Silicon film layer deposition method, and method for manufacturing heterojunction solar cell

By passing the reaction gas and inert gas into the reaction chamber in the microcrystalline silicon process of heterojunction solar cells and providing radio frequency signals on the electrode plate, the slow deposition speed and inconsistency of film formation in the microcrystalline silicon process are solved. The problem improves battery efficiency.

WO2024250258A1PCT designated stage expired Publication Date: 2024-12-12IDEAL ENERGY (SHANGHAI) SUNFLOWER THIN FILM EQUIPMENT LTD

Patent Information

Application Number
PCT/CN2023/099263
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-09
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

The existing microcrystalline silicon process has problems such as slow deposition speed, uneven film formation, and susceptible to air erosion, causing dark decay, which affects battery efficiency.

Method used

Reaction gas and inert gas are introduced into the reaction chamber, and the electrode plate is provided with very high frequency and low frequency radio frequency signals, which stimulate gas dissociation and increase the self-biasing voltage and ion movement of the electrode plate, and improve the film formation rate of the silicon film layer. and compactness.

Benefits of technology

The film formation rate and density of the silicon film layer are improved, the corrosion of water vapor and oxygen in the air is reduced, the defects of microcrystalline silicon film are improved, and the battery efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099263_12122024_PF_FP_ABST
    Figure CN2023099263_12122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention are a silicon film layer deposition method and a method for manufacturing a heterojunction solar cell. The silicon film layer deposition method comprises: first, introducing a reaction gas into a reaction chamber; then introducing inert gas into the reaction chamber; simultaneously providing a very high-frequency radio frequency signal and a low-frequency radio frequency signal to an electrode plate in the reaction chamber, using the very high-frequency radio frequency signal to excite and dissociate the gas in the reaction chamber into plasma, and using the low-frequency radio frequency signal to direct the plasma onto the electrode plate, such that the self-bias voltage of the electrode plate is increased, ion motion is accelerated, and ion energy are increased, thereby depositing and forming a silicon film layer on a silicon wafer placed on the electrode plate. According to the present invention, the film forming rate and film forming compactness of a silicon film layer can be increased, erosion by water vapor in the air and oxygen is reduced, dark attenuation is reduced, the shortcomings of a microcrystalline silicon thin film are overcome, and battery efficiency is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon film deposition method and method for manufacturing heterojunction solar cell Technical Field

[0001] The present invention relates to the field of solar energy manufacturing, and in particular to a silicon film deposition method and a method for manufacturing heterojunction solar cells. Background Art

[0002] Thin-film / crystalline silicon heterojunction solar cells (hereinafter referred to as heterojunction solar cells, also known as HIT or HJT or SHJ solar cells) belong to the third generation of high-efficiency solar cell technology. It combines the advantages of crystalline silicon and silicon thin film, and has the characteristics of high conversion efficiency and low temperature coefficient. It will gradually replace PERC cells and become the mainstream of photovoltaic cells.

[0003] The core manufacturing process of heterojunction solar cells in the existing technology is the formation of its various amorphous silicon films, specifically including: using a plasma enhanced chemical vapor deposition (PECVD) process to deposit an intrinsic I-type intrinsic amorphous silicon film and a P-type amorphous silicon film on one side of the N-type crystalline silicon after surface texturing or velveting, and depositing an intrinsic I-type intrinsic amorphous silicon film and an N-type amorphous silicon film on the other side of the crystalline silicon.

[0004] Compared to the various amorphous silicon doped layers mentioned above, microcrystalline silicon doped layers offer improved light transmittance, greater carrier mobility, and a higher effective doping concentration. This results in microcrystalline silicon heterojunction cells with improved short-circuit current, fill factor, and cell efficiency. Microcrystalline silicon processes are gradually replacing traditional amorphous silicon processes. Microcrystalline silicon processes utilize very high frequency (VHF) radio frequency power supplies. Due to the high electron oscillation frequency, VHF radio frequency power supplies generate high plasma density, resulting in faster microcrystalline deposition rates.

[0005] However, the microcrystalline silicon process still has the following shortcomings: First, the deposition rate is relatively slow, requiring the addition of multiple film-forming chambers to match the current amorphous silicon passivation process, resulting in relatively high equipment costs. Second, the microcrystalline silicon film is not dense enough and is easily corroded by water vapor and oxygen in the air, resulting in dark decay (a decrease in cell efficiency). Some in the industry have tried adding argon gas to the PECVD reaction chamber to improve the density of the microcrystalline silicon formed in the microcrystalline silicon process, but the bombardment effect of argon gas at very high frequencies is affected, making the improvement in microcrystalline silicon density ineffective.

[0006] Therefore, how to provide a silicon film deposition method and a method for manufacturing heterojunction solar cells to increase the silicon film formation rate and film density, reduce the erosion of water vapor and oxygen in the air, reduce dark decay, improve microcrystalline silicon film defects, and improve cell efficiency has become a technical problem that needs to be urgently solved in the industry.

[0007] Summary of the Invention

[0008] In view of the above problems in the prior art, the present invention proposes a silicon film deposition method, comprising:

[0009] introducing reaction gas into the reaction chamber;

[0010] introducing an inert gas into the reaction chamber; and

[0011] A very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber, the very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the self-bias voltage of the electrode plate, accelerating the movement of ions, and increasing the ion energy, thereby depositing a silicon film layer on a silicon wafer placed on the electrode plate.

[0012] In one embodiment, the inert gas is argon or helium.

[0013] In one embodiment, the reaction gas includes hydrogen and silane, and further includes phosphine, diborane, or trimethylborane.

[0014] In one embodiment, the reaction gas further includes carbon dioxide and / or methane.

[0015] In one embodiment, the volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of silane to phosphine or diborane or trimethylboron is 1:0.5-2.

[0016] In one embodiment, the frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W; the frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0017] The present invention also provides a method for preparing a heterojunction solar cell, comprising the following steps:

[0018] The monocrystalline silicon wafer is textured and cleaned through the texturing and cleaning process;

[0019] Forming a first intrinsic amorphous / microcrystalline silicon layer and a second intrinsic amorphous / microcrystalline silicon layer on the front and back sides of the single crystal silicon wafer respectively by an intrinsic PECVD process;

[0020] forming an N-type amorphous silicon / microcrystalline silicon layer on the first intrinsic amorphous silicon / microcrystalline silicon layer by an N-type PECVD process;

[0021] forming a P-type amorphous silicon / microcrystalline silicon layer on the second intrinsic amorphous / microcrystalline silicon layer by a P-type PECVD process;

[0022] forming a first transparent conductive film and a second transparent conductive film on the N-type amorphous silicon / microcrystalline silicon layer and the P-type amorphous silicon / microcrystalline silicon layer, respectively; and

[0023] forming a first electrode and a second electrode on the first transparent conductive film and the second transparent conductive film respectively;

[0024] The intrinsic PECVD process, the N-type PECVD process, and the P-type PECVD process each include:

[0025] introducing corresponding reaction gas into the reaction chamber;

[0026] introducing an inert gas into the reaction chamber; and

[0027] A very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber, the very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the self-bias voltage of the electrode plate, accelerating the movement of ions, and increasing the ion energy, thereby depositing a corresponding type of silicon film layer on a silicon wafer placed on the electrode plate.

[0028] In one embodiment, the intrinsic PECVD process includes:

[0029] introducing reaction gases including hydrogen and silane into the reaction chamber;

[0030] introducing an inert gas including argon or helium into the reaction chamber; and

[0031] Simultaneously providing a very high frequency radio frequency signal and a low frequency radio frequency signal to an electrode plate in a reaction chamber, using the very high frequency radio frequency signal to excite and dissociate gas in the reaction chamber into plasma, and using the low frequency radio frequency signal to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias voltage, accelerating ion motion, and increasing ion energy, thereby depositing the first intrinsic amorphous / microcrystalline silicon layer or the second intrinsic amorphous / microcrystalline silicon layer on a silicon wafer placed on the electrode plate;

[0032] The volume ratio of the inert gas to silane is 10-100:1, and the flow ratio of the inert gas to hydrogen is 1-10:20-50.

[0033] In one embodiment, the N-type PECVD process includes:

[0034] introducing reaction gases including hydrogen, silane and phosphine into the reaction chamber;

[0035] introducing an inert gas including argon or helium into the reaction chamber; and

[0036] Simultaneously providing a very high frequency radio frequency signal and a low frequency radio frequency signal to an electrode plate in the reaction chamber, using the very high frequency radio frequency signal to excite and dissociate the gas in the reaction chamber into plasma, and using the low frequency radio frequency signal to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias voltage, accelerating ion motion, and increasing ion energy, thereby depositing an N-type amorphous silicon / microcrystalline silicon layer on a silicon wafer placed on the electrode plate;

[0037] The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of the silane to phosphine is 1:0.5-2.

[0038] In one embodiment, the P-type PECVD process includes:

[0039] introducing a reaction gas comprising hydrogen, silane, and diborane or trimethylboron into the reaction chamber;

[0040] introducing an inert gas including argon or helium into the reaction chamber; and

[0041] A very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to an electrode plate in a reaction chamber, the very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the self-bias voltage of the electrode plate, accelerating ion motion, and increasing ion energy, thereby depositing a P-type amorphous silicon / microcrystalline silicon layer on a silicon wafer placed on the electrode plate;

[0042] The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of the silane to diborane or trimethylboron is 1:0.5-2.

[0043] In one embodiment, the frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W; the frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0044] In one embodiment, the reaction gas further includes carbon dioxide and / or methane.

[0045] In one embodiment, the thickness ranges of the first intrinsic amorphous / microcrystalline silicon layer, the second intrinsic amorphous / microcrystalline silicon layer, the P-type amorphous silicon / microcrystalline silicon layer, and the N-type amorphous silicon / microcrystalline silicon layer are 5-15 nm, 5-15 nm, 20-40 nm, and 20-40 nm, respectively.

[0046] Compared to the prior art method of introducing only inert gas under very high frequency (VHF) excitation, which only slightly improves the film formation speed and film density of microcrystalline silicon, the silicon film deposition method of the present invention first introduces a reaction gas into the reaction chamber, then introduces an inert gas into the reaction chamber, and finally simultaneously provides a very high frequency radio frequency signal and a low frequency radio frequency signal to the electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias voltage, accelerating ion motion, and increasing ion energy, thereby depositing a silicon film layer on a silicon wafer placed on the electrode plate. The present invention can increase the film formation speed and film density of the silicon film layer, reduce the erosion of water vapor and oxygen in the air, reduce dark decay, improve microcrystalline silicon film defects, and improve battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The above features and advantages of the present invention will be better understood after reading the detailed description of the embodiments of the present disclosure in conjunction with the following drawings. In the drawings, the components are not necessarily drawn to scale, and components with similar related properties or characteristics may have the same or similar reference numerals.

[0048] FIG1 is a schematic flow chart of an embodiment of a method for depositing a silicon film according to the present invention.

[0049] FIG2 is a schematic flow chart of an embodiment of a method for preparing a heterojunction solar cell according to the present invention.

[0050] FIG3 is a schematic flow chart showing an embodiment of the intrinsic PECVD process in step S210 of FIG2 .

[0051] FIG. 4 is a schematic flow chart showing a first embodiment of the N-type PECVD process in step S220 of FIG. 2 .

[0052] FIG. 5 is a schematic flow chart showing a second embodiment of the N-type PECVD process in step S230 of FIG. 2 . Specific implementation plan

[0053] The present invention is described in detail below in conjunction with the accompanying drawings and examples so that the objects, features and advantages of the present invention are more clearly understood. It should be understood that the aspects described below in conjunction with the accompanying drawings and examples are merely exemplary and should not be construed as limiting the scope of protection of the present invention in any way. Unless the context clearly indicates otherwise, the singular forms "one" and "the" include plural referents. It should be noted that, in this article, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply the existence of any such actual relationship or order between these entities or operations.

[0054] Referring to FIG1 , which is a schematic flow diagram of an embodiment of a silicon film deposition method of the present invention. As shown in FIG1 , the silicon film deposition method 10 first performs step S100, where a reaction gas is introduced into a reaction chamber. In this embodiment, the reaction gas includes hydrogen and silane, and also includes phosphine, diborane, or trimethylboron. The reaction gas may also include carbon dioxide and / or methane. The flow rate of the hydrogen is in the range of 90-120 slm (liters per minute under standard conditions), the flow rate of the silane is in the range of 160-600 sccm (milliliters per minute under standard conditions), and the flow rate of the phosphine, diborane, or trimethylboron, carbon dioxide, or methane is in the range of 80-1200 sccm.

[0055] Method 10 proceeds to step S110, where an inert gas is introduced into the reaction chamber. In this embodiment, the inert gas is argon (Ar) or helium (He). The flow rate of the inert gas ranges from 5 to 30 slm. The volume ratio of the inert gas to silane is 10-100:1, the flow rate ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of the silane to phosphine, diborane, or trimethylboron is 1:0.5-2.

[0056] Method 10 proceeds to step S120, where a very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma. The low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias, accelerating ion motion, and increasing ion energy, thereby depositing a silicon film layer on the silicon wafer placed on the electrode plate. In this embodiment, the pressure range of the reaction chamber during deposition of the silicon film layer is 2-3.6 mbar, and the deposition time range is 30-120 seconds. The frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W. The frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0057] It should be noted that the silicon film layer in the present invention refers to an amorphous / microcrystalline silicon layer including a mixture of amorphous silicon and microcrystalline silicon, wherein the proportion of microcrystalline silicon is the crystallization rate of the amorphous / microcrystalline silicon layer. The crystallization rate of the amorphous / microcrystalline silicon layer in the present invention is 40%-70%.

[0058] The hydrogen included in the reaction gas in step S100 is primarily used to etch the amorphous silicon during the deposition process. Because amorphous silicon has a relatively loose structure, hydrogen atoms etch amorphous silicon at a higher rate than microcrystalline silicon particles. Using a larger amount of hydrogen can increase the proportion of microcrystalline silicon (crystallization rate). The carbon dioxide and / or methane included in the reaction gas in step S100 can adjust the optical band gap of the silicon film layer, improving the light transmittance of the window layer.

[0059] The inert gas argon or helium in step S110 is a monatomic gas that is very easy to dissociate and is usually used to assist plasma ignition. The dissociated electrons of argon or helium collide with other gas molecules, helping to dissociate the gas and increase the plasma density, thereby also increasing the film formation rate. Argon itself has a large mass. Under low-frequency RF signals (13M or 2M), it can increase the bombardment energy of Ar on the microcrystalline film, thereby improving the density of the film and reducing the dark decay of the microcrystalline silicon cell.

[0060] The higher frequency of VHF signals leads to faster electron oscillations, which in turn generate more ionization, increase plasma density, and enhance the degree of gas dissociation within the cavity. Under VHF and LF signals, Ar or He can bombard amorphous silicon, allowing it to enter the voids between microcrystalline silicon, enhancing the gap-filling effect and improving defects and voids in the microcrystalline silicon film, resulting in a 0.2%-0.3% increase in the conversion efficiency of heterojunction solar cells. The power of the auxiliary LFRF signal (13M or 2M) and the argon flow rate can be adjusted at different stages of microcrystalline growth to achieve optimal efficiency and dark decay results.

[0061] Referring to FIG. 2 , a flow chart illustrating an embodiment of a method for preparing a heterojunction solar cell according to the present invention is shown. As shown in FIG. 2 , the method 20 for preparing a heterojunction solar cell first proceeds to step S200 , in which a monocrystalline silicon wafer is textured and cleaned using a texturing and cleaning process. In this embodiment, the monocrystalline silicon wafer in step S200 is an N-type monocrystalline silicon wafer, and an alkaline etching solution (e.g., a mixture of sodium hydroxide solution or potassium hydroxide solution, isopropyl alcohol, and Na₂SiO₃) is used to remove the damage layer and form a pyramid-shaped textured surface on the N-type monocrystalline silicon wafer.

[0062] The method 20 proceeds to step S210, where a first intrinsic amorphous / microcrystalline silicon layer and a second intrinsic amorphous / microcrystalline silicon layer are formed on the front and back sides of the single-crystalline silicon wafer, respectively, using an intrinsic PECVD process. The specific steps of the intrinsic PECVD process are shown in FIG3 . In step S210, the first intrinsic amorphous / microcrystalline silicon layer and the second intrinsic amorphous / microcrystalline silicon layer can be formed simultaneously on the front and back sides of the N-type single-crystalline silicon wafer using the intrinsic PECVD process performed in the same PECVD reaction chamber, or the first intrinsic amorphous / microcrystalline silicon layer and the second intrinsic amorphous / microcrystalline silicon layer can be formed sequentially on the front and back sides of the N-type single-crystalline silicon wafer using the intrinsic PECVD process performed in different PECVD reaction chambers. The thicknesses of the first intrinsic amorphous / microcrystalline silicon layer and the second intrinsic amorphous / microcrystalline silicon layer range from 5 to 15 nm and 5 to 15 nm, respectively.

[0063] FIG3 shows a flow chart of an embodiment of the intrinsic PECVD process in FIG2 . As shown in FIG3 , the intrinsic PECVD process in step S210 in FIG2 first proceeds to step S2100, where a reaction gas comprising hydrogen and silane is introduced into the reaction chamber. The reaction gas may also include carbon dioxide and / or methane. The hydrogen flow rate range is 90-120 slm, the silane flow rate range is 160-600 sccm, and the carbon dioxide or methane flow rate range is 80-1200 sccm.

[0064] The intrinsic PECVD process continues with step S2110, where an inert gas, including argon or helium, is introduced into the reaction chamber. The inert gas flow rate ranges from 5 to 30 slm. The volume ratio of the inert gas to silane is 10 to 100:1, and the flow ratio of the inert gas to hydrogen is 1 to 10:20 to 50.

[0065] The intrinsic PECVD process proceeds to step S2120, where a very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias, accelerating ion motion, and increasing ion energy, thereby depositing a first intrinsic amorphous / microcrystalline silicon layer and / or a second intrinsic amorphous / microcrystalline silicon layer on the silicon wafer placed on the electrode plate. In this embodiment, the pressure range of the reaction chamber during deposition of the first intrinsic amorphous / microcrystalline silicon layer or the second intrinsic amorphous / microcrystalline silicon layer is 2-3.6 mbar, and the deposition time range is 30-120 seconds. The frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W. The frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0066] 2 , the method 20 proceeds to step S220, where an N-type amorphous silicon / microcrystalline silicon layer is formed on the first intrinsic amorphous silicon / microcrystalline silicon layer by an N-type PECVD process. The specific steps of the N-type PECVD process are shown in FIG4 . In this embodiment, the thickness of the N-type amorphous silicon / microcrystalline silicon layer is 20-40 nanometers.

[0067] As shown in Figure 4, a flow chart of the embodiment of the N-type PECVD process in Figure 2 is shown. As shown in Figure 4, the N-type PECVD process in step S220 in Figure 2 first proceeds to step S2200, where a reaction gas comprising hydrogen, silane, and phosphine is introduced into the reaction chamber. The reaction gas may also include carbon dioxide and / or methane. The flow rate of the hydrogen is in the range of 90-120 slm, the flow rate of the silane is in the range of 160-600 sccm, and the flow rate of the phosphine, carbon dioxide, or methane is in the range of 80-1200 sccm.

[0068] The N-type PECVD process continues with step S2210, where an inert gas, including argon or helium, is introduced into the reaction chamber. The inert gas flow rate ranges from 5 to 30 slm. The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of silane to phosphine is 1:0.5-2.

[0069] The N-type PECVD process proceeds to step S2220, where a very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias, accelerating ion motion, and increasing ion energy, thereby depositing an N-type amorphous silicon / microcrystalline silicon layer on the first intrinsic amorphous / microcrystalline silicon layer. In this embodiment, the pressure in the reaction chamber during deposition of the N-type amorphous silicon / microcrystalline silicon layer is in the range of 2-3.6 mbar, and the deposition time is in the range of 30-120 seconds. The frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W. The frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0070] 2, the method 20 proceeds to step S230, forming a P-type amorphous silicon / microcrystalline silicon layer on the second intrinsic amorphous / microcrystalline silicon layer by a P-type PECVD process. The specific steps of the P-type PECVD process are shown in FIG5. In this embodiment, the thickness of the P-type amorphous silicon / microcrystalline silicon layer is 20-40 nanometers.

[0071] As shown in Figure 5, it shows a flow chart of an embodiment of the P-type PECVD process in step S230 in Figure 2. As shown in Figure 5, the P-type PECVD process in step S230 in Figure 2 first performs step S2300, where a reaction gas including hydrogen, silane, and diborane or trimethylboron is introduced into the reaction chamber. The reaction gas may also include carbon dioxide and / or methane. The flow rate of the hydrogen is in the range of 90-120 slm, the flow rate of the silane is in the range of 160-600 sccm, and the flow rate of the diborane or trimethylboron, carbon dioxide, or methane is in the range of 80-1200 sccm.

[0072] The P-type PECVD process continues with step S2310, where an inert gas, including argon or helium, is introduced into the reaction chamber. The inert gas flow rate ranges from 5 to 30 slm. The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of the silane to diborane or trimethylboron is 1:0.5-2.

[0073] The P-type PECVD process proceeds to step S2320, where a very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias, accelerating ion motion, and increasing ion energy, thereby depositing a P-type amorphous silicon / microcrystalline silicon layer on the second intrinsic amorphous / microcrystalline silicon layer. In this embodiment, the pressure range of the reaction chamber during deposition of the P-type amorphous silicon / microcrystalline silicon layer is 2-3.6 mbar, and the deposition time range is 30-120 seconds. The frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W. The frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

[0074] Continuing with FIG. 2 , the method 20 proceeds to step S240 to form a first transparent conductive film and a second transparent conductive film on the N-type amorphous silicon / microcrystalline silicon layer and the P-type amorphous silicon / microcrystalline silicon layer, respectively. In step S140, the first transparent conductive film and the second transparent conductive film are formed on the N-type amorphous silicon / microcrystalline silicon layer and the P-type amorphous silicon / microcrystalline silicon layer, respectively, by a reactive plasma deposition process or a physical vapor deposition process. Both the first transparent conductive film and the second transparent conductive film may be indium tin oxide (ITO), a ZnO-based film, an IWO-based film, or an ITIO-based transparent conductive film, which may be deposited on the N-type amorphous silicon / microcrystalline silicon layer and the P-type amorphous silicon / microcrystalline silicon layer by sputtering.

[0075] The method 20 proceeds to step S250, where a first electrode and a second electrode are formed on the first transparent conductive film and the second transparent conductive film, respectively. The first electrode and the second electrode can be formed on the first transparent conductive film and the second transparent conductive film, respectively, using a screen printing process or an electroplating process. The first electrode and the second electrode in step S250 can be formed by screen printing and sintering silver paste, commonly used in the industry.

[0076] The silicon film deposition method of the present invention first introduces a reaction gas into a reaction chamber, then introduces an inert gas into the reaction chamber, and finally simultaneously provides a very high frequency radio frequency signal and a low frequency radio frequency signal to an electrode plate in the reaction chamber. The very high frequency radio frequency signal is used to excite and dissociate the gas in the reaction chamber into a plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate, thereby increasing the electrode plate self-bias voltage, accelerating ion motion, and increasing ion energy, thereby depositing a silicon film layer on the silicon wafer in the reaction chamber. The present invention can increase the film formation rate and film density of the silicon film layer, reduce the erosion of water vapor and oxygen in the air, reduce dark decay, improve defects in microcrystalline silicon thin films, and improve battery efficiency.

[0077] The above embodiments are provided to persons familiar with the art for implementing or using the present invention. Personnel familiar with the art may make various modifications or changes to the above embodiments without departing from the inventive concept of the present invention. Therefore, the scope of protection of the present invention is not limited to the above embodiments, but should be the maximum scope of the innovative features mentioned in the claims.

Claims

1. A method for depositing a silicon film, comprising: introducing reaction gas into the reaction chamber; introducing an inert gas into the reaction chamber; as well as A very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber, the very high frequency radio frequency signal is used to excite the gas in the reaction chamber to dissociate into plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate so that the self-bias voltage of the electrode plate is increased, the movement of ions is accelerated, and the energy of ions is increased, thereby depositing a silicon film layer on a silicon wafer placed on the electrode plate.

2. The silicon film deposition method according to claim 1, characterized in that: The inert gas is argon or helium.

3. The silicon film deposition method according to claim 1, characterized in that: The reaction gas includes hydrogen and silane, and also includes phosphine, diborane or trimethylborane.

4. The silicon film deposition method according to claim 3, characterized in that: The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of silane to phosphine or diborane or trimethylboron is 1:0.5-2.

5. The silicon film deposition method according to claim 1, characterized in that: The frequency of the very high frequency radio frequency signal is 40 MHz, and the power range is 6000-10000 W. The frequency of the low frequency radio frequency signal is 13 MHz or 2 MHz, and the power range is 50-1500 W.

6. A method for preparing a heterojunction solar cell, comprising the following steps: The monocrystalline silicon wafer is textured and cleaned through the texturing and cleaning process; Forming a first intrinsic amorphous / microcrystalline silicon layer and a second intrinsic amorphous / microcrystalline silicon layer on the front side and the back side of the single crystal silicon wafer respectively by an intrinsic PECVD process; Forming an N-type amorphous silicon / microcrystalline silicon layer on the first intrinsic amorphous / microcrystalline silicon layer by an N-type PECVD process; forming a P-type amorphous silicon / microcrystalline silicon layer on the second intrinsic amorphous / microcrystalline silicon layer by a P-type PECVD process; Forming a first transparent conductive film and a second transparent conductive film on the N-type amorphous silicon / microcrystalline silicon layer and the P-type amorphous silicon / microcrystalline silicon layer, respectively; as well as forming a first electrode and a second electrode on the first transparent conductive film and the second transparent conductive film respectively; The intrinsic PECVD process, the N-type PECVD process, and the P-type PECVD process each include: introducing corresponding reaction gas into the reaction chamber; introducing an inert gas into the reaction chamber; and A very high frequency radio frequency signal and a low frequency radio frequency signal are simultaneously provided to the electrode plate in the reaction chamber, the very high frequency radio frequency signal is used to excite the gas in the reaction chamber to dissociate into plasma, and the low frequency radio frequency signal is used to strike the plasma onto the electrode plate so that the self-bias voltage of the electrode plate is increased, the movement of ions is accelerated, and the energy of ions is increased, thereby depositing a corresponding type of silicon film layer on a silicon wafer placed on the electrode plate.

7. The method for preparing a heterojunction solar cell according to claim 6, characterized in that: The intrinsic PECVD process comprises: introducing a reaction gas including hydrogen and silane into the reaction chamber; introducing an inert gas including argon or helium into the reaction chamber; and The electrode plate in the reaction chamber is provided with the very high frequency radio frequency signal and the low frequency radio frequency signal at the same time, the gas in the reaction chamber is excited and dissociated into plasma by the very high frequency radio frequency signal, and the plasma is struck on the electrode plate by the low frequency radio frequency signal. The electrode plate self-bias voltage is increased, the ion movement is accelerated, and the ion energy is increased, so that a first intrinsic amorphous / microcrystalline silicon layer or a second intrinsic amorphous / microcrystalline silicon layer is deposited on a silicon wafer placed on the electrode plate; The volume ratio of the inert gas to silane is 10-100:1, and the flow ratio of the inert gas to hydrogen is 1-10:20-50.

8. The method for preparing a heterojunction solar cell according to claim 6, characterized in that: The N-type PECVD process comprises: introducing a reaction gas including hydrogen, silane and phosphine into the reaction chamber; introducing an inert gas including argon or helium into the reaction chamber; and The electrode plate in the reaction chamber is provided with the very high frequency radio frequency signal and the low frequency radio frequency signal at the same time, the gas in the reaction chamber is excited and dissociated into plasma by using the very high frequency radio frequency signal, and the plasma is struck on the electrode plate by using the low frequency radio frequency signal so that the self-bias voltage of the electrode plate is increased, the movement of ions is accelerated, and the energy of ions is increased, thereby depositing an N-type amorphous silicon / microcrystalline silicon layer on the silicon wafer placed on the electrode plate; The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of silane to phosphine is 1:0.5-2.

9. The method for preparing a heterojunction solar cell according to claim 6, characterized in that: The P-type PECVD process includes: introducing a reaction gas including hydrogen, silane, and diborane or trimethylboron into the reaction chamber; introducing an inert gas including argon or helium into the reaction chamber; and The electrode plate in the reaction chamber is provided with the very high frequency radio frequency signal and the low frequency radio frequency signal at the same time, the gas in the reaction chamber is excited and dissociated into plasma by using the very high frequency radio frequency signal, and the plasma is struck on the electrode plate by using the low frequency radio frequency signal so that the self-bias voltage of the electrode plate is increased, the movement of ions is accelerated, and the energy of ions is increased, thereby depositing a P-type amorphous silicon / microcrystalline silicon layer on a silicon wafer placed on the electrode plate; The volume ratio of the inert gas to silane is 10-100:1, the flow ratio of the inert gas to hydrogen is 1-10:20-50, and the volume ratio of silane to diborane or trimethylboron is 1:0.5-2.

10. The method for preparing a heterojunction solar cell according to claim 7, 8 or 9, characterized in that: The frequency of the very high frequency radio frequency signal is 40MHz, and the power range is 6000-10000W; the frequency of the low frequency radio frequency signal is 13M or 2M, and the power range is 50-1500W; the reaction gas also includes carbon dioxide and / or methane; the thickness ranges of the first intrinsic amorphous / microcrystalline silicon layer, the second intrinsic amorphous / microcrystalline silicon layer, the P-type amorphous silicon / microcrystalline silicon layer, and the N-type amorphous silicon / microcrystalline silicon layer are 5-15nm, 5-15nm, 20-40nm, and 20-40nm, respectively.

Citation Information

Patent Citations

  • Plasma treatment device with adjustable plasma concentration distribution and processing method thereof

    CN102983051A

  • Method for manufacturing graphene

    CN103311104A

  • Low-temperature plasma processing device and method

    CN103458599A

  • Method for manufacturing heterojunction solar cell and heterojunction solar cell

    CN113921661A

  • Preparation method of heterojunction solar cell and heterojunction solar cell

    CN115360267A

Cited By

  • Preparation method of double-layer thick-film high-resistance single crystal epitaxial wafer for semiconductor device

    CN120311309A