Thermoplastic polyester elastomer resin and preparation method therefor

The integration of PO3G and EO-PPG in thermoplastic polyester elastomer resin addresses the limitations of TPEE by improving mechanical strength and elasticity, enabling broader application in various products.

WO2024248592A1PCT designated stage expired Publication Date: 2024-12-05SK CHEMICALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/095855
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional thermoplastic polyester elastomer (TPEE) resins face limitations in achieving optimal mechanical strength, elasticity, and compression-elastic recovery due to the incompatibility and crystallinity issues between hard and soft blocks, leading to restricted use in various applications.

Method used

The development of a thermoplastic polyester elastomer resin incorporating polytrimethylene ether glycol (PO3G) for soft blocks to control crystallinity and ethylene oxide-added polypropylene glycol (EO-PPG) to enhance phase separation and compatibility with hard blocks, resulting in improved mechanical strength and elasticity.

Benefits of technology

The resin exhibits enhanced mechanical strength, elasticity, and compression-elastic recovery, making it suitable for diverse applications such as automobile parts, electrical components, fibers, films, and shoe materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024095855-APPB-IMG-000001
    Figure PCTKR2024095855-APPB-IMG-000001
  • Figure PCTKR2024095855-APPB-IMG-000002
    Figure PCTKR2024095855-APPB-IMG-000002
  • Figure PCTKR2024095855-APPB-IMG-000003
    Figure PCTKR2024095855-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention relates to a thermoplastic polyester elastomer resin, a preparation method therefor, and an article comprising same. The thermoplastic polyester elastomer resin can have excellent elasticity and compression-elastic recovery while having high mechanical strength, elongation, etc. Accordingly, the thermoplastic polyester elastomer resin can be utilized in the manufacturing of various articles (e.g., fibers, foams, shoe parts, etc.).
Need to check novelty before this filing date? Find Prior Art

Description

Thermoplastic polyester elastomer resin and method for producing the same

[0001] The present invention relates to a thermoplastic polyester elastomer resin having excellent physical properties such as mechanical strength, elasticity, and compression-elastic recovery force, and a method for producing the same, while including a hard block having thermoplastic properties and a soft block having elastomeric properties (introducing PO3G and EO-PPG).

[0002] Thermoplastic elastomer (TPE) resins comprise a hard segment derived from a thermoplastic polymer and possessing thermoplastic properties, and a soft segment derived from an elastomer, a rubber-like material, and possessing elastomeric properties. Compared to typical thermosetting rubbers, the hard segments, which are physically bonded by crystals, resemble chemical cross-linking known as "vulcanization," while the soft segments resemble amorphous rubber-like properties.

[0003] Among the above TPE resins, thermoplastic polyester elastomer (TPEE) resin has high mechanical strength and excellent impact resistance, heat resistance, flexibility, and moldability, and is used in the manufacture of automobile parts, electrical and electronic parts, fibers, films, etc.

[0004] The above TPEE resin mainly includes a tetramethylene ester crystalline hard block and a polyether polyol ester amorphous soft block. As raw materials for manufacturing the soft block of the TPEE resin, polyethylene ether glycol (PEG), poly(1,2-propylene) glycol (PPG), ethylene oxide-added polypropylene glycol (EO-PPG), polytetramethylene ether glycol (PTMG), etc. have been used. However, the TPEE resin manufactured using the PEG as a raw material has a disadvantage of high moisture content, and the PPG has poor polymerization reactivity, so they are not often used as raw materials for manufacturing the TPEE resin. Therefore, the PTMG, the EO-PPG, or a combination thereof are mainly used for manufacturing the soft block of the TPEE resin.

[0005] The TPEE resin manufactured using the above PTMG as a raw material exhibits excellent physical properties such as mechanical strength and elongation, but has limitations in increasing physical properties such as elasticity and compressive elasticity beyond the desired level. In addition, the TPEE resin manufactured using the above EO-PPG as a raw material exhibits high crystallinity and thus excellent formability, but has poor physical properties such as mechanical strength and elongation.

[0006] Therefore, there is a need to develop a new TPEE resin that has excellent properties such as mechanical strength and elongation, as well as high elasticity and compressive elasticity recovery, and can be used in the manufacture of various products.

[0007] In order to solve the above-mentioned conventional problems, the inventors of the present invention have conducted various studies, and as a result, they have confirmed that a thermoplastic polyester elastomer (TPEE) resin having excellent mechanical strength and improved elasticity and compressive elasticity recovery is obtained by increasing the incompatibility between hard blocks and soft blocks and controlling the crystallinity and crystallization rate of the soft block to a low level.

[0008] Accordingly, the object of the present invention is to provide a thermoplastic polyester elastomer resin having excellent mechanical strength, elasticity and compression-elastic recovery, and a method for producing the same.

[0009] In addition, another object of the present invention is to provide a composition or article comprising the thermoplastic polyester elastomer resin.

[0010] To solve the above problem, the present invention provides a thermoplastic polyester elastomer resin comprising a repeating unit (a) represented by the following chemical formula 1; a repeating unit (b) represented by the following chemical formula 2; and a repeating unit (c) represented by the following chemical formula 3:

[0011] [Chemical Formula 1]

[0012]

[0013] [Chemical Formula 2]

[0014]

[0015] [Chemical Formula 3]

[0016]

[0017] In the above chemical formulas 1 to 3,

[0018] R 1 Inland R 3 are each independently C1 to C 12 A straight-chain, branched, or cyclic divalent aliphatic hydrocarbon group; or C6 to C 12 The second is an aromatic hydrocarbon group,

[0019] m is an integer from 2 to 6, n is an integer from 2 to 3, p is an integer from 10 to 30, t is an integer from 1 to 30, and s is an integer from 1 to 40.

[0020] In addition, the present invention provides a method for producing a thermoplastic polyester elastomer resin, comprising: (1-1) a step of reacting a glycol component; a dicarboxylic acid component; and a high molecular weight glycol component to obtain a reactant; and (1-2) a step of subjecting the reactant to a condensation polymerization reaction, wherein the method comprises: a repeating unit (a) represented by the chemical formula 1; a repeating unit (b) represented by the chemical formula 2; and a repeating unit (c) represented by the chemical formula 3.

[0021] In addition, the present invention provides a composition comprising the thermoplastic polyester elastomer resin.

[0022] In addition, the present invention provides an article comprising the thermoplastic polyester elastomer resin.

[0023] The thermoplastic polyester elastomer resin according to the present invention can exhibit excellent mechanical strength by applying polytrimethylene ether glycol (PO3G) in the production of a soft block. In addition, the thermoplastic polyester elastomer resin according to the present invention can exhibit excellent elasticity and compressive elasticity recovery by applying ethylene oxide-added polypropylene glycol (EO-PPG), which has a methylene side branch attached to the polyol chain main chain to restrict the movement of the polymer chain of the soft block and create sufficient free volume between the polymer chains to lower crystallinity and crystallization speed and increase incompatibility with the hard block to promote phase separation from the hard block.

[0024] In this way, the thermoplastic polyester elastomer resin according to the present invention exhibits excellent mechanical strength, elasticity, and compressive elasticity recovery while exhibiting a desired level of hardness, and can be utilized in the manufacture of various articles such as automobile parts, electrical and electronic parts, fibers, films, matrices, cushioning materials, foams, and shoe parts.

[0025] Hereinafter, the present invention will be described in detail. Herein, the present invention is not limited to the contents described below, and may be modified in various forms as long as the gist of the invention is not changed.

[0026] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.

[0027] In this specification, terms such as first, second, etc. are used to describe various components, and the components are not limited to these terms. These terms are used to distinguish one component from another.

[0028] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification can be understood to be modified by the term “about” in all cases unless otherwise specified.

[0029]

[0030] Thermoplastic polyester elastomer (TPEE) resins form an elastomer matrix by phase separation due to the incompatibility of crystalline hard blocks and amorphous soft blocks, thereby exhibiting rubber-like elastic properties. In order to improve the elastic properties of such thermoplastic polyester elastomer resins, it is necessary to clearly control the boundary distinction between the hard blocks and the soft blocks. Specifically, by increasing the difference in crystallinity / amorphism of the hard blocks and the soft blocks to improve the incompatibility while increasing the free volume of the polymer chains, the phase separation can occur more clearly. That is, the hard blocks need to crystallize as quickly as possible, and the soft blocks need to crystallize as late as possible, thereby obtaining a thermoplastic polyester elastomer resin having high mechanical strength and excellent elastic properties.

[0031] Based on these points, the present invention applies polytrimethylene ether glycol (PO3G) when forming a soft block of a thermoplastic polyester elastomer resin to lower the crystallinity and crystallization speed of the soft block, and applies ethylene oxide-added polypropylene glycol (EO-PPG) to increase incompatibility with the hard block, thereby making phase separation distinct. This will be specifically described as follows.

[0032]

[0033] thermoplastic polyester elastomer resin

[0034] The thermoplastic polyester elastomer resin according to the present invention comprises a repeating unit (a) represented by the following chemical formula 1; a repeating unit (b) represented by the following chemical formula 2; and a repeating unit (c) represented by the following chemical formula 3.

[0035] [Chemical Formula 1]

[0036]

[0037] [Chemical Formula 2]

[0038]

[0039] [Chemical Formula 3]

[0040]

[0041] In the above chemical formulas 1 to 3,

[0042] R 1 Inland R 3 are identical or different from each other, and each independently, C1 to C 12 A straight-chain, branched, or cyclic divalent aliphatic hydrocarbon group; or C6 to C 12 The second is an aromatic hydrocarbon group,

[0043] m is an integer from 2 to 6, n is an integer from 2 to 3, p is an integer from 10 to 30, t is an integer from 1 to 30, and s is an integer from 1 to 40.

[0044] The repeating unit (a) represented by the above chemical formula 1 may be a repeating unit constituting a hard block of the thermoplastic polyester elastomer resin. In the above chemical formula 1, R 1 Specifically, C5 to C 12 The fantasy of the two aliphatic hydrocarbon groups, or C6 to C 12 is an aromatic hydrocarbon group, and m may be an integer from 3 to 5. For example, the R 1 may be a cyclohexylene group or a phenylene group, and m may be an integer of 4.

[0045] The repeating unit (b) represented by the above chemical formula 2 and the repeating unit (c) represented by the above chemical formula 3 may be repeating unit(s) constituting the soft block of the thermoplastic polyester elastomer resin. In the above chemical formula 2, R 2 Specifically, C5 to C 12 The fantasy of the two aliphatic hydrocarbon groups, or C6 to C 122 of the group may be an aromatic hydrocarbon group. In addition, n may be an integer of 2 or 3, and p may be an integer of 15 to 25. For example, the R 2 may be a cyclohexylene group or a phenylene group, n is an integer of 3, and p may be an integer of 18 to 22. In the above chemical formula 3, R 3 Specifically, C5 to C 12 The fantasy of the two aliphatic hydrocarbon groups, or C6 to C 12 2 of may be an aromatic hydrocarbon group. In addition, t may be an integer from 5 to 25, and s may be an integer from 5 to 35. For example, the R 3 may be a cyclohexylene group or a phenylene group, t may be an integer from 10 to 20, and s may be an integer from 10 to 30.

[0046] For example, the thermoplastic polyester elastomer resin according to the present invention may include a repeating unit represented by the following chemical formula 4 and / or a repeating unit represented by the following chemical formula 5, in which the repeating unit (a) represented by the above chemical formula 1, the repeating unit (b) represented by the above chemical formula 2, and the repeating unit (c) represented by the above chemical formula 3 are bonded to each other.

[0047] [Chemical Formula 4]

[0048]

[0049] [Chemical Formula 5]

[0050]

[0051] In the above chemical formulas 4 and 5, R 1 , R 2 , R 3 , m, n, p, t and s are the same as described above, and x, y and z are weight ratios.

[0052] According to the present invention, the repeating unit (a) represented by the above chemical formula 1 can be derived from the reaction of a glycol component including 1,4-butanediol and a dicarboxylic acid component, the repeating unit (b) represented by the above chemical formula 2 can be derived from the reaction of a dicarboxylic acid component and a high molecular weight glycol component (first high molecular weight glycol component) including polytrimethylene ether glycol, and the repeating unit (c) represented by the above chemical formula 3 can be derived from the reaction of a dicarboxylic acid component and a high molecular weight glycol component (second high molecular weight glycol component) including ethylene oxide-added polypropylene glycol.

[0053] Specifically, the thermoplastic polyester elastomer resin according to the present invention may be a resin obtained by using a dicarboxylic acid component, a glycol component, and a high molecular weight glycol component (a first high molecular weight glycol component and a second high molecular weight glycol component) as reaction raw materials.

[0054] The above dicarboxylic acid component (e.g., a dicarboxylic acid, an ester thereof, a chloride thereof, or an anhydride thereof) may be an aliphatic dicarboxylic acid component, an aromatic dicarboxylic acid component, or a combination thereof.

[0055] The aliphatic dicarboxylic acid component may be a linear, branched, or cyclic aliphatic dicarboxylic acid component. The aliphatic dicarboxylic acid component may have 4 or more, 5 or more, 6 or more, or 7 or more carbon atoms, and may be 20 or less, 15 or less, 13 or less, 12 or less, or 10 or less. Specifically, the aliphatic dicarboxylic acid component may have 4 to 20, 5 to 15, or 6 to 10 carbon atoms.

[0056] For example, the aliphatic dicarboxylic acid component may include, but is not limited to, one or more selected from the group consisting of adipic acid, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, fumaric acid, glutaric acid, azelaic acid, 1,4-cyclohexanedicarboxylic acid, and 1,3-cyclohexanedicarboxylic acid.

[0057] The number of carbon atoms of the aromatic dicarboxylic acid component may be 6 or more, 7 or more, 8 or more, or 10 or more, and 25 or less, 20 or less, or 15 or less. Specifically, the number of carbon atoms of the aromatic dicarboxylic acid component may be 6 to 25, 6 to 15, or 6 to 10.

[0058] For example, the aromatic dicarboxylic acid component may include, but is not limited to, one or more selected from the group consisting of terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, 4,4'-stilbenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,5-thiophenedicarboxylic acid, and dimethyl terephthalate.

[0059] Preferably, the dicarboxylic acid component may include at least one selected from the group consisting of terephthalic acid and dimethyl terephthalate. The amount used (the amount added during the reaction) of at least one selected from the group consisting of terephthalic acid and dimethyl terephthalate (at least one component) is not particularly limited, but may be 50 mol% or more, 65 mol% or more, 70 mol% or more, 85 mol% or more, 90 mol% or more, or 95 mol% or more, based on the total mol% of the dicarboxylic acid component. Specifically, the amount used of the terephthalic acid, the dimethyl terephthalate, or a combination thereof may be 50 to 100 mol%, 55 to 100 mol%, 60 to 100 mol%, 70 to 100 mol%, 85 to 100 mol%, or 90 to 95 mol%.

[0060] The glycol component may be a component that forms a tetramethylene ester hard block (e.g., repeating unit (a) of chemical formula 1) through an esterification reaction or an ester exchange reaction with the dicarboxylic acid component. The glycol component may have 2 or more, 3 or more, or 4 or more carbon atoms, and may be 15 or less, 12 or less, 10 or less, or 8 or less. Specifically, the glycol component may have 2 to 15, 3 to 10, or 4 to 8 carbon atoms.

[0061] For example, the glycol component may be ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyhexamethylene glycol, copolymer of ethylene oxide and tetrahydrofuran, polycarbonate diol, It may include at least one selected from the group consisting of polyneopentyl glycol, poly-3-methylpentanediol, and poly-1,5-pentanediol, but is not limited thereto. Specifically, the glycol component may include at least one selected from the group consisting of ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol.

[0062] Preferably, the glycol component may include 1,4-butanediol. The amount of 1,4-butanediol used (amount added during reaction) is not particularly limited, but may be 75 mol% or more, 80 mol% or more, 83 mol% or more, 85 mol% or more, 90 mol% or more, or 95 mol% or more, based on the total mol% of the glycol component. Specifically, the amount of 1,4-butanediol used may be 75 to 100 mol%, 80 to 100 mol%, 83 to 100 mol%, 85 to 100 mol%, 90 to 100 mol%, or 90 to 95 mol%.

[0063] The number average molecular weight of these glycol components is not particularly limited, but may be less than 400 g / mol, less than 350 g / mol, less than 300 g / mol, or less than 250 g / mol.

[0064] The high molecular weight glycol component may be a component that forms a poly(alkylene oxide) ester soft block (e.g., repeating unit (b) of chemical formula 2 and repeating unit (c) of chemical formula 3) through an esterification reaction or an ester exchange reaction with the dicarboxylic acid component. The high molecular weight glycol component may include polytrimethylene ether glycol (PO3G) and ethylene oxide-added polypropylene glycol (EO-PPG). Since the high molecular weight glycol component includes the polytrimethylene ether glycol (PO3G), the mechanical strength of the thermoplastic polyester elastomer resin can be significantly increased. In addition, since the high molecular weight glycol component includes the ethylene oxide-added polypropylene glycol (EO-PPG), the elasticity and compression-elastic recovery force of the thermoplastic polyester elastomer resin can be significantly increased.

[0065] Preferably, the high molecular weight glycol component may be composed of polytrimethylene ether glycol (PO3G) and ethylene oxide-added polypropylene glycol (EO-PPG). The amount of polytrimethylene ether glycol (PO3G) used (amount added during reaction) is not particularly limited, but may be 50 mol% or more, 60 mol% or more, 75 mol% or more, 85 mol% or more, 95 mol% or more, or 97 mol% or more, based on the total mol% of the high molecular weight glycol component (the sum of the first high molecular weight glycol component and the second high molecular weight glycol component). Specifically, the amount of polytrimethylene ether glycol (PO3G) used may be 50 to 99.5 mol%, 60 to 99 mol%, 65 to 95 mol%, 70 to 90 mol%, 75 to 90 mol%, or 75 to 85 mol%. In addition, the amount of the ethylene oxide-added polypropylene glycol (EO-PPG) used (amount added during reaction) is not particularly limited, but may be 50 mol% or less, 40 mol% or less, 25 mol% or less, 15 mol% or less, 5 mol% or less, or 3 mol% or less, based on the total mol% of the high molecular weight glycol component (the sum of the first high molecular weight glycol component and the second high molecular weight glycol component). Specifically, the amount of the ethylene oxide-added polypropylene glycol (EO-PPG) used may be 0.5 to 50 mol%, 1 to 40 mol%, 5 to 35 mol%, 10 to 30 mol%, 15 to 30 mol%, or 15 to 25 mol%.

[0066] The number average molecular weight of the high molecular weight glycol component including the above polytrimethylene ether glycol (PO3G) and the above ethylene oxide-added polypropylene glycol (EO-PPG) is not particularly limited, but may be 400 g / mol or more, 500 g / mol or more, 600 g / mol or more, 700 g / mol or more, or 800 g / mol or more, and may be 6,000 g / mol or less, 5,000 g / mol or less, 4,000 g / mol or less, or 3,000 g / mol or less. Specifically, in order to ensure good phase separation from the hard block, the number average molecular weight of the high molecular weight glycol component may be 400 to 5,000 g / mol, or 1,000 to 3,000 g / mol.

[0067] For example, the number average molecular weight of the polytrimethylene ether glycol (PO3G) may be 500 to 4,000 g / mol, 600 to 4,000 g / mol, 800 to 3,500 g / mol, or 1,000 to 3,000 g / mol. In addition, the number average molecular weight of the ethylene oxide-added polypropylene glycol (EO-PPG) may be 1,000 to 4,000 g / mol, 1,500 to 3,500 g / mol, 2,000 to 3,500 g / mol, or 2,000 to 3,000 g / mol.

[0068] Meanwhile, according to the present invention, the content (x) of the repeating unit (a) represented by the above chemical formula 1 is not particularly limited, but may be 20 to 70 wt%, 22 to 68 wt%, 24 to 65 wt%, 26 to 63 wt%, or 27 to 60 wt% based on the total weight of the thermoplastic polyester elastomer resin. When the content (x) of the repeating unit (a) is within the above range, a thermoplastic polyester elastomer resin in which mechanical strength (e.g., tensile strength) and hardness are secured at a desired level can be provided.

[0069] In addition, the content (y) of the repeating unit (b) represented by the above chemical formula 2 is not particularly limited, but may be 5 to 70 wt%, 7 to 65 wt%, 9 to 60 wt%, 12 to 55 wt%, or 20 to 50 wt% based on the total weight of the thermoplastic polyester elastomer resin. When the content (y) of the repeating unit (b) is within the above range, a thermoplastic polyester elastomer resin having excellent mechanical strength and elongation, etc., and having elasticity and compressive-elastic recovery force secured at a desired level can be provided.

[0070] In addition, the content (z) of the repeating unit (c) represented by the above chemical formula 3 is not particularly limited, but may be 0.5 to 40 wt%, 1 to 38 wt%, 5 to 35 wt%, 10 to 30 wt%, or 15 to 25 wt% based on the total weight of the thermoplastic polyester elastomer resin. When the content (z) of the repeating unit (c) is within the above range, a thermoplastic polyester elastomer resin having excellent elasticity and compressive-elastic recovery force while securing mechanical strength and elongation at the desired level can be provided.

[0071] The thermoplastic polyester elastomer resin according to the present invention may be a resin comprising the repeating unit (a), the repeating unit (b), and the repeating unit (c), wherein the content ratio (weight ratio) between these repeating units is controlled within a specific range.

[0072] Specifically, the thermoplastic polyester elastomer resin according to the present invention can satisfy the following formula 1. As the thermoplastic polyester elastomer resin satisfies the following formula 1, it can have a desired high molecular weight and higher mechanical strength.

[0073] [Formula 1]

[0074] 0.5 ≤ (y + z) / x ≤ 3.0

[0075] In the above equation 1,

[0076] x is the weight occupied by the repeating unit (a) represented by the above chemical formula 1 in the thermoplastic polyester elastomer resin (total weight of the thermoplastic polyester elastomer resin),

[0077] y is the weight occupied by the repeating unit (b) represented by the above chemical formula 2 in the thermoplastic polyester elastomer resin (total weight of the thermoplastic polyester elastomer resin),

[0078] z is the weight occupied by the repeating unit (c) represented by the above chemical formula 3 in the thermoplastic polyester elastomer resin (total weight of the thermoplastic polyester elastomer resin).

[0079] Specifically, in the above formula 1, the ratio of (y + z) / x may be 0.55 to 2.95, 0.6 to 2.85, 0.65 to 2.75, 0.7 to 2.65, 0.75 to 2.5, 0.9 to 2.5, 1 to 2.5, or 1.1 to 2.45.

[0080] In addition, the thermoplastic polyester elastomer resin according to the present invention can satisfy the following equation 2. As the thermoplastic polyester elastomer resin satisfies the following equation 2, the elasticity and compression-elastic recovery force can be better.

[0081] [Formula 2]

[0082] 0.3 ≤ y / z ≤ 35

[0083] In the above equation 2,

[0084] y is the weight occupied by the repeating unit (b) represented by the above chemical formula 2 in the thermoplastic polyester elastomer resin (total weight of the thermoplastic polyester elastomer resin),

[0085] z is the weight occupied by the repeating unit (c) represented by the above chemical formula 3 in the thermoplastic polyester elastomer resin (total weight of the thermoplastic polyester elastomer resin).

[0086] Specifically, the ratio of y / z in the above formula 2 may be 0.4 to 30, 0.45 to 20, 0.5 to 15, 0.5 to 10, 0.8 to 8, 0.9 to 6, 1 to 5, or 1.2 to 4.

[0087] Meanwhile, the thermoplastic polyester elastomer resin according to the present invention may further comprise a repeating unit (d) derived from a reactive compatibilizer. As the thermoplastic polyester elastomer resin further comprises the repeating unit (d), the mechanical strength, elongation, etc., as well as the elasticity and compressive elasticity recovery force, may be further improved.

[0088] The above reactive compatibilizer is an additive that helps improve miscibility by preventing phase separation between each raw material component in a raw material mixture (resin mixture) of two or more types and enabling the formation of a stable and long-term continuous phase. Specifically, the reactive compatibilizer is a reactive polymer that is compatibilizable with one of the raw material components among the mixed raw material components and reacts with a functional group of the other raw material component. When this is added to the raw material mixture and a reactive extrusion process is performed, the formation of a block copolymer or a graft copolymer can be induced.

[0089] Such reactive compatibilizers may be selected from the group consisting of isocyanate compounds, carbodiimide compounds (e.g., polycarbodiimide compounds having two or more structures of -N=C=N- in the molecule), epoxy compounds, oxazoline compounds, compounds having a glycidyl group, and compounds having a maleic anhydride structure. Here, the isocyanate compound may have too high a reactivity with moisture, making it difficult to control the reactivity and handle (storage), and the carbodiimide compound may be expensive, making it difficult to economically produce. In addition, the epoxy compound may have a large difference in the degree of reactivity depending on the epoxy equivalent and the number of functional groups, making it difficult to control the reactivity, and the oxazoline compound may have low reactivity compared to other compounds, making it difficult to expect an effect of improving the miscibility between raw material components. Therefore, it may be preferable to use a compound having the glycidyl group or the maleic anhydride structure as the reactive compatibilizer.

[0090] The compound having the glycidyl group may specifically be a glycidyl group-modified olefin rubber polymer, and preferably may be a polymer in which glycidyl (meth)acrylate is grafted onto a polyolefin rubber copolymer (Glycidyl methacrylate grafted polyolefin elastomers). The compound having the maleic anhydride structure may specifically be a polymer in which maleic anhydride is grafted onto a polyolefin rubber copolymer (Maleic anhydride grafted polyolefin elastomers).

[0091] For example, the reactive compatibilizer may be poly(ethylene-co-methylacrylate-co-glycidyl methacrylate), whereby the repeating unit (d) may have a structure represented by the following chemical formula 6. In addition, the reactive compatibilizer may be poly(ethylene-co-ethylacrylate-co-maleic anhydride), whereby the repeating unit (d) may be represented by the following chemical formula 7.

[0092] [Chemical Formula 6]

[0093]

[0094] [Chemical Formula 7]

[0095]

[0096] When the above poly(ethylene-co-methylacrylate-co-glycidyl methacrylate) is used, in the above chemical formula 6, a is an integer from 116 to 268, b is an integer from 12 to 29, and c is an integer from 2 to 7.

[0097] Also, when it is poly(ethylene-co-ethylacrylate-co-maleic anhydride), in the chemical formula 7, d is an integer from 129 to 300, e is an integer from 8 to 25, and f is an integer from 1 to 3.

[0098] As such reactive commercialization agents, commercially available products include Rotader AX8840, Rotader AX8900, and Rotader AX4720.

[0099] According to the present invention, the content of the repeating unit (d) derived from the reactive compatibilizer is not particularly limited, but may be 0.1 to 10 wt%, 0.5 to 10 wt%, 1 to 5 wt%, or 2 to 4 wt% based on the total weight of the thermoplastic polyester elastomer resin. When the content of the repeating unit (d) is within the above range, a desired level of melt viscosity can be secured, thereby improving the moldability (processability) of the thermoplastic polyester elastomer resin.

[0100]

[0101] The thermoplastic polyester elastomer resin according to the present invention can exhibit improved physical properties by controlling the amount of each reaction raw material used while applying the high molecular weight glycol component (PO3G, EO-PPG) to form a soft block as described above.

[0102] Specifically, the thermoplastic polyester elastomer resin according to the present invention has a tensile strength of 190 kgf / cm as measured according to ASTM D638. 2 Above, 195 kgf / cm 2 Above, 200 kgf / cm 2 Above, 205 kgf / cm 2 Above, 220 kgf / cm 2 Above, 230 kgf / cm 2 Above, 240 kgf / cm 2 or more than 250 kgf / cm 2 It can be more than that. More specifically, the tensile strength is 190 to 350 kgf / cm. 2 , 195 to 345 kgf / cm 2 , 205 to 340 kgf / cm 2 , or 230 to 335 kgf / cm 2 It could be.

[0103] The thermoplastic polyester elastomer resin according to the present invention may have an intrinsic viscosity (IV) of 1.0 to 2.4 ㎗ / g, specifically 1.05 to 2.35 ㎗ / g, 1.08 to 2.3 ㎗ / g, 1.1 to 2 ㎗ / g, 1.2 to 1.9 ㎗ / g, 1.3 to 1.88 ㎗ / g, or 1.4 to 1.85 ㎗ / g.

[0104] The thermoplastic polyester elastomer resin according to the present invention may have a Shore D hardness of 20 to 60, specifically 25 to 55, 28 to 53, 28 to 50, 30 to 48, or 30 to 45.

[0105] The thermoplastic polyester elastomer resin according to the present invention may have a compression set (compression-elastic recovery) of 30 to 60%, 30 to 59%, 31 to 58%, 31 to 57%, 32 to 56%, 32 to 55%, 33 to 53%, 33 to 50%, 34 to 49%, or 34 to 48%.

[0106] The thermoplastic polyester elastomer resin according to the present invention may have a resilience (elasticity) of 50 to 75%, 53 to 74%, 55 to 73%, 56 to 72%, 57 to 71%, 58 to 70%, 59 to 70%, 60 to 69%, or 62 to 68%.

[0107] The thermoplastic polyester elastomer resin according to the present invention can have excellent mechanical strength, elasticity, and compressive elasticity recovery by satisfying the following formula 3 and / or formula 4.

[0108] [Formula 3]

[0109] H / R ≤ 0.75

[0110] [Formula 4]

[0111] 0.8 ≤ H / CS

[0112] In the above equations 3 and 4,

[0113] H is the Shore D hardness of the thermoplastic polyester elastomer resin measured according to ASTM D2240,

[0114] R is the resilience of the thermoplastic polyester elastomer resin measured according to ASTM D2632,

[0115] CS is the compression set of thermoplastic polyester elastomer resin measured according to ISO 816 Method B.

[0116] Specifically, the H / R ratio may be 0.3 to 0.75, 0.32 to 0.73, 0.34 to 0.7, 0.35 to 0.68, 0.38 to 0.65, 0.4 to 0.63, or 0.4 to 0.6.

[0117] Additionally, the H / CS ratio may be 0.8 to 0.95, 0.8 to 0.93, 0.81 to 0.92, 0.82 to 0.91, 0.83 to 0.9, 0.84 to 0.89, or 0.85 to 0.88.

[0118]

[0119] The thermoplastic polyester elastomer resin according to the present invention can be utilized in the manufacture of various products because it has excellent mechanical strength, elasticity, and compressive elastic recovery while securing basic physical properties (e.g., heat resistance, impact resistance, moldability, etc.). Specifically, the thermoplastic polyester elastomer resin can be useful in the manufacture of fibers, films, foams (foam-type molded products), shoe parts (e.g., cushioning materials for shoe midsoles, shoe outsoles, and shoe insoles), etc.

[0120]

[0121] Method for producing thermoplastic polyester elastomer resin

[0122] The thermoplastic polyester elastomer resin according to the present invention can be manufactured through a process of esterification reaction or ester exchange reaction followed by polycondensation reaction. Specifically, the method for manufacturing the thermoplastic polyester elastomer resin according to the present invention comprises the step of (1-1) reacting a glycol component; a dicarboxylic acid component; and a high molecular weight glycol component to obtain a reactant; and the step of (1-2) subjecting the reactant to a polycondensation reaction, which will be specifically described as follows.

[0123] Step (1-1): Esterification reaction, or transesterification reaction

[0124] According to the present invention, step (1-1) is a step of introducing a glycol component, a dicarboxylic acid component, and a high molecular weight glycol component, which are reaction raw materials, into a reactor (esterification reactor or ester exchange reactor) and performing an esterification reaction or an ester exchange reaction to obtain a reactant. At this time, the glycol component includes 1,4-butanediol, and the high molecular weight glycol component includes polytrimethylene ether glycol (PO3G) and ethylene oxide-added polypropylene glycol (EO-PPG). Since the description of these components is the same as described above, it is omitted. In addition, since the description of the dicarboxylic acid component is the same as described above, it is omitted.

[0125] The glycol component, the dicarboxylic acid component, and the high molecular weight glycol component may be fed into the reactor at once, or the glycol component and the dicarboxylic acid component may be fed and the temperature of the reactor may be increased to a certain level, and then the high molecular weight glycol may be fed. For example, the feeding of the high molecular weight glycol may be performed at a temperature of 180 to 280°C under a nitrogen atmosphere while removing by-products such as water or methanol.

[0126] The above esterification reaction or ester exchange reaction can be performed in the presence of a catalyst. That is, a catalyst can be introduced together with the reaction raw material when it is introduced into the reactor. The catalyst is not particularly limited as long as it is a commonly known catalyst, and specifically, at least one selected from the group consisting of a titanium-based catalyst, a germanium-based catalyst, an antimony-based catalyst, an aluminum-based catalyst, and a tin-based catalyst can be used.

[0127] For example, the titanium-based catalyst may specifically include at least one selected from the group consisting of tetraethyl titanate, acetyltripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, triethanolamine titanate, acetylacetonate titanate, ethylacetoacetic ester titanate, isostearyl titanate, and titanium dioxide. The germanium-based catalyst may specifically include at least one selected from the group consisting of germanium dioxide, germanium tetrachloride, germanium ethyleneglycoxide, and germanium acetate.

[0128] The amount of the catalyst used (the amount introduced during the reaction) can be appropriately adjusted depending on the reaction conditions and the type of catalyst. For example, the catalyst can be introduced so that the weight of the metal component (e.g., Ti, Ge, Sb, Al, Sn, etc.) contained in the catalyst is 0.0001 to 0.005 parts by weight based on the total weight of the glycol component, the dicarboxylic acid component, and the high molecular weight glycol component introduced into the reactor.

[0129] Meanwhile, in the esterification reaction or ester exchange reaction, one or more additives selected from the group consisting of a crystallizer, an antioxidant, and a polymerization reaction branching agent may be further added.

[0130] As the above crystallizer, a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, or a polyamide resin can be used.

[0131] As the above antioxidant, at least one selected from the group consisting of hindered phenol compounds, phosphite compounds, and thioether compounds may be used.

[0132] As the above polymerization reaction branching agent, a polyol having 3 to 6 hydroxyl groups; a polycarboxylic acid having 3 to 4 carboxyl groups, or an anhydride thereof; or a hydroxy acid having a total of 3 to 6 hydroxyl groups and carboxyl groups may be used. Specifically, the polyol may include at least one selected from the group consisting of glycerol, sorbitol, pentaerythritol, 1,1,4,4-tetrakis(hydroxymethyl)cyclohexane, trimethylol propane, and 1,2,6-hexane triol. In addition, the polycarboxylic acid may include at least one selected from the group consisting of hemimellitic acid, trimellitic acid, trimespyromellitic acid, 1,1,2,2-ethanetetracarboxylic acid, 1,1,2-ethanetricarboxylic acid, 1,3,5-pentanetricarboxylic acid, and 1,2,3,4-cyclopentanetetracarboxylic acid. For example, trimellitic acid, trimellitic anhydride, trimethylol propane, or a combination thereof may be used as the polymerization reaction branching agent to control the melt index (MI) of the thermoplastic polyester elastomer resin to a desired level.

[0133] The amount of this polymerization reaction branching agent used (amount added during reaction) is not particularly limited, but a concentration of 0.00015 to 0.005 equivalents per 100 g of thermoplastic polyester elastomer resin may be applied.

[0134] The above esterification reaction, or ester exchange reaction, is usually carried out without the addition of a solvent, but an inert solvent such as water or a diol may be added to facilitate the removal of volatile components.

[0135] The conditions of the esterification reaction or ester exchange reaction can be appropriately controlled depending on the reaction environment and the molecular weight of the desired reactant. Specifically, the pressure applied to the esterification reaction or ester exchange reaction may be 0.01 kg / cm2 or more, 0.05 kg / cm2 or more, or 0.1 kg / cm2 or more, and may be 1.5 kg / cm2 or less, 1 kg / cm2 or less, 0.5 kg / cm2 or less, or 0.3 kg / cm2 or less. In addition, the temperature applied to the esterification reaction or ester exchange reaction may be 140°C or more, 160°C or more, 180°C or more, or 200°C or more, and may be 300°C or less, 280°C or less, 270°C or less, 250°C or less, or 220°C or less. The esterification reaction or ester exchange reaction may be performed under a nitrogen atmosphere. For example, the esterification reaction or ester exchange reaction can be performed under conditions of 0.05 to 1.5 kg / cm2 and 180 to 280°C under a nitrogen atmosphere.

[0136] The above esterification reaction or ester exchange reaction can be performed in a batch or continuous manner.

[0137] The end point of the above esterification reaction or ester exchange reaction can be determined by considering the theoretical amount of water or methanol, which are by-products generated from the dicarboxylic acid component, or when the outflow of by-products no longer occurs.

[0138] Step (1-2): Condensation polymerization reaction

[0139] According to the present invention, step (1-2) is a step of subjecting the reactant obtained in step (1-1) to a polycondensation reaction. The conditions under which the polycondensation reaction is performed may not be particularly limited.

[0140] Specifically, the polycondensation reaction may be carried out under a vacuum atmosphere. In addition, the pressure applied to the polycondensation reaction may be 0.01 to 600 mmHg, 0.05 to 200 mmHg, 0.1 to 100 mmHg, 0.5 to 50 mmHg, or 1 to 10 mmHg. In addition, the temperature applied to the polycondensation reaction may be 150 to 300°C, 200 to 290°C, 220 to 280°C, or 230 to 260°C. For example, the polycondensation reaction may be carried out under reduced pressure conditions of 0.1 to 10 mmHg and at 200 to 260°C for 1 to 24 hours in a vacuum atmosphere. By performing a polycondensation reaction under the above conditions, a thermoplastic polyester elastomer resin having a desired molecular weight and intrinsic viscosity (IV) can be manufactured while sufficiently removing by-products.

[0141] By going through these steps (1-1) and (1-2), a thermoplastic polyester elastomer resin including repeating units ((a), (b), (c)) represented by the chemical formulas 1 to 3 described above can be manufactured in high yield.

[0142]

[0143] Meanwhile, the thermoplastic polyester elastomer resin according to the present invention can be manufactured by a process of producing a first thermoplastic polyester elastomer resin and a second thermoplastic polyester elastomer resin as reaction raw materials through a process of condensation polymerization after an esterification reaction or an ester exchange reaction, and then melt-kneading them. Specifically, the method for producing the thermoplastic polyester elastomer resin according to the present invention comprises the steps of: (2-1) reacting a first glycol component comprising 1,4-butanediol; a first dicarboxylic acid component; and a first high molecular weight glycol component comprising polytrimethylene ether glycol to obtain a first reactant; (2-2) reacting a second glycol component comprising 1,4-butanediol; a second dicarboxylic acid component; and a second high molecular weight glycol component comprising ethylene oxide addition polypropylene glycol to obtain a second reactant; and (2-3) reacting the first reactant; The second reactant and the reactive compatibilizer are melt-mixed, and this is specifically described as follows.

[0144] Step (2-1): First esterification reaction, or first ester exchange reaction

[0145] According to the present invention, step (2-1) is a step of introducing a first glycol component, a first dicarboxylic acid component, and a first high molecular weight glycol component as reaction raw materials into a reactor (esterification reactor or ester exchange reactor), performing an esterification reaction or an ester exchange reaction to obtain a reactant (intermediate reactant), and subjecting the reactant to a condensation polymerization reaction to obtain a first reactant (first thermoplastic polyester elastomer resin).

[0146] Descriptions of the first glycol component and the first dicarboxylic acid component are the same as those of the glycol component and the dicarboxylic acid component, and are therefore omitted. The first high molecular weight glycol component may include polytrimethylene ether glycol (PO3G), and specifically, may be composed solely of polytrimethylene ether glycol (PO3G).

[0147] Meanwhile, the description of the esterification reaction, or ester exchange reaction and polycondensation reaction for producing the first reactant is omitted as it is the same as described above.

[0148] Step (2-2): Second esterification reaction, or second ester exchange reaction

[0149] According to the present invention, step (2-2) is a step of introducing a second glycol component, a second dicarboxylic acid component, and a second high molecular weight glycol component as reaction raw materials into a reactor (esterification reactor or ester exchange reactor), performing an esterification reaction or an ester exchange reaction to obtain a reactant (intermediate reactant), and subjecting this to a condensation polymerization reaction to obtain a second reactant (second thermoplastic polyester elastomer resin).

[0150] Descriptions of the second glycol component and the second dicarboxylic acid component are the same as those of the glycol component and the dicarboxylic acid component, and are therefore omitted. The second high molecular weight glycol component may include ethylene oxide-added polypropylene glycol (EO-PPG), and specifically, may be composed solely of ethylene oxide-added polypropylene glycol (EO-PPG).

[0151] Meanwhile, the description of the esterification reaction, or ester exchange reaction and polycondensation reaction for producing the second reactant is omitted as it is the same as described above.

[0152] Step (2-3): Melt mixing

[0153] According to the present invention, step (2-3) is a step of melt-mixing the first reactant obtained in step (2-1) and the second reactant obtained in step (2-2). In the melt-mixing of step (2-3), a reactive compatibilizer capable of maximizing the dispersibility of the first and second reactants while allowing chemical cross-linking is introduced, thereby securing basic physical properties while producing a thermoplastic polyester elastomer resin having excellent mechanical strength, elasticity, and compressive elasticity recovery. In particular, by applying the reactive compatibilizer, the first and second reactants are dispersed and combined without causing micro-phase separation of the soft block having a repeating unit (repeating unit (c) of chemical formula 3) derived from ethylene oxide-added polypropylene glycol (EO-PPG) having an energy repulsive elastic effect and the soft block having a repeating unit (repeating unit (b) of chemical formula 2) derived from polytrimethylene ether glycol (PO3G) that determines mechanical strength, thereby producing a thermoplastic polyester elastomer resin having excellent elasticity and compressive elasticity recovery. The description of the reactive compatibilizer is the same as described above and therefore is omitted.

[0154] Meanwhile, the above melt mixing can be performed under heating and / or pressurization conditions using a single-screw extruder, a twin-screw extruder, a mixing roll, a Banbury mixer, a batch mixer, a molding machine, etc.

[0155] For the above melt mixing, the first reactant and the second reactant may go through a preliminary mixing process. Specifically, the preliminary mixing process may be performed by putting the first reactant and the second reactant into various mixers such as a V-type blender, a ribbon blender, a Henschel mixer, a rocking mixer, a tubular mixer, a planetary mixer, a Banbury mixer, a mill blender, a mixing roll, and a tumbler and mixing them in advance in a solid state. The mixing time in the solid state may vary depending on the type of mixer, but the mixing time may be adjusted so that the standard deviation is within 1% and at most 2% compared to the target mixing ratio when five random locations are sampled after mixing.

[0156] In this preliminary mixing process, commonly known additives (e.g., coloring agents, fillers, UV blockers, heat stabilizers, etc.) may be further added as needed. Here, the first and second reactants may be directly added to a single-screw extruder, twin-screw extruder, mixing roll, Banbury mixer, batch mixer, molding machine, etc. for melt mixing without going through the preliminary mixing process. In addition, a thermoplastic polyester elastomer resin may be manufactured by mixing some of the raw material components in advance and then melt mixing the resulting reactant to form a masterbatch, mixing the remaining raw material components into the masterbatch, and then melt mixing again.

[0157] Meanwhile, the mixing ratio of the first reactant and the second reactant during the melt mixing is not particularly limited, but considering the desired properties of the thermoplastic polyester elastomer resin, it may be a weight ratio of 40:60 to 99:1, a weight ratio of 45:55 to 99:1, a weight ratio of 50:50 to 98:2, a weight ratio of 55:45 to 98:2, a weight ratio of 60:40 to 95:5, a weight ratio of 60:40 to 90:10, a weight ratio of 65:35 to 90:10, a weight ratio of 70:30 to 85:15, or a weight ratio of 75:25 to 85:15.

[0158] Specifically, the melt mixing can be performed in the single-screw extruder or the twin-screw extruder. The temperature at which the melt mixing is performed through the extruder(s) (e.g., the barrel temperature of the extruder) is not particularly limited and can be determined in consideration of miscibility, ease of extrusion, extrusion reaction efficiency, etc. Specifically, the melt mixing is performed at the melting temperature (T) of the desired thermoplastic polyester elastomer resin. m ) can be performed at a temperature 20 to 30 ℃ higher than that of the extruder. For example, the temperature at which the melt mixing is performed may be 170 to 230 ℃, 180 to 225 ℃, 190 to 220 ℃, 195 to 215 ℃, or 200 to 210 ℃. Meanwhile, the extrusion speed (screw rotation speed) of the extruder(s) is not particularly limited, and may be specifically 150 to 230 rpm, 160 to 225 rpm, 170 to 220 rpm, 180 to 210 rpm, 190 to 205 rpm, or 195 to 200 rpm. As the melt mixing is performed under these conditions, sufficient melt mixing and reactive extrusion can be performed while ensuring an appropriate throughput per unit time. If the above conditions are exceeded, the thermoplastic polyester elastomer resin may undergo thermal decomposition or the melting characteristics may be poor, resulting in a deterioration in the melt mixing and reactive extrusion characteristics of the compatibilizer.

[0159] As the above reactive compatibilizer is introduced and melt-mixed, the hydroxyl group (-OH) or carboxyl group (-COOH) present in each of the first reactant and the second reactant can react with the glycidyl group or maleic anhydride structure of the reactive compatibilizer to form an ether bond or an ester bond.

[0160] Specifically, by going through steps (2-1) to (2-3), a thermoplastic polyester elastomer resin including the repeating unit (d) described above together with the repeating units ((a), (b), (c)) represented by the chemical formulae 1 to 3 described above can be manufactured in high yield.

[0161]

[0162] Compositions and articles

[0163] The composition according to the present invention comprises the thermoplastic polyester elastomer resin described above. Specifically, the composition according to the present invention can be used for the manufacture of various products because it comprises a thermoplastic polyester elastomer resin with excellent mechanical strength, elasticity, and compression-elastic recovery.

[0164] The composition according to the present invention may further include commonly known solvents and additives as needed.

[0165] Meanwhile, the article according to the present invention comprises the thermoplastic polyester elastomer resin described above. The article according to the present invention is not particularly limited, but may be a fiber, a foam (a molded article in the form of foam), or a shoe part.

[0166] The fibers may be monocomponent fibers and / or multicomponent fibers (e.g., bicomponent fibers). Such fibers may be used to produce woven, knitted, or nonwoven fabrics.

[0167] The above foam (a molded product in the form of foam) can be manufactured through a process of physically or chemically foaming the thermoplastic polyester elastomer resin described above in a mold or autoclave. The density of the foam is not particularly limited, but is 0.15 to 0.45 g / cm. 3 This foam can be used as straps, reporting gears, high-elasticity buffer parts, etc., because it has high elasticity and energy return properties due to the thermoplastic polyester elastomer resin described above.

[0168] The above shoe part is obtained by injecting the above-described thermoplastic polyester elastomer resin into a mold and molding it, and can be specifically a cushioning material for a shoe midsole, a shoe outersole, or a shoe insole.

[0169] The present invention is described in more detail through the following examples. However, the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention.

[0170]

[0171] [Example 1]

[0172] Step (1-1): Preparation of reactants through ester exchange reaction

[0173] Into a 1.2 ㎥ volume ester exchange reactor connected to a water-coolable condenser and column, 24.2 kg of 1,4-butanediol (BD) as a glycol component; 43.9 kg of polytrimethylene ether glycol (PO3G) and 13.2 kg of ethylene oxide-added polypropylene glycol (EO-PPG) as high molecular weight glycol components; 40.0 kg of dimethyl terephthalate (DMT) as a dicarboxylic acid component; 0.06 kg of trimellitic anhydride (TMA) as a polymerization reaction branching agent; 0.25 kg of tetrabutyl titanate (TBT) as a reaction catalyst; 0.15 kg of I1098 and 0.15 kg of I1019 as primary antioxidants; and 0.1 kg of I168 as a secondary antioxidant were charged. Next, the reactor was evacuated and nitrogen was flowed to backfill the pressure inside the reactor to 1 kg / cm2 to create an inert atmosphere. Thereafter, the input raw materials were stirred and heated under a nitrogen atmosphere, and when the temperature inside the reactor reached approximately 200°C, the transesterification reaction was performed while maintaining the temperature at 200°C for 3 hours. At this time, methanol, a by-product, was discharged through a column and a condenser during the transesterification reaction, and the transesterification reaction was continued until the outflow of methanol stopped. After the transesterification reaction was completed, the nitrogen inside the pressurized reactor was discharged to the outside to lower the pressure inside the reactor to normal pressure, and the reactant (result) inside the reactor was transferred to a polycondensation reactor with a volume of 0.75 m3 capable of vacuum reaction.

[0174] Step (1-2): Preparation of thermoplastic polyester elastomer resin through polycondensation reaction

[0175] The pressure of the polycondensation reactor was lowered from atmospheric pressure to 5 Torr (absolute pressure: 5 mmHg) over 30 minutes, and at the same time, the temperature of the polycondensation reactor was raised to 245 ℃ over 1 hour. The polycondensation reaction was performed while maintaining the pressure of the polycondensation reactor below 1 Torr (absolute pressure: 1 mmHg). At this time, the stirring speed was set high in the early stage of the polycondensation reaction, and as the polycondensation reaction progressed, the glycol component, which is a by-product, was discharged through the column and condenser. If the stirring force weakened due to the increase in the viscosity of the reactant or the temperature of the reactant rose above the set temperature, the stirring speed was appropriately adjusted. Thereafter, the polycondensation reaction was performed until the intrinsic viscosity (IV) of the reactant (melt) inside the reactor became 1.85 dl / g, and when the intrinsic viscosity (IV) of the reactant reached the desired level, the reactant was discharged outside the reactor to form a strand. Next, a thermoplastic polyester elastomer resin was obtained by going through a pelletizing process so that the average weight of 100 cut pellets after solidification with a cooling liquid was approximately 2.5 to 4.0 g.

[0176]

[0177] [Examples 2 to 6]

[0178] A thermoplastic polyester elastomer resin was obtained through the same process as Example 1, except that the content (unit: kg) of each input raw material was applied as shown in Table 1 below.

[0179]

[0180] [Comparative Examples 1 to 6]

[0181] A thermoplastic polyester elastomer resin was obtained through the same process as Example 1, except that the content (unit: kg) of each input raw material was applied as shown in Table 2 below.

[0182]

[0183] Input raw materials Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 DMT 4 0.03 2.24 4.04 0.15 6.13 7.11,4-BD 2 4.21 8.227 4 24.136 0 2 1.9 PO 3 G 4 3.9 4 3.7 29 0 5 5.3 1 1.3 4 6.5 PO 3 G Mn 2 0.00 2 0.00 2 0.00 2 0.00 2 0.00 2 0.00 1 0.00 2 0.00 0 EO-PPG 1 3.22 2.5 23.21 7 27.11 4.0 EO-PPG Mn2,4002,4002,4002,4002,4002,400TMA0.060.050.070.060.090.06I10980.150.150.150.150.150.150.15I10190.150.150.150.150.150.150.15I1680.10.10.10.10.10.10.1TBT0.250.250.250.250.250.25DMT: Dimethyl terephthalate1,4-BD: 1,4-butanediolPO3G: Polytrimethylene ether glycolEO-PPG: Ethylene oxide addition polypropylene glycolTMA: Trimellitic anhydrideTBT: Tetrabutyl titanate

[0184] Input raw material comparison example 1 Comparative example 2 Comparative example 3 Comparative example 4 Comparative example 5 Comparative example 6 DMT29.432.340.060.935.853.11,4-BD15.818.124.137.921.334.5 PO3G-66.257.033.8--PO3G Mn-2,0002,0001,000--PTMG69.7-----PTMG Mn2,000-----EO-PPG----61.741.3EO-PPG Mn----2,4002,400TMA0.050.110.120.11--TMP----0.150.14I10980.150.150.150.150.150.150.15I10190.150.150.150.150.150.150.15I1680.100.100.100.100.100.100.10TBT0.250.250.250.250.250.25DMT: Dimethyl Terephthalate1,4-BD: 1,4-ButanediolPO3G: Polytrimethylene Ether GlycolEO-PPG: Ethylene Oxide Added Polypropylene GlycolPTMG: Polytetramethylene Ether GlycolTMA: Trimellitic AnhydrideTMP: Trimethylol PropaneTBT: Tetrabutyl titanate

[0185]

[0186] The composition and properties of the thermoplastic polyester elastomer resins obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were evaluated as follows, and the results are shown in Tables 3 and 4 below.

[0187]

[0188] [Test Example 1] Contents of hard block (chemical formula 1) and soft block (chemical formula 2 and 3)

[0189] After dissolving the thermoplastic polyester elastomer resin in CDCl3 solvent at a concentration of 3 mg / mL, the result was analyzed using a nuclear magnetic resonance device (JEOL, 600 MHz FT-NMR) at 25 ℃. 1 H-NMR spectra were obtained. By analyzing the spectra, the contents (weight %) of BD, PO3G, and EO-PPG were calculated based on the total mole number of residues derived from all glycols (BD, PO3G, EO-PPG, etc.), and this was used to confirm the contents of the hard and soft blocks.

[0190]

[0191] [Test Example 2] Shore D hardness (H)

[0192] The hardness of thermoplastic polyester elastomer resin was measured according to ASTM D2240 (Durometer Type D). Specifically, thermoplastic polyester elastomer resin pellets were injection-molded using an injection molding machine (ENGEL, Victory 80) to produce test specimens measuring 100 mm in width, 100 mm in length, and 2 mm in thickness. Hardness was measured by applying a test specimen of 6 mm in thickness, which was made by overlapping three of these.

[0193]

[0194] [Test Example 3] Intrinsic viscosity (IV)

[0195] A thermoplastic polyester elastomer resin was dissolved in orthochlorophenol (OCP) at a concentration of 0.12% at 150°C to obtain a solution, and then the intrinsic viscosity of the thermoplastic polyester elastomer resin was measured using a Ubbelrod viscometer in a constant temperature bath at 35°C. Specifically, the temperature of the viscosity tube was maintained at 35°C, and the time it took for the solvent to pass through a specific internal section of the viscosity tube (efflux time) and the time it took for the solution to pass through were measured to obtain the specific viscosity, which was then used to calculate the intrinsic viscosity.

[0196]

[0197] [Test Example 4] Melting Index (MI)

[0198] According to ASTM D1238, the melt index was calculated by averaging the amount of discharged material per hour three times after allowing the thermoplastic polyester elastomer resin to remain at 220°C and a 2.16 kg load for 4 minutes.

[0199]

[0200] [Experimental Example 5] Melting Point (Tm)

[0201] Thermoplastic polyester elastomer resin was dried under reduced pressure at 50°C for 15 hours, melted and rapidly cooled, and then scanned at a temperature of 10°C / min using a differential scanning calorimeter (DSC, TA Instruments). The highest point of the endothermic peak due to resin melting was then measured as the melting point (T m ) was used.

[0202]

[0203] [Test Example 6] Tensile strength

[0204] The tensile strength of thermoplastic polyester elastomer resin was measured according to ASTM D638. Specifically, thermoplastic polyester elastomer resin pellets were injection-molded using an injection molding machine (ENGEL, Victory 80) to produce test specimens measuring 120 mm in width, 120 mm in length, and 2 mm in thickness. These were then punched to prepare tensile test specimens of ASTM Type I (dumbbell-shaped bars). Next, the tensile strength of the tensile test specimens was measured using a tensile tester (Zwick Roell, Z010) at a speed of 50 mm / min.

[0205]

[0206] [Test Example 7] Compression Set (CS)

[0207] The compression set of thermoplastic polyester elastomer resin was measured according to ISO 816 Method B. Specifically, thermoplastic polyester elastomer resin pellets were injection-molded using a compression mold (WithLab, WL1700) to produce test specimens with a diameter of 29 mm and a thickness of 12.5 mm, which were then compressed at 70°C with a compression ratio of 25% for 22 hours. After the compressive force was removed, the residual strain was obtained, which was then used to calculate the compression set.

[0208]

[0209] [Example 8] Resilience (R)

[0210] The resilience of thermoplastic polyester elastomer resins was measured according to ASTM D2632. Specifically, thermoplastic polyester elastomer resin pellets were injection-molded using a compression mold (WithLab, WL1700) to produce test specimens with a diameter of 29 mm and a thickness of 12.5 mm. Next, a 28 g weight was dropped onto the test specimen, and the rebound height was obtained, which was used to calculate the resilience.

[0211]

[0212] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Repeating unit of chemical formula 2 (b) Weight % (y) 46.75 46.58 30.90 58.89 12.75 49.56 Repeating unit of chemical formula 3 (c) Weight % (z) 13.88 23.71 24.46 1.79 28.54 14.72 Repeating unit of chemical formula 1 (a) Weight % (x) 39.37 29.71 44.64 39.32 58.71 35.72 y / z (weight ratio of soft block) 3.37 1.96 1.26 32.90 0.45 3.37 (y+z) / x (weight ratio of soft block / hard block) Weight ratio) 1.542.371.241.540.701.80H(shore D) 403045404838IV(㎗ / g) 1.851.701.511.751.211.71MI(g / 10min,220℃) 172012151417Tm(℃) 201196218194217200Tensile strength(kgf / cm 2 )260230300260340230Permanent Compression Set (CS, %)493455505645Resilience (R, %)657161576465H / CS0.820.880.820.80.860.84H / R0.620.420.740.70.750.58

[0213] Classification Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Repeating unit of chemical formula 2 (b) weight % (y) 74.3 (PTMG derived repeating unit) 70.56 0.83 8.2 -- Repeating unit of chemical formula 3 (c) weight % (z) ---- 65.04 3.5 Repeating unit of chemical formula 1 (a) weight % (x) 25.72 9.53 9.26 1.83 5.05 6.5 y / z (weight ratio of soft block) ------ (y + z) / x (weight ratio of soft block / hard block) 2.89 2.39 1.55 0.62 1.86 0.77 H (shore D)303040552847IV(㎗ / g)1.871.851.791.311.381.08MI(g / 10min,220℃151711132411Tm(℃)180174195203194216Tensile strength(kgf / cm 2)270220260380120180Permanent Compression Set (CS, %)474460645355Resilience (R, %)657051505550H / CS0.640.680.670.860.530.85H / R0.460.430.781.100.510.94

[0214] Referring to Tables 3 and 4 above, it can be confirmed that the resins of Examples 1 to 6, which are thermoplastic polyester elastomer resins according to the present invention, have excellent mechanical strength, elasticity (resilience), and compression set, which is elastic recovery after long-term deformation, because they include soft blocks containing PO3G and EO-PPG derived repeating units (chemical formulae 2 and 3) and hard blocks (chemical formulae 1).

[0215] On the other hand, it can be confirmed that the thermoplastic polyester elastomer resin of Comparative Example 1, in which PTMG was used alone, and the thermoplastic polyester elastomer resins of Comparative Examples 2 to 4, in which PO3G was used alone, have good mechanical strength but poor elasticity or elastic recovery. In addition, it can be confirmed that the thermoplastic polyester elastomer resins of Comparative Examples 5 and 6, in which EO-PPG was used alone, have significantly poor mechanical strength.

Claims

1. A repeating unit (a) represented by the following chemical formula 1; A repeating unit (b) represented by the following chemical formula 2; and A thermoplastic polyester elastomer resin comprising a repeating unit (c) represented by the following chemical formula 3: [Chemical Formula 1] [Chemical Formula 2] [Chemical Formula 3] In the above chemical formulas 1 to 3, R 1 Inland R 3 are each independently C1 to C 12 A straight-chain, branched, or cyclic divalent aliphatic hydrocarbon group; or C6 to C 12 The second is an aromatic hydrocarbon group, m is an integer from 2 to 6, n is an integer from 2 to 3, p is an integer between 10 and 30, t is an integer from 1 to 30, s is an integer from 1 to 40.

2. In paragraph 1, A thermoplastic polyester elastomer resin satisfying the following equation 1: [Formula 1] 0.5 ≤ (y + z) / x ≤ 3.0 In the above equation 1, x is the weight occupied by the repeating unit (a) represented by the above chemical formula 1 in the thermoplastic polyester elastomer resin, y is the weight occupied by the repeating unit (b) represented by the above chemical formula 2 in the thermoplastic polyester elastomer resin, z is the weight occupied by the repeating unit (c) represented by the above chemical formula 3 in the thermoplastic polyester elastomer resin.

3. In paragraph 1, A thermoplastic polyester elastomer resin satisfying the following equation 2: [Formula 2] 0.3 ≤ y / z ≤ 35 In the above equation 2, y is the weight occupied by the repeating unit (b) represented by the above chemical formula 2 in the thermoplastic polyester elastomer resin, z is the weight occupied by the repeating unit (c) represented by the above chemical formula 3 in the thermoplastic polyester elastomer resin.

4. In paragraph 1, Tensile strength measured according to ASTM D638 is 190 kgf / cm 2 Ideal, thermoplastic polyester elastomer resin.

5. In paragraph 1, A thermoplastic polyester elastomer resin satisfying the following equation 3: [Formula 3] H / R ≤ 0.75 In the above equation 3, H is the Shore D hardness of the thermoplastic polyester elastomer resin measured according to ASTM D2240, R is the resilience of the thermoplastic polyester elastomer resin as measured according to ASTM D2632.

6. In paragraph 1, A thermoplastic polyester elastomer resin satisfying the following equation 4: [Formula 4] 0.8 ≤ H / CS In the above equation 4, H is the Shore D hardness of the thermoplastic polyester elastomer resin measured according to ASTM D2240, CS is the compression set of thermoplastic polyester elastomer resin measured according to ISO 816 Method B.

7. In paragraph 1, A thermoplastic polyester elastomer resin having an intrinsic viscosity of 1.0 to 2.4 ㎗ / g.

8. In paragraph 1, The repeating unit (a) represented by the above chemical formula 1 is derived from the reaction of a glycol component including 1,4-butanediol; and a dicarboxylic acid component, The repeating unit (b) represented by the above chemical formula 2 is derived from the reaction of a dicarboxylic acid component; and a high molecular weight glycol component including polytrimethylene ether glycol, A thermoplastic polyester elastomer resin, wherein the repeating unit (c) represented by the above chemical formula 3 is derived from the reaction of a dicarboxylic acid component; and a high molecular weight glycol component including ethylene oxide-added polypropylene glycol.

9. In paragraph 8, Based on the total mol% of the above glycol component, the amount of 1,4-butanediol used is 75 mol% or more, A thermoplastic polyester elastomer resin in which the amount of polytrimethylene ether glycol used is 50 mol% or more based on the total mol% of the high molecular weight glycol component.

10. In paragraph 8, The above dicarboxylic acid component includes at least one selected from the group consisting of terephthalic acid and dimethyl terephthalate, A thermoplastic polyester elastomer resin in which at least one selected from the group consisting of terephthalic acid and dimethyl terephthalate is used in an amount of 50 mol% or more based on the total mol% of the dicarboxylic acid component.

11. In paragraph 8, A thermoplastic polyester elastomer resin, wherein the number average molecular weights of the high molecular weight glycol component including the above polytrimethylene ether glycol and the high molecular weight glycol component including the above ethylene oxide-added polypropylene glycol are each 400 to 5,000 g / mol.

12. In paragraph 8, A thermoplastic polyester elastomer resin, wherein the number average molecular weights of the high molecular weight glycol component including the polytrimethylene ether glycol and the high molecular weight glycol component including the ethylene oxide-added polypropylene glycol are each 1,000 to 3,000 g / mol. 13.(1-1) A step of obtaining a reactant by reacting a glycol component; a dicarboxylic acid component; and a high molecular weight glycol component; and (1-2) comprising a step of subjecting the above reactants to a condensation polymerization reaction, A method for producing a thermoplastic polyester elastomer resin, comprising a repeating unit (a) represented by the following chemical formula 1; a repeating unit (b) represented by the following chemical formula 2; and a repeating unit (c) represented by the following chemical formula 3: [Chemical Formula 1] [Chemical Formula 2] [Chemical Formula 3] In the above chemical formulas 1 to 3, R 1 Inland R 3 are each independently C1 to C 12 A straight-chain, branched, or cyclic divalent aliphatic hydrocarbon group; or C6 to C 12 The second is an aromatic hydrocarbon group, m is an integer from 2 to 6, n is an integer from 2 to 3, p is an integer between 10 and 30, t is an integer from 1 to 30, s is an integer from 1 to 40.

14. A composition comprising a thermoplastic polyester elastomer resin according to any one of claims 1 to 12.

15. An article comprising a thermoplastic polyester elastomer resin according to any one of claims 1 to 12.

16. In paragraph 15, An article wherein the above article is a fiber, foam, or shoe part.

Citation Information

Patent Citations

  • Preparation of polyester elastomer

    JP1990283759A

  • Flexible polyester-polyether elastomers, compositions and keypads

    JP2990437B2

  • Polyether ester elastomer comprising polytrimethyleneether ester soft segment and tetramethylene ester hardsegment

    KR100933411B1

  • Methods for preparing polyether ester elastomer composition

    US20110021697A1

  • Polytrimethylene ether ester elastomer flexible films

    US7422795B2