Water-disintegratable cardboard sheet and tube
A bleached hardwood pulp cardboard sheet with CMC, PVP, and PEPA binding agents addresses the low disintegration rate and water hardness issues, achieving rapid and uniform disintegration in cold water, enhancing the solubility and strength of water-soluble cardboard sleeves for sanitary products.
Patent Information
- Application Number
- PCT/RU2024/050038
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-02-13
- Publication Date
- 2024-12-05
AI Technical Summary
Existing water-soluble cardboard sheets and sleeves have low disintegration rates in cold water and are affected by water hardness variations, which is a concern given the varying quality of water across different regions, impacting their effectiveness in dissolving uniformly.
A bleached hardwood pulp cardboard sheet with a specific binding agent composition, including carboxymethylcellulose (CMC), polyvinylpyrrolidone (PVP), and polyethylene polyamine (PEPA), is developed to enhance the solubility in cold water under variable hardness conditions, ensuring rapid disintegration within 7 seconds.
The solution achieves rapid and uniform disintegration in cold water across different water hardness levels, outperforming existing solutions like the Zewa Aqua Tube, with improved strength and manufacturing ease using available raw materials and standard adhesives.
Smart Images

Figure 000011 
Figure 000012 
Figure 000013
Abstract
Description
[0001] CARDBOARD SHEET AND SLEEVE THAT DISINTEGRATE IN WATER
[0002] The invention relates to the paper industry and consists of developing a cardboard made from bleached hardwood pulp, glued in the mass with a binding agent, which dissolves in cold water under conditions of variable hardness, with the aim of obtaining a water-soluble toilet paper roll similar to Zewa Aqua Tube®.
[0003] The core or bushing is a consumable material in industrial production as a base for winding foil, packaging stretch film, scotch tape, adhesive tapes, receipt tapes in cash registers, paper, cardboard, linoleum and other rolled materials for the purpose of their preservation.
[0004] The core material must be sufficiently rigid to withstand the loads and forces that act on the rolls during their production, transportation and storage. If the core material is not strong enough, the roll is subject to deformation. This has a negative impact on the quality of the resulting product and on all output products.
[0005] In the present invention, a cardboard core is used in the production of sanitary and hygienic products, in particular, toilet paper. The core has an additional property - solubility in water. This solution is relevant, because it is convenient for the end user (the core does not need to be thrown into the trash can, thereby adding to the mass of solid household waste), and is environmentally friendly.
[0006] The prior art discloses the invention "Method for manufacturing a paper sheet disintegrating in water, using such a paper sheet to manufacture a core that is a support element for a roll, a paper sheet disintegrating in water, and a core made from such a paper sheet" (Patent RU No. 2517129, published on 27.01.2013). This method includes the following stages: ensuring the presence of at least one tape of a water-soluble binder in the form of a dry film, ensuring the presence of at least two tapes, each of which is formed from at least one layer of cellulose fibers, placing the said tape of a water-soluble binder between the said two tapes of cellulose fibers, moistening, joining and compressing the said three tapes, drying the composite tape thus obtained.The sheet obtained in this way can be used to make a core, which is a supporting element for a roll, for which one or more strips obtained from the said sheet are wound along a helical line on a cylindrical core form. The sheet in a dry state contains a water-soluble binder in an amount of 20% to 70%, preferably 25 - 50% of the mass of the finished sheet. For example, polyvinyl alcohol can be used as a binder.
[0007] The invention "A sheet of fibrous material that disintegrates in water, a method for producing such a sheet and the use of a sheet of fibrous material for producing a core for a roll of absorbent material" is known (Patent RU No. 2575071, published 10.09.2013). This invention relates to a sheet of fibrous material with a base density of 20 to 1000 g / m 2, which is manufactured by the wet papermaking process and dried by heat exchange, disintegrates in water in less than 120 s when measured according to NFQ 34-020 and contains from 10 to 70% starch and at least 30% paper-forming fibres by total dry sheet weight of fibrous material, the starch being distributed uniformly throughout the thickness of the sheet.
[0008] The closest analogue (prototype) is the invention "Roll of an absorbent sheet without a core and a method for its manufacture" (Patent RU No. 2754029, published on 08 / 25 / 2021), which proposes a coreless technology, but with the preservation of the strength properties of a toilet paper roll by gluing individual turns of the main product in the area of the hollow axial channel. In this case, a water-soluble composite coating is used, which gives the paper strength in a dry state and does not prevent its disintegration in water after use for its intended purpose. The coating consists of a polymer (for example, a polyether polyol) and a binder - PVP (PVP) - polyvinylpyrrolidone. The mass ratio of the polymer to the binder according to the patent is at least 92: 8, preferably at least 96: 4.
[0009] The disadvantages of the analogues and the prototype are the low speed of disintegration of sheets of fibrous material in cold water and the lack of information on the effect of water hardness on the disintegration of such sheets.
[0010] Water hardness in different regions can vary widely and is not constant throughout the year. As is known, the solubility of substances is affected by whether the water contains other substances, i.e. the solubility of substances may differ in hard and soft water.
[0011] The relevance of assessing the ability of a cardboard core to dissolve in water of variable hardness is due to the different quality of water in households in different regions of the country. In accordance with SanPiN 1.2.3685-21, the total mineralization of drinking water from central water supply systems should not exceed 1 g / l, i.e. it is classified as soft water.
[0012] However, in Russia, according to RBC data for 2019, more than 12 million residents do not have access to central water supply and another 11 million people in 83 regions are not provided with quality water.
[0013] [https: / / realty.rbc.ru / news / 5d9dc79e9a79472e2f90ccb3?ysclid=lgv9tvjrbs721258083].
[0014] According to Rosstat data for 2023, 9.7% of the country's citizens do not have central water supply at all.
[0015] [https: / / news.rambler.ru / other / 41978824 / ?utm_content=news_media&utm_medium=read_more &utm_source=copylink] .
[0016] Toilet paper is a mass-market product and is used regardless of the region and water quality. Therefore, the water-degradable core must show good ability to dissolve regardless of the quality and hardness of the water.
[0017] The objective of the proposed invention is to obtain a water-soluble (dissolving in water) cardboard sheet and a core made from it with an increased dissolving speed in cold water under conditions of its variable hardness.
[0018] The technical result coincides with the task, and also additionally includes the simplicity of manufacturing a cardboard core (use of available raw materials, single-layer or double-layer cardboard, standard single-component glue suitable both for manufacturing cardboard as a binder and for manufacturing a core as an adhesive agent), increased specific strength of cardboard for the core.
[0019] In order to create cardboard that disintegrates in water at a speed of no more than 7 s, bleached commercial hardwood pulp was used.
[0020] All unbleached, semi-bleached pulps and mechanical pulps are unsuitable for producing high-speed water-dissolving cardboard. Such semi-finished products are characterized by an increased content of residual lignin, which after drying becomes keratinized (vitrified), clogs the pores on the surface of the cell wall of the cellulose fiber and, as a result, leads to a sharp decrease in the absorption capacity of the fibrous semi-finished product and, as a consequence, cardboard.
[0021] The cardboard samples were manufactured in laboratory conditions using the wet method by depositing an interwoven structure of cellulose fibers on a mesh in accordance with GOST 14363.4-89. The samples were standard and had an isotropic structure. The base density of the samples (the weight of one square meter in grams) was 180, 250, and 340 g / m 2 . Grinding of fibrous semi-finished products was carried out in a centrifugal grinding apparatus of the Iokro type. The adopted degree of grinding was 18 and 20 °ШР.
[0022] At the stage of preparing the cardboard mass, a binding agent in the form of an aqueous solution was introduced into the cellulose suspension and fed through a filling device to a grid for forming a cardboard sheet. Excess water was removed from the sheet formed on the grid by pressing and subsequent drying. Drying temperature (temperature of the surface of the drying cylinders) 110-115 °C.
[0023] The following chemicals were used as water-soluble binding agents in the production of cardboard:
[0024] - CMC - carboxymethyl cellulose in the form of a white powder. The solution was prepared by dissolving a sample of CMC in water at room temperature of 20-25 °C, with a concentration of 0.5% - 1.0% (preferably 0.5%) with constant stirring. The prepared solution was kept before use for 2 - 4 hours for complete swelling of the CMC particles. The greatest efficiency is observed when using the glue within 4 hours after swelling. The shelf life of the glue is no more than 7 days. It has hazard class 3 - moderately hazardous substances, in accordance with GOST 12.1.007.
[0025] - PVP - polyvinylpyrrolidone grade K-30 in the form of a white fine powder. The solution was prepared by dissolving a sample of PVP in warm water at a temperature of no higher than 50-60 °C, with a concentration of 1% - 15% (preferably 1%, for ease of dosing) with constant stirring until the powder is completely dissolved. The finished solution does not require aging. The shelf life of the glue is no more than 7 days. It is not classified as hazardous to the aquatic environment. It is not categorized by hazard class according to the degree of impact on the body, GOST 12.1.007.
[0026] - NEPA - polyethylenepolyamine, does not require preparation, was used in the form of a yellow-brown solution. The shelf life of the solution is no more than 6 months. It has hazard class 3 - moderately hazardous substances, in accordance with GOST 12.1.007. The specified additives were dosed separately from each other and with the production of different cardboard samples. All of them participate in the formation of bonds, which leads to an increase in the strength of the cardboard sheet in a dry state and an increase in the ability to dissolve in water. Dissolution in water is ensured by the water-soluble nature of the used binding additives.
[0027] The content of the binding agent in the cardboard sample is 0.3-1.0 wt.%, cellulose - 99.0 - 99.7 wt.%.
[0028] The results of tests for strength and elongation of cardboard samples under tension according to GOST ISO 1924-1 showed that samples glued with HDPE and PEPA have satisfactory results: 5 - 9 kN / m and 1.4 - 1.6%, respectively.
[0029] The ability of cardboard samples (cores) to disintegrate was determined using the Afnor NFQ 34-020 method at a stirrer speed of 400-800 min 1 , water temperature of 16-20 °C. The sample weight of the cardboard was 3.88 g or the sample size was 9x8 cm. Dissolution was carried out on a laboratory hydropulper - disintegrator model N2101, with a volume of 8 l (shown in Fig. 1). The rotation speed of the stirrer was regulated in the range of 400-800 min 4 .
[0030] All cardboard samples, regardless of weight, grinding degree and glue, had satisfactory ability to disintegrate in cold water. The size of undisintegrated particles averaged 20 ± 10 mm when disintegrated for 5 sec.
[0031] Figures 2, 3 and 4 show photographs of unblown pieces when dispersing cardboard samples with a grinding degree of 20 °SR of different base densities (1 - 180 g / m 2 , 2 - 250 g / m 2 , 3 - 340 g / m 2 ) and with different binding additives with a dissolution time of 5 sec.
[0032] The largest unblown pieces were found in samples glued with CMC.
[0033] The size of the unblown cardboard pieces does not depend on the unblown time. The variations in the size of the unblown cardboard fragments during 5 and 7 s are within the experimental error for all the samples studied.
[0034] With a cellulose grinding degree of 18 °TTTR, the sizes of unblown pieces are approximately 1.5 times smaller than with a grinding degree of 20 °TTTR.
[0035] Increasing the weight of 1 square meter of cardboard from 180 to 340 g leads to worse unraveling.
[0036] Thus, the best result of solubility in water was shown by the cardboard sample consisting of cellulose with a grinding degree of 18 °TTGR, a base density of 180 g / m 2in the amount of 99 wt.%, glued with PVP or PEPA binding agents in the amount of 1 wt.% (preferred composition). The core for winding sanitary and hygienic products was made from the cardboard sheet described above by screw winding in one or two layers (for cardboard with a base density of 250 - 340 g / m 2 in one layer, for cardboard with a base density of 180 g / m 2 - in two layers). As a water-soluble binding agent for gluing, solutions of PVP or PEPA or CMC, prepared according to the methods described above, were used with a consumption of no more than 5 g / m 2 .
[0037] The solubility of the manufactured bushings in water of variable hardness was assessed in comparison with the Zewa Aqua Tube bushing. It should be noted that no data on the ability of this bushing to dissolve in water of variable hardness are presented in open sources.
[0038] Water with different degrees of hardness was simulated in laboratory conditions. CaCh and MgSC salts were used as hardness salts in a ratio of 4: 1. Water hardness varied in the range of 1 - 10 mg-eq / l: 1-2 mg-eq / l - soft, 5 mg-eq / l - medium hardness, 10 mg-eq / l - hard.
[0039] Tests of tubes for dissolving in cold water of variable hardness showed that the developed cardboard and tubes made from it have significant advantages not only in terms of dissolving speed, but also in terms of the ability to dissolve in water of variable hardness compared to the Zewa Aqua Tube tube.
[0040] The Zewa Aqua Tube sleeve, coated with starch glue over its entire surface, is wetted worse in hard and medium-hard water and does not dissolve in 5 seconds or more. This is explained by the formation of a hydrogel on its surface as a result of the interaction of the calcium cation in the water with the adhesive substance (starch) on the surface of the sleeve. [The effect of Ca ions on the pasting, morphological, structural, vibrational, and 2+ mechanical properties of the starch-water system Mana de los Angeles Cornejo-Villegas, Natalia Rincon-Londono, Alicia Del RealLdpez, Mario E. Rodriguez-Garcfa]. The hydrogel, in turn, prevents further penetration of water deep into the sleeve and, as a result, its disintegration. This effect is felt tactilely. The use of CMC, PVP and PEPA as water-soluble binding agents, which have active reactive groups (amide, carboxyl, etc.) that react with hardness salts, primarily with the Ca cation 2+, neutralizes hardness salts in water. At the same time, the cardboard surface remains wettable and does not prevent the disintegration of the core. Figures 5-8 show photographs of unblown pieces of cores with PVP, PEPA and CMC binding agents and the Zewa Aqua Tube core under conditions of variable water hardness. Dissolution time is 7 sec. As can be seen from these figures, the Zewa Aqua Tube core did not dissolve into individual fibers in medium-hard and hard water, but only disintegrated into 2-4 large fragments that partially retained the shape of the core. When dissolving cores with CMC, PVP, PEPA binding agents, after 7 sec. the core disintegrated into individual fragments with an average size of 30-40 mm for medium-hard and hard water. In soft water, all the tested samples of the tube, including the Zewa Aqua Tube tube, unraveled equally well, the size of the unraveled fragments did not exceed 15-20 mm.Thus, the water-soluble cardboard core according to the proposed invention is characterized by a high rate of dissolution in cold water with a general hardness index higher than 4 mg-eq / l. The core can be used for winding sanitary and hygienic products, including toilet paper.
Claims
8 CLAUSES OF THE INVENTION 1. A water-soluble cardboard sheet, the weight of one square meter of which is in the range from 180 g to 340 g, characterized in that it is obtained by a wet process from bleached hardwood pulp fibers, the connection between which is achieved with the help of a water-soluble binding agent - a solution of carboxymethyl cellulose or polyvinylpyrralidone, or polyethylene polyamine, while the content of the binding agent in the sheet is 0.3-1.0 wt.%, cellulose - 99.0-99.7 wt.%, and the binding agent is added to the cellulose suspension at the stage of preparing the cardboard mass.
2. A core for winding sanitary and hygienic products from a water-soluble cardboard sheet, made by screw winding it in one or two layers, and for gluing the core, a solution of polyvinylpyrralidone or polyethylenepolyamine, or carboxymethylcellulose is used with a consumption of no more than 5 g / m2, the core is made with the ability to unravel in no more than 7 seconds in water with a hardness in the range of 1-10 mg-eq / l at a temperature of 16-20 ° C, while the weight of one square meter of water-soluble cardboard sheet is in the range from 180 g to 340 g, the water-soluble cardboard sheet is obtained by a wet process from bleached hardwood cellulose fibers, the connection between which is achieved using a water-soluble binding agent - a solution of carboxymethylcellulose or polyvinylpyrralidone, or polyethylenepolyamine, and the content of the binding agent in the sheet is 0.3-1.0 wt.%, cellulose - 99.0-99.7 wt.%, while the binding agent is added to the cellulose suspension at the stage of preparing the cardboard mass.
Citation Information
Patent Citations
Paper or cardboard laminated material and method for manufacturing the same
RU2202021C2
Sheet of fibrous material decomposable in water, method of manufacturing such sheet and application of sheet of fibrous material for manufacturing core for roll of absorbent material
RU2575071C2
Fibrous sheet that disintegrates in water, process for manufacturing said fibrous sheet and core for roll of absorbent material made from strips of said fibrous sheet
RU2599367C2
Method for producing cardboard-base and cardboard-base for laminate material
RU2623405C2
Paper towel rolls
US11447916B2