Information
Patent Citations
Polishing pad
JP2005305570A