Organic material for semiconductor cmp, and slurry composition comprising same

Polymer micelles with tailored amphiphilic structures address the size limitations of inorganic nanoparticles in CMP processes, offering improved control and performance in semiconductor manufacturing by adjusting particle size and surface bonding forces, thus enhancing CMP efficacy.

WO2024248455A1PCT designated stage expired Publication Date: 2024-12-05IND ACADEMIC COOP FOUND YONSEI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007194
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-21
Filing Date
2024-05-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional inorganic nanoparticles used as abrasives or anti-polishing agents in semiconductor CMP processes have limitations in size and effectiveness for smaller scales, particularly as semiconductor device line widths narrow and integration increases.

Method used

The development of polymer micelles with specific amphiphilic structures, including hydrophilic polyglycerol and hydrophobic phenol groups, which can be adjusted in size and surface bonding force, replacing inorganic nanoparticles as CMP slurry additives.

Benefits of technology

The polymer micelles enable precise control of particle size and surface interactions, enhancing CMP performance by improving recess and polishing rates, and can be applied as abrasives or anti-polishing agents in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007194_05122024_PF_FP_ABST
    Figure KR2024007194_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in one embodiment of the present invention is a polymer micelle having a micelle structure composed of an amphiphilic material with both a hydrophilic group and a hydrophobic group, wherein the hydrophilic group includes a polyglycerol functional group, and the hydrophobic group includes a phenol group having a hydrophobic substituent bonded to the end thereof and modified to be hydrophobic.
Need to check novelty before this filing date? Find Prior Art

Description

Organic material for semiconductor CMP and slurry composition containing the same

[0001] The present invention relates to a novel material and a slurry composition containing the same, and more particularly, to a novel material that can replace inorganic nanoparticles that have been conventionally used as abrasives or anti-abrasives for CMP, and a slurry composition containing the same.

[0002] The CMP process is a process of planarizing the surface of a wafer using a polishing pad and a slurry composition during semiconductor manufacturing. It is a process of bringing the polishing pad and the wafer into contact, and then polishing the polishing pad and the wafer using a slurry composition containing an abrasive while performing an orbital motion that mixes rotational and linear motion.

[0003] The slurry composition used in the CMP process is largely composed of compounds such as abrasive particles, which exert physical action, and etchants, which exert chemical action. Therefore, the slurry composition selectively etches exposed areas of the wafer surface through physical and chemical actions, thereby performing a more optimized and comprehensive planarization process.

[0004] In performing the above CMP process, inorganic nanoparticles have been used as CMP slurry additives in the past. However, since the inorganic nanoparticles have limitations in the size that can be produced, they have limitations as CMP slurry additives targeting smaller scales.

[0005] Recently, due to the narrowing of the line width of semiconductor devices and the high integration of ICs, there is a need to overcome the above limitations.

[0006] Prior patent document: Republic of Korea Patent No. 10-1178236

[0007]

[0008] The technical problem to be achieved by the present invention is to provide a novel material that can replace inorganic nanoparticles that have been conventionally used as abrasives or anti-abrasives for CMP, and a slurry composition containing the same.

[0009]

[0010] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.

[0011]

[0012] To achieve the above technical task, one embodiment of the present invention provides a polymer micelle.

[0013] According to one embodiment of the present invention, the polymer micelle is

[0014] It may be a polymer micelle having a micelle structure composed of an amphiphilic substance having both a hydrophilic group and a hydrophobic group, wherein the hydrophilic group includes a polyglycerol functional group, and the hydrophobic group includes a phenol group hydrophobically modified by bonding a hydrophobic substituent to the terminal.

[0015]

[0016] Additionally, according to one embodiment of the present invention, there may be a polymer micelle characterized in that the hydrophobic substituent is an alkyl group of C7 to C9.

[0017] In addition, according to one embodiment of the present invention, there may be a polymer micelle characterized in that the polyglycerol functional group is a hyperbranched type polyglycerol functional group.

[0018] Additionally, according to one embodiment of the present invention, the amphiphilic material may be a polymer micelle characterized by a degree of branching of 0.4 to 0.8.

[0019] In addition, according to one embodiment of the present invention, there may be a polymer micelle characterized in that the degree of polymerization of the polymer micelle is 10 to 17.

[0020] In addition, according to one embodiment of the present invention, the amphiphilic material may be a polymer micelle characterized by being represented by the following chemical formula 1.

[0021] [Chemical Formula 1]

[0022]

[0023] In addition, according to one embodiment of the present invention, there may be a polymer micelle characterized in that the polyglycerol functional group is a linear type polyglycerol functional group.

[0024] In addition, according to one embodiment of the present invention, the amphiphilic material may be a polymer micelle characterized by being represented by the following chemical formula 2.

[0025] [Chemical Formula 2]

[0026]

[0027] In the above chemical formula 2, n is an integer from 1 to 200.

[0028] More preferably, n may be an integer from 14 to 17.

[0029]

[0030] Additionally, according to one embodiment of the present invention, there may be a polymer micelle characterized in that the micelle structure has a diameter of 5 nm to 7 nm.

[0031]

[0032] In order to achieve the above technical task, another embodiment of the present invention provides a polymer material.

[0033] According to one embodiment of the present invention, the polymer material is

[0034] A polymer material may be a polymer comprising a 1,1,1-Tris(hydroxymethyl)propane group and a hyperbranched type polyglycerol functional group, wherein the 1,1,1-Tris(hydroxymethyl)propane group is characterized in that some of the hydroxyl groups are substituted or unsubstituted.

[0035]

[0036] Additionally, according to one embodiment of the present invention, the polymer material may be a polymer material characterized by a degree of branching of 0.4 to 0.8.

[0037] In addition, according to one embodiment of the present invention, the polymer material may be a polymer material characterized by being represented by the following chemical formula 3.

[0038] [Chemical Formula 3]

[0039]

[0040] In the above chemical formula 3, R represents a functional group represented by the following chemical formula 4.

[0041] [Chemical Formula 4]

[0042]

[0043] In the above chemical formula 4, the * part is the part where a bond is formed.

[0044]

[0045] In addition, according to one embodiment of the present invention, there may be a polymer material characterized in that the degree of polymerization of the polymer material is 10 to 17.

[0046]

[0047] In order to achieve the above technical task, another embodiment of the present invention provides an abrasive for CMP.

[0048] According to one embodiment of the present invention, the abrasive for CMP is

[0049] It may be a CMP abrasive comprising the polymer micelles described above, characterized in that it can be applied to at least one material selected from the group consisting of tungsten (W), silica (SiO2), cobalt (Co), and rubidium (Rb).

[0050]

[0051] In addition, according to one embodiment of the present invention, there may be a CMP abrasive comprising the aforementioned polymer material, characterized in that it can be applied to at least one material selected from the group consisting of tungsten (W), silica (SiO2), cobalt (Co), and rubidium (Rb).

[0052]

[0053] In order to achieve the above technical task, another embodiment of the present invention provides an anti-abrasive agent for CMP.

[0054] According to one embodiment of the present invention, the CMP anti-abrasive agent is:

[0055] It may be a CMP anti-polishing agent characterized in that it can be applied to molybdenum, including the polymer micelles described above.

[0056]

[0057] In order to achieve the above technical task, another embodiment of the present invention provides a slurry composition for CMP.

[0058] According to one embodiment of the present invention, the slurry composition for CMP comprises:

[0059] It may be a slurry composition for CMP characterized by including the abrasive for CMP described above.

[0060] In addition, according to one embodiment of the present invention, there may be a slurry composition for CMP, characterized in that the abrasive is contained in a ratio of 0.5 wt% to 2.5 wt% with respect to the entire composition.

[0061] Additionally, according to one embodiment of the present invention, there may be a slurry composition for CMP characterized by including the above-described anti-polishing agent.

[0062] In addition, according to one embodiment of the present invention, there may be a slurry composition for CMP, characterized in that the anti-abrasive agent is contained in a ratio of 0.5 wt% to 2.5 wt% with respect to the entire composition.

[0063]

[0064] According to one embodiment of the present invention, a novel material that can replace inorganic nanoparticles that have been conventionally used as an abrasive or anti-abrasive for CMP and a slurry composition including the same can be provided.

[0065] According to one embodiment of the present invention, in the case of polymer micelles, the particle size can be controlled to a level of several nanometers, and the strength and surface bonding force can also be easily controlled depending on the composition, and can replace inorganic nanoparticles used as conventional CMP abrasives or anti-abrasives.

[0066] In addition, according to one embodiment of the present invention, a novel polymer micelle for a CMP slurry additive that can be used for recess improvement, polishing rate improvement, and other components can be provided compared to conventional CMP slurry additives.

[0067]

[0068] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0069]

[0070] Figure 1 is a synthesis table of novel materials according to one embodiment of the present invention.

[0071] Figure 2 is TMP-hbPG according to one embodiment of the present invention. 13 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0072] Figure 3 is an OP-hbPG according to one embodiment of the present invention. 13 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0073] Figure 4 is a linPG according to an embodiment of the present invention. 14 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0074] Figure 5 is an OP-hbPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0075] Figure 6 is a table summarizing quantitative data of the materials used in the synthesis of Figure 5.

[0076] Figure 7 is an OP-hbPG according to an embodiment of the present invention. 13 Chemical reaction formula and when potassium naphthalenide is used in the manufacturing process 1 This is a graph showing the results of H-NMR analysis.

[0077] Figure 8 is an OP-hbPG according to an embodiment of the present invention. 13This graph shows the results of C-NMR analysis when potassium naphthalenide was used in the manufacturing process.

[0078] Figure 9 is a table summarizing quantitative data of the materials used in the synthesis of Figure 7.

[0079] Figure 10 is an OP-linearPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0080] Figure 11 is a table summarizing quantitative data of the materials used in the synthesis of Figure 10.

[0081] Figure 12 is an OP-linearPG according to an embodiment of the present invention. 13 This is a graph and table showing the GPC analysis results data when MeOK was used in the manufacturing process.

[0082] Figure 13 is an OP-linPG according to an embodiment of the present invention. 13 This is a table and graph measuring the polishing performance.

[0083] Figure 14 is a table and graph showing the polishing performance according to DP of OP-hbPG according to one embodiment of the present invention.

[0084]

[0085] Hereinafter, the present invention will be described with reference to the attached drawings. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein. It should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.

[0086] In addition, in order to clearly explain the present invention in the drawings, parts unrelated to the description are omitted, and similar parts are given similar drawing reference numerals throughout the specification.

[0087] Throughout the specification, when a part is said to be "connected (connected, contacted, coupled)" to another part, this includes not only cases where it is "directly connected" but also cases where it is "indirectly connected" with another part in between.

[0088] In addition, when it is said that a part such as a layer, film, region, or plate is “on” another part, this includes not only the case where it is “directly above” the other part, but also the case where there is another part in between. In addition, in the present specification, when it is said that a part such as a layer, film, region, or plate is formed on another part, the direction in which it is formed is not limited to the upper direction, but also includes the case where it is formed in the side or lower direction. Conversely, when it is said that a part such as a layer, film, region, or plate is “under” another part, this includes not only the case where it is “directly below” the other part, but also the case where there is another part in between.

[0089] In this specification, the terms "upper surface" and "lower surface" are used as relative concepts to facilitate understanding of the technical concepts of the present invention. Therefore, "upper surface" and "lower surface" do not refer to specific directions, locations, or components, and are interchangeable.

[0090] For example, 'upper surface' can be interpreted as 'lower surface', and 'lower surface' can be interpreted as 'upper surface'. Accordingly, 'upper surface' can be expressed as 'first' and 'lower surface' can be expressed as 'second', or 'lower surface' can be expressed as 'first' and 'upper surface' can be expressed as 'second'. However, within one embodiment, 'upper surface' and 'lower surface' are not used interchangeably.

[0091] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and shall not be interpreted in an idealized or overly formal sense unless explicitly defined herein.

[0092] Additionally, when a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0093] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0094]

[0095] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0096] A polymer micelle according to one embodiment of the present invention is described.

[0097]

[0098] As an example of the above embodiment, there may be a polymer micelle having a micelle structure composed of an amphiphilic substance having both a hydrophilic group and a hydrophobic group, wherein the hydrophilic group includes a polyglycerol functional group, and the hydrophobic group includes a phenol group hydrophobically modified by bonding a hydrophobic substituent to the terminal.

[0099] Inorganic nanoparticles, which have been used as abrasives or anti-abrasives for CMP, have limitations in the size that can be produced, and thus have limitations as CMP slurry additives targeting smaller scales.

[0100] On the other hand, in the case of the polymer micelle according to the above embodiment, the particle size can be controlled to a level of several nanometers (nm), and the strength and surface bonding force can also be easily controlled depending on the composition, so the above-described limitations can be overcome.

[0101] As described above, the particle size, strength, surface bonding force, etc. of the polymer micelle may vary greatly depending on the monomer constituting the polymer micelle, the functional group included in the monomer, the composition of the constituent materials, etc., and therefore, in order to have properties suitable for the intended use, the above elements may be important components, and the above embodiment of the present invention is a novel material not previously disclosed.

[0102]

[0103] As an example of the above embodiment, there may be a polymer micelle characterized in that the hydrophobic substituent is an alkyl group of C7 to C9.

[0104] As an example of the above embodiment, the hydrophobic substituent may be a C8 alkyl group,

[0105] More specifically, the hydrophobic substituent may be a tert-Octyl group.

[0106]

[0107] As an example of the above embodiment, there may be a polymer micelle characterized in that the polyglycerol functional group is a hyperbranched type polyglycerol functional group.

[0108] At this time, the multi-branched polyglycerol functional group has a hydroxyl group (-OH) at the end of many branches, and the hydroxyl group (-OH) interacts with the surface of the metal in the CMP process.

[0109]

[0110] At this time, the PG (polyglycerol) included in the above embodiment has the advantage of being able to easily control the shape into different forms of linear type and hyperbranched type.

[0111]

[0112] As an example of the above embodiment, the amphiphilic material may be a polymer micelle characterized by a degree of branching of 0.4 to 0.8.

[0113]

[0114] As an example of the above embodiment, there may be a polymer micelle characterized in that the degree of polymerization of the polymer micelle is 10 to 17.

[0115]

[0116] The lower the above polymerization value, the lower the mechanical removal rate (MRR) value, and the less significant the effect on the static etching rate (SER).

[0117] The MRR / SER value tends to be higher as the polymerization degree value is lower, which means that the physical polishing effect is higher as the polymerization degree value is lower.

[0118] In the above example, the polymerization degree value of the polymer micelle can be formed at a low level of 10 to 17.

[0119]

[0120] As an example of the above embodiment, the amphiphilic material may be a polymer micelle characterized by being represented by the following chemical formula 1.

[0121] [Chemical Formula 1]

[0122]

[0123] The reaction formula for synthesizing the polymer micelle corresponding to the above chemical formula 1 is as shown in the following chemical reaction formula 1.

[0124]

[0125] [Chemical Reaction Formula 1]

[0126]

[0127] There may be a polymer micelle, which is distinguished from the polymer micelle corresponding to the above chemical formula 1, characterized in that the polyglycerol functional group is a linear type polyglycerol functional group.

[0128]

[0129] The amphiphilic substance having the linear type polyglycerol functional group can be expressed by the following chemical formula 2.

[0130]

[0131] [Chemical Formula 2]

[0132]

[0133] In the above chemical formula 2, n is an integer from 1 to 200.

[0134] More preferably, n may be an integer from 14 to 17.

[0135]

[0136] When the above material is used in a CMP slurry, high efficiency can be obtained even at a relatively low molecular weight with an n value of 14 to 17.

[0137]

[0138] The reaction formula for synthesizing the polymer micelle corresponding to the above chemical formula 2 is as shown in the following chemical reaction formula 2.

[0139]

[0140] [Chemical Reaction Formula 2]

[0141]

[0142] As described above, in the case of the polymer micelle according to the above embodiment, the particle size can be controlled to a level of several nanometers (nm), and among them, there may be a polymer micelle characterized by having a diameter of 5 nm to 7 nm.

[0143]

[0144] As described above, the polymer micelle has an extremely small particle size of 5 nm to 7 nm in diameter, which is much smaller than the inorganic silica nanoparticles used previously, and thus has the advantage of enabling more reliable etching of the edge portion in CMP etching.

[0145]

[0146] A polymer material according to another embodiment of the present invention is described.

[0147]

[0148] As an example of the above embodiment, it includes a 1,1,1-Tris(hydroxymethyl)propane group and a hyperbranched type polyglycerol functional group,

[0149] The above 1,1,1-Tris(hydroxymethyl)propane group may be a polymer material characterized in that some of the hydroxyl groups are substituted or unsubstituted.

[0150]

[0151] The hydroxyl group included in the above 1,1,1-Tris(hydroxymethyl)propane group may be substituted with one or more substances selected from the group consisting of an aliphatic group, aromatic, nitro, ether, and ester.

[0152] However, it is not suitable when substituted with amine because the reaction may be initiated.

[0153]

[0154] As an example of the above embodiment, the polymer material may be characterized by a degree of branching of 0.4 to 0.8.

[0155]

[0156] As an example of the above embodiment, the polymer material may be a polymer material characterized by being represented by the following chemical formula 3.

[0157] [Chemical Formula 3]

[0158]

[0159] In the above chemical formula 3, R represents a functional group represented by the following chemical formula 4.

[0160] [Chemical Formula 4]

[0161]

[0162] In the above chemical formula 4, the * part is the part where a bond is formed.

[0163]

[0164] The reaction formula for synthesizing the polymer micelle corresponding to the above chemical formula 3 is as shown in the following chemical reaction formula 3.

[0165]

[0166] [Chemical Reaction Formula 3]

[0167]

[0168]

[0169] As an example of the above embodiment, there may be a polymer micelle characterized in that the degree of polymerization of the polymer micelle is 10 to 17.

[0170]

[0171] As mentioned above, the lower the polymerization degree value, the lower the mechanical removal rate (MRR) value, and the effect on the static etching rate (SER) is not large.

[0172] The MRR / SER value tends to be higher as the polymerization degree value is lower, which means that the physical polishing effect is higher as the polymerization degree value is lower.

[0173] In the above example, the polymerization degree value of the polymer micelle can be formed at a low level of 10 to 17.

[0174]

[0175] An abrasive for CMP according to another embodiment of the present invention is described.

[0176]

[0177] As an example of the above embodiment, there may be a CMP abrasive comprising a polymer micelle having a hyperbranched type polyglycerol functional group among the polymer micelles described above, and characterized in that it can be applied to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

[0178]

[0179] As an example of the above embodiment, there may be a CMP abrasive comprising a polymer material characterized in that it includes the above-described 1,1,1-Tris(hydroxymethyl)propane group and a hyperbranched type polyglycerol functional group, wherein the 1,1,1-Tris(hydroxymethyl)propane group is characterized in that some hydroxyl groups are substituted or unsubstituted, and is applicable to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

[0180]

[0181] An anti-abrasive agent for CMP according to another embodiment of the present invention is described.

[0182]

[0183] As an example of the above embodiment, there may be a CMP polishing inhibitor characterized in that it can be applied to molybdenum, which comprises a polymer micelle having a hyperbranched type polyglycerol functional group among the polymer micelles described above.

[0184]

[0185] As an example of the above embodiment, there may be a CMP polishing inhibitor characterized in that it includes a polymer micelle having a linear type polyglycerol functional group among the polymer micelles described above, and can be applied to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

[0186]

[0187] A slurry composition according to another embodiment of the present invention is described.

[0188]

[0189] As an example of the above embodiment, there may be a slurry composition for CMP characterized by including a CMP abrasive including a polymer micelle having a hyperbranched type polyglycerol functional group among the polymer micelles described above.

[0190] There may be a CMP slurry composition characterized in that the CMP abrasive is contained in a ratio of 0.5 wt% to 2.5 wt% with respect to the total mass of the CMP slurry composition.

[0191]

[0192] When the ratio of the CMP abrasive to the total mass of the CMP slurry composition is 0.5 wt% to 2.5 wt%, the MRR and DER are formed high, and in particular, the DER value at 0.5 wt% and 1 wt% is formed higher than that of the existing material (Triton-X).

[0193] This is explained in more detail in Experimental Example 4 below.

[0194]

[0195] As an example of the above embodiment, there may be a slurry composition for CMP characterized by including an anti-abrasive agent for CMP including a polymer micelle having the linear type polyglycerol functional group described above.

[0196] There may be a CMP slurry composition characterized in that the CMP anti-abrasive agent is contained in a ratio of 0.5 wt% to 2.5 wt% with respect to the total mass of the CMP slurry composition.

[0197] As can be confirmed in Experimental Example 4 below, it can be confirmed that the inhibitor effect is the greatest at 1.0 wt%.

[0198]

[0199] As an example of the above embodiment, there may be a slurry composition for CMP characterized in that it includes a CMP abrasive including a polymer material including the above-described 1,1,1-Tris(hydroxymethyl)propane group and a hyperbranched type polyglycerol functional group, wherein some of the 1,1,1-Tris(hydroxymethyl)propane groups are substituted or unsubstituted.

[0200] There may be a CMP slurry composition characterized in that the CMP abrasive is contained in a ratio of 0.5 wt% to 2.5 wt% with respect to the total mass of the CMP slurry composition.

[0201]

[0202] When the concentration of the above abrasive is 2.5 wt%, it has the same level of MRR effect as the existing material (Triton-X), but at a lower concentration, it shows a low MRR effect.

[0203] In the case of DER, it shows performance that is more than 5% better than the existing material (Triton-X) at 0.5 wt% or 2.5 wt%.

[0204]

[0205] [Manufacturing example]

[0206] Referring to Figure 1, examples of synthesis of novel materials according to one embodiment of the present invention can be confirmed.

[0207] The above synthetic examples go through the following steps.

[0208]

[0209] 1. Dissolve each initiator in MeOH, add the base potassium methoxide (MeOK), mix evenly, and remove the solvent to form the initiator salt.

[0210] 2. After that, add NMP solvent, raise the temperature to dissolve the salt, then inject the monomer in 12-hour increments and proceed with the reaction for an additional 6 hours.

[0211]

[0212] At this time, the optimal synthesis conditions were optimized by adjusting the equivalent amount of the base.

[0213]

[0214] As can be seen in the experimental examples below,

[0215] The initiator and polyether backbone were confirmed through 1H NMR, and based on this, the degree of polymerization (DP) of each polymer was calculated, and it was confirmed that the solvent was sufficiently removed.

[0216] The calculated DP is summarized in the table in Figure 1 for each polymer.

[0217] In addition, the degree of branching (DB) of hbPG was calculated through 13C NMR, and it was confirmed to have a value of approximately 0.6 corresponding to the DB of hbPG.

[0218] The figures for this are also organized in the table in Figure 1 above.

[0219]

[0220] Preparation Example 1. OP-hbPG13 (MeOK).

[0221] Figure 5 is an OP-hbPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0222] Figure 6 is a table summarizing quantitative data of the materials used in the synthesis of Figure 5.

[0223]

[0224] Referring to FIGS. 5 and 6, the above manufacturing example 1 is described.

[0225] The above material is synthesized through the following manufacturing process, and the information on the material used is as shown in Fig. 6.

[0226]

[0227]

[0228] 1. Dissolve 4-tert-octylphenol in MeOH, add MeOK, and stir for 30 min to perform the initiator activation step.

[0229] 2. Dry at 40 °C under vacuum conditions, add dry toluene and repeat the blowing process twice.

[0230] 3. Add 4 mL of NMP and heat to 80 °C.

[0231] 4. Inject glycidol using a syringe pump for 12 hours and react for an additional 6 hours. (Consumption of monomer can be confirmed through crude 1H-NMR.)

[0232] 5. After cooling the polymer solution, quench it with MeOH+HCl.

[0233] 6. After precipitation and recovery in cold diethyl ether, dissolve in MeOH and perform exchange resin filtering.

[0234] 7. Afterwards, the solvent is dried to obtain the final product.

[0235]

[0236] Preparation Example 2. OP-hbPG13 (potassium naphthalenide)

[0237] Figure 7 is an OP-hbPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and H-NMR analysis results when potassium naphthalenide was used in the manufacturing process.

[0238] Figure 8 is an OP-hbPG according to an embodiment of the present invention.13 This graph shows the results of C-NMR analysis when potassium naphthalenide was used in the manufacturing process.

[0239] Figure 9 is a table summarizing quantitative data of the materials used in the synthesis of Figure 7.

[0240]

[0241] Referring to FIGS. 7 to 9, the above manufacturing example 2 is described.

[0242] The above material is synthesized through the following manufacturing process, and the information on the material used is as shown in Fig. 9 above.

[0243]

[0244] 1. Dissolve 4-tert-octylphenol in MeOH, add potassium naphthalenide, and stir for 30 min to perform the initiator activation step.

[0245] Afterwards, the same process is performed from “Step 2” of Manufacturing Example 1 above.

[0246]

[0247] Preparation Example 3. OP-linearPG13 (MeOK)

[0248] Figure 10 is an OP-linearPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0249] Figure 11 is a table summarizing quantitative data of the materials used in the synthesis of Figure 10.

[0250]

[0251] Referring to FIGS. 10 and 11, the above manufacturing example 3 is described.

[0252] The above material is synthesized through the following manufacturing process, and the information on the material used is as shown in Fig. 11 above.

[0253]

[0254] 1. Dissolve 4-tert-octylphenol in MeOH, add MeOK, and stir for 30 min to perform the initiator activation step.

[0255] 2. Dry at 40 °C under vacuum conditions, add dry toluene and repeat the blowing process twice.

[0256] 3. Add 4 mL of NMLP and heat to 80 °C.

[0257] 4. Inject EEGE monomer using a syringe pump for 12 hours and react for an additional 6 hours. (crude 1 (Monomer consumption can be confirmed through H-NMR)

[0258] 5. After cooling the polymer solution, quench it with MeOH and HCl solutions.

[0259] 6. After precipitation and recovery in cold diethyl ether, dissolve in MeOH and perform exchange resin filtering.

[0260] 7. Afterwards, the solvent is dried to obtain the final product.

[0261]

[0262]

[0263] Experimental Example 1. TMP-hbPG13 analysis data.

[0264] The above experimental example 1 is described with reference to Fig. 2.

[0265]

[0266] Figure 2 is TMP-hbPG according to one embodiment of the present invention. 13 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0267]

[0268] Through the reaction of the above chemical reaction formula 3, the TMP-hbPG 13 was synthesized.

[0269]

[0270] Referring to a in Fig. 2, 1 The initiator and polyether backbone can be identified through H NMR, and the degree of polymerization (DP) of the material can be calculated based on this, confirming that the solvent has been sufficiently removed.

[0271] The above calculated DP can be confirmed in the TMP Entry of Fig. 1.

[0272] Referring to b in Fig. 2, 13 The degree of branching (DB) of hbPG can be calculated using C NMR, which can be confirmed in the TMP Entry of Figure 1.

[0273] Referring to the TMP Entry of Figure 1, it can be confirmed that the DB of the hbPG has a value of approximately 0.6.

[0274] Referring to c of Fig. 2, it can be confirmed that the material was synthesized uniformly through the fact that the graph has a unimodal shape.

[0275] Referring to Fig. 2d, the size distribution analysis results of the 5 wt% TMP-hbPG13 solution after syringe filtration can be confirmed through dynamic light scattering (DLS) with intensity, number, and volume weighted distributions, respectively.

[0276] Referring to d in Fig. 2, some particles with large diameters are observed in the intensity, but when viewed in terms of number or volume, particles with large diameters that are similar in size to the main peak of intensity are not observed, confirming that they have a constant small size.

[0277]

[0278]

[0279] Experimental example 2. OP-hbPG13 analysis data.

[0280] The above experimental example 2 is described with reference to FIGS. 3 and 5 to 9.

[0281]

[0282] Figure 3 is an OP-hbPG according to one embodiment of the present invention. 13 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0283] Referring to a in Fig. 3, 1 The initiator and polyether backbone can be identified through H NMR, and the degree of polymerization (DP) of the material can be calculated based on this, confirming that the solvent has been sufficiently removed.

[0284] The above calculated DP can be confirmed in the HB Entry of Fig. 1.

[0285] Referring to b in Fig. 3, 13 The degree of branching (DB) of hbPG can be calculated using C NMR, which can be confirmed in the HB Entry in Figure 1.

[0286] Referring to the HB Entry of Fig. 1, it can be confirmed that the DB of the hbPG has a value of about 0.6 to 0.8.

[0287] Referring to c of Figure 3, it can be confirmed that the material was synthesized uniformly through the fact that the graph has a unimodal shape.

[0288] Referring to Fig. 3d, the size distribution analysis results of the 2.5 wt% OP-hbPG13 solution after syringe filtration can be confirmed through dynamic light scattering (DLS) with intensity, number, and volume weighted distributions, respectively.

[0289] Referring to d in Fig. 3, it can be confirmed that it has a constant size.

[0290]

[0291] Figure 5 is an OP-hbPG according to one embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0292] Figure 6 is a table summarizing quantitative data of the materials used in the synthesis of Figure 5.

[0293]

[0294] In Figs. 5 and 6, measurements were taken after cold ether precipitation and cationic resin filtering, followed by solvent drying.

[0295] Referring to FIGS. 5 and 6, it can be seen that the polymer is well grown in the initiator, but it can be seen that the polymer is synthesized with a DP twice the target DP, so it can be seen that the equivalent amount of the base must be increased to obtain a more desirable result.

[0296] Please add the meaning, significance, and emphasized parts of the experimental results of Figures 5 and 6 above.

[0297]

[0298] Figure 7 is a graph showing a chemical reaction formula and H-NMR analysis results when potassium naphthalenide is used in the manufacturing process of OP-hbPG13 according to one embodiment of the present invention.

[0299] Figure 8 is a graph showing the results of C-NMR analysis when potassium naphthalenide was used in the manufacturing process of OP-hbPG13 according to one embodiment of the present invention.

[0300] Figure 9 is a table summarizing quantitative data of the materials used in the synthesis of Figure 7.

[0301]

[0302] Referring to FIGS. 7 to 9, it can be seen that the polymer is well grown in the initiator and that a multi-branched structure is well formed. However, it can be seen that the polymer is synthesized with a DP that is twice the target DP, so it can be seen that the equivalent amount of the base must be increased to obtain a more desirable result.

[0303]

[0304] Experimental Example 3. OP-linPG13 analysis data.

[0305] The above experimental example 3 is described with reference to FIG. 4 and FIG. 10 to FIG. 12.

[0306]

[0307] Figure 4 is a linPG according to an embodiment of the present invention. 14 This graph shows the results of NMR analysis, GPC analysis, and DLS analysis.

[0308] Referring to a in Fig. 4, 1 The initiator and polyether backbone can be identified through H NMR, and the degree of polymerization (DP) of the material can be calculated based on this, confirming that the solvent has been sufficiently removed.

[0309] The above calculated DP can be confirmed in L Entry of Fig. 1.

[0310] Referring to b of Fig. 4, it can be confirmed that the material was synthesized uniformly through the fact that the graph has a unimodal shape.

[0311] Referring to c and d of Fig. 4, the size distribution analysis results of 25 wt% and 2.5 wt% linPG14 solutions after syringe filtration can be confirmed through dynamic light scattering (DLS) with intensity, number, and volume weighted distributions, respectively.

[0312] Referring to c and d in Fig. 4, some particles with large diameters are observed in the intensity, but when viewed in terms of number or volume, particles with large diameters that are similar in size to the main peak of intensity are not observed, confirming that they have a constant small size.

[0313]

[0314] Figure 10 is an OP-linearPG according to an embodiment of the present invention. 13 This is a graph showing the chemical reaction formula and NMR analysis results when MeOK was used in the manufacturing process.

[0315] Figure 11 is a table summarizing quantitative data of the materials used in the synthesis of Figure 10.

[0316] Referring to Figures 10 and 11, it can be seen that all monomers are consumed, and after purification through precipitation, it can be confirmed that the polymer of the target DP is well grown in the initiator.

[0317]

[0318] Figure 12 is an OP-linearPG according to an embodiment of the present invention. 13 This is a graph and table showing the GPC analysis results data when MeOK was used in the manufacturing process.

[0319] Referring to Figure 12, it can be confirmed that it has a constant molecular weight and a molecular weight close to the theoretical value.

[0320]

[0321] Experimental Example 4. CMP performance test results.

[0322] Polishing performance was evaluated based on the synthesized polymer micelles.

[0323] Experimental Example 4 is described above through Figures 13 and 14.

[0324]

[0325] Figure 13 is an OP-linPG according to an embodiment of the present invention. 13 This is a table and graph measuring the polishing performance.

[0326] Referring to Fig. 13, when the recess rate (RR) is calculated based on the reference, it can be confirmed that when the dynamic etching rate (DER) testing the RR effect is measured at 70 °C, a value of approximately 0.2 is observed at a concentration of 0.5%.

[0327] This means that polishing occurs, but the performance is only 20% of that of the original material.

[0328]

[0329] On the other hand, when examining the effect of machine removal rate (MRR), a negative RR value was observed at a concentration of 1.0 wt%. This can be interpreted as the polymer not being easily removed from the tungsten surface after being attached, implying that it can be used as an inhibitor to slow down polishing properties.

[0330]

[0331] Figure 14 is a table and graph showing the polishing performance according to DP of OP-hbPG according to one embodiment of the present invention.

[0332] Referring to Figure 14, it can be confirmed that the MRR value is higher as the DP is smaller, and the DER maintains a similar value.

[0333] This is because at low temperatures, the polymer is adsorbed onto the tungsten surface, but at high temperatures, the mobility of the polymer increases and decreases.

[0334] At this time, the MRR / SER value is highest at DP 11, which means that the physical polishing effect is high.

[0335]

[0336] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.

[0337] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

Claims

1. It has a micelle structure composed of an amphiphilic substance having both hydrophilic and hydrophobic groups. The hydrophilic group includes a polyglycerol functional group, A polymer micelle characterized in that the hydrophobic group includes a phenol group modified to be hydrophobic by bonding a hydrophobic substituent to the terminal thereof.

2. A polymer micelle according to claim 1, characterized in that the hydrophobic substituent is an alkyl group of C7 to C9.

3. A polymer micelle according to claim 1, wherein the polyglycerol functional group is a hyperbranched type polyglycerol functional group.

4. In the third paragraph, the amphiphilic material is a polymer micelle characterized by a degree of branching of 0.4 to 0.

8.

5. A polymer micelle according to claim 1, characterized in that the degree of polymerization of the polymer micelle is 10 to 17.

6. In the first paragraph, the amphiphilic material is a polymer micelle characterized by being represented by the following chemical formula 1: [Chemical Formula 1] 7. A polymer micelle according to claim 1, characterized in that the polyglycerol functional group is a linear type polyglycerol functional group.

8. In the 7th paragraph, the amphiphilic material is a polymer micelle characterized by being represented by the following chemical formula 2: [Chemical Formula 2] In the above chemical formula 2, n is an integer from 1 to 200.

9. A polymer micelle according to claim 1, characterized in that the micelle structure has a diameter of 5 nm to 7 nm. Containing a 10.1,1,1-Tris(hydroxymethyl)propane group and a hyperbranched type polyglycerol functional group, A polymer material characterized in that the above 1,1,1-Tris(hydroxymethyl)propane group has some hydroxyl groups substituted or unsubstituted.

11. In the 10th paragraph, the polymer material is characterized in that the degree of branching is 0.4 to 0.

8.

12. In the 10th paragraph, the polymer material is characterized by being expressed by the following chemical formula 3: [Chemical Formula 3] In the above chemical formula 3, R represents a functional group represented by the following chemical formula 4. [Chemical Formula 4] In the above chemical formula 4, the * part is the part where a bond is formed.

13. A polymer material according to claim 10, characterized in that the degree of polymerization of the polymer material is 10 to 17.

14. Containing the polymer micelle of clause 3, An abrasive for CMP, characterized in that it can be applied to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

15. Containing the polymer micelle of clause 3, An anti-abrasive agent for CMP characterized in that it can be applied to molybdenum.

16. Containing the polymer micelle of Article 7, An anti-abrasive for CMP, characterized in that it can be applied to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

17. Containing the polymer material of Article 10, An abrasive for CMP, characterized in that it can be applied to at least one material selected from the group consisting of tungsten, silica, cobalt, and rubidium.

18. A slurry composition for CMP characterized by containing the abrasive of clause 14.

19. In the 18th paragraph, the abrasive is, for the entire composition, A slurry composition for CMP, characterized in that it contains a ratio of 0.5 wt% to 2.5 wt%.

20. A slurry composition for CMP characterized by containing the anti-abrasive agent of Article 16.

21. In the 20th paragraph, the anti-abrasive agent is, for the entire composition, A slurry composition for CMP, characterized in that it contains a ratio of 0.5 wt% to 2.5 wt%.

22. A slurry composition for CMP characterized by containing the abrasive of clause 17.

23. In paragraph 22, the abrasive is, for the entire composition, A slurry composition for CMP, characterized in that it contains a ratio of 0.5 wt% to 2.5 wt%.

Citation Information

Patent Citations

  • Slurry comprising micelle for chemical-mechanicalpolishing silicon

    KR1020070002865A