Method for treating tailings pond liquor

The two-stage carbonization process for sludge water, optimizing pH conditions and using waste gases, addresses the challenges of producing high-purity pseudoboehmite aluminum hydroxide, enhancing product quality and sustainability.

WO2024253563A1PCT designated stage expired Publication Date: 2024-12-12OBSHCHESTVO S OGRANICHENNOY OTVETSTVENNOSTYU OBEDINENNAYA KOMPANIYA RUSAL INZHENERNO TEKHNOLOGICHESKIY TSENTR
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/RU2024/050116
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2024-05-31
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Current methods for producing aluminum hydroxide with a pseudoboehmite structure face challenges such as phase separation difficulties during filtration, formation of liquid waste, high energy costs for evaporation, incomplete removal of acid anions, and increased production costs due to multi-stage purification processes, which negatively impact the quality and environmental sustainability of the final product.

Method used

A two-stage carbonization process for processing sludge water, where the first stage is carried out at a pH of 11-10.5 to precipitate amorphous aluminum hydroxide, followed by filtration and washing, and the second stage at a pH of 9-8 to produce pseudoboehmite, using gases containing carbon dioxide, such as exhaust gases from sintering furnaces or lime kilns, to achieve high purity and reduce impurity content.

Benefits of technology

This method effectively produces aluminum hydroxide with a pseudoboehmite structure of high purity and specific surface area, suitable for use in cement mixtures and catalyst supports, while minimizing environmental impact and reducing production costs by utilizing waste gases and optimizing pH conditions for each carbonization stage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000012_0001
    Figure IMGF000012_0001
  • Figure IMGF000019_0001
    Figure IMGF000019_0001
  • Figure IMGF000020_0001
    Figure IMGF000020_0001
Patent Text Reader

Abstract

A method for treating tailings pond liquor resulting from alumina production includes filtering tailings pond liquor, carbonating the liquor by saturation with carbon dioxide, separating the precipitates formed, washing same with water, and drying. The tailings pond liquor is carbonated in two stages. The first stage is carried out to a slurry pH value at which a precipitate in the form of amorphous aluminium hydroxide is produced. The carbonated solution is then sent to a second stage of carbonation to a slurry pH value at which pseudoboehmite is precipitated. The result is that of producing powders of aluminium hydroxide with a pseudoboehmite structure and a low level of impurities, which can be used in the production of cement mortar mixes and aluminium oxide catalyst supports.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD OF PROCESSING SLUDGE WATER

[0002] Field of technology

[0003] The invention relates to chemical technology, in particular to a method for producing amorphous aluminum hydroxide and aluminum hydroxide with a pseudoboehmite structure, and can also be used to produce granulated active aluminum oxide, catalysts, carriers, and in other areas of industry.

[0004] State of the art

[0005] In the water cycle of alumina production, a significant part is occupied by subsludge water, which participates in many technological processes. The content of aluminum oxide in subsludge water allows it to be used as a raw material source for obtaining various products based on aluminum hydroxide, including amorphous aluminum hydroxide, used as an active additive to building mixtures and aluminum hydroxide of pseudoboehmite structure, used as a feedstock for obtaining granulated active aluminum oxide, catalysts and carriers.

[0006] Aluminum hydroxides used as raw materials for catalyst carriers have specific requirements.

[0007] Firstly, pseudoboehmite should not contain impurity phases of bayerite, gibbsite or X-ray amorphous aluminum trihydroxide in quantities greater than 1-2 wt.% each.

[0008] Secondly, the content of a number of impurities is strictly regulated, since they are catalytic poisons for most industrial catalytic processes. Among the controlled impurities, iron, sodium and other alkaline and alkaline earth metals are especially distinguished. As a rule, metallic aluminum or aluminum hydroxide is used as a raw material for obtaining pseudoboehmite. The most common method for obtaining pseudoboehmite is the reprecipitation of crystalline aluminum hydroxide by mixing an alkaline and an acidic solution, one or both of which contain aluminum.

[0009] For example, in the method for producing pseudoboehmite according to US 4154812(A), published 15.05.1979, an aluminate solution and an aluminum sulfate solution are mixed. This method includes holding the pulp at 60-82 °C to achieve a final pH value in the range from 9.5 to 10.5, separating the precipitate by filtration, washing and drying to obtain pseudoboehmite, a sodium sulfate solution and industrial water from washing the precipitate.

[0010] According to CN1 02219245 (B), published on 05.06.2013, pseudoboehmite is obtained by performing neutralizing precipitation on a sodium aluminate solution and an aluminum sulfate solution, holding, filtering, washing and drying, wherein, in terms of oxide, the concentration of the solution is from 180 to 320 g ACO3 g / l, and the alkali ratio is from 1.3 to 2.5; and based on the characteristics of the ultraviolet (UV) spectrum, the absorption value of the UV spectrum of the solution at the position of 270 nm is from 0.8 to 5.5. Compared with the prior art, pseudoboehmite can be directly used to produce aluminum oxide with a large pore volume, such as gamma-alumina with a pore volume of 1.1 to 1.5 ml / g.

[0011] The disadvantages of the known technologies are difficulties in separating phases during filtration, as well as the formation of liquid waste, the disposal of which is difficult due to low concentrations. Evaporation of such solutions is associated with high energy costs, which are incomparable with the effect of selling the salts obtained. As a result, this waste pollutes the water basin, worsening the environmental situation. In addition, the acid anion cannot be completely removed from the sediment by washing, which worsens the quality of the resulting pseudoboehmite. According to RU 2234460 Cl, published 20.08.2004, aluminum hydroxide of pseudoboehmite structure is obtained by heat treatment of the original aluminum trihydroxide on a rotating surface heated to 100-700 °C for 0.5-5 s, with subsequent hydrothermal treatment of the resulting product at a temperature of 105-170 °C for 2-48 hours in the presence of inorganic or organic substances.

[0012] The disadvantage of this method is that, during thermochemical activation of gibbsite, depending on the conditions of its implementation, a mixture of various phases from trihydrate and monohydrate to aluminum oxides can be formed. As a result, during further hydrothermal treatment, it is impossible to ensure the monophase nature of the resulting product, which subsequently negatively affects the specific surface area and strength of the catalyst.

[0013] There are a number of methods for producing aluminum hydroxide of pseudoboehmite structure based on the carbonization of aluminate solutions with a gas-air mixture with different CO2 contents.

[0014] A method for producing pseudoboehmite is also known, which includes preparing aluminum hydroxide using the Bayer method, dissolving this hydroxide in caustic alkali to obtain an aluminate solution with a concentration of 20-200 g / l AI2O3, carbonizing the aluminate solution at a temperature of 0-60 °C until a pH of 7-11.5 is obtained in the final solution with the precipitation of an X-ray amorphous precipitate, separating the precipitate, washing it with an aqueous solution at a temperature of about 30 °C, and treating the precipitate with a solution of mineral acid (see EP 85592, published 02.07.1986).

[0015] The disadvantages of the method are the use of Al(OH)3 as the starting product for the preparation of the aluminate solution, due to the increase in production costs, the difficulty of regulating the process, and the need to dispose of waste.

[0016] A method for processing aluminum-containing raw materials is known (RU 2197429, published 27.01.2003), which includes the following stages: sintering with limestone and alkali-containing material to form gas products and sinter;

[0017] - leaching of sinter to obtain an aluminate solution, desiliconization of the aluminate solution;

[0018] - dilution of the desiliconized solution with a carbonate solution until a molar ratio of carbonate alkali to total alkali of 0.15-0.6 is obtained;

[0019] - carbonization of the diluted solution with gaseous sintering products at a temperature of 10-50°C and a consumption of CO2 / AI2O3 = 1-5 dm 3 / G;

[0020] - separation of the precipitate formed during carbonation from the carbonate solution;

[0021] - washing of sediment to obtain pseudoboehmite and industrial water with the separation of alkali metal carbonates from the carbonate solution and industrial water.

[0022] The main problem with this known method is that the raw material used is desiliconized aluminate solution from alumina production, which is the main raw material source for obtaining alumina. When organizing production using this method, the need to use an aluminate solution leads to a decrease in the productivity of alumina production, or an increase in the costs of producing an additional amount of aluminate solution.

[0023] The closest to the declared technical solution (prototype) is the method for removing impurities from sludge water and obtaining pseudoboehmite according to CN 107973327 (A), published 01.05.2018, consisting of the following stages:

[0024] 1. Treatment of sludge water with lime milk at 80 - 90 °C with a molar ratio of CaO / 8 s 2' = 1.1 - 1.3: 1 and subsequent filtration. 2. Treatment of the filtrate obtained in stage 1 with a flocculant at 70-80 °C, followed by filtration. Polyacrylamide is used as a flocculant.

[0025] 3. Adding BaAhO4 to the filtrate obtained in step 2, followed by filtration of the precipitate.

[0026] 4. Treatment of the filtrate with H2C2O4 at 40-50 °C to remove excess Ca 2+ and Va 2+ .

[0027] 5. Carbonization of the purified NaAlCh solution with carbon dioxide of 90-99% concentration at a temperature of 85 - 90 °C, for 2-3 minutes, washing the resulting precipitate with deionized water, grinding and drying.

[0028] The disadvantages of this method are the use of multi-stage purification of sludge water with a large number of expensive reagents, the need for an independent source of carbon dioxide, such as gas cylinders, and the lack of the ability to utilize solutions after filtration and washing of sediment.

[0029] Disclosure of invention

[0030] The technical task and technical result of the claimed method is the development of a low-cost method for processing the sludge water of alumina production to obtain from it aluminum hydroxide powders of pseudoboehmite structure with a low content of impurities, which also makes it possible to expand the raw materials market in the production of cement building mixtures and alumina catalyst carriers.

[0031] The problem is solved and the result is achieved by the proposed method of processing subsludge water, alumina production, including filtration of subsludge water, its carbonization by bubbling with gases containing carbon dioxide, separation of the resulting sediments, their washing with water and drying.In this case, according to the claimed invention, the carbonation of the subslurry water is carried out in two stages, wherein the first stage of carbonation of the subslurry water is carried out until the pH value of the pulp is preferably equal to 11 - 10.5, the resulting pulp is filtered to obtain a precipitate, which is washed to obtain a product in the form of amorphous aluminum hydroxide, suitable for use as a modifier of cement building mixtures and a carbonate solution, which is sent to the second stage of carbonation until the pH value of the pulp is preferably equal to 9 - 8, the resulting pulp is filtered, the precipitate is washed at a wash water temperature of 40 - 90 °C, to obtain a product in the form of pseudoboehmite, suitable for use as a precursor in the production of alumina catalyst carriers.

[0032] The claimed method is supplemented by features that characterize the invention in particular cases of its implementation.

[0033] The gases containing carbon dioxide can be exhaust gases from furnaces sintering aluminum-containing raw materials with limestone and / or soda.

[0034] Gases from lime kilns or gases produced by burning thermal coal or hydrocarbons can also be used as gases containing carbon dioxide.

[0035] At the end of carbonization at a pulp pH of 11 - 10.5, the sediment is represented by amorphous aluminum hydroxide. At the end of carbonization at a pulp pH of 9 - 8, the sediment is represented by the pseudoboehmite phase.

[0036] To ensure high purity of the pseudo-boehmite obtained during carbonization of the subsludge water, a two-stage carbonization process is carried out. The end of the first stage of carbonization must be ensured at a pulp pH of 11 - 10.5. Under these conditions, aluminum hydroxide, which has an amorphous structure, precipitates from the solution. Due to its sorption properties, the precipitated aluminum hydroxide concentrates the impurities contained in the subsludge water. Thus, intermediate filtration of amorphous aluminum hydroxide obtained after the first stage of carbonation allows purifying the carbonate solution from the main impurities and obtaining a product with a low impurity content at the second stage.

[0037] Intermediate filtration of sediment at pulp pH >11 allows removing only part of the main impurities contained in the subslurry water. Filtration of sediment at pulp pH <10.5 helps reduce the yield of the target product.

[0038] Amorphous aluminum hydroxide obtained after the first stage of carbonization can be used as an active additive to building mixtures, accelerating the strength gain of concrete and building mortars.

[0039] Completion of the second stage of carbonization at pulp pH >9 promotes incomplete precipitation of AI2O3 from the production solution. Completion of carbonization at pulp pH <8 does not affect the degree of AI2O3 precipitation, but promotes a significant increase in the duration of the process and leads to an increase in production costs, and also promotes the formation of impurity phases of gibbsite and bayerite.

[0040] The temperature of the washing water during washing of the precipitate obtained in the second stage of carbonation below 40 °C is insufficient for removing soluble impurities and completely converting the precipitate into pseudoboehmite, and washing at a temperature of washing water above 90 °C requires the installation of special equipment for working under pressure. The phase composition of the precipitates in the first and second stages of carbonation is necessarily subject to control. The precipitates are dried, crushed and analyzed by X-ray diffraction analysis on an X-ray diffractometer, for example, X Pert PRO from PANanalytical.

[0041] The speed of the process depends on the gas consumption and the CO2 content in it; the higher the CO2 content, the faster the process. Before carbonization, the exhaust gases must be cooled (to a temperature of about 40-50 °C) and subjected to air cleaning to reduce the possibility of sinter dust or other undesirable mechanical impurities getting into the resulting products.

[0042] For the sludge water selected as a raw material source, the initial pH is within 12 +- 0.2, which is due to the presence of free caustic alkali (FCA). The content of AI2O3, Na2O3, and Na2O is important for the process. Ky in the subsludge water. The increased content of AI2O3 contributes to an increase in the yield of target products. The duration of the process depends on the content of Na2O3 in the initial solution: the higher the content, the greater the KV the more CO2 is required to overcome the buffer zone and bind Na2CO3 into Na2CO3 and NaHCO3.

[0043] Increased content of Na2O in the initial solution К b (Na2CO3) leads to the formation of an impurity phase of sodium hydrocarboaluminate (Na2CO3 + 2H2O) in the carbonation precipitates, thereby increasing the content of Na2O in the carbonation products.

[0044] The above NaOH is the total content of all Na compounds (the total content of NaOH, NaOHCO3, NaHCO3), converted to NaOHO, NaOHO is the content in the NaOH solution (caustic alkali) converted to NaOHO, Na2O K 6 is the content of Na2CO3 in the solution converted to Na2O.

[0045] The drawings show:

[0046] Fig. 1 - Example of a process flow diagram for processing subslurry water from alumina production.

[0047] Fig. 2 - An example of a hardware and process flow diagram for processing subslurry water from alumina production.

[0048] The subslurry water from the slurry pond is sent to the control filtration (CF) stage to remove residual slurry content. The slurry from the filters is sent to the slurry removal unit of the alumina production, and the purified subslurry water enters the subslurry water receiving mixer Ml. From the mixer Ml, the subslurry water is pumped to the first carbonization stage in the carbonizer KB1. The carbonizer KB1 receives flue gases pre-cooled to a temperature of 40-50 °C in the heat exchanger TO1 and purified in the bag filter F1 using the gas blower GD1. The condensate obtained during the cooling of the flue gases in the condensate drain KO1 is sent to the alumina production.

[0049] The first stage of carbonization is carried out until the pH value of the pulp is preferably equal to 11-10.5. In this case, amorphous aluminum hydroxide precipitates from the subslurry water. The pulp obtained after the first stage of carbonization is sent through the pulp receiving mixer M2 to filtration on the press filter PF1. The filtrate is sent to the collecting mixer M3.

[0050] The sediment obtained in the filter press PF1 is washed with wash water from the pseudoboehmite filtration and washing unit, and then washed with condensate from the alumina production. When using the resulting sediment as a commercial product, the sediment from the PF1 filter is sent to the repulpator RP1, where it is repulped with condensate from the alumina production. The resulting pulp is sent to the spray dryer RS1, where the process of drying amorphous aluminum hydroxide takes place in a stream of air preheated by the heater KL1, supplied by the gas blower GD2. The air after the spray dryer RS1 undergoes a two-stage cleaning stage in the cyclone Ts1 and the bag filter F2 and is released into the atmosphere.

[0051] The obtained amorphous aluminum hydroxide in powder form is sent to the finished product filling unit using the Ш1 screw.

[0052] In case of defects at the first stage of carbonization, the sediment is mixed with industrial waters in the M5 mixer and sent to the alumina production batch preparation unit.

[0053] The filtrate after the first stage of carbonization from the mixer M3 is sent to the second stage of carbonization, carried out in carbonizers KB2 - KB5. Carbonization is carried out using pre-cleaned and cooled flue gases to the pH of the pulp, preferably equal to 9-8. Upon reaching the specified pH, the pulp is sent to the collector M4, from where it is fed for filtration on the press filter PF2. To avoid loss of sediment together with the filtrate, the first part of the filtrate is sent to tank M4 for repeated filtration through a sediment layer on the press filter PF2.

[0054] The filtered sediment is washed with condensate from alumina production at a temperature of 80 - 90 °C.

[0055] After completion of filtration, the filtrate is mixed with part of the industrial water in the SF mixer and sent to meet the needs of alumina production.

[0056] Part of the industrial water from the second stage of filtration is sent to wash off amorphous aluminum hydroxide on the PF 1 press filter.

[0057] The sediment from the PF2 press filter is sent to the RP2 repulpator, where it is pulped with condensate from the alumina production. The resulting pulp is sent to the RS2 spray dryer, where the pseudoboehmite is dried in a stream of air preheated by the KL2 heater, supplied by the GDZ gas blower. The air after the RS2 spray dryer undergoes a two-stage cleaning stage in the C2 cyclone and the FZ bag filter and is released into the atmosphere.

[0058] The resulting pseudoboehmite in powder form is sent to the finished product filling unit using the Ш2 auger.

[0059] Below is an example of a specification for the hardware and process diagram according to Fig. 2. Implementation of the invention

[0060] Example 1

[0061] The subsludge water containing the following components: AI2O3 - 7.3 g / l, Na2Ototal - 10.4 g / l, Na2Ok - 10.4 g / l was filtered to a solids content of 0.01 g / l.

[0062] The filtered sludge water with a volume of 40 l was carbonized with the exhaust gases of the sintering furnaces with a CO2 content of 5 wt.% at a temperature of 25 °C. Carbonization was carried out until the pH of the pulp was 8.5. The duration of carbonization was 2 hours. Upon completion of carbonization, the pulp was filtered on a Nutsche filter under a vacuum of 0.8 kgf / cm 2 . Pure condensate at T = 90 °C was used as the washing liquid. The amount of condensate for one wash was calculated from the ratio L: T = 2: 1 by the weight of the wet sediment. A total of 5 washes were carried out. The washed sediment was dried at a temperature of 120 °C until moisture loss ceased.

[0063] Phase composition of the obtained product: pseudoboehmite, S yj =278 m 2 / G.

[0064] The process parameters are shown in Table 2.

[0065] Example 2

[0066] The original sludge water underwent a filtration stage similar to Example 1.

[0067] Filtered sludge water with a volume of 40 liters was carbonized with exhaust gases from sintering furnaces with a CO2 content of 5 wt.%.

[0068] Carbonization was carried out in 2 stages. The temperature of the subslurry water during the first stage of carbonization was 25 °C. The end of the first stage of carbonization was recorded at a pulp pH of 11. The duration of carbonization was 15 minutes. Upon completion of carbonization, the pulp was filtered on a Nutsche filter under a vacuum of 0.8 kgf / cm 2. Pure condensate at T = 90 °C was used as the washing liquid. The amount of condensate for one wash was calculated from the ratio of W : T = 2 : 1 by the weight of the wet sediment. A total of 5 washes were carried out. The washed sediment was dried at a temperature of 120 °C until moisture loss ceased, crushed and analyzed. The amount of AI2O3 transferred to the sediment at the first stage of carbonation was 25% of the initial content in the subsludge water.

[0069] Phase composition of the sediment obtained after the first stage of carbonization: amorphous aluminum hydroxide.

[0070] The parameters of the first stage of carbonization are shown in Table 1.

[0071] The carbonate solution obtained at the stage of filtration of amorphous aluminum hydroxide was sent to the second stage of carbonization. Carbonization was carried out to the pH of the pulp of 8.5. The duration of carbonization was 1.5 hours. The stages of filtration, washing, drying and grinding of the product were carried out similarly to Example 1.

[0072] Phase composition of the sediment obtained after the second stage of carbonation: pseudoboehmite, 8 уд = 280 m 2 / G.

[0073] The parameters of the second stage of carbonization are shown in Table 2.

[0074] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3.

[0075] Example 3

[0076] The process was carried out similarly to Example 2, the end of the first stage of carbonization was recorded at a pulp pH of 11.5. The amount of AI2O3 that passed into the sediment at the first stage of carbonization was 17% of the initial content in the subslurry water.

[0077] Phase composition of the sediment obtained after the first stage of carbonization: amorphous aluminum hydroxide.

[0078] The phase composition of the sediment obtained after the second stage of carbonization: pseudoboehmite, with an admixture of bayerite. The parameters of the first and second stages of carbonization are given in Tables 1 and 2, respectively.

[0079] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3.

[0080] Example 4

[0081] The process was carried out similarly to Example 2, the end of the first stage of carbonation was recorded at pH = 10. The amount of ACO3 that passed into the sediment at the first stage of carbonation was 60% of the initial content in the subsludge water.

[0082] Phase composition of the sediment obtained after the first stage of carbonation: pseudoboehmite, amorphous aluminum hydroxide, gibbsite, bayerite.

[0083] Phase composition of the sediment obtained after the second stage of carbonation: pseudoboehmite.

[0084] The parameters of the first and second stages of carbonization are shown in Tables 1 and 2, respectively.

[0085] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3.

[0086] Example 5

[0087] The process was carried out similarly to Example 2, the end of the second stage of carbonization was recorded at a pulp pH of 9.5. The amount of ACO3 that passed into the sediment after the second stage of carbonization was 75% of the initial content in the subslurry water.

[0088] Phase composition of the sediment obtained after the second stage of carbonation: pseudoboehmite, 8 уд = 268 m 2 / G.

[0089] The parameters of the first and second stages of carbonization are shown in Tables 1 and 2, respectively.

[0090] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3. Example 6

[0091] The process was carried out similarly to Example 2, the end of the second stage carbonization was recorded at a pulp pH of 7. The duration of carbonization was 6 hours.

[0092] Phase composition of the sediment obtained after the second stage of carbonation: pseudoboehmite, gibbsite, bayerite.

[0093] The parameters of the first and second stages of carbonization are shown in Tables 1 and 2, respectively.

[0094] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3.

[0095] Example 7

[0096] The process was carried out similarly to Example 2. Washing was carried out with condensate at T = 25 °C.

[0097] Phase composition of the sediment obtained after the second stage of carbonation: pseudoboehmite, dawsonite.

[0098] The parameters of the first and second stages of carbonization are shown in Tables 1 and 2, respectively.

[0099] The content of impurities in the sediment obtained after the second stage of carbonation is given in Table 3.

[0100] During the research and testing, the authors found that processing of sludge water by means of single-stage carbonization (Example 1) allows obtaining a sediment with a pseudoboehmite structure with an increased content of impurities.

[0101] In Example 2, the authors demonstrate the achievement of a technical result by adding an additional carbonation stage in the process of processing subsludge water with the separation of amorphous aluminum hydroxide at a pulp pH of 11. Carrying out the process of processing subsludge water with the specified parameters makes it possible to obtain aluminum hydroxide with a pseudoboehmite structure with a low content of impurity elements after the second stage of carbonation.

[0102] In Examples 3 and 4, the authors demonstrate the influence of pulp pH after the first stage of carbonation on the properties and yield of the resulting products.

[0103] In Example 3, the authors showed that the completion of the first stage of carbonation of the sludge water at a pulp pH of 11.5 helps to reduce the precipitation of Al2O3 in the form of amorphous aluminum hydroxide, but entails an increased content of impurity elements in the sediment obtained after the second stage of carbonation, which leads to a deterioration in the quality of the final product.

[0104] In Example 4, the authors show that the end of the first stage of carbonization of the subslurry water at a pulp pH of 10 contributes to a significant increase in the formation of sediment after the first stage of carbonization, characterized by a heterogeneous phase composition, which negatively affects its quality and the possibility of using it as an additive to dry building mixtures. In addition, the yield of sediment after the second stage of carbonization, which is pseudoboehmite, decreases to 40% of the initial Al2O3 content in the subslurry water, which is economically inexpedient.

[0105] In Examples 5 and 6, the authors demonstrate the influence of the pH of the second stage carbonation pulp on the properties and yield of the final product.

[0106] In Example 5, the authors show that the completion of the second stage of carbonation of subslurry water at a pulp pH of 9.5 does not affect the impurity content, but contributes to a 15% reduction in the yield of the final product.

[0107] In Example 6, the authors found that the end of the second stage of carbonization of the sludge water at a pulp pH of 7 contributes to a significant increase in the duration of the process from 2 to 6 hours and the formation of impurity phases of gibbsite and bayerite in the final product, which negatively affects its quality. In Example 7, the authors showed that changing the temperature of the wash water (condensate) to 20 °C leads to an increase in the NaiO content in the sediment after the second stage of carbonization, which reduces the quality of the resulting product and makes it unsuitable for use as a precursor for most catalysts.

[0108] Increasing the temperature of the wash water above 90 °C is not advisable due to the high energy costs for heating and the presence of steam formation.

[0109] Taking into account the given description and examples, the scope of legal protection of the proposed invention is requested for a method for processing subsludge water from alumina production, including filtering the subsludge water, carbonizing it by saturating it with carbon dioxide, separating the resulting sediments, washing them with water and drying, in which the carbonization of the subsludge water is carried out in two stages. The first stage of carbonization is carried out to a pulp pH value at which a precipitate in the form of amorphous aluminum hydroxide precipitates from the solution, the resulting pulp is filtered to obtain a sediment, which is washed to obtain a product in the form of amorphous aluminum hydroxide suitable for use as a modifier for cement building mixtures, and a carbonate solution, which is sent to the second stage of carbonization to a pulp pH value at which the maximum amount of the target sediment precipitates.The obtained pulp is filtered, the sediment is washed to obtain a product in the form of pseudoboehmite suitable for use as a precursor in the production of alumina catalyst carriers. Carbonization of the subslurry water is preferably carried out by bubbling with gases containing carbon dioxide, wherein the gases containing carbon dioxide are exhaust gases from sintering furnaces of aluminum-containing raw materials with limestone and / or soda, and / or the gases containing carbon dioxide are gases from lime kilns, and / or the gases forming during combustion of power-generating coal or hydrocarbons are used as gases containing carbon dioxide. The first stage of carbonization is carried out until the pH value of the pulp is preferably 11-10.5. The obtained pulp after the first stage of carbonization of the subslurry water is filtered until the sediment on the filter is dried, the preferred moisture content of the sediment is 60-80 wt.%.The second stage of carbonization is carried out until the pH value of the pulp is preferably 9-8. After the second stage of carbonization, the sediment is washed at a wash water temperature of preferably 40-90°C.

[0110] The aluminum hydroxide of pseudoboehmite structure obtained by the proposed method contains at least 90 wt.% pseudoboehmite and is characterized by a high specific surface area and a low impurity content.

[0111] Table 1 Table 2

[0112] Table 3

Claims

CLAUSE OF THE INVENTION 1. A method for processing subsludge water from alumina production, including filtering the subsludge water, carbonizing it by saturating it with carbon dioxide, separating the resulting precipitates, washing them with water and drying, characterized in that the carbonization of the subsludge water is carried out in two stages, the first stage of carbonization is carried out until the pH of the pulp is reached, at which a precipitate in the form of amorphous aluminum hydroxide precipitates from the solution, the resulting pulp is filtered to obtain a precipitate, which is washed to obtain a product in the form of amorphous aluminum hydroxide suitable for use as a modifier for cement building mixtures, and a carbonate solution, which is sent to the second stage of carbonization until the pH of the pulp is reached, at which the maximum amount of the target precipitate precipitates, the resulting pulp is filtered, the precipitate is washed to obtain a product in the form of pseudoboehmite suitable for use as a precursor in the production of alumina catalyst carriers.

2. The method according to paragraph 1, characterized in that the carbonization of the subslurry water is carried out by bubbling gases containing carbon dioxide, wherein the gases containing carbon dioxide are waste gases from furnaces for sintering aluminum-containing raw materials with limestone and / or soda, and / or the gases containing carbon dioxide are gases from lime kilns, and / or the gases containing carbon dioxide are gases formed during the combustion of power-generating coal or hydrocarbons.

3. The method according to item 1, characterized in that the first stage of carbonization is carried out until the pH value of the pulp is preferably 11-10.

5.

4. The method according to item 1, characterized in that the pulp obtained after the first stage of carbonization of the subsludge water is filtered before drying. sediment on the filter, with the preferred moisture content of the sediment being 60-80 wt%.

5. The method according to item 1, characterized in that the second stage of carbonization is carried out until the pH value of the pulp is preferably 9-8.

6. The method according to item 1, characterized in that after the second stage of carbonization, the sediment is washed at a wash water temperature of preferably 40-90 °C.

Citation Information

Patent Citations

  • Pseudoboehmite and aluminium oxide prepared from same

    CN102219245B

  • Impurity removal method of red mud washing liquid and production method of pseudoboehmite

    CN107973327A

  • Boehmites and extremely pure pseudoboehmites, and process for their manufacture

    EP0085592A1

  • Method of processing aluminum-containing raw material

    RU2197429C2

  • Method of production of aluminum hydroxide of pseudo-boehmite structure and gamma aluminum oxide on its base

    RU2234460C1