Method for the flameless composite repair of through-wall pipeline defects

The fireless composite repair method addresses the complexity and cost issues of existing pipeline repair technologies by using composite materials and crimping clamps to restore pipeline integrity without altering pumping conditions, ensuring long-term reliability and reduced costs.

WO2024253561A1PCT designated stage expired Publication Date: 2024-12-12VINOKUROV VALERIY IVANOVICH +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/RU2024/050015
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2024-01-22
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Existing pipeline repair methods for through defects, such as conical repair structures, are complex and costly, limiting their use in medium and low-pressure gas pipelines, and do not provide permanent solutions without changing pumping modes.

Method used

A fireless composite repair method using a repair structure made entirely of composite materials, which involves cleaning, preparing the surface, applying adhesive and composite paste, and installing internal and external composite sleeves with crimping clamps to create uniform pressure, thereby restoring the pipeline's structural strength without altering pumping conditions.

Benefits of technology

This method enhances the operational reliability of repaired sections for at least 30 years, reduces repair time, and optimizes costs by providing a permanent solution that prevents further defect development and maintains pipeline integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure RU2024050015_12122024_PF_FP_ABST
    Figure RU2024050015_12122024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to the field of pipeline construction and repair. The present method entails performing an emergency procedure in which a section of pipeline on one side of a through-wall defect is cleaned of contaminants, a sealing assembly is mounted, the pipeline is marked together with the sealing assembly for the purpose of positioning the assembly on the through-wall defect, and the assembly is tightened and clamped with the aid of two pipe clamps temporarily attached thereto until the product being transported ceases to leak from beneath the sealing assembly. Following this emergency procedure, subsequent work to repair the through-wall defect and reinforce the pipeline is carried out in a working procedure. Composite repair rings adhered to the pipeline and reinforcing composite rings overlaid thereon firmly attach the repair structure to the defective section of the pipeline. The method makes it possible to restore the hermeticity and pressure-containing capability of the repaired section of pipeline to the state of a non-defective pipe.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD OF FIRELESS COMPOSITE REPAIR OF THROUGH-THROUGH DEFECTS IN PIPELINES

[0002] Description

[0003] The invention relates to the field of repair of main, field, process and other pipelines of any type of installation.

[0004] During the construction and operation of the above facilities, as a result of corrosion, mechanical, electrochemical and other processes, defects such as ulcers, cavities, caverns, pittings, cracks and other defects appear on the pipe wall, which over time can develop to a through state and turn into fistulas, the leakage of the pumped product from which often leads to invaluable damage to the environment, fines imposed on the owners of leaky pipelines, image losses and enormous material costs due to the shutdown of the pipeline to replace leaky sections. Due to these possible consequences, all pipeline owners are concerned about the problem of early detection of through defects and their rapid elimination.The emergency repair of pipelines carried out for this purpose must be fast, reliable and completely restore the tightness, as well as the load-bearing capacity of pipes damaged by defects for the entire remaining service life of the pipeline, that is, it must be a permanent repair method and, if possible, carried out without changing the pumping modes.

[0005] Cone repair structures (RU 148064 U1, 27.11.2014 and RU 174392 Ul, 11.10.2017) allow repairing through pipeline defects without long-term changes in pumping modes. They include a sealing sleeve, with the help of which the leak is first eliminated, and then a conical bushing with a recess for the sealing sleeve and an outer shell made of metal or composite material is installed on top of it. The listed cone repair structures have one drawback - this is the complexity of the design and, as a result, high cost, which limits their wider use, in particular, on medium and low pressure gas pipelines.

[0006] The design chosen as a prototype for repairing pipelines according to the method of fireless repair of defective sections of pipelines without changing the pumping modes and the device for its implementation (RU 2788782 C1, 24.01.2023) is free of the specified drawback.

[0007] The prototype method is implemented by sequentially performing the following operations. Cleaning the section of the pipeline to be repaired from residual soil, insulation and other contaminants, preparing the surface of the section to be repaired to the first degree of cleaning according to GOST 9.402-2004 (or St 3 according to ISO 8501), dust removal with a damp cloth, removing moisture and degreasing the cleaned surface with acetone. Treatment with a rust converter, which also acts as a primer. Filling the cavity of the defect with a quick-hardening composite paste. Applying a thin, uniform layer of adhesive composition to the section to be repaired within the length of a single repair structure. Installation on the pipeline of an internal composite bushing with a factory recess for a vertical welded joint, or with a special recess so thatso that the horizontal joint of the inner bushing is located on the opposite side from the defect. Applying a thin uniform layer of adhesive to the surface of the mounted inner bushing. Mounting an outer composite bushing with smooth surfaces over the inner bushing so that its horizontal joint is located on the opposite side from the horizontal joint of the inner bushing. Installing one or more single-bolt composite couplings over the outer bushing, consisting of two half couplings connected to each other to grip the pipe on one side by a hinge, and on the other side by means of coupling screws tightened with a calibrated force (one on each coupling), due to which each coupling is tightly pressed through two bushings to the surface of the pipeline, squeezing it from the outside and creating an external contact effect on the pipe that is uniform over the entire surface of the section being repaired, with a magnitude commensurate with the effect on the wall of the pipeline from the inside,created by the product under working pressure, pumped through the pipeline, which reduces to zero the total impact on the wall of the pipeline in the area of ​​the installation of the repair structure, thereby removing both hoop and longitudinal stresses from it, which leads to the prevention of further development of existing and the formation of new defects, which, coupled with the strengthening of the wall of the defective section of the pipeline by thickening it due to gluing in two layers of composite bushings, returns it to the state of a defect-free pipe and restores the original structural strength of the pipeline.

[0008] The method selected as a prototype does not provide for the permanent repair of through defects of pipelines (fistulas) regardless of the method of their installation without a long-term reduction in pressure and flow rate of the pumped product, i.e. without changing the pumping modes. The proposed invention is aimed at solving this problem. The technical result achieved due to the use of the proposed invention is an increase in the operational reliability of repaired sections of pipelines with through defects and ensuring their safe operation during the remaining service life, but not less than 30 years, as well as a significant reduction in the time frame for repair work and optimization of their cost.

[0009] The essence of the proposed method is as follows.

[0010] Main, field, process and other pipelines of underground, ground, above-ground and underwater laying for pumping hydrocarbons, water and other liquid and gaseous products are subject to mechanical, electrochemical and / or other effects during operation, the consequence of which is the formation of such pipeline defects as corrosion ulcers, pitting and other defects that have developed to a through state - a fistula. Operation of pipelines with through defects is prohibited. In this regard, on sections of pipelines with through defects, it is necessary to carry out repair work to restore their tightness and reinforce them in order to restore their load-bearing capacity. The present invention proposes a method for carrying out this repair without changing the pumping modes using a fireless method by a constant method using a repair structure made entirely of composite materials.

[0011] The proposed method of fireless composite repair by a permanent method of through-hole pipeline defects without changing the pumping modes is carried out in stages in the following step-by-step sequence.

[0012] The first stage of repair is carried out in an emergency, without stopping pumping through the pipeline being repaired (a short-term pressure reduction is possible to carry out preparatory work near the through defect with the pumped product flowing out of it) and includes the following steps: Step 1. Cleaning of soil, dirt, peeling insulation and separating corrosion products from sections of the pipeline on one side of the through defect with a length equal to the width of the repair structure, on the other - equal to half the width of the repair structure.

[0013] Step 2. Assembly on the longer of the cleaned sections, at the minimum safe distance from the through defect, around the pipeline of the sealing unit of the repair structure, consisting of an internal composite sleeve, to which a sealing element-gasket is attached from the inside in factory conditions, and an external composite sleeve, which is glued in the field with a composite paste of rapid curing to the internal composite sleeve with the placement of their longitudinal joints in a staggered manner.

[0014] Step 3. Marking the sealing unit and pipeline so that after moving the sealing unit to the defect, its middle falls under the section of the sealing unit structurally allocated for this purpose.

[0015] Step 4. Shifting the sealing unit to the through defect according to the markings made.

[0016] Step 5. Tightening and crimping the sealing unit using two power crimping clamps temporarily attached to it as a tool until the product pumped through the pipeline stops flowing from under the sealing unit. If the pressure in the pipeline decreased during Steps 1-4, bring it to the operating pumping mode. If the product pumped from under the sealing unit resumes flowing, continue tightening and crimping the sealing unit until the flow completely stops.

[0017] The second stage of repair is carried out immediately after the flow of the pumped product from under the sealing unit mounted on the pipeline has stopped, and includes steps that are no longer performed in an emergency, but in a working order, namely:

[0018] Step 6. Cleaning from insulation and other contaminants to the first degree of cleaning according to GOST 9.402-2004 (or St 3 according to ISO 8501) the surface of the pipeline sections to the left and right of the sealing unit with a length equal to the width of the technological composite rings, plus a reserve of 50-00 mm on each side.

[0019] Step 7. Cleaning the installed sealing unit, as well as sections of the pipeline along the repair zone boundaries with a length of at least 100 mm with the existing insulation, from the pumped product and contaminants that got on them during Step 6.

[0020] Step 8. Dedusting, drying and degreasing with acetone the sections of the pipeline and sealing unit prepared according to Steps 6 and 7, especially its ends.

[0021] Step 9. Gluing two technological composite rings to the degreased sections of the pipeline and the ends of the sealing unit using a fast-curing composite paste. This Step, together with Steps 11 and 12, is necessary to ensure a tight and rigid connection of the repair structure with the pipeline being repaired and to strengthen the repair structure as a whole.

[0022] Step 10. Filling all the resulting vertical and horizontal joints with composite paste, such as for gluing, or any other special filling composite paste.

[0023] Step 11. Installation of two reinforcing composite rings on the fast-curing composite paste over the vertical joints between the sealing unit and the process composite rings close to the power clamps, but so that the outer edges of the reinforcing composite rings are at a distance of 25-40 mm from the outer edge of the process ring in order to minimize the edge stress of the repair structure. Step 12. Installation of the third reinforcing composite ring on the fast-curing composite paste in the gap between the power clamps close to them over that part of the sealing unit that is directly located above the through defect.

[0024] Step 13. After the composite paste has gained strength, eliminating the recoil of the reinforcing composite rings, dismantle both power compression clamps for use as a tool when installing other repair structures of the same type.

[0025] Step 14. After completing the installation of the repair structure, all gaps and joints of the repair structure are carefully sealed with a quick-hardening composite paste.

[0026] Step 15. To restore the insulation of the repaired section of the pipeline, the sections of the pipeline, previously prepared according to Steps 6-8, and the installed repair structure are coated with an adhesive compound, on top of which, in accordance with standard technology, new pipeline insulation is applied.

[0027] The illustrations in Fig. 1 and Fig. 2 explain the proposed invention.

[0028] Fig. 1 shows the front and side projection (section along line A-A) of the composite repair structure for implementing the proposed method of fireless composite repair of through pipeline defects by a permanent method without changing the pumping modes, where the following symbols are used: 1 - pipeline; 2 - process composite ring; 2.1 - vertical joint; 3 - reinforcing composite ring; 4 - outer composite sleeve; 5 - inner composite sleeve; 5.1 - longitudinal joint of the inner composite sleeve; 6 - through defect; 7 - sealing element - seal; 7.1 - longitudinal joint of the sealing element - seal; 8 - longitudinal joint of the process composite ring; 9 - longitudinal joint of the outer composite sleeve; L - width of the repair structure; Lr - width of the sealing unit; LTK - width of the process ring; Ьук - width of the reinforcing ring; a - technological indent.

[0029] The repair structure according to the proposed invention is mounted, among other things, using compression power clamps of any design variants. Fig. 2 shows the front and side projections (left view and right view) of one of the design variants of the compression power clamp, where 10 is an elongated opening; 11 is a tightening screw; 12 is a washer; 13 is a nut; 14 is a hinged joint. The bolted connections, by means of which the compression power clamp is temporarily attached to the outer composite bushing 4 through the elongated openings 10, so as not to clutter Fig. 1, are not illustrated.

[0030] The sealing unit of the repair structure consists of a sealing element - a seal 7, an internal composite sleeve 5, an external composite sleeve 4 and two power clamps (see Fig. 2), temporarily attached over the external composite sleeve 4 within the boundaries of rings of width X and dismantled after the leak from the through defect 6 has been eliminated.

[0031] The installation of the repair structure shown in Fig. 1 is carried out as follows.

[0032] At the closest safe distance from the through defect 6, on a section of pipeline 1 with a length equal to the width of the repair structure L, previously cleared of soil, dirt, peeling insulation, separating corrosion products and pumped product, a sealing unit of the repair structure is assembled around the pipe so that, when it is shifted along the axis of pipeline 1 to the through defect 6, its center would fall on the middle of the sealing unit (see Fig. 1, section line A-A). In order for this condition to be met, upon completion of the preparation of pipeline 1 for installation of the repair structure, the position of the middle of the through defect 6 being repaired is transferred to the adjacent sections of pipeline 1 not covered by the repair structure, by applying marks in any available way, for example, with chalk lines.

[0033] According to the proposed invention, the sealing element-gasket 7 is manufactured under factory conditions from a sealing material inert with respect to the product pumped through the pipeline 1, from the series: natural rubber, synthetic rubber, polyacetal, caprolon, rubber, silicone, polyurethane, fluoroplastic, paronite, fiberglass, basalt fiber, carbon fiber, thermally expanded graphite, aramid fiber by a woven or non-woven method, as well as by combining them, including casting, pressing, cutting, printing on a 3D printer in the form of a cuff cut lengthwise for installation in the girth of the pipeline 1 with a smooth, foamed, or waffle working surface of a deep or shallow profile of various configurations, is attached to the internal composite sleeve 5, for example, glued under factory conditions.The outer composite sleeve 4 is glued around the pipe to the inner composite sleeve 5 using a quick-hardening composite paste so that it covers the longitudinal joint of the inner composite sleeve, sealing it. Two compression clamps are temporarily attached to the outer composite sleeve 4 within the boundaries of the rings of width X through the elongated openings 10 using, for example, bolted connections, which are the power elements of the sealing unit of the repair structure for implementing the proposed method. The compression power clamps can be of any design, for example, consisting of two half-clamps (see Fig. 2), connected to each other on one side using a hinged connection 14, and on the other side using a bolted connection: the tightening screw 11 is screwed into the nut 13 through the washer 12.

[0034] Upon completion of the assembly of the sealing unit, before moving it onto the through defect 6, a special mark is applied to the outer surface of the outer composite bushing 4 with chalk or a marker, for example, in the form of a target (a ring with a crosshair), under which the middle of the through defect 6 being repaired should fall.

[0035] Then, the sealing unit is shifted along the axis of the pipeline 1 onto the through defect 6 so that the special mark applied to it coincides with the marks that were applied to the pipeline to mark the middle of the defect. After that, the power compression clamps (see Fig. 2) are tightened using the tightening screws 11 until the flow of the pumped product from under the sealing element-seal 7 stops. Due to the elongated shape of the holes 10, the compression clamps, when tightened, shift along the outer composite sleeve 4 within the length of the said holes, which ensures the appropriate pressing force of the sealing element-seal 7 to the through defect 6 to achieve the necessary sealing effect and crimping of the repair structure as a whole.

[0036] If the pressure in pipeline 1 decreased during the emergency, then after the sealing unit of the repair structure has been compressed, i.e. after the leak has been eliminated, the pipeline is brought to the operating pumping mode. If, after pipeline 1 has been brought to the operating mode, the flow of the pumped product from under the sealing element-seal 7 has resumed, then the tightening of screws 11 is resumed until it has completely stopped.

[0037] After the final elimination of the leak, no longer in an emergency, but in the normal course of business, the sections of the pipeline along the boundaries of the sealing unit with a width equal to the width of the TK plus a reserve of 5SN100 mm on each side are cleaned of insulation and other contaminants to the first degree of cleaning according to GOST 9.402-2004 (or St 3 according to ISO 8501). The specified reserve is needed to ensure proper adhesion of the insulation to the metal of pipeline 1, during its restoration, upon completion of the installation of the repair structure. Then the cleaned sections of pipeline 1, the sealing unit of the repair structure mounted on the pipeline, especially its ends, as well as sections of the existing insulation at a distance of at least 100 mm along the boundaries of the repair zone are thoroughly cleaned of all contaminants, dried and degreased. The specified sections are needed to ensure the overlap of the restored insulation on the existing pipeline insulation. The overlap is necessary to seal the transition from the existing insulation to the restored one and vice versa.Then, to the prepared sections of the pipeline 1 and the ends of the sealing unit, for a hermetic and rigid connection of the repair structure with the pipeline 1, two composite process rings 2 are glued with a quick-hardening composite paste so that the longitudinal joint of each process ring 8 does not coincide with the longitudinal joint of the outer composite sleeve 9. The vertical joint 2.1 formed on each side between the sealing unit and the corresponding process ring 2 is filled with a quick-hardening composite paste, flush with the jointless surface +0.5 mm for shrinkage, during its polymerization.

[0038] Then, in order to minimize the edge stress of the repair structure, at a distance of the technological indent a from the outer edge of the technological ring 2, equal to 25^-50 mm, over the vertical joints 2.1, close to the clamps, two reinforcing composite rings 3, for example, from a field-made composite laminate, are installed on a quick-hardening composite paste, for example, by the spiral winding method. The third reinforcing composite ring 3 is installed over the through defect 6 in the gap between the power clamps, also close to them. After the composite paste has gained strength, eliminating the recoil of the reinforcing composite rings 3, both power clamps are removed for use as a tool, when installing other repair structures of the same type.

[0039] After completion of installation works, in order to prevent moisture ingress, as well as to smooth out the internal angles of the installed repair structure, which is desirable for a higher-quality restoration of the insulation of pipeline 1, all gaps and abutments are carefully sealed with a quick-hardening composite paste. Next, pre-cleaned, dried and degreased sections of the existing insulation at a distance of at least 100 mm along the boundaries of the repair zone, sections of pipeline 1 with a width of 5SN-100 mm from both ends from the installed repair structure and the repair structure itself are coated with an adhesive composition, for example, a primer, according to which new external insulation is applied to the repaired section of pipeline 1 over the installed repair structure with an overlap on both sides of it on the existing insulation of the pipeline, observing the standard technology of its application.

[0040] For the production of composite parts of the repair structure according to the proposed method, high-strength and elastic structural composite materials are used, including reinforced polymers from the list: fiberglass; basalt fiberglass; carbon fiberglass; a mixture of basalt, fiberglass, carbon fiberglass based on epoxy, polyester, organosilicon resins, polyethylene, polypropylene, polystyrene, polychloride, polyamide, polycarbonate, polytetrafluoroethylene and textolite by pressing, vacuuming, winding a bundle, and impregnation under pressure. In this case, the inner composite bushing 5 is made elastically deformed to fit the outer diameter of the pipeline 1 with a sealing element - seal 7 located on top of it, and the outer composite bushing 4 is elastically deformed to fit the outer diameter of the pipeline 1 taking into account the inner composite bushing 5 mounted on it together with the sealing element - seal 7.The elastic deformation of both composite bushings under the specified diameters allows them to self-fasten after the tensile force is removed from them during installation around pipeline 1.

[0041] As a fast-hardening composite paste, for the purposes of the present invention, it is possible to use the composite polymerizing paste GAMMAFIX manufactured by NPO GAMMA-KOMPOZIT LLC (INN 7723406020).

[0042] The repair structure according to the proposed method does not have metal parts, therefore it does not require the use of active protection against soil corrosion.

[0043] The proposed method allows for pipeline repairs not only on land but also underwater.

[0044] The repair structure according to the proposed method is a crimping one. In addition, gluing technological composite rings 2 to the pipe and through them rigidly connecting the repair structure to the pipeline by installing reinforcing composite rings 3 removes both ring and axial stresses from the defective section of the pipeline, i.e. removes it from the stress-strain state, which not only prevents the development of the repaired through defect 6, but also generally stops further defect formation on the repaired section of the pipeline 1.Taking into account the fact that, according to the documentation of the manufacturers of composite materials used for the production of the proposed repair structure, their service life is at least 30 years, and taking into account that, as a result of repairing the through defect 6, the tightness and load-bearing capacity of the repaired section of the pipeline 1 is restored to the state of a defect-free pipe, it becomes obvious that the repair structure according to the proposed method has all the features of a means for the permanent repair of pipelines. This means that the method of fireless composite repair without changing the pumping modes according to the proposed invention pertains to permanent methods of repairing pipelines.

[0045] The proposed method of fireless composite repair of through pipeline defects by a constant method without changing the pumping modes has undergone a full cycle of factory and bench tests, which have shown its industrial applicability and high efficiency in comparison with any of the fire repair methods due to the reduction of repair work periods, due to the absence of the need to change the pumping modes, namely its complete stop for emptying (swinging, drying, etc.) of the pipeline being repaired, optimization of their cost, including due to the reduction of organizational and technical measures for carrying out repairs, due to the lack of need for the use of welding equipment, lifting mechanisms, pumping equipment and other technical devices.

[0046] Thus, the proposed invention solves the problem set before it, namely, repairing through defects in pipelines using a fireless composite method using a permanent method without changing the pumping modes.

Claims

Formula 1. A method of fireless composite repair by a permanent method of through-hole pipeline defects without changing the pumping modes, consisting of cleaning, carried out in an emergency manner, without stopping pumping through the pipeline being repaired, of soil, dirt, peeling insulation and separating corrosion products on one side of the through-hole defect of a section of the pipeline with a length equal to the width of the installed repair structure, on the other - half this width, assembly on the first of the cleaned sections at a minimum safe distance from the through-hole defect in the girth of the pipeline of a sealing unit of the repair structure, marking the pipeline and the sealing unit so that, after its displacement, the middle of the through-hole defect would fall under the section of the sealing unit structurally allocated for this, displacement of the sealing unit onto the through defect in accordance with the marking made,tightening and crimping the sealing unit with two crimping power tools until the pumped product stops flowing out from under it, after stopping the flow of the pumped product, no longer in an emergency, but in the working order, cleaning the surface of the pipeline at both ends from the installed sealing unit with a length equal to the width of the technological composite rings of the repair structure with a reserve of 50-400 mm on each side, removing the pumped product and contaminants, dust removal, drying and degreasing the installed sealing unit, as well as sections of the pipeline with existing insulation along the boundaries of the repair line with a length of at least 100 mm, gluing two technological composite rings to these sections of the pipeline and the ends of the sealing unit with a composite paste of rapid curing, filling all the resulting vertical and horizontal joints with a composite paste of rapid curing flush with the seamless surface +0.5 mm,mounting two reinforcing composite rings on the vertical joints using a fast-hardening composite paste so that their outer edges are at a distance of 5-40 mm from the outer edges of the process rings, mounting a third reinforcing composite ring on a fast-hardening composite paste in the gap between the power clamps over the through defect, dismantling both power clamps, after the fast-hardening composite paste used for mounting the reinforcing composite rings has achieved strength that prevents them from recoiling.

2. The method according to item 1, characterized in that the sealing unit of the repair structure installed around the pipeline with a through defect consists of an internal composite sleeve, to which a sealing element-gasket is attached from the inside under factory conditions, and an external composite sleeve, which is glued under field conditions with a composite paste of rapid hardening to the internal composite sleeve by placing their longitudinal joints in a staggered manner.

3. The method according to claim 1, characterized in that the sealing unit of the repair structure includes two sludge elements temporarily attached to the outer composite sleeve in the form of tightening clamps of any model, used as a tool and removed upon completion of their function, which, when tightened, develop a compressive effect, including acting on the sealing element - the sealant with a force of such magnitude as to create a stress in its surface layers, residual for their deformation and to ensure the proper sealing effect due to filling all micro-roughnesses of the contact surface of the through defect of the pipeline with the sealant material.

4. The method according to item 1, characterized in that the sealing element-seal included in the sealing element is manufactured in factory conditions from a material that is non-metallic in relation to the product pumped through the pipeline being repaired, 8 sealing material from the following series: natural rubber, synthetic rubber, polyacetal, caprolon, rubber, silicone, polyurethane, fluoroplastic, paronite, fiberglass, basalt fiber, carbon fiber, thermally expanded graphite, aramid fiber by woven or non-woven method, as well as by their combination, including casting, pressing, cutting, printing on a 3D printer in the form of a cuff cut lengthwise for installation in the girth of a pipeline with a smooth, foamed, or waffle working surface of a deep or shallow profile of various configurations.

5. The method according to paragraph 1, characterized in that the internal composite sleeve and the external composite sleeve of the sealing unit, as well as the technological composite rings of the repair structure, are manufactured in factory conditions by pressing, vacuuming, winding, impregnation under pressure from high-strength and elastic structural materials, including reinforced, hardenable composite materials, from the series: fiberglass, basalt fiberglass, carbon fiberglass, a mixture of basalt, glass fiber and carbon fiber based on epoxy, polyester, organosilicon resins, polyethylene, polypropylene, polystyrene, polychloride, polyamide, polycarbonate, polytetrafluoroethylene, ekstolite.

6. The method according to claim 1, characterized in that the reinforcing rings of the repair structure are made from high-strength and elastic structural laminates, including reinforced, hardenable composite laminates of field and factory manufacture using the method of pressing, vacuuming, impregnation under pressure, winding with the use of threads, tow, roving, tapes, as well as prepregs from the series of fiberglass, azalt fiberglass, carbon fiber, a mixture of basalt, fiberglass and carbon fiber based on epoxy, oleaster, organosilicon resins, polyethylene, polypropylene, polystyrene, olichloride, polyamide, polycarbonate, polytetrafluoroethylene, textolite.

7. The method according to item 2, characterized in that the inner composite sleeve and the outer composite sleeve of the sealing unit, for self-fastening after the tensile force is removed from them during installation around the pipeline, are made spring-deformed, wherein the inner composite sleeve is made to fit the outer diameter of the pipeline being installed, taking into account the sealing element-sealer glued to it from the inside, and the outer composite sleeve is made to fit the outer diameter of the pipeline being installed, taking into account the inner composite sleeve with the sealing element-sealer glued to it. 9

Citation Information

Patent Citations

  • Water supply steel pipe welding seam leakage repairing method

    CN115076508A

  • Method for repairing concreted portion of underwater pipeline and device for its implementation

    RU2619954C1

  • Method of pipeline repair without decommissioning

    RU2687476C1

  • Universal repair kit for pipelines

    RU2730268C1

  • Method for fire-free repair of defective sections of pipelines without changing pumping modes

    RU2788782C1